Patterning method in preparation of solar cell, application of patterning method and solar cell

Through the combined method of local laser activation and wet thermal oxidation treatment, the negative impact of patterning technology on solar cell performance and complex process problems in the prior art are solved, and the process is simplified and mass production capacity is improved, which is suitable for industrial-scale production.

CN118919585APending Publication Date: 2024-11-08LAPLACE (WUXI) SEMICON TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410976863.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-19
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

The existing patterning technology is prone to negatively affecting performance in the preparation of high-efficiency crystalline silicon solar cells and the process is complicated, making it difficult to adapt to industrial mass production.

Method used

The local laser activation combined with wet thermal oxidation treatment is used to form the oxide layer thickness difference of the doped layer, and the retained mask layer is selectively etched to achieve patterning, thereby simplifying the process and reducing the requirements of the laser equipment and avoiding laser-induced damage.

Benefits of technology

It improves the performance of solar cells, reduces production difficulty, improves production yield and efficiency, and is suitable for industrial mass production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118919585A_ABST
    Figure CN118919585A_ABST
Patent Text Reader

Abstract

The invention provides a novel patterning method in solar cell preparation, and the method comprises the steps: carrying out the local laser activation of a first doping layer disposed on a silicon substrate, and enabling the first doping layer to form a first non-laser activation region and a first laser activation region with the doping concentration higher than that of the first non-laser activation region; wet thermal oxidation treatment is carried out on the first doping layer, so that an oxidation layer is formed on the side, away from the silicon substrate, of the first doping layer, the oxidation layer comprises a first oxidation region corresponding to the first laser active region and a second oxidation region corresponding to the first non-laser active region, and the thickness of the first oxidation region is larger than that of the second oxidation region; etching to remove the second oxidation region, thinning and reserving the first oxidation region as a mask layer; and carrying out alkali washing on the first doped layer to remove or thin the first non-laser active region so as to obtain a doped pattern region. The method is simple in process, is beneficial to improving the performance of the solar cell, and is suitable for industrial mass production. The invention also provides a solar cell and a preparation process thereof.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The embodiments of the present application relate to the technical field of photovoltaic solar cells, and in particular to a patterning method in the preparation of solar cells, a preparation process of solar cells using the patterning method in the preparation of solar cells, and a solar cell prepared using the preparation process of solar cells. Background Art

[0002] In the preparation of some high-efficiency crystalline silicon solar cells, such as BC (Back Contact) cells and TOPCon (Tunnel Oxide Passivated Contact) cells, it is necessary to use patterning technology to form controllable, localized doping areas to achieve excellent emitter and / or surface field effects. However, existing patterning methods are prone to negatively affect the performance of solar cells or have complex processes. Summary of the invention

[0003] In view of this, the present application provides a novel patterning method for solar cells, which has a simple process and is beneficial to improving the performance of solar cells and is suitable for industrial-scale mass production.

[0004] In addition, a process for preparing a solar cell using the graphic method in preparing the solar cell and a solar cell prepared using the process for preparing a solar cell are also provided, which are beneficial to ensuring the performance of the solar cell and reducing the production difficulty to improve the production yield and production efficiency, and are suitable for industrial-scale mass production.

[0005] In a first aspect, the present application provides a patterning method in the preparation of a solar cell, comprising: locally laser activating a first doping layer disposed on a silicon substrate so that the first doping layer forms a first laser activation region and a first non-laser activation region, wherein the doping concentration of the first laser activation region is higher than the doping concentration of the first non-laser activation region; performing wet thermal oxidation treatment on the first doping layer to form an oxide layer on a side of the first doping layer away from the silicon substrate, wherein the oxide layer comprises a first oxide region corresponding to the first laser activation region and a second oxide region corresponding to the first non-laser activation region, and the thickness of the first oxide region is greater than the thickness of the second oxide region; etching to remove the second oxide region while thinning and retaining the first oxide region as a mask layer; and alkali washing the first doping layer provided with the mask layer to remove or thin the first non-laser activation region to achieve patterning to obtain a doped pattern region.

[0006] In the above-mentioned patterning method for preparing solar cells, the thickness of the oxide layer corresponding to the first laser activation area and the first non-laser activation area is different by combining local laser activation with the differential growth of the oxide layer on the first laser activation area and the first non-laser activation area during wet thermal oxidation treatment, so that the oxide layer corresponding to the first laser activation area and the first non-laser activation area can be selectively retained as a mask layer during subsequent etching to achieve subsequent patterning. The above-mentioned patterning method does not require the use of high-pulse energy lasers, and while reducing the requirements for laser equipment, it is also beneficial to avoid laser-induced damage such as but not limited to microcracks, point defects, etc., thereby helping to reduce the negative impact on product performance. In addition, the above-mentioned patterning method is simple, stable and repeatable, which is easy to apply to mass production and is beneficial to ensuring production yield and efficiency.

[0007] In some possible implementations, the first doped layer is a phosphorus-doped crystalline silicon layer. Before laser activation, the doping concentration of the phosphorus-doped crystalline silicon layer is 5×10 18 cm -3 Up to 5×10 20 cm -3 , The phosphorus-doped crystalline silicon layer may be a phosphorus-doped single crystal silicon layer or a phosphorus-doped polycrystalline silicon layer.

[0008] In some possible embodiments, when the laser is activated, the wavelength of the laser is 300 nm to 1200 nm, and the pulse energy density of the laser is 0.1 J / cm 2 Up to 4J / cm 2 , the laser pulse width is 10ns to 250ns.

[0009] In some possible implementations, the doping concentration of the first laser active region is one order of magnitude or more higher than the doping concentration of the first laser inactive region.

[0010] In some possible implementations, the wet thermal oxidation treatment is performed in a water vapor atmosphere, and the temperature of the wet thermal oxidation treatment is 700° C. to 850° C., and the time of the wet thermal oxidation treatment is 20 min to 60 min.

[0011] In some possible implementations, the thickness of the first oxidized region is at least twice the thickness of the second oxidized region.

[0012] In some possible implementations, the thickness of the mask layer obtained after etching is not less than 20 nm.

[0013] The second aspect of the present application provides a process for preparing a solar cell, comprising: cleaning and texturing an N-type silicon substrate, the silicon substrate comprising a first side and a second side opposite to each other; sequentially depositing a first tunneling oxide layer and a first doping layer on the first side of the cleaned and texturized silicon substrate; patterning the first doping layer to remove or thin the first non-laser activated area based on the patterning method in the preparation of the solar cell as described above to obtain an N-type patterned area; sequentially depositing a second tunneling oxide layer and a second doping layer on the first side, wherein the second doping layer is formed by diffusing boron after depositing a second intrinsic amorphous silicon layer on the first side, or the second doping layer is formed by depositing an in-situ doped polycrystalline silicon layer on the first side; locally laser activating the second doping layer to form a second laser activated area, wherein the second laser activated area is spaced apart from the first laser activated area; alkaline washing the second doping layer to remove the portion of the second doping layer other than the second laser activated area, thereby obtaining a P-type patterned area; acid washing to remove the mask layer; depositing a passivation layer on the first side and the second side of the silicon substrate respectively; and preparing an electrode on the first side of the silicon substrate.

[0014] The third aspect of the present application provides a process for preparing a solar cell, comprising: cleaning and texturing an N-type silicon substrate, the silicon substrate comprising a first side and a second side opposite to each other; diffusing boron on the first side of the cleaned and texturized silicon substrate; etching and polishing the second side of the silicon substrate, and then sequentially depositing a first tunneling oxide layer and a first doping layer; patterning the first doping layer based on the patterning method in the preparation of the solar cell as described above to thin the first non-laser activated area; acid washing to remove the mask layer; depositing a passivation layer on the first side and the second side of the silicon substrate, respectively; and preparing electrodes on the first side and the second side of the silicon substrate, respectively.

[0015] In the above-mentioned solar cell preparation process, the oxide layer on the first laser activation area and the first non-laser activation area is grown differently by local laser activation combined with the wet thermal oxidation process, so that the oxide layer has different thicknesses corresponding to the first laser activation area and the first non-laser activation area, so that the oxide layer corresponding to the first laser activation area can be selectively retained as a mask layer during subsequent etching to achieve subsequent patterning. The above-mentioned patterning method does not require the use of high-pulse energy lasers, which reduces the requirements for laser equipment and is also conducive to avoiding laser-induced damage, such as but not limited to microcracks, point defects, etc., thereby helping to reduce the negative impact on the performance of solar cells. In addition, the above-mentioned solar cell preparation process is simple, stable and repeatable, which is easy to apply to the mass production of solar cells and is conducive to ensuring production yield and efficiency.

[0016] The fourth aspect of the present application provides a solar cell, wherein the solar cell is manufactured using the above-mentioned solar cell manufacturing process. The solar cell manufactured using the above-mentioned solar cell manufacturing process is conducive to realizing the structure of the solar cell and ensuring the performance of the solar cell. BRIEF DESCRIPTION OF THE DRAWINGS

[0017] Figure 1 A flowchart of a graphical method for preparing a solar cell provided in an embodiment of the present application.

[0018] Figures 2 to 6 A schematic cross-sectional view of a structure corresponding to a step in a graphic method for preparing a solar cell provided in an embodiment of the present application, and Figures 2 to 6 Only the structure on one side of the silicon substrate is shown.

[0019] Figure 7 A flow chart of a process for preparing a solar cell provided in an embodiment of the present application.

[0020] Figures 8 to 14 A schematic cross-sectional view of a structure corresponding to a step in a solar cell manufacturing process provided in an embodiment of the present application, and Figures 8 to 13 Only the structure on the first side of the silicon substrate is illustrated.

[0021] Fig.15 A flow chart of another process for preparing a solar cell provided in an embodiment of the present application.

[0022] Fig.16 A cross-sectional schematic diagram of a solar cell provided in an embodiment of the present application.

[0023] Main component symbols

[0024] 10. Silicon substrate; 20. First doped layer; 21. First laser active region; 23. First non-laser active region; 30. Oxide layer; 31. First oxide region; 33. Second oxide region; 31a. Mask layer; 10a. First side; 10b. Second side; 13. First tunnel oxide layer; 13a. Second tunnel oxide layer; 40a. Second doped layer; 41. Second laser active region; 50. Passivation layer; 60. Electrode; 17. Doped layer; 100A. Back contact solar cell; 100B. Tunnel oxide layer passivation contact cell.

[0025] The following specific implementation methods will further illustrate the present application in conjunction with the above-mentioned drawings. DETAILED DESCRIPTION

[0026] In order to further illustrate the technical means and effects adopted by the present application to achieve the intended application purpose, the following is combined with the drawings and implementation methods. Obviously, the described embodiments are only part of the embodiments of the present application, rather than all the embodiments.

[0027] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art to which this application belongs. The terms used herein in the specification of this application are only for the purpose of describing specific embodiments and are not intended to limit this application.

[0028] In the description of the embodiments of the present application, when an element is considered to be "connected" to another element, it may be directly connected to the other element or there may be a centrally disposed element at the same time. When an element is considered to be "disposed on" another element, it may be directly disposed on the other element or there may be a centrally disposed element at the same time. In the present application, unless otherwise clearly specified and limited, the terms "installed", "connected", "connected", "fixed" and the like should be understood in a broad sense, for example, it may be a fixed connection, a detachable connection, or an integral connection; it may be a mechanical connection or an electrical connection; it may be directly connected, or it may be indirectly connected through an intermediate medium, or it may be internal communication between the two elements. For those of ordinary skill in the art, the specific meanings of the above terms in the present application can be understood according to the specific circumstances.

[0029] In conjunction with the accompanying drawings, some embodiments of the present application are described in detail below. In the absence of conflict, the following embodiments and features in the embodiments can be combined with each other.

[0030] See also Figure 1 , an embodiment of the present application provides a method for patterning in the preparation of a solar cell, which comprises the following steps:

[0031] Step S11, please refer to Figure 2 , locally laser activates the first doping layer 20 disposed on the silicon substrate 10, so that the first doping layer 20 includes a first laser activation region 21 and a first non-laser activation region 23, wherein the doping concentration of the first laser activation region 21 is higher than the doping concentration of the first non-laser activation region 23.

[0032] The silicon substrate 10 may be an N-type silicon substrate. The first doped layer 20 may be a phosphorus-doped crystalline silicon layer. In this case, before laser activation, the doping concentration of the first doped layer 20 may be, but is not limited to, 5×10 18 cm -3 Up to 5×10 20 cm -3 , for example, 5×10 18 cm -3 , 8×10 18 cm -3 , 2×10 19 cm -3 , 5×10 19 cm-3 , 8×10 19 cm -3 , 3×10 20 cm -3 , 5×10 20 cm -3 Or any specific value between any two adjacent values ​​mentioned above, which is helpful to avoid high square resistance and large contact resistance in the metallized area caused by too low doping concentration, thereby helping to avoid reducing the performance parameters and conversion efficiency of the solar cell. It is also helpful to avoid excessive doping concentration that causes a large amount of impurity atoms to be doped into the silicon substrate, thereby causing Auger recombination, thereby helping to avoid the subsequent decrease in passivation quality and conversion efficiency.

[0033] The wavelength of the laser during the laser activation may be 300 nm to 1200 nm, for example, 300 nm, 355 nm, 365 nm, 405 nm, 515 nm, 532 nm, 540 nm, 660 nm, 1064 nm, 1080 nm, 1200 nm or any specific value between any two adjacent values ​​mentioned above; the pulse energy density of the laser may be 0.1 J / cm 2 Up to 4J / cm 2 , for example, 0.1 J / cm 2 , 0.5J / cm 2 , 1J / cm 2 , 1.5J / cm 2 , 2J / cm 2 , 2.5J / cm 2 , 3J / cm 2 , 3.5J / cm 2 , 4J / cm 2 or any specific value between any two adjacent values ​​mentioned above; the pulse width of the laser can be 10ns to 250ns, for example, 10ns, 30ns, 50ns, 70ns, 100ns, 130ns, 150ns, 180ns, 200ns, 230ns, 250ns or any specific value between any two adjacent values ​​mentioned above. The spot of the laser can be, for example, but not limited to, a square flat-top spot. The above laser parameters are conducive to reducing laser-induced damage while achieving the activation effect, thereby helping to ensure the performance of subsequent solar cells.

[0034] Furthermore, the doping concentration of the first laser activated region 21 may be one order of magnitude or more higher than the doping concentration of the first non-laser activated region 23, which is beneficial to achieving enhanced oxidation characteristics of the first laser activated region 21 compared to the first non-laser activated region 23, that is, it is beneficial to ensure the thickness difference between the portion of the subsequent oxidation layer corresponding to the first laser activated region 21 and the portion corresponding to the first non-laser activated region 23.

[0035] Step S12, please refer to Figure 2 and Figure 3 The first doped layer 20 is subjected to a wet thermal oxidation treatment to form an oxide layer 30 on a side of the first doped layer 20 away from the silicon substrate 10, wherein the oxide layer 30 includes a first oxide region 31 corresponding to the first laser activated region 21 and a second oxide region 33 corresponding to the first non-laser activated region 23, and the thickness of the first oxide region 31 is greater than the thickness of the second oxide region 33.

[0036] The wet thermal oxidation treatment may be carried out in a water vapor atmosphere. In some embodiments, the temperature of the wet thermal oxidation treatment may be 700°C to 850°C, for example, 700°C, 730°C, 750°C, 770°C, 800°C, 820°C, 850°C, or any specific value between any two adjacent values ​​mentioned above; the time of the wet thermal oxidation treatment may be 20min to 60min, for example, 20min, 30min, 40min, 50min, 60min, or any specific value between any two adjacent values ​​mentioned above. The above parameters of the wet thermal oxidation treatment are conducive to ensuring the growth rate of the oxide layer, thereby facilitating the industrial mass production of solar cells.

[0037] In some embodiments, the thickness of the first oxide region 31 may be at least twice the thickness of the second oxide region 33, which is beneficial for the oxide layer 30 to be retained to form a mask layer corresponding to the first laser active region 21 after subsequent etching. Specifically, in some embodiments, the thickness of the first oxide region 31 may be not less than 100 nm.

[0038] Step S13, please refer to Figure 3 and Figure 4 , etching to remove the second oxide region 33 while thinning and retaining the first oxide region 31 as a mask layer 31a.

[0039] In some embodiments, the thickness of the mask layer 31 a may be no less than 20 nm.

[0040] The above etching may be performed using a hydrofluoric acid solution as a cleaning solution, wherein the concentration of the hydrofluoric acid solution may be, but is not limited to, 1 vol% to 10 vol%, such as 2 vol%.

[0041] Step S13, please refer to Figure 4 , Figure 5 and Figure 6 The first doping layer 20 provided with the mask layer 31a is alkali washed to remove or thin the first non-laser activated area 23 to achieve patterning to obtain a doped pattern area.

[0042] like Figure 5 As shown, after removing the first non-laser activated area 23, the first laser activated area 21 is retained as the doped pattern area. Figure 6 As shown, after the first non-laser activated region 23 is thinned, the first laser activated region 21 and the thinned first non-laser activated region 23 are used together as a doped pattern region, wherein the doped pattern region can be an N-type pattern region or a P-type pattern region.

[0043] The above-mentioned alkaline washing can be achieved, for example, by using, but not limited to, an alkaline washing solution of an inorganic base or an organic base.

[0044] In the above-mentioned patterning method for preparing solar cells, the differential growth of the oxide layer 30 on the first laser activation area 21 and the first non-laser activation area 23 during wet thermal oxidation treatment is combined by local laser activation, so that the thickness of the oxide layer 30 corresponding to the first laser activation area 21 and the first non-laser activation area 23 is different, so that in the subsequent etching, the oxide layer corresponding to the first laser activation area 21 can be selectively retained as a mask layer 31a to achieve subsequent patterning. The above-mentioned patterning method does not require the use of high-pulse energy lasers, and while reducing the requirements for laser equipment, it is also beneficial to avoid laser-induced damage, such as but not limited to microcracks, point defects, etc., thereby helping to reduce the negative impact on product performance, and the above-mentioned patterning method is simple, stable and repeatable, which is easy to apply to mass production and is conducive to ensuring production yield and efficiency.

[0045] See also Figure 7 One embodiment of the present application also provides a process for preparing a solar cell, which is a process for preparing a back-contact solar cell. The process comprises the following steps:

[0046] Step S20, please refer to Figure 8 , the N-type silicon substrate 10 is cleaned and textured, and the silicon substrate 10 includes a first side 10a and a second side 10b opposite to each other.

[0047] Step S21, please refer to Figure 8 , a first tunneling oxide layer 13 and a first doping layer 20 are sequentially deposited on the first side 10a of the cleaned and textured silicon substrate 10 .

[0048] In some embodiments, see Figure 8 , the formation method of the first doping layer 20 may include but is not limited to:

[0049] In the first step, a first intrinsic amorphous silicon layer (not shown) is formed on the first tunnel oxide layer 13 .

[0050] In the second step, phosphorus is diffused into the first intrinsic amorphous silicon layer to form the above-mentioned first doping layer 20 and PSG (phosphosilicate glass, not shown).

[0051] The third step is pickling to remove PSG.

[0052] In some embodiments, the first tunnel oxide layer 13 and the first intrinsic amorphous silicon layer may be formed by, but not limited to, low pressure chemical vapor deposition (LPCVD). In some embodiments, the first tunnel oxide layer 13 may also be formed by other methods such as wet chemical methods.

[0053] Among them, the thickness of the first tunneling oxide layer 13 can be 1nm to 2nm, for example, it can be 1nm, 1.2nm, 1.4nm, 1.6nm, 1.8nm, 2nm or any specific value between any two adjacent values ​​mentioned above; the thickness of the first intrinsic amorphous silicon layer 15 can be 100nm to 200nm, for example, it can be 100nm, 120nm, 150nm, 170nm, 190nm, 200nm or any specific value between any two adjacent values ​​mentioned above.

[0054] In some embodiments, the first doping layer 20 may be formed by diffusing a phosphorus source using, but not limited to, a low-pressure tubular diffusion furnace, wherein the phosphorus source may be, but not limited to, phosphorus oxychloride (POCl 3 ).

[0055] Step S22, please refer to Fig. 9 , Figures 1 to 5 and Fig.10 The first doping layer 20 is patterned by the above-mentioned patterning method in the preparation of the solar cell to remove the first non-laser activated area 23.

[0056] It can be understood that, in some embodiments, the area of ​​the first tunnel oxide layer 13 not covered by the first laser active region 21 may also be removed.

[0057] Step S23, please refer to Fig.10 , a second tunneling oxide layer 13a and a second intrinsic amorphous silicon layer (not shown) are sequentially deposited on the first side 10a, wherein the second intrinsic amorphous silicon layer also covers the mask layer 31a. It can be understood that the second tunneling oxide layer 13a and the second doped layer are sequentially deposited on the first side 10a, wherein the second doped layer is formed by diffusing boron after depositing the second intrinsic amorphous silicon layer on the first side, or the second doped layer is formed by depositing an in-situ doped polysilicon layer on the first side, and the deposition of the in-situ doped polysilicon layer can be understood as the simultaneous deposition of polysilicon and impurity atoms. This embodiment is exemplified by forming the second doped layer by diffusing boron after depositing the second intrinsic amorphous silicon layer on the first side.

[0058] In some embodiments, the second intrinsic amorphous silicon layer may be formed by, but is not limited to, low pressure chemical vapor deposition (LPCVD).

[0059] The thickness of the second intrinsic amorphous silicon layer may be 100 nm to 200 nm, for example, 100 nm, 120 nm, 150 nm, 170 nm, 190 nm, 200 nm or any specific value between any two adjacent values ​​mentioned above.

[0060] Step S24, please refer to Fig.10 , boron is diffused into the second intrinsic amorphous silicon layer to form a second doping layer 40a.

[0061] In some embodiments, the boron source may be, but is not limited to, a boron source for boron diffusion including at least one of boron trichloride and boron tribromide (BBr 3 ).

[0062] Specifically, when boron is diffused, BSG (borosilicate glass) is formed on the surface of the second doping layer 40a, and before the subsequent steps, BSG can be removed by, but not limited to, etching. Among them, BSG can be removed by, but not limited to, cleaning with a hydrofluoric acid solution.

[0063] Step S25, please refer to Fig.10 and Fig.11 The second doping layer 40a is locally laser activated to make the local boron-doped polysilicon oversaturated to form a second laser activation area 41, wherein the second laser activation area 41 is spaced apart from the N-type graphic area, namely the first laser activation area 21.

[0064] In some embodiments, the doping concentration of the second laser active region 41 may be no less than 5×10 20 cm -3 .

[0065] In this embodiment, the wavelength of the laser for local laser activation of the second doping layer 40a may be 300nm to 1200nm, for example, 300nm, 355nm, 365nm, 405nm, 515nm, 532nm, 540nm, 660nm, 1064nm, 1080nm, 1200nm or any specific value between any two adjacent values ​​of the foregoing; the pulse energy density of the laser may be 0.1J / cm 2 Up to 4J / cm 2 , for example, 0.1 J / cm 2 , 0.5J / cm 2 , 1J / cm 2 , 1.5J / cm 2 , 2J / cm 2 , 2.5J / cm 2 , 3J / cm 2 , 3.5J / cm 2 , 4J / cm 2or any specific value between any two adjacent values ​​mentioned above; the pulse width of the laser may be 10ns to 250ns, for example, 10ns, 30ns, 50ns, 70ns, 100ns, 130ns, 150ns, 180ns, 200ns, 230ns, 250ns or any specific value between any two adjacent values ​​mentioned above. The spot of the laser may be, for example, but not limited to, a square flat-top spot. The specific parameters for selecting the local laser activation of the second doped layer 40a may be the same as or different from the specific parameters for selecting the local laser activation of the first doped layer 20.

[0066] Step S26, please refer to Fig.11 and Fig.12 , the second doping layer 40a is alkali washed to remove the portion of the second doping layer 40a except the second laser activation region 41, thereby obtaining a P-type graphic region, namely, the second laser activation region 41.

[0067] Step S27, see Fig.12 and Fig.13 , and remove the mask layer 31a by pickling.

[0068] Step S28, see Fig.14 , a passivation layer 50 is deposited on the first side 10 a and the second side 10 b of the silicon substrate 10 , respectively, and then an electrode 60 is prepared on the first side 10 a of the silicon substrate 10 .

[0069] The passivation layer 50 may be, but is not limited to, an aluminum oxide and / or silicon nitride layer, which may be formed by, but is not limited to, ALD atomic deposition equipment coating and plasma enhanced chemical vapor deposition (PECVD).

[0070] The electrode 60 can be manufactured by, but is not limited to, screen printing followed by sintering. In the present application, the specific manufacturing method of the electrode 60 is not limited.

[0071] Correspondingly, such as Fig.14 As shown, one embodiment of the present application further provides a back-contact solar cell 100A manufactured by the above-mentioned solar cell manufacturing process.

[0072] See also Fig.15 and Fig.16 One embodiment of the present application also provides a process for preparing a solar cell, which is a process for preparing a tunnel oxide layer passivation contact cell, and the preparation process includes the following steps:

[0073] Step S40, as in the above step S20, the N-type silicon substrate 10 is cleaned and textured, and the silicon substrate 10 includes a first side 10a and a second side 10b opposite to each other.

[0074] Step S41 , performing boron diffusion on the first side 10 a of the cleaned and textured silicon substrate 10 to form a doping layer 17 .

[0075] In some embodiments, the boron source may be, but is not limited to, a boron source for boron diffusion including at least one of boron trichloride and boron tribromide (BBr 3 ).

[0076] Specifically, when boron is diffused, a BSG layer (borosilicate glass) is formed on the surface of the doping layer 17 .

[0077] Step S42 , after etching and polishing the second side 10 b of the silicon substrate 10 , a first tunneling oxide layer and a first doping layer are sequentially deposited as in the above step S21 .

[0078] Step S43, patterning the first doping layer by the patterning method in the above solar cell preparation to thin the first non-laser active region 23 and reduce parasitic absorption.

[0079] Step S44, as in the above step S28, the mask layer is removed by pickling.

[0080] In step S45 , a passivation layer 50 is deposited on the first side 10 a and the second side 10 b of the silicon substrate 10 , respectively, and then electrodes 60 are prepared on the first side 10 a and the second side 10 b of the silicon substrate 10 , respectively.

[0081] Correspondingly, such as Fig.16 As shown, an embodiment of the present application further provides a tunneling oxide layer passivation contact cell 100B manufactured by the above-mentioned solar cell manufacturing process.

[0082] In the above-mentioned solar cell preparation process, the oxide layer on the first laser activation area and the first non-laser activation area is grown differently by local laser activation combined with the wet thermal oxidation process, so that the oxide layer has different thicknesses corresponding to the first laser activation area and the first non-laser activation area, so that the oxide layer corresponding to the first laser activation area can be selectively retained as a mask layer during subsequent etching to achieve subsequent patterning. The above-mentioned patterning method does not require the use of high-pulse energy lasers, and while reducing the requirements for laser equipment, it is also beneficial to avoid laser-induced damage such as but not limited to microcracks, point defects, etc., thereby helping to reduce the negative impact on the performance of solar cells. In addition, the above-mentioned solar cell preparation process is simple, stable and repeatable, which is easy to apply to the mass production of solar cells and is beneficial to ensuring production yield and efficiency.

[0083] The solar cell produced by the above-mentioned solar cell preparation process is beneficial to ensuring the performance of the solar cell.

[0084] In addition, those skilled in the art should recognize that the above embodiments are only used to illustrate the present application and are not intended to limit the present application. As long as they are within the spirit of the present application, appropriate changes and modifications to the above embodiments are within the scope of the present application.

Claims

1. A method for patterning in the preparation of solar cells, characterized in that: include: Locally laser activating a first doped layer disposed on a silicon substrate so that the first doped layer forms a first laser activated region and a first non-laser activated region, wherein the doping concentration of the first laser activated region is higher than the doping concentration of the first non-laser activated region; Performing a wet thermal oxidation treatment on the first doped layer to form an oxide layer on a side of the first doped layer facing away from the silicon substrate, wherein the oxide layer includes a first oxide region corresponding to the first laser active region and a second oxide region corresponding to the first non-laser active region, and a thickness of the first oxide region is greater than a thickness of the second oxide region; Etching to remove the second oxide region while thinning and retaining the first oxide region as a mask layer; and The first doping layer provided with the mask layer is subjected to alkali washing to remove or thin the first non-laser activated area to achieve patterning to obtain a doping pattern area.

2. The method for patterning in preparing a solar cell according to claim 1, characterized in that: The first doped layer is a phosphorus-doped crystalline silicon layer. Before the laser activation, the doping concentration of the phosphorus-doped crystalline silicon layer is 5×10 18 cm -3 Up to 5×10 20 cm -3 .

3. The method for patterning in preparing a solar cell according to claim 1 or 2, characterized in that: When the laser is activated, the wavelength of the laser is 300nm to 1200nm, and the pulse energy density of the laser is 0.1J / cm 2 Up to 4J / cm 2 , the pulse width of the laser is 10ns to 250ns.

4. The method for patterning in preparing a solar cell according to claim 1, characterized in that: The doping concentration of the first laser active region is one order of magnitude or more higher than the doping concentration of the first laser inactive region.

5. The method for patterning in preparing a solar cell according to claim 1, characterized in that: The wet thermal oxidation treatment is performed in a water vapor atmosphere, and the temperature of the wet thermal oxidation treatment is 700° C. to 850° C., and the time of the wet thermal oxidation treatment is 20 min to 60 min.

6. The method for patterning in preparing a solar cell according to claim 1, characterized in that: The thickness of the first oxidized region is at least twice the thickness of the second oxidized region.

7. The method for patterning in preparing a solar cell according to claim 1, characterized in that: The thickness of the mask layer obtained after the etching is not less than 20 nm.

8. A process for preparing a solar cell, characterized in that: include: Cleaning and texturing an N-type silicon substrate, wherein the silicon substrate comprises a first side and a second side opposite to each other; Sequentially forming a first tunneling oxide layer and a first doping layer on the first side of the cleaned and textured silicon substrate; Based on the patterning method in the preparation of a solar cell according to any one of claims 1 to 7, patterning the first doping layer to remove or thin the first non-laser activated area to obtain an N-type patterned area; Depositing a second tunneling oxide layer and a second doped layer on the first side in sequence, wherein the second doped layer is formed by depositing a second intrinsic amorphous silicon layer on the first side and then performing boron diffusion, or the second doped layer is formed by depositing an in-situ doped polysilicon layer on the first side; Performing local laser activation on the second doping layer to form a second laser activation region, wherein the second laser activation region is spaced apart from the first laser activation region; Performing alkali washing on the second doped layer to remove the portion of the second doped layer except the second laser activated region, thereby obtaining a P-type pattern region; Pickling to remove the mask layer; depositing a passivation layer on the first side and the second side of the silicon substrate respectively; and An electrode is fabricated on the first side of the silicon substrate.

9. A process for preparing a solar cell, characterized in that: include: Cleaning and texturing an N-type silicon substrate, wherein the silicon substrate comprises a first side and a second side opposite to each other; Performing boron diffusion on the first side of the cleaned and textured silicon substrate; After etching and polishing the second side of the silicon substrate, a first tunneling oxide layer and a first doping layer are sequentially deposited; Patterning the first doping layer to thin the first non-laser active area based on the patterning method in the preparation of a solar cell according to any one of claims 1 to 7; Pickling to remove the mask layer; Depositing a passivation layer on the first side and the second side of the silicon substrate respectively; as well as Electrodes are respectively prepared on the first side and the second side of the silicon substrate.