Negative pole piece and lithium ion battery
By combining uncoated graphite primary particles, carbon-coated graphite primary particles, and secondary particles, the negative electrode of lithium-ion batteries is optimized, solving the problems of poor charging rate and high-temperature storage recovery performance of graphite materials, and achieving good high-temperature storage recovery capacity and charging rate.
Patent Information
- Application Number
- CN202410950107.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-16
- Publication Date
- 2024-11-08
AI Technical Summary
The existing graphite materials used as negative electrodes in lithium-ion batteries suffer from low charging rate performance and poor high-temperature storage recovery performance.
A negative electrode sheet was prepared by combining uncoated primary graphite particles, carbon-coated primary graphite particles, and carbon-coated secondary graphite particles. The lithium-ion migration channel was optimized by controlling the appropriate particle size and specific surface area.
This achieves good storage capacity recovery rate and good charging rate performance of the negative electrode material at high temperatures, thus improving the overall performance of the battery.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of lithium batteries, and in particular to a negative electrode sheet and a lithium ion battery. Background Art
[0002] With the development and progress of science and technology, lithium-ion batteries are increasingly used in power, energy storage, 3C and other fields, and the market has higher and higher requirements for the energy density of lithium-ion batteries. Battery negative electrode materials are an important component of secondary batteries and have a great impact on the battery's charging characteristics, battery capacity and battery life.
[0003] Among them, graphite material is the most widely used negative electrode material in the current lithium-ion battery market because of its advantages such as high theoretical specific capacity, low working potential and good structural stability. However, graphite material also has the disadvantages of low charging rate performance and poor high-temperature storage recovery performance. Summary of the invention
[0004] In order to solve the above technical problems, the present invention discloses a negative electrode sheet and a lithium-ion battery. The technical solution of the present invention is implemented as follows:
[0005] The first aspect of the present invention is to provide a negative electrode plate, the negative electrode plate comprising a current collector and a negative electrode active material, the negative electrode active material is a graphite material;
[0006] The graphite material includes primary particles D1, primary particles C1 and secondary particles C2;
[0007] The primary particles D1 are graphite particles not coated with carbon, and the primary particles C1 and the secondary particles C2 are graphite particles coated with carbon.
[0008] Preferably, the primary particles D1, primary particles C1 and secondary particles C2 are made of the same graphite material, wherein the graphite material includes natural graphite and artificial graphite.
[0009] Preferably, the primary particles D1, primary particles C1 and secondary particles C2 are different types of graphite materials, wherein the rate performance of the graphite materials is ranked as C2>C1>D1, and the high temperature storage performance of the graphite materials is ranked as D1>C1>C2.
[0010] Preferably, the particle size D50 of the graphite material is 11 μm-13 μm, and the BET specific surface area of the graphite material is 0.8 m 2 / g-1.2m 2 / g.
[0011] Preferably, the mass fraction of the primary particles D1 in the graphite material is 5%-15%; the mass fraction of the primary particles C1 in the graphite material is 20%-30%; and the mass fraction of the secondary particles C2 in the graphite material is 60%-70%.
[0012] Carbon-coated graphite secondary particles are obtained by taking graphite primary particles as raw materials and subjecting them to secondary granulation and then carbon coating. This type of graphite material contains a large amount of carbon-coated graphite secondary particles, which can effectively shorten the path of lithium ion migration channels. Compared with carbon-coated primary graphite particles, it can further improve the rate performance of the battery.
[0013] In the present invention, the uncoated carbon graphite primary particles D1 provide good high temperature storage performance and dynamic performance, the carbon coated graphite primary particles C1 provide good rate performance, and the carbon coated graphite secondary particles C2 further provide good rate performance.
[0014] Preferably, the mass fraction of the primary particles D1 in the graphite material is 10%.
[0015] Preferably, the carbon coating amount of the primary particles C1 is 4wt%-6wt%, and the carbon coating amount of the secondary particles C2 is 4wt%-8wt%.
[0016] Preferably, the thickness of the carbon coating layer of the primary particle C1 is 8 nm-20 nm, and the thickness of the carbon coating layer of the secondary particle C2 is 6 nm-20 nm.
[0017] The second aspect of the present invention is to provide a lithium-ion battery, wherein the lithium-ion battery uses the negative electrode plate provided in the first aspect of the present invention.
[0018] By simultaneously using uncoated carbon graphite particles with good high temperature stability and graphite particles with good rate performance to prepare the negative electrode plate, the lithium ion battery of the present invention has good high temperature storage recovery capacity recovery rate and good charging rate.
[0019] Advantages of the present invention:
[0020] The present invention adopts a compounding method of uncoated carbon primary graphite particles, carbon-coated graphite primary particles and carbon-coated secondary graphite particles. The prepared negative electrode material has the characteristics of good high-temperature storage recovery performance of uncoated graphite particles, and at the same time has the advantages of good charging rate of carbon-coated primary graphite particles and carbon-coated secondary graphite particles. DETAILED DESCRIPTION
[0021] The technical solution of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0022] Unless otherwise defined, all technical and scientific terms used in the present invention have the same meanings as those commonly understood by technicians in the technical field to which the present invention belongs; the terms used in the specific implementation methods are only for the purpose of describing specific embodiments and are not intended to limit the present invention; the terms "including" and "having" in the description and claims of the present invention and any variations thereof are intended to cover non-exclusive inclusions.
[0023] In the description of the specific implementation methods of the present invention, the technical terms "first", "second", etc. are only used to distinguish different objects, and cannot be understood as indicating or implying relative importance or implicitly indicating the number, specific order or primary and secondary relationship of the indicated technical features. In the description of the embodiments of the present invention, the meaning of "multiple" is more than two, unless otherwise clearly and specifically defined.
[0024] Reference to "embodiments" in the present invention means that a particular feature, structure, or characteristic described in conjunction with the embodiments may be included in at least one embodiment of the present invention. The appearance of the phrase in various places in the specification does not necessarily refer to the same embodiment, nor is it an independent or alternative embodiment that is mutually exclusive with other embodiments. It is explicitly and implicitly understood by those skilled in the art that the embodiments described in the present invention may be combined with other embodiments.
[0025] In the description of the embodiments of the present invention, the term "and / or" is only a description of the association relationship of associated objects, indicating that three relationships may exist. For example, A and / or B can represent: A exists alone, A and B exist at the same time, and B exists alone. In addition, the character " / " in the present invention generally indicates that the associated objects before and after are in an "or" relationship.
[0026] Throughout the present invention, numerical values represent approximate measures or limits of ranges to cover minor deviations from given values as well as embodiments with about the values mentioned and embodiments with the exact values mentioned. Except for the working examples provided at the end of the detailed description, all numerical values of parameters (e.g., amounts or conditions) in this specification (including the appended claims) should be understood to be modified by the term "about" in all cases, regardless of whether "about" actually appears before the numerical value. "About" indicates that the stated numerical value allows some minor imprecision (close to the exact value of the value to some extent; approximately or reasonably close to the value; almost). If the imprecision provided by "about" is not otherwise understood in this ordinary sense in the art, "about" as used in the present invention at least indicates the variation that can be produced by the ordinary methods of measuring and using such parameters. For example, "about" may include a variation of less than or equal to 5%, optionally less than or equal to 4%, optionally less than or equal to 3%, optionally less than or equal to 2%, optionally less than or equal to 1%, optionally less than or equal to 0.5%, and in some aspects, optionally less than or equal to 0.1%.
[0027] Additionally, disclosure of ranges includes disclosure of all values within the entire range and further divided ranges, including endpoints and sub-ranges given for such ranges.
[0028] The first aspect of the present invention is to provide a negative electrode plate, the negative electrode plate comprising a current collector and a negative electrode active material, the negative electrode active material is a graphite material;
[0029] The graphite material includes primary particles D1, primary particles C1 and secondary particles C2;
[0030] The primary particles D1 are graphite particles not coated with carbon, and the primary particles C1 and the secondary particles C2 are graphite particles coated with carbon.
[0031] Graphite particles without carbon coating have good high temperature stability. Carbon coating of graphite can effectively improve the rate performance of graphite. However, after carbon coating, there will be residual carbon on the surface of graphite. These residual carbon will react with electrolyte to generate gas under high temperature, affecting the high temperature storage capacity recovery rate of the battery. In the present invention, the primary particles of graphite without carbon coating, the primary particles of carbon coating and the secondary particles of carbon coating are compounded to make the negative electrode material have both good high temperature storage capacity recovery rate and good charging rate. The primary particles have good kinetic performance, and the secondary particles have good low temperature cycle performance.
[0032] In some embodiments, the particle size D50 of the graphite material is 11 μm-13 μm, and the BET specific surface area of the graphite material is 0.8 m 2 / g-1.2m 2 / g. In specific applications, the particle size of the graphite material can be 11 μm, 12 μm, or 13 μm; the BET specific surface area of the graphite material can be 0.8 m 2 / g, 0.9m 2 / g, 1.0m 2 / g, 1.1m 2 / g, 1.2m 2 The above values are only examples and are not limiting.
[0033] When the specific surface area of graphite material is too small, it is not conducive to the deintercalation of lithium ions, which will affect the rate performance of the secondary battery; when the specific surface area of graphite material is too large, it is easy to have side reactions with the electrolyte, which will affect the service life of the secondary battery. The present invention controls the particle size of the constituent graphite particles to make the three graphite particles densely stacked, thereby increasing the compaction density of the negative electrode active material and thus improving the energy density of the battery. The present invention controls the specific surface area to mix the three graphite particles, complement each other's advantages, and thus balance the high temperature storage performance and charging rate of the battery.
[0034] In some embodiments, the mass fraction of the primary particles D1 in the graphite material is 5%-15%; the mass fraction of the primary particles C1 in the graphite material is 20%-30%; and the mass fraction of the secondary particles C2 in the graphite material is 60%-70%. In specific applications, the mass fraction of the primary particles D1 can be 5%, 6%, 7%, 8%, 9%, 10%, 11%, 12%, 13%, 14% or 15%, etc.; the mass fraction of the primary particles C1 can be 20%, 21%, 22%, 23%, 24%, 25%, 26%, 27%, 28%, 29% or 30%, etc.; the mass fraction of the secondary particles C2 can be 60%, 61%, 62%, 63%, 64%, 65%, 66%, 67%, 68%, 69% or 70%, etc. The above values are only examples and are not limited.
[0035] Carbon-coated graphite secondary particles are obtained by carbon coating after secondary granulation of graphite primary particles as raw materials. This graphite material contains more carbon-coated graphite secondary particles, which can effectively shorten the path of lithium ion migration channel and further improve the rate performance of the battery compared with carbon-coated primary graphite particles. In this application, three kinds of particles are mixed as negative electrode materials, and carbon-coated secondary particles are the main components in the negative electrode material, so that the high temperature storage recovery rate of the negative electrode material can be taken into account while ensuring the charging rate.
[0036] In the present invention, the uncoated carbon graphite primary particles D1 provide good high temperature storage performance and dynamic performance, the carbon coated graphite primary particles C1 provide good rate performance, and the carbon coated graphite secondary particles C2 further provide good rate performance.
[0037] In some preferred embodiments, the primary particles D1, primary particles C1 and secondary particles C2 are made of the same graphite material, wherein the graphite material includes natural graphite and artificial graphite.
[0038] In some preferred embodiments, the primary particles D1, primary particles C1 and secondary particles C2 are different types of graphite materials, wherein the rate performance of the graphite materials is ranked as C2>C1>D1, and the high temperature storage performance of the graphite materials is ranked as D1>C1>C2.
[0039] In some preferred embodiments, the mass fraction of the primary particles D1 in the graphite material is 10%.
[0040] In some embodiments, the carbon coating amount of the primary particles C1 is 4wt%-6wt%, and the carbon coating amount of the secondary particles C2 is 4wt%-8wt%. In specific applications, the carbon coating amount of the primary particles C1 can be selected as 4wt%, 5wt%, 6wt%; the carbon coating amount of the secondary particles C2 can be selected as 4wt%, 5wt%, 6wt%, 7wt%, 8wt%. The above values are only examples and are not limited.
[0041] If the carbon coating amount is too low, the rate performance of the battery will deteriorate, while if the carbon coating amount is too high, side reactions will increase during use, causing the high-temperature storage recovery performance of the battery to deteriorate. Therefore, the present invention can better improve the overall performance of the battery by controlling the carbon coating amount.
[0042] In some embodiments, the thickness of the carbon coating layer of the primary particle C1 is 8nm-20nm, and the thickness of the carbon coating layer of the secondary particle C2 is 6nm-20nm. In specific applications, the thickness of the carbon coating layer of the primary particle C1 can be 8nm, 9nm, 10nm, 11nm, 12nm, 13nm, 14nm, 15nm, 16nm, 17nm, 18nm, 19nm, 20nm; the thickness of the carbon coating layer of the secondary particle C2 can be 6nm, 7nm, 8nm, 9nm, 10nm, 11nm, 12nm, 13nm, 14nm, 15nm, 16nm, 17nm, 18nm, 19nm, 20nm. The above values are only examples and are not limited.
[0043] In the present invention, the thickness of the carbon coating layer of the primary particle C1 and the secondary particle C2 is within this range, so that the graphite material has better processing performance and better lithium ion transmission rate, and can better improve the overall performance of the battery.
[0044] The second aspect of the present invention is to provide a lithium-ion battery, wherein the lithium-ion battery uses the negative electrode plate provided in the first aspect of the present invention.
[0045] By simultaneously using uncoated carbon graphite particles with good high temperature stability and graphite particles with good rate performance to prepare the negative electrode plate, the lithium ion battery of the present invention has good high temperature storage recovery capacity recovery rate and good charging rate.
[0046] The embodiments of the present invention will be described in more detail below through examples and comparative examples. It should be noted that the embodiments of the present invention are not limited to these examples.
[0047] Example 1
[0048] A lithium-ion battery comprises a negative electrode sheet, a positive electrode sheet and an electrolyte. The steps for preparing the lithium-ion battery are as follows:
[0049] 1. Preparation of negative electrode sheet
[0050] A negative electrode active material was obtained by mixing 10% by mass of carbon-uncoated graphite primary particles D1, 20% by mass of carbon-coated graphite primary particles C1, and 70% by mass of carbon-coated graphite secondary particles C2.
[0051] The preparation method of carbon-coated graphite secondary particles is to mix graphite primary particles and perform secondary granulation to obtain graphite secondary particles, and then carbon-coat the graphite secondary particles to obtain carbon-coated graphite secondary particles. The carbon coating method is not limited here.
[0052] The negative electrode active material, conductive agent (Super P), binder (styrene-butadiene rubber emulsion) and thickener (CMC-Na) prepared above were fully stirred and mixed in an appropriate amount of deionized water at a mass ratio of 96.2:0.8:1.8:1.2 to form a uniform negative electrode slurry; the negative electrode slurry was coated on the surface of the negative electrode current collector copper foil, and after drying and cold pressing, a negative electrode sheet was obtained.
[0053] 2. Preparation of positive electrode sheet
[0054] The positive electrode active material LiNi 0.5 Co 0.2 Mn 0.3O2 (NCM523), conductive agent (Super P) and binder PVDF are fully stirred and mixed in a proper amount of NMP at a weight ratio of 96.2:2.7:1.1 to form a uniform positive electrode slurry; the positive electrode slurry is coated on the surface of the positive electrode current collector aluminum foil, and after drying and cold pressing, a positive electrode sheet is obtained.
[0055] 3. Preparation of electrolyte
[0056] Ethylene carbonate (EC), ethyl methyl carbonate (EMC) and diethyl carbonate (DEC) are mixed in a volume ratio of 1:1:1, and then LiPF6 is uniformly dissolved in the above solution to obtain an electrolyte, wherein the concentration of LiPF6 is 1 mol / L.
[0057] 4. Preparation of batteries
[0058] The positive electrode sheet and negative electrode sheet prepared above are stacked in order with the separator so that the separator is between the positive and negative electrode sheets, and then wound to obtain a bare cell. The bare cell is placed in an outer packaging shell, and after drying, an electrolyte is injected. After vacuum packaging, standing, forming, shaping and other processes, a lithium-ion battery is obtained.
[0059] Example 2
[0060] A lithium-ion battery comprises a negative electrode sheet, a positive electrode sheet and an electrolyte. The steps for preparing the lithium-ion battery are as follows:
[0061] 1. Preparation of negative electrode sheet
[0062] A negative electrode active material was obtained by mixing 10% by mass of carbon-uncoated graphite primary particles D1, 30% by mass of carbon-coated graphite primary particles C1, and 60% by mass of carbon-coated graphite secondary particles C2.
[0063] The preparation method of the carbon-coated graphite secondary particles is as follows: mixing the graphite primary particles and performing secondary granulation to obtain graphite secondary particles, and then carbon-coating the graphite secondary particles to obtain carbon-coated graphite secondary particles.
[0064] The negative electrode active material, conductive agent (Super P), binder (styrene-butadiene rubber emulsion) and thickener (CMC-Na) prepared above were fully stirred and mixed in an appropriate amount of deionized water at a mass ratio of 96.2:0.8:1.8:1.2 to form a uniform negative electrode slurry; the negative electrode slurry was coated on the surface of the negative electrode current collector copper foil, and after drying and cold pressing, a negative electrode sheet was obtained.
[0065] 2. Preparation of positive electrode sheet
[0066] The positive electrode active material LiNi 0.5 Co 0.2 Mn0.3 O2 (NCM523), conductive agent (Super P) and binder PVDF are fully stirred and mixed in a proper amount of NMP at a weight ratio of 96.2:2.7:1.1 to form a uniform positive electrode slurry; the positive electrode slurry is coated on the surface of the positive electrode current collector aluminum foil, and after drying and cold pressing, a positive electrode sheet is obtained.
[0067] 3. Preparation of electrolyte
[0068] Ethylene carbonate (EC), ethyl methyl carbonate (EMC) and diethyl carbonate (DEC) are mixed in a volume ratio of 1:1:1, and then LiPF6 is uniformly dissolved in the above solution to obtain an electrolyte, wherein the concentration of LiPF6 is 1 mol / L.
[0069] 4. Preparation of batteries
[0070] The positive electrode sheet and negative electrode sheet prepared above are stacked in order with the separator so that the separator is between the positive and negative electrode sheets, and then wound to obtain a bare cell. The bare cell is placed in an outer packaging shell, and after drying, an electrolyte is injected. After vacuum packaging, standing, forming, shaping and other processes, a lithium-ion battery is obtained.
[0071] Example 3
[0072] A lithium-ion battery comprises a negative electrode sheet, a positive electrode sheet and an electrolyte. The steps for preparing the lithium-ion battery are as follows:
[0073] 1. Preparation of negative electrode sheet
[0074] A negative electrode active material was obtained by mixing 5% by mass of carbon-uncoated graphite primary particles D1, 25% by mass of carbon-coated graphite primary particles C1, and 70% by mass of carbon-coated graphite secondary particles C2.
[0075] The preparation method of the carbon-coated graphite secondary particles is as follows: mixing the graphite primary particles and performing secondary granulation to obtain graphite secondary particles, and then carbon-coating the graphite secondary particles to obtain carbon-coated graphite secondary particles.
[0076] The negative electrode active material, conductive agent (Super P), binder (styrene-butadiene rubber emulsion) and thickener (CMC-Na) prepared above were fully stirred and mixed in an appropriate amount of deionized water at a mass ratio of 96.2:0.8:1.8:1.2 to form a uniform negative electrode slurry; the negative electrode slurry was coated on the surface of the negative electrode current collector copper foil, and after drying and cold pressing, a negative electrode sheet was obtained.
[0077] 2. Preparation of positive electrode sheet
[0078] The positive electrode active material LiNi 0.5 Co 0.2Mn 0.3 O2 (NCM523), conductive agent (Super P) and binder PVDF are fully stirred and mixed in a proper amount of NMP at a weight ratio of 96.2:2.7:1.1 to form a uniform positive electrode slurry; the positive electrode slurry is coated on the surface of the positive electrode current collector aluminum foil, and after drying and cold pressing, a positive electrode sheet is obtained.
[0079] 3. Preparation of electrolyte
[0080] Ethylene carbonate (EC), ethyl methyl carbonate (EMC) and diethyl carbonate (DEC) are mixed in a volume ratio of 1:1:1, and then LiPF6 is uniformly dissolved in the above solution to obtain an electrolyte, wherein the concentration of LiPF6 is 1 mol / L.
[0081] 4. Preparation of batteries
[0082] The positive electrode sheet and negative electrode sheet prepared above are stacked in order with the separator so that the separator is between the positive and negative electrode sheets, and then wound to obtain a bare cell. The bare cell is placed in an outer packaging shell, and after drying, an electrolyte is injected. After vacuum packaging, standing, forming, shaping and other processes, a lithium-ion battery is obtained.
[0083] Example 4
[0084] A lithium-ion battery comprises a negative electrode sheet, a positive electrode sheet and an electrolyte. The steps for preparing the lithium-ion battery are as follows:
[0085] 1. Preparation of negative electrode sheet
[0086] A negative electrode active material was obtained by mixing 5% by mass of carbon-uncoated graphite primary particles D1, 35% by mass of carbon-coated graphite primary particles C1, and 65% by mass of carbon-coated graphite secondary particles C2.
[0087] The preparation method of the carbon-coated graphite secondary particles is as follows: mixing the graphite primary particles and performing secondary granulation to obtain graphite secondary particles, and then carbon-coating the graphite secondary particles to obtain carbon-coated graphite secondary particles.
[0088] The negative electrode active material, conductive agent (Super P), binder (styrene-butadiene rubber emulsion) and thickener (CMC-Na) prepared above were fully stirred and mixed in an appropriate amount of deionized water at a mass ratio of 96.2:0.8:1.8:1.2 to form a uniform negative electrode slurry; the negative electrode slurry was coated on the surface of the negative electrode current collector copper foil, and after drying and cold pressing, a negative electrode sheet was obtained.
[0089] 2. Preparation of positive electrode sheet
[0090] The positive electrode active material LiNi 0.5 Co0.2 Mn 0.3 O2 (NCM523), conductive agent (Super P) and binder PVDF are fully stirred and mixed in a proper amount of NMP at a weight ratio of 96.2:2.7:1.1 to form a uniform positive electrode slurry; the positive electrode slurry is coated on the surface of the positive electrode current collector aluminum foil, and after drying and cold pressing, a positive electrode sheet is obtained.
[0091] 3. Preparation of electrolyte
[0092] Ethylene carbonate (EC), ethyl methyl carbonate (EMC) and diethyl carbonate (DEC) are mixed in a volume ratio of 1:1:1, and then LiPF6 is uniformly dissolved in the above solution to obtain an electrolyte, wherein the concentration of LiPF6 is 1 mol / L.
[0093] 4. Preparation of batteries
[0094] The positive electrode sheet and negative electrode sheet prepared above are stacked in order with the separator so that the separator is between the positive and negative electrode sheets, and then wound to obtain a bare cell. The bare cell is placed in an outer packaging shell, and after drying, an electrolyte is injected. After vacuum packaging, standing, forming, shaping and other processes, a lithium-ion battery is obtained.
[0095] Example 5
[0096] A lithium-ion battery comprises a negative electrode sheet, a positive electrode sheet and an electrolyte. The steps for preparing the lithium-ion battery are as follows:
[0097] 1. Preparation of negative electrode sheet
[0098] A negative electrode active material was obtained by mixing 15% by mass of carbon-uncoated graphite primary particles D1, 20% by mass of carbon-coated graphite primary particles C1, and 65% by mass of carbon-coated graphite secondary particles C2.
[0099] The preparation method of the carbon-coated graphite secondary particles is as follows: mixing the graphite primary particles and performing secondary granulation to obtain graphite secondary particles, and then carbon-coating the graphite secondary particles to obtain carbon-coated graphite secondary particles.
[0100] The negative electrode active material, conductive agent (Super P), binder (styrene-butadiene rubber emulsion) and thickener (CMC-Na) prepared above were fully stirred and mixed in an appropriate amount of deionized water at a mass ratio of 96.2:0.8:1.8:1.2 to form a uniform negative electrode slurry; the negative electrode slurry was coated on the surface of the negative electrode current collector copper foil, and after drying and cold pressing, a negative electrode sheet was obtained.
[0101] 2. Preparation of positive electrode sheet
[0102] The positive electrode active material LiNi 0.5Co 0.2 Mn 0.3 O2 (NCM523), conductive agent (Super P) and binder PVDF are fully stirred and mixed in a proper amount of NMP at a weight ratio of 96.2:2.7:1.1 to form a uniform positive electrode slurry; the positive electrode slurry is coated on the surface of the positive electrode current collector aluminum foil, and after drying and cold pressing, a positive electrode sheet is obtained.
[0103] 3. Preparation of electrolyte
[0104] Ethylene carbonate (EC), ethyl methyl carbonate (EMC) and diethyl carbonate (DEC) are mixed in a volume ratio of 1:1:1, and then LiPF6 is uniformly dissolved in the above solution to obtain an electrolyte, wherein the concentration of LiPF6 is 1 mol / L.
[0105] 4. Preparation of batteries
[0106] The positive electrode sheet and negative electrode sheet prepared above are stacked in order with the separator so that the separator is between the positive and negative electrode sheets, and then wound to obtain a bare cell. The bare cell is placed in an outer packaging shell, and after drying, an electrolyte is injected. After vacuum packaging, standing, forming, shaping and other processes, a lithium-ion battery is obtained.
[0107] Example 6
[0108] A lithium-ion battery comprises a negative electrode sheet, a positive electrode sheet and an electrolyte. The steps for preparing the lithium-ion battery are as follows:
[0109] 1. Preparation of negative electrode sheet
[0110] A negative electrode active material was obtained by mixing 15% by mass of carbon-uncoated graphite primary particles D1, 25% by mass of carbon-coated graphite primary particles C1, and 60% by mass of carbon-coated graphite secondary particles C2.
[0111] The preparation method of carbon-coated graphite secondary particles is to mix graphite primary particles and perform secondary granulation to obtain graphite secondary particles, and then carbon-coat the graphite secondary particles to obtain carbon-coated graphite secondary particles. The carbon coating method is not limited here.
[0112] The negative electrode active material, conductive agent (Super P), binder (styrene-butadiene rubber emulsion) and thickener (CMC-Na) prepared above were fully stirred and mixed in an appropriate amount of deionized water at a mass ratio of 96.2:0.8:1.8:1.2 to form a uniform negative electrode slurry; the negative electrode slurry was coated on the surface of the negative electrode current collector copper foil, and after drying and cold pressing, a negative electrode sheet was obtained.
[0113] 2. Preparation of positive electrode sheet
[0114] The positive electrode active material LiNi 0.5 Co 0.2 Mn 0.3 O2 (NCM523), conductive agent (Super P) and binder PVDF are fully stirred and mixed in a proper amount of NMP at a weight ratio of 96.2:2.7:1.1 to form a uniform positive electrode slurry; the positive electrode slurry is coated on the surface of the positive electrode current collector aluminum foil, and after drying and cold pressing, a positive electrode sheet is obtained.
[0115] 3. Preparation of electrolyte
[0116] Ethylene carbonate (EC), ethyl methyl carbonate (EMC) and diethyl carbonate (DEC) are mixed in a volume ratio of 1:1:1, and then LiPF6 is uniformly dissolved in the above solution to obtain an electrolyte, wherein the concentration of LiPF6 is 1 mol / L.
[0117] 4. Preparation of batteries
[0118] The positive electrode sheet and negative electrode sheet prepared above are stacked in order with the separator so that the separator is between the positive and negative electrode sheets, and then wound to obtain a bare cell. The bare cell is placed in an outer packaging shell, and after drying, an electrolyte is injected. After vacuum packaging, standing, forming, shaping and other processes, a lithium-ion battery is obtained.
[0119] Comparative Example 1
[0120] A lithium-ion battery comprises a negative electrode sheet, a positive electrode sheet and an electrolyte. The steps for preparing the lithium-ion battery are as follows:
[0121] 1. Preparation of negative electrode sheet
[0122] A negative electrode active material was obtained by mixing 50% by mass of carbon-coated graphite primary particles C1 and 50% by mass of carbon-coated graphite secondary particles C2.
[0123] The preparation method of carbon-coated graphite secondary particles is to mix graphite primary particles and perform secondary granulation to obtain graphite secondary particles, and then carbon-coat the graphite secondary particles to obtain carbon-coated graphite secondary particles. The carbon coating method is not limited here.
[0124] The negative electrode active material, conductive agent (Super P), binder (styrene-butadiene rubber emulsion) and thickener (CMC-Na) prepared above were fully stirred and mixed in an appropriate amount of deionized water at a mass ratio of 96.2:0.8:1.8:1.2 to form a uniform negative electrode slurry; the negative electrode slurry was coated on the surface of the negative electrode current collector copper foil, and after drying and cold pressing, a negative electrode sheet was obtained.
[0125] 2. Preparation of positive electrode sheet
[0126] The positive electrode active material LiNi 0.5 Co 0.2 Mn 0.3 O2 (NCM523), conductive agent (Super P) and binder PVDF are fully stirred and mixed in a proper amount of NMP at a weight ratio of 96.2:2.7:1.1 to form a uniform positive electrode slurry; the positive electrode slurry is coated on the surface of the positive electrode current collector aluminum foil, and after drying and cold pressing, a positive electrode sheet is obtained.
[0127] 3. Preparation of electrolyte
[0128] Ethylene carbonate (EC), ethyl methyl carbonate (EMC) and diethyl carbonate (DEC) are mixed in a volume ratio of 1:1:1, and then LiPF6 is uniformly dissolved in the above solution to obtain an electrolyte, wherein the concentration of LiPF6 is 1 mol / L.
[0129] 4. Preparation of batteries
[0130] The positive electrode sheet and negative electrode sheet prepared above are stacked in order with the separator so that the separator is between the positive and negative electrode sheets, and then wound to obtain a bare cell. The bare cell is placed in an outer packaging shell, and after drying, an electrolyte is injected. After vacuum packaging, standing, forming, shaping and other processes, a lithium-ion battery is obtained.
[0131] Comparative Example 2
[0132] A lithium-ion battery comprises a negative electrode sheet, a positive electrode sheet and an electrolyte. The steps for preparing the lithium-ion battery are as follows:
[0133] 1. Preparation of negative electrode sheet
[0134] A negative electrode active material was obtained by mixing 70% by mass of carbon-coated graphite primary particles C1 and 30% by mass of carbon-coated graphite secondary particles C2.
[0135] The preparation method of carbon-coated graphite secondary particles is to mix graphite primary particles and perform secondary granulation to obtain graphite secondary particles, and then carbon-coat the graphite secondary particles to obtain carbon-coated graphite secondary particles. The carbon coating method is not limited here.
[0136] The negative electrode active material, conductive agent (Super P), binder (styrene-butadiene rubber emulsion) and thickener (CMC-Na) prepared above were fully stirred and mixed in an appropriate amount of deionized water at a mass ratio of 96.2:0.8:1.8:1.2 to form a uniform negative electrode slurry; the negative electrode slurry was coated on the surface of the negative electrode current collector copper foil, and after drying and cold pressing, a negative electrode sheet was obtained.
[0137] 2. Preparation of positive electrode sheet
[0138] The positive electrode active material LiNi 0.5 Co 0.2 Mn 0.3 O2 (NCM523), conductive agent (Super P) and binder PVDF are fully stirred and mixed in a proper amount of NMP at a weight ratio of 96.2:2.7:1.1 to form a uniform positive electrode slurry; the positive electrode slurry is coated on the surface of the positive electrode current collector aluminum foil, and after drying and cold pressing, a positive electrode sheet is obtained.
[0139] 3. Preparation of electrolyte
[0140] Ethylene carbonate (EC), ethyl methyl carbonate (EMC) and diethyl carbonate (DEC) are mixed in a volume ratio of 1:1:1, and then LiPF6 is uniformly dissolved in the above solution to obtain an electrolyte, wherein the concentration of LiPF6 is 1 mol / L.
[0141] 4. Preparation of batteries
[0142] The positive electrode sheet and negative electrode sheet prepared above are stacked in order with the separator so that the separator is between the positive and negative electrode sheets, and then wound to obtain a bare cell. The bare cell is placed in an outer packaging shell, and after drying, an electrolyte is injected. After vacuum packaging, standing, forming, shaping and other processes, a lithium-ion battery is obtained.
[0143] Comparative Example 3
[0144] A lithium-ion battery comprises a negative electrode sheet, a positive electrode sheet and an electrolyte. The steps for preparing the lithium-ion battery are as follows:
[0145] 1. Preparation of negative electrode sheet
[0146] The negative electrode active material was obtained by mixing 10% by mass of non-carbon-coated graphite primary particles D1 and 90% by mass of carbon-coated graphite secondary particles C2.
[0147] The preparation method of carbon-coated graphite secondary particles is to mix graphite primary particles and perform secondary granulation to obtain graphite secondary particles, and then carbon-coat the graphite secondary particles to obtain carbon-coated graphite secondary particles. The carbon coating method is not limited here.
[0148] The negative electrode active material, conductive agent (Super P), binder (styrene-butadiene rubber emulsion) and thickener (CMC-Na) prepared above were fully stirred and mixed in an appropriate amount of deionized water at a mass ratio of 96.2:0.8:1.8:1.2 to form a uniform negative electrode slurry; the negative electrode slurry was coated on the surface of the negative electrode current collector copper foil, and after drying and cold pressing, a negative electrode sheet was obtained.
[0149] 2. Preparation of positive electrode sheet
[0150] The positive electrode active material LiNi 0.5 Co 0.2 Mn 0.3 O2 (NCM523), conductive agent (Super P) and binder PVDF are fully stirred and mixed in a proper amount of NMP at a weight ratio of 96.2:2.7:1.1 to form a uniform positive electrode slurry; the positive electrode slurry is coated on the surface of the positive electrode current collector aluminum foil, and after drying and cold pressing, a positive electrode sheet is obtained.
[0151] 3. Preparation of electrolyte
[0152] Ethylene carbonate (EC), ethyl methyl carbonate (EMC) and diethyl carbonate (DEC) are mixed in a volume ratio of 1:1:1, and then LiPF6 is uniformly dissolved in the above solution to obtain an electrolyte, wherein the concentration of LiPF6 is 1 mol / L.
[0153] 4. Preparation of batteries
[0154] The positive electrode sheet and negative electrode sheet prepared above are stacked in order with the separator so that the separator is between the positive and negative electrode sheets, and then wound to obtain a bare cell. The bare cell is placed in an outer packaging shell, and after drying, an electrolyte is injected. After vacuum packaging, standing, forming, shaping and other processes, a lithium-ion battery is obtained.
[0155] Comparative Example 4
[0156] A lithium-ion battery comprises a negative electrode sheet, a positive electrode sheet and an electrolyte. The steps for preparing the lithium-ion battery are as follows:
[0157] 1. Preparation of negative electrode sheet
[0158] A negative electrode active material was obtained by mixing 10% by mass of non-carbon-coated graphite primary particles D1 and 90% by mass of carbon-coated graphite primary particles C1.
[0159] The negative electrode active material, conductive agent (Super P), binder (styrene-butadiene rubber emulsion) and thickener (CMC-Na) prepared above were fully stirred and mixed in an appropriate amount of deionized water at a mass ratio of 96.2:0.8:1.8:1.2 to form a uniform negative electrode slurry; the negative electrode slurry was coated on the surface of the negative electrode current collector copper foil, and after drying and cold pressing, a negative electrode sheet was obtained.
[0160] 2. Preparation of positive electrode sheet
[0161] The positive electrode active material LiNi 0.5 Co 0.2 Mn 0.3O2 (NCM523), conductive agent (Super P) and binder PVDF are fully stirred and mixed in a proper amount of NMP at a weight ratio of 96.2:2.7:1.1 to form a uniform positive electrode slurry; the positive electrode slurry is coated on the surface of the positive electrode current collector aluminum foil, and after drying and cold pressing, a positive electrode sheet is obtained.
[0162] 3. Preparation of electrolyte
[0163] Ethylene carbonate (EC), ethyl methyl carbonate (EMC) and diethyl carbonate (DEC) are mixed in a volume ratio of 1:1:1, and then LiPF6 is uniformly dissolved in the above solution to obtain an electrolyte, wherein the concentration of LiPF6 is 1 mol / L.
[0164] 4. Preparation of batteries
[0165] The positive electrode sheet and negative electrode sheet prepared above are stacked in order with the separator so that the separator is between the positive and negative electrode sheets, and then wound to obtain a bare cell. The bare cell is placed in an outer packaging shell, and after drying, an electrolyte is injected. After vacuum packaging, standing, forming, shaping and other processes, a lithium-ion battery is obtained.
[0166] Lithium battery performance test
[0167] 1) Sample selection
[0168] Ten lithium-ion batteries prepared in Examples 1-6 and Comparative Examples 1-4 were selected to form 10 groups of samples.
[0169] 2) High temperature storage recovery rate test
[0170] The 10 groups of samples were placed in a 25℃ constant temperature box in turn and left to stand for 30 minutes to allow the lithium-ion battery to reach a constant temperature of 25℃. They were charged to 3.65V at a constant current of 1C, charged to 0.05C at a constant voltage, and then discharged to 2.5V at a constant current of 1C. The discharge capacity of each group was recorded as the initial capacity and the average value was C0. After that, they were charged to 3.65V at a constant current of 0.5C, charged to 0.05C at a constant voltage, and transferred to a 55℃ constant temperature box for storage for 7 days. The samples were then transferred to a 25℃ constant temperature box, left to stand for 60 minutes, and discharged to 2.5V at a constant current of 1C. The discharge capacity of each group of samples was recorded as the residual capacity and the average value was C1; then they were charged to 3.65V at a constant current of 1C, charged to 0.05C at a constant voltage, and then discharged to 2.5V at a constant current of 1C. The discharge capacity of each group of samples was recorded as the recovery capacity and the average value was C2.
[0171] The remaining capacity retention rate and the recovery capacity retention rate of the lithium-ion batteries in the 10 groups of samples were calculated according to the following formula as indicators for evaluating the 100% SOC high temperature storage performance of the lithium-ion batteries.
[0172] 100% SOC high temperature storage recovery capacity retention rate = C2 / C0×100%.
[0173] 3) Charging rate test
[0174] At 25°C, the batteries prepared in the embodiments and comparative examples are fully charged at xC and fully discharged at 1C for 10 times, and then the batteries are fully charged at xC again, and then the negative electrode plates are disassembled, and the lithium deposition on the surface of the negative electrode plates is observed. If no lithium is deposited on the negative electrode surface, the charging rate xC is increased by 0.1C and tested again until lithium is deposited on the negative electrode surface. The test is stopped, and the charging rate (x-0.1)C at this time is the charging rate of the battery.
[0175] The final test result data is shown in the following table.
[0176]
[0177] According to the above table, by comparing Examples 1-6 and Comparative Examples 1-4, it can be seen that the present invention adopts a compounding method of uncoated carbon primary graphite particles D1, carbon-coated primary graphite particles C1 and carbon-coated secondary graphite particles C2 to obtain a negative electrode sheet having good charge rate performance and good high temperature storage recovery capacity recovery rate.
[0178] It should be pointed out that the above is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A negative electrode sheet, comprising a current collector and a negative electrode active material, wherein the negative electrode active material is a graphite material, characterized in that: The graphite material includes primary particles D1, primary particles C1 and secondary particles C2; The primary particles D1 are graphite particles that are not coated with carbon, and the primary particles C1 and the secondary particles C2 are graphite particles that are coated with carbon.
2. The negative electrode sheet according to claim 1, characterized in that: The primary particles D1, primary particles C1 and secondary particles C2 are made of the same graphite material, wherein the graphite material includes natural graphite and artificial graphite.
3. The negative electrode sheet according to claim 1, characterized in that: The primary particles D1, primary particles C1 and secondary particles C2 are different types of graphite materials, wherein the rate performance of the graphite materials is ranked as C2>C1>D1, and the high temperature storage performance of the graphite materials is ranked as D1>C1>C2.
4. The negative electrode sheet according to claim 1, characterized in that: The particle size D50 of the graphite material is 11 μm-13 μm, and the BET specific surface area of the graphite material is 0.8 m2 / g-1.2 m2 / g.
5. The negative electrode sheet according to claim 1, characterized in that: The mass fraction of the primary particles D1 in the graphite material is 5%-15%; The mass fraction of the primary particles C1 in the graphite material is 20%-30%; The mass fraction of the secondary particles C2 in the graphite material is 60%-70%.
6. The negative electrode sheet according to claim 5, characterized in that: The mass fraction of the primary particles D1 in the graphite material is 10%.
7. The negative electrode sheet according to claim 1, characterized in that: The carbon coating amount of the primary particles C1 is 4wt%-6wt%, and the carbon coating amount of the secondary particles C2 is 4wt%-8wt%.
8. The negative electrode sheet according to claim 1, characterized in that: The thickness of the carbon coating layer of the primary particle C1 is 8nm-20nm, and the thickness of the carbon coating layer of the secondary particle C2 is 6nm-20nm.
9. A lithium ion battery, characterized in that: It comprises a negative electrode sheet as described in any one of claims 1 to 8.