Cover article with high hardness and anti-reflective properties for infrared sensors
By using a combination of chemically strengthened glass or glass-ceramic substrates with multilayer outer films in infrared sensor applications, the problems of wear and insufficient strength are solved, achieving optical performance with high hardness, low reflectivity and high transmittance.
Patent Information
- Application Number
- CN202380029251.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2023-03-08
- Filing Date
- 2023-03-17
- Publication Date
- 2024-11-08
AI Technical Summary
Existing cover products are susceptible to wear, abrasion, and scratch damage in infrared sensor applications, leading to a decline in optical performance. Furthermore, the combination of traditional substrates and outer layer films results in insufficient product strength.
It uses chemically strengthened glass or glass-ceramic substrate, combined with an outer layer film. The outer layer film consists of multiple alternating high and low refractive index layers, including scratch-resistant layers and anti-reflection areas. It has high hardness and low reflectivity characteristics and is suitable for infrared and visible light ranges.
It improves the durability and optical performance of the cover, ensuring low reflectivity and high transmittance in the infrared and visible light range, and enhances scratch resistance and mechanical strength.
Smart Images

Figure CN118922748A_ABST
Abstract
Description
[0001] Priority claim
[0002] This application claims priority under the patent law to U.S. Provisional Application No. 63 / 321,905 filed on March 21, 2022, and claims priority under the patent law to U.S. Provisional Application No. 63 / 450,687 filed on March 8, 2023, which applications are incorporated herein by reference in their entirety. Technical Field
[0003] The present invention relates to durable and / or scratch resistant cover articles for electronic devices, and more particularly, to durable and / or scratch resistant cover articles for infrared sensors and other sensors. Background Art
[0004] Cover products are often used to protect key devices within electronic products, to provide user interfaces for input and / or display, and / or many other functions. Such products include mobile devices such as smart phones, mp3 players, and computer tablets. Cover products also include architectural products, transportation products (e.g., products for automotive applications, trains, airplanes, marine vessels, etc.), electrical products, or any product that requires a certain degree of transparency, scratch resistance, abrasion resistance, or a combination thereof.
[0005] These applications typically require scratch resistance and strong optical performance properties in terms of maximum light transmittance and minimum reflectivity. In addition, some cover applications require that the color displayed or perceived in reflection and / or transmission does not change noticeably with changes in viewing angle. In display applications, this is because if the color in reflection or transmission changes to a noticeable degree with viewing angle, the user of the product will perceive a change in the color or brightness of the display, which can reduce the perceived quality of the display. In other applications, the change in color may negatively impact aesthetic requirements or other functional requirements.
[0006] Recently, infrared (IR) sensors have been increasingly deployed in these same applications, for example, in LIDAR or time-of-flight infrared sensing applications, such as distance sensing for camera focus and facial recognition. These IR sensors (which may include IR cameras) typically operate at wavelengths where semiconductor IR devices have historically been developed, driven by semiconductor band gap factors (e.g., silicon, gallium arsenide (GaAs), germanium, indium phosphide (InP), InGaAs, GaInAsP, AlGaInAs, (Ga)InAs+ quantum dots, and GaInNAs (Sb) emission and absorption wavelengths), emission wavelengths of rare earth and other emitting elements and compounds (e.g., erbium, ytterbium, neodymium yttrium aluminum garnet), and telecommunication (e.g., silica optical fiber) transparency window factors, as well as wavelength division multiplexing telecommunication applications operating in a wavelength window of approximately 1260-1675 nm. Typical exemplary wavelengths include those at or near (eg, within 50 nm) center wavelengths around 850 nm, 940 nm, 1060 nm, 1260 nm, 1310 nm, and 1550 nm.
[0007] The optical performance of a cover article can be improved by using various anti-reflective coatings. However, known anti-reflective (AR) coatings are susceptible to wear, abrasion and / or scratch damage. Such wear, abrasion and scratch damage may compromise any optical performance improvement achieved by the AR coating. In addition, some known anti-reflective coatings exhibit good performance in the visible spectrum, but also exhibit high reflectivity and / or low transmittance in the infrared spectrum (e.g., 1000-1700 nm) utilized by IR sensors.
[0008] In addition, conventional cover articles employing glass or glass-ceramic substrates and outer layer films may have reduced overall mechanical properties. Specifically, the inclusion of outer layer films and AR coatings on these substrates provides advantages in terms of optical performance and certain mechanical properties (e.g., scratch resistance); however, conventional combinations of these substrates with outer layer films (e.g., optimized with high modulus and / or hardness for improved scratch resistance) result in poor strength levels in the resulting articles. It should be noted that the presence of an outer layer film on a substrate can adversely reduce the strength level of the article to less than the strength of the substrate in its bare form without the outer layer film.
[0009] Therefore, there is a need for cover articles for electronic devices (e.g., which employ IR sensors) that are durable (e.g., having high hardness, damage resistance and / or residual strength) and / or scratch resistant, and have improved optical properties (e.g., low reflectivity and / or high transmittance), particularly in a spectrum that includes both visible light and infrared light or in a spectrum of infrared light. Summary of the invention
[0010] According to an aspect of the present invention, there is provided a cover product for a sensor, comprising: a substrate having a thickness of 50 μm to 5000 μm, an outer major surface and an inner major surface, wherein the outer major surface and the inner major surface are opposite to each other; and an outer layered film disposed on the outer major surface of the substrate. The substrate is a chemically strengthened glass substrate or a glass ceramic substrate. The cover product exhibits a first surface average reflectivity of less than 10% for a wavelength of 1000 nm to 1700 nm at at least one incident angle of 8° to 60°.
[0011] According to another aspect of the present invention, there is provided a cover article for a sensor, comprising: a substrate comprising a thickness of 50 μm to 5000 μm, an outer major surface and an inner major surface, wherein the outer major surface and the inner major surface are opposite to each other; and an outer layered film disposed on the outer major surface of the substrate. The substrate is a chemically strengthened glass substrate or a glass ceramic substrate. The outer layered film exhibits a hardness of at least 8 GPa, as measured by a Berkovich indenter hardness test from the outermost surface of the outer layered film to a depth of about 100 nm to about 500 nm. In addition, the cover article exhibits a first surface average reflectivity of less than 10% for wavelengths of 1000 nm to 1700 nm at at least one incident angle of 8° to 60°.
[0012] According to a further aspect of the present invention, a cover product for a sensor is provided, comprising: a substrate comprising a thickness of 50 μm to 5000 μm, an outer major surface and an inner major surface, wherein the outer major surface and the inner major surface are opposite to each other; and an outer layered film disposed on the outer major surface of the substrate. The substrate is a chemically strengthened glass substrate or a glass ceramic substrate. The outer layered film comprises a plurality of alternating high refractive index layers and low refractive index layers. Each of the high refractive index layers comprises a nitride or an oxynitride, and the refractive index is greater than the refractive index of each of the low refractive index layers. The outer layered film comprises an anti-scratch layer having a thickness of about 80 nm to 10000 nm. One of the low refractive index layers is a cap layer defining the outermost surface of the outer layered film, and the cap layer has a thickness of at least 110 nm. In addition, the outer layered film comprises an anti-reflection region above the anti-scratch layer, and the anti-reflection region comprises a thickness of about 100 nm to about 525 nm. In addition, the low refractive index layer of the anti-reflection region comprises a total thickness of less than 275 nm. In addition, the outer layer film exhibits a hardness of at least 8 GPa, as measured by a Berkovich indenter hardness test from the outermost surface of the outer layer film to a depth of about 100 nm to about 500 nm. In addition, the cover article exhibits a first surface average reflectivity of less than 10% for wavelengths from 1000 nm to 1700 nm at at least one incident angle of 8° to 60°.
[0013] According to a further aspect of the present invention, there is provided a cover article for a sensor, comprising: a substrate comprising a thickness of 50 μm to 5000 μm, an outer major surface and an inner major surface, wherein the outer major surface and the inner major surface are opposite to each other; and an outer layered film disposed on the outer major surface of the substrate. The substrate is a chemically strengthened glass substrate or a glass ceramic substrate. The cover article exhibits a first surface average reflectivity of less than 10% for a wavelength of 1000 nm to 1700 nm at at least one incident angle of 8° to 60°. In addition, the outer layered film exhibits a residual compressive stress greater than or equal to 700 MPa and an elastic modulus greater than or equal to 140 GPa.
[0014] According to a further aspect of the present invention, a cover article is provided, comprising: a glass ceramic substrate including a first major surface and a second major surface, the major surfaces being opposite to each other; and an outer layer film defining an outer surface, the outer layer film being disposed on the first major surface. The cover article exhibits a hardness greater than 15 GPa, as measured by a Berkovich hardness test at an indenter depth of about 125 nm from the outer surface of the outer layer film. In addition, the cover article exhibits a first surface average reflectivity of less than 10% for wavelengths of 1000 nm to 1700 nm at at least one incident angle of 8° to 60°.
[0015] Additional features and advantages will be set forth in the following detailed description, and some features and advantages will be readily apparent to those skilled in the art from that description or by practicing the embodiments described herein, including the following detailed description, claims, and drawings.
[0016] It should be understood that the foregoing general description and the following detailed description are only exemplary and are intended to provide an overview or framework for understanding the nature and features of the claims. The accompanying drawings are included to provide a further understanding and are incorporated into and constitute a part of this specification. The accompanying drawings illustrate one or more embodiments and, together with the description, are used to explain the principles and operations of the various embodiments. BRIEF DESCRIPTION OF THE DRAWINGS
[0017] Figure 1 is a cross-sectional side view of a cover article according to one or more embodiments described herein;
[0018] Figure 1A is a cross-sectional side view of a cover article according to one or more embodiments described herein;
[0019] Figure 1B is a cross-sectional side view of a cover article according to one or more embodiments described herein;
[0020] Figure 1C is a cross-sectional side view of a cover article according to one or more embodiments described herein;
[0021] Figure 1D is a cross-sectional side view of a cover article according to one or more embodiments described herein;
[0022] Figure 1E is a cross-sectional side view of a cover article according to one or more embodiments described herein;
[0023] Figure 1F is a cross-sectional side view of a cover article according to one or more embodiments described herein;
[0024] Figure 2A is a plan view of an exemplary electronic product incorporating any of the cover articles disclosed herein;
[0025] Figure 2B yes Figure 2A A perspective view of an exemplary electronic product;
[0026] Figure 3A is a graph showing the relationship between the first surface reflectivity and wavelength of the comparative cover product at incident angles of 8°, 30°, 40° and 60°;
[0027] Figure 3B yes Figure 3A A graph of the first surface reflected color of the comparative cover product at all viewing angles from 0 degrees to 90 degrees using a D65 light source;
[0028] Figure 3C yes Figure 3A A graph of the dual surface transmission color of the comparative cover product at all viewing angles from 0 degrees to 90 degrees with a D65 light source;
[0029] Figure 4A is a graph of first surface reflectivity versus wavelength for an exemplary cover product of the present invention at incident angles of 8°, 30°, 40°, and 60°;
[0030] Figure 4B yes Figure 4A A graph of the first surface reflected color of an exemplary cover product at all viewing angles from 0 degrees to 90 degrees with a D65 light source;
[0031] Figure 4C yes Figure 4A A graph of dual surface transmission color of an exemplary cover product at all viewing angles from 0 degrees to 90 degrees with a D65 light source;
[0032] Figure 5A is a graph of first surface reflectivity versus wavelength for an exemplary cover product of the present invention at incident angles of 8°, 30°, 40°, and 60°;
[0033] Figure 5B yes Figure 5AA graph of the first surface reflected color of an exemplary cover product at all viewing angles from 0 degrees to 90 degrees with a D65 light source;
[0034] Figure 5C yes Figure 5A A graph of dual surface transmission color of an exemplary cover product at all viewing angles from 0 degrees to 90 degrees with a D65 light source;
[0035] Fig. 6A is a graph of first surface reflectivity versus wavelength for an exemplary cover product of the present invention at incident angles of 8°, 30°, 40°, and 60°;
[0036] Figure 6B yes Fig. 6A A graph of the first surface reflected color of an exemplary cover product at all viewing angles from 0 degrees to 90 degrees with a D65 light source;
[0037] Figure 6C yes Fig. 6A A graph of dual surface transmission color of an exemplary cover product at all viewing angles from 0 degrees to 90 degrees with a D65 light source;
[0038] Fig. 7A is a graph of first surface reflectivity versus wavelength for an exemplary cover product of the present invention at incident angles of 8°, 30°, 40°, and 60°;
[0039] Figure 7B yes Fig. 7A A graph of the first surface reflected color of an exemplary cover product at all viewing angles from 0 degrees to 90 degrees with a D65 light source;
[0040] Figure 7C yes Fig. 7A A graph of dual surface transmission color of an exemplary cover product at all viewing angles from 0 degrees to 90 degrees with a D65 light source;
[0041] Fig. 8A is a graph of first surface reflectivity versus wavelength for an exemplary cover product of the present invention at incident angles of 8°, 30°, 40°, and 60°;
[0042] Figure 8B yes Fig. 8A A graph of the first surface reflected color of an exemplary cover product at all viewing angles from 0 degrees to 90 degrees with a D65 light source;
[0043] Figure 8C yes Fig. 8A A graph of dual surface transmission color of an exemplary cover product at all viewing angles from 0 degrees to 90 degrees with a D65 light source;
[0044] Fig.9Ais a graph of first surface reflectivity versus wavelength for an exemplary cover product of the present invention at incident angles of 8°, 30°, 40°, and 60°;
[0045] Fig. 9B yes Fig.9A A graph of the first surface reflected color of an exemplary cover product at all viewing angles from 0 degrees to 90 degrees with a D65 light source;
[0046] Fig. 9C yes Fig.9A A graph of dual surface transmission color of an exemplary cover product of for all viewing angles from 0 degrees to 90 degrees using a D65 light source;
[0047] Fig. 10A is a graph of first surface reflectivity versus wavelength for an exemplary cover product of the present invention at incident angles of 8°, 30°, 40°, and 60°;
[0048] Fig. 10B yes Fig. 10A A graph of the first surface reflected color of an exemplary cover product at all viewing angles from 0 degrees to 90 degrees with a D65 light source; and
[0049] Fig. 10C yes Fig. 10A A graph of the dual surface transmission color of an exemplary cover product at all viewing angles from 0 degrees to 90 degrees with a D65 illuminant.
[0050] Fig.11A is a graph of first surface reflectivity versus wavelength at an incident angle of 8° for an exemplary cover article of the present invention;
[0051] Fig. 11B yes Fig.11A Graph of first surface reflected color measured for exemplary cover products at incident angles ranging from 0° to 90° at various optical film structure thickness scaling factors.
[0052] Fig. 12A is a graph of first surface reflectance versus wavelength for an exemplary cover article of the present invention at an incident angle of 8°;
[0053] Fig. 12B yes Fig. 12A Graph of first surface reflected color measured for exemplary cover products at incident angles ranging from 0° to 90° at various optical film structure thickness scaling factors.
[0054] Fig.13A is a graph of first surface reflectivity versus wavelength at an incident angle of 8° for an exemplary cover article of the present invention;
[0055] Fig. 13B yes Fig.13AGraph of first surface reflected color measured for exemplary cover products at incident angles ranging from 0° to 90° at various optical film structure thickness scaling factors.
[0056] Fig.14A is a graph of the first surface reflectivity versus wavelength for a comparative cover product at an incident angle of 8°;
[0057] Fig. 14B yes Fig.14A A graph of first surface reflected color of a comparative cover product measured at various optical film structure thickness ratio factors at incident angles of 0° to 90°;
[0058] Fig.15A Is has Fig.11A To 13B of the optical properties of the present invention, the cover product, the control product without the outer layer structure and having Fig.14A and Fig. 14B Box plot of the average product failure stress measured in the ring-on-ring test for comparative products with medium optical properties;
[0059] Fig. 15B is a graph of the hardness versus depth of the outer delamination film of the lid articles of Examples 8-10, as measured in the Berkovich Hardness Test; and
[0060] Fig. 15C is a graph of the elastic modulus of the outer layered film of the lid articles of Examples 8-10 versus depth, as measured in the Berkovich Hardness Test. DETAILED DESCRIPTION
[0061] In the following detailed description, for the purpose of explanation rather than limitation, example embodiments disclosing specific details are set forth to provide a thorough understanding of the various principles of the present invention. However, it will be apparent to one of ordinary skill in the art, having obtained the benefit of the present invention, that the present invention may be practiced in other embodiments that deviate from the specific details disclosed herein. In addition, descriptions of known devices, methods, and materials may be omitted so as not to obscure the description of the various principles of the present invention. Finally, where applicable, the same reference numerals refer to the same components.
[0062] Ranges herein may be expressed as "about" one particular value, and / or to "about" another particular value. When such a range is expressed, another embodiment includes from the one particular value and / or to the other particular value. Similarly, when a value is expressed as an approximation by using the antecedent "about," it will be understood that the particular value forms another embodiment. It will be further understood that the endpoints of each range are both related to and independent of the other endpoint.
[0063] Directional terms used herein, for example, “upper,” “lower,” “right,” “left,” “front,” “back,” “top,” and “bottom,” refer only to the figures drawn and are not intended to imply an absolute orientation.
[0064] Unless expressly stated otherwise, any method described herein should not be interpreted as requiring that its steps be performed in a specific order. Therefore, if a method claim does not actually list the order in which its steps are to be followed, or if there is no specific statement in the claim or description that the steps are to be limited to a specific order, no order is intended to be inferred. This applies to any possible non-express basis for interpretation, including: logical matters regarding the arrangement of steps or operational flow; plain meaning derived from grammatical organization or punctuation; the number or type of embodiments described in the specification.
[0065] As used herein, the singular forms "a," "an," and "the" include plural references unless the context clearly dictates otherwise. Thus, for example, reference to "a component" includes aspects having two or more such components unless the context clearly dictates otherwise.
[0066] As used herein, the term "disposed" includes coating, depositing and / or forming a material on a surface using any method known or to be developed in the art. The disposed material may constitute a layer as defined herein. As used herein, the phrase "disposed on" includes forming a material on a surface such that the material is in direct contact with the surface, as well as embodiments in which the material is formed on a surface with one or more intervening materials disposed between the material and the surface. The intervening material may constitute a layer as defined herein.
[0067] As used herein, the terms "low RI layer", "medium RI layer" and "high RI layer" refer to the relative values of the refractive index ("refractive index, RI") of the layers of the outer layered film of the cover product according to the present invention. Therefore, unless otherwise clearly indicated in the present invention, the RI of the low RI layer is < the RI of the medium RI layer < the RI of the high RI layer. Therefore, the low RI layer has a refractive index value that is less than the refractive index values of the medium RI layer and the high RI layer. In addition, as used herein, "low RI layer" and "low refractive index layer" are interchangeable and have the same meaning. Similarly, "medium RI layer" and "medium refractive index layer" are interchangeable and have the same meaning. Similarly, "high RI layer" and "high refractive index layer" are interchangeable and have the same meaning.
[0068] As used herein, the term "strengthened substrate" refers to a substrate employed in the cap product of the present invention that has been strengthened, for example, by ion exchange of larger ions with smaller ions in the surface of the substrate. However, other strengthening methods known in the art may be used to form a strengthened substrate, such as thermal tempering, or utilizing a mismatch in the coefficient of thermal expansion between portions of the substrate to produce compressive stress and a central tension region.
[0069] As used herein, "Berkovich indenter hardness test" and "Berkovic hardness test" are used interchangeably and refer to a test for measuring the hardness of a material on a surface of the material by pressing a diamond Berkovich indenter into the surface. The Berkovich indenter hardness test comprises pressing a diamond Berkovich indenter into the outermost surface (e.g., exposed surface) of the outer layered film of the cover article of the present invention to form an indentation with a depth ranging from about 50 nm to about 1000 nm (or the entire thickness of the outer layered film, whichever is less), and measuring the maximum hardness from this indentation along the entire indentation depth range or a portion of this indentation depth range (e.g., a depth of about 100 nm to about 600 nm, about 100 nm to about 500 nm to 200 nm). The hardness and elastic modulus are generally determined by Oliver, WC & Pharr, GM's Improved Technique of Determining Hardness and Elastic Modulus Using Load and Displacement Sensing Indentation Test (J. Mater. Res., Vol. 7, No. 6, 1992, 1564-1583) and Oliver, WC & Pharr, GM's Methods of Measuring Hardness and Elastic Modulus by Instrumental Indentation: Advanced Understanding and Improved Methods (J. Mater. Res., Vol. 19, No. 1, 2004, 3-20). As used herein, each of "hardness" and "maximum hardness" interchangeably refers to the maximum hardness measured along the range of indentation depth, rather than the average hardness.
[0070] Typically, in nanoindentation measurement methods (such as the Berkovich indenter hardness test) of a coating or film that is harder than the underlying substrate, the measured hardness may initially appear to increase due to the development of the plastic zone at a shallow indentation depth, then increase and reach a maximum or plateau at a deeper indentation depth. Thereafter, the hardness begins to decrease at even deeper indentation depths due to the influence of the underlying substrate. The same effect can be seen in the case of using a substrate with increased hardness compared to the coating; however, the hardness increases at deeper indentation depths due to the influence of the underlying substrate. The indentation depth range and the hardness values at a particular indentation depth range can be selected to identify the specific hardness response of the outer layered films and their layers described herein without being affected by the underlying substrate.
[0071] When the hardness of the outer layered film of the cover article of the present invention is measured according to the Berkovich Indenter Hardness Test, the permanent deformation zone (plastic zone) of the material is associated with the hardness of the material. During indentation, the elastic stress field extends far beyond this permanent deformation zone. As the indentation depth increases, the apparent hardness and modulus are affected by the interaction with the stress field of the underlying substrate. The effect of the substrate on the hardness occurs at deeper indentation depths (i.e., typically at depths greater than about 10% of the thickness of the outer layered film or layer). In addition, a further complication is that the hardness response requires a certain minimum load to produce complete plasticity during the indentation process. Prior to the specific minimum load, the hardness shows a generally increasing trend.
[0072] At small indentation depths (which can also be characterized as small loads) (e.g., up to about 50 nm) in the outer layered film of the cover article of the present invention, the apparent hardness of the material appears to increase significantly relative to the indentation depth. This small indentation depth range does not represent a true measure of hardness, but rather reflects the development of the plastic zone described above, which is related to the finite radius of curvature of the indenter. At intermediate indentation depths, the apparent hardness approaches a maximum level. At deeper indentation depths, the effect of the substrate (e.g., substrate 110, as described in detail below) becomes more pronounced as the indentation depth increases. Once the indentation depth exceeds the outer layered film of the cover article of the present invention (e.g., substrate 110, as described in detail below), the apparent hardness of the material appears to increase significantly relative to the indentation depth. Figures 1 to 1F The hardness may begin to drop sharply when the outer layer film 120 (shown in FIG. 1 and discussed in detail below) is approximately 30% of the outer layer film 120 .
[0073] For the "model hardness" values cited in the following examples (see the section entitled "Examples"), the nanoindentation process of the coated glass was modeled using the finite element method (FEM) in the commercial software suite ABAQUS v.2018. An axisymmetric model was used to reduce the computational time, and a conical indenter tip with a half angle of 70.3° was assumed, which produced the same contact area to depth ratio as the Berkovich tip. In practice, there is no sharp Berkovich indenter with zero tip radius. The radius of the new indenter tip is in the range of 40nm-50nm and may increase to 100-200nm or more as it wears. In the present invention, it is assumed that the indenter has a tip bluntness of 100nm, which is incorporated into the model. In the modeling analysis adopted in the present invention, it is assumed that all materials are homogeneous, isotropic, perfectly elastic-plastic, and the Max Sir yield criterion is adopted. The displacement history from the experiment (e.g., the nanoindentation results of the manufactured monolayer film) is used as the input of the FEM simulation. The nanoindentation load as a function of a prescribed displacement is the output of the simulation. In order to extract the hardness as a function of the nanoindentation depth, a continuous stiffness measurement (CSM) nanoindentation is simulated. For this purpose, a small amplitude vibration is imparted to the nanoindentation tip during the loading phase. The load vs. nanoindentation depth curve is extracted from the numerical simulation. The hardness response is then calculated using the Oliver-Pharr method.
[0074] As used herein, the term "ring-on-ring test" or "ROR test" refers to a test for determining the breaking strength or breaking stress (in MPa) of the cover product of the present invention and comparative products. Each ring-on-ring (ROR) test is conducted with a test configuration using a load ring and a support ring made of high-strength steel having diameters of 12.7 mm and 25.4 mm, respectively. In addition, the load-bearing surfaces of the load ring and the support ring are machined to a radius of about 0.0625 inches to minimize stress concentration in the contact area between the ring and the cover product. In addition, the load ring is placed on the outermost major surface of the cover product (e.g., on the outer surface of its outer layered film), and the support ring is placed on the innermost major surface of the cover product (e.g., on the second major surface of its substrate). The load ring incorporates a mechanism that enables the load ring to be articulated and ensures proper alignment and uniform loading of the tes sample. In addition, each ROR test is conducted by applying a load ring to the cover product at a load rate of 1.2 mm / min. In the context of the ROR test, the term "average" is the mathematical mean of the failure stress measurements based on five (5) samples. In addition, unless otherwise specified in a specific example of the present invention, all failure stress values and measurements described herein refer to measurements from a ROR test, which places the outer surface of the article under tension, as described in International Publication No. WO2018 / 125676, entitled "Coated Articles with Optical Coatings Having Residual Compressive Stress," published on July 5, 2018, which is incorporated herein by reference in its entirety. Failure in each ROR test typically occurs on the side of the sample opposite the load ring, which is under tension, and finite element modeling is used to provide an appropriate conversion from the failure load to the failure stress at the location of the failure. It should also be understood that other failure strength tests can be used to determine the failure strength of the cover article of the present invention, and the ROR values in the present invention and the results reported herein are appropriately correlated based on differences in test conditions, test specimen geometry, and other technical factors understood by a person of ordinary skill in the art. However, unless otherwise stated, all average breaking strength values reported for the inventive lid articles and comparative articles are values obtained from ROR test measurements.
[0075] As also used herein, the term "stress-induced failure" refers to stress at which a crack propagates simultaneously in the outer layered film, substrate, or both of the cover article of the present invention without the application of additional loads, typically resulting in catastrophic failure in a given material, layer, or film, and possibly even across another material, layer, or film, as defined herein. That is, failure of the outer layered film without failure of the substrate constitutes failure, and failure of the substrate also constitutes failure. The term "average", when related to average stress-induced failure or any other property, is a mathematical mean based on the measurement of such property for 5 samples. Typically, crack initiation stress measurements are repeatable under normal laboratory conditions, and the standard deviation of crack initiation stresses measured in multiple samples may be as low as 0.01% of the observed stress. The term "average stress-induced failure" as used herein is measured using a ring-on-ring (ROR) test. However, unless otherwise noted, the stress-induced failure measurements described herein refer to measurements from a ring-on-ring test, as described in International Publication No. WO2018 / 125676, entitled “Coated Articles Having Optical Coatings with Residual Compressive Stress,” published on July 5, 2018, which is incorporated herein by reference in its entirety.
[0076] As used herein, the term "transmittance" is defined as the percentage of incident light power transmitted through a material (e.g., a cover article, substrate, outer layer film, or portion thereof) within a given wavelength range. The term "reflectivity" is similarly defined as the percentage of incident light power reflected from a material (e.g., a cover article, substrate, or outer layer film, or portion thereof) within a given wavelength range. Transmittance and reflectivity are measured using a specific line width. As used herein, "average transmittance" refers to the average amount of incident light power transmitted through a material within a defined wavelength range. As used herein, "average reflectivity" refers to the average amount of incident light power reflected by a material.
[0077] As used herein, "light reflectance" simulates the response of the human eye by weighting the reflectance or transmittance and the wavelength spectrum according to the sensitivity of the human eye. Light reflectance can also be defined as the brightness or tristimulus Y value of the reflected light according to known conventions such as the CIE color space convention. As used herein, the "average light reflectance" in the wavelength range of 380nm to 720nm is defined in the following equation as the spectral reflectance R(λ) multiplied by the light source spectrum I(λ) and the CIE color matching function is related to the spectral response of the eye and is given by equation (1):
[0078]
[0079] In addition, "average reflectivity" can be determined in accordance with measurement principles understood by those skilled in the art over the visible spectrum or in other wavelength ranges, for example, in the infrared spectrum from 840 nm to 950 nm, etc. Unless otherwise specified, all reflectivity values reported or otherwise referenced in the present invention are associated with tests through the outer layered film of the cover article and away from the major surface of the substrate on which the outer layered film is disposed, for example, "first surface" average light reflectivity, "first surface" average reflectivity in a specified wavelength range, etc.
[0080] The usability of a camera system in an electronic device and / or the usability of a cover product (e.g., as a protective cover) may be related to the total amount of reflectivity in the camera system. Light reflectivity is particularly important for visible light camera systems and display devices that employ visible light. Lower reflectivity of a cover product over a camera system or camera lens or display may reduce multiple bounce reflections in the system that may produce "ghost images." Therefore, reflectivity is important for image quality in camera systems and devices that employ cover products. In addition, low reflectivity displays may enable better readability, reduce eye fatigue, and speed up user response time. Low reflectivity displays may also allow for reduced display energy consumption, increasing device battery life, because the display brightness of a low reflectivity display may be reduced compared to a standard display while still maintaining a target level of display readability in bright environments.
[0081] As used herein, "light transmittance" is defined as the spectral transmittance T(λ) multiplied by the light source spectrum I(λ) and the CIE color matching function in the following equation: is related to the spectral response of the eye and is given by equation (2):
[0082]
[0083] In addition, the "average transmittance" can be determined in the visible spectrum or other wavelength ranges according to measurement principles understood by those skilled in the art, for example, in the infrared spectrum from 840nm to 950nm, etc. Unless otherwise specified, all transmittance values reported or otherwise referenced in this disclosure are relative to the transmittance through the major surfaces of both the substrate and the outer layer film of the cover article (e.g., substrate 110, major surfaces 112, 114 and outer layer film 120, such as Figures 1 to 1F and described below), for example, "dual-surface" average light transmittance, "dual-surface" average transmittance within a specified wavelength range, etc.
[0084] As used herein, "transmitted color" and "reflected color" refer to the color transmitted or reflected through the cover product of the present invention in terms of color in the CIE L*, a*, b* colorimetric system under a D65 illuminant. More specifically, "transmitted color" and "reflected color" are given by √(a*2+b*2) because these color coordinates are obtained by transmitting a D65 illuminant through a major surface of the substrate of the cover product (e.g., substrate 110, major surfaces 112, 114, and outer layered film 120, such as the substrate 110, major surfaces 112, 114, and outer layered film 120, such as the substrate 110, major surfaces 112, 114, and outer layered film 120) over a range of incident angles (e.g., 0 to 10 degrees, 0 to 45 degrees, 0 to 90 degrees, etc.). Figures 1 to 1F Measured by transmission or reflection of a material (as shown in and described below).
[0085] Generally speaking, the present invention is directed to a method of using a chemically strengthened glass substrate (e.g., The present invention relates to a cover article having an outer layered film on a glass-ceramic substrate (e.g., an infrared product) or a glass-ceramic substrate. These cover articles have high hardness and scratch resistance, as well as low optical reflectivity, especially in the infrared spectrum. The outer layered film of the cover article is an engineered multilayer film structure, and the cover article of the present invention reflects a new system-level design configured for camera lens, sensor and / or light source protection glass. Scratches and reflections are both detrimental to camera, sensor and light source performance, resulting in signal loss, image distortion and related artifacts. However, as the number of cameras, sensors and light sources in electronic devices increases, and the demand for imaging and sensing continues to grow, especially for sensors operating in the infrared spectrum, the demand for protective cover articles with optimized scratch resistance and damage resistance and optical transmission over a wide spectrum also continues to grow. The cover article of the present invention utilizes a new outer layered film and system-level design to address these developing needs.
[0086] The cover products of the present invention can be used for camera lens, sensor and light source protection, as well as protection of other components (e.g., buttons, speakers, microphones, etc.). These cover products can also be used as covers for displays, camera lenses, sensors and / or light source components or other parts of electronic devices in electronic devices. These cover products use an outer layered film that exhibits a combination of high hardness and / or damage resistance, as well as desired optical properties, including high light transmittance and infrared transmittance. The cover products include a scratch-resistant layer in the outer layered film. In addition, the outer layered films of these products include a plurality of alternating high refractive index layers and low refractive index layers. In addition, each high refractive index layer comprises a nitride or an oxynitride, and each low refractive index layer may comprise an oxide. According to some embodiments, the outer layered film may be configured with a high RI layer and a scratch-resistant layer (e.g., SiO x N y or SiN y ) in contact with at least one middle RI layer (e.g., SiO x N y), and / or low RI layers in the outer structure (e.g., SiO 2 or SiO x N y ) is limited to about 75 nm or less.
[0087] Aspects of the cover articles of the present invention include outer layered films (e.g., hard optical coatings) on chemically strengthened glass or glass ceramic substrates that are optimized to give a desired combination of hardness, reflectivity, color, and color shift over a range of viewing angles. These outer layered films are intended to improve the scratch resistance and optical performance (lower reflectivity and / or higher transmittance) of chemically strengthened glass or glass ceramic substrates on which they are disposed. These outer layered films target low reflectivity and color shift in the visible range. Notably, the cover articles of the present invention exhibit controlled, lower levels of reflectivity and higher levels of transmittance at infrared wavelengths in the broad band of about 800-1700 nm, particularly 1000-1700 nm.
[0088] Aspects of the cover articles of the present invention have the following combinations: 1) high hardness; 2) low visible light reflectance; 3) controlled reflective color; 4) low infrared reflectance and high infrared transmittance over infrared wavelengths of 800-1700 nm; and 5) low reflectance (e.g., less than 1.5% light average at near normal incidence) and well controlled color over a wide viewing angle range (e.g., first surface reflected color is -8 to +3 in b* and -4 to +4 in a* at all viewing angles from 0 degrees to 90 degrees).
[0089] Additional aspects of the invention include devices and systems incorporating the cover articles of the invention as protective cover glasses, cover lenses, or cover windows. These devices and systems may include, for example, smart watches, smart phones, camera modules (which may be on smart phones), smart glasses (e.g., AR / VR glasses), glass screen protectors with adhesive backing placed over the smart phone cover glass, and LIDAR sensing systems for distance sensing in cameras or motor vehicles. These devices or systems may further include one or more semiconductor optical emitters or detectors made of materials including elements or compounds such as silicon, gallium arsenide (GaAs), germanium, indium phosphide (InP), InGaAs, GaInAsP, AlGaInAs, (Ga)InAs+ quantum dots, GaInNAs (Sb), erbium, ytterbium, and neodymium yttrium aluminum garnet. These systems may further include display modules such as LCD or OLED displays. Furthermore, in the implementation of a glass screen protector for a smartphone, the screen protector includes a cover glass and an adhesive backing disposed on the cover glass, wherein at least a portion of the cover glass includes the cover article of the present invention, and the adhesive backing is used to attach to the smartphone (e.g., to the display of the smartphone). More generally, the cover article of the present invention can be manufactured or configured in a device or system so that the cover article acts as a protective window covering more than one of the components mentioned herein, for example, covering a combination of components such as: a) a display plus a camera plus an IR sensor; b) a camera plus an IR sensor; and c) multiple cameras and multiple IR sensors.
[0090] With respect to mechanical properties, the cover articles of the present invention may exhibit a maximum hardness of 8 GPa or greater, 10 GPa or greater, or 12 GPa or greater (even greater than 14 GPa in some cases), as measured by the Berkovich hardness test in an indentation depth range of 100 nm to about 500 nm in the outer layered film. The glass-ceramic substrates employed in these articles may have an elastic modulus greater than 85 GPa, or greater than 95 GPa in some cases. These substrates may also exhibit a fracture toughness greater than 0.8 MPa·√m, or greater than 1 MPa·√m in some cases.
[0091] According to some embodiments of the lid products of the present invention (e.g., lid product 100 described in detail below), favorable product-level failure stress levels can be achieved by controlling the composition, configuration and / or treatment of the outer layer film used in the lid product. Notably, the composition, configuration and / or treatment of the outer layer film can be adjusted to obtain a residual compressive stress level of at least 700 MPa (e.g., 700 to 1100 MPa) and an elastic modulus of at least 140 GPa (e.g., 140 to 170 GPa, or 140 to 180 GPa). The mechanical properties of these outer layer films are unexpectedly associated with an average failure stress level of 700 MPa or greater (or an average failure stress level of 800 MPa or greater) in lid products using these outer layer films, as measured in a ROR test in which the outer layer film of the product is placed under tension.
[0092] Reference will now be made in detail to various embodiments of the cover articles, examples of which are illustrated in the accompanying drawings. Figure 1 According to one or more embodiments disclosed herein, the cover article 100 may include a substrate 110 and an outer layer film 120 disposed on the substrate. The substrate 110 may include opposing major surfaces 112, 114. The outer layer film 120 may be disposed on the substrate. Figure 1 100; however, in addition to or instead of being disposed on the outer major surface 112, the outer layered film 120 can also be disposed on the inner major surface 114 of the substrate 110. The outer layered film 120 forms an outermost surface 122. In addition, the outer layered film 120 can include an anti-scratch layer 150. In some implementations, the outer layered film 120 can include an anti-reflective region 130 above the anti-scratch layer 150. In some embodiments, the outer layered film 120 further includes an interference layer between the substrate 110 and the anti-scratch layer 150. In addition, the outermost surface 122 of the outer layered film 120 forms an air interface and generally defines the edge of the outer layered film 120 and the edge of the entire cover article 100. The substrate 110 can be substantially transparent, as described herein.
[0093] The outer layered film 120 includes at least one layer of at least one material. The term "layer" may include a single layer, or may include one or more sublayers. Such sublayers may be in direct contact with each other. The sublayers may be formed of the same material or two or more different materials. In one or more alternative embodiments, such sublayers may have an intermediate layer of different materials disposed therebetween. In one or more embodiments, the layer may include one or more continuous and uninterrupted layers and / or one or more discontinuous and discontinuous layers (i.e., layers of different materials formed adjacent to each other). One or more sublayers may be formed by any known method in the art, including discrete deposition or continuous deposition processes. In one or more embodiments, the layer may be formed using only a continuous deposition process, or alternatively, only a discrete deposition process.
[0094] In one or more embodiments, a single layer or multiple layers of the outer layer film 120 may be deposited onto the substrate 110 by a vacuum deposition technique such as, for example, chemical vapor deposition (e.g., plasma enhanced chemical vapor deposition (PECVD), low pressure chemical vapor deposition, atmospheric pressure chemical vapor deposition, and plasma enhanced atmospheric pressure chemical vapor deposition), physical vapor deposition (e.g., reactive or non-reactive sputtering or laser ablation), thermal evaporation or e-beam evaporation and / or atomic layer deposition. Liquid-based methods such as spraying, dipping, spin coating, or slot coating (e.g., using sol-gel materials) may also be used. In general, vapor deposition techniques may include a variety of vacuum deposition methods that may be used to produce thin films. For example, physical vapor deposition uses a physical process (such as heating or sputtering) to generate a vapor of a material that is then deposited on a coated article. Preferred methods for making the outer layer film 120 may include reactive sputtering, metal mode reactive sputtering, and PECVD processes.
[0095] The thickness of the outer layer film 120 may be about 0.10 μm or more, or about 0.25 μm or more. In some examples, the thickness of the outer layer film 120 may be in the range of about 0.10 μm to about 20 μm, about 0.10 μm to about 10 μm, about 0.25 μm to about 20 μm, about 0.25 μm to about 15 μm, about 0.25 μm to about 10 μm, about 0.25 μm to about 5 μm, about 0.5 μm to about 10 μm, about 0.5 μm to about 5 μm, about 0.5 μm to about 4 μm, and all thickness values of the outer layer film 120 between these thickness values. For example, the thickness of the outer layer film 120 may be approximately 0.25μm, 0.3μm, 0.4μm, 0.5μm, 0.6μm, 0.7μm, 0.8μm, 0.9μm, 1μm, 1.25μm, 1.5μm, 1.75μm, 2μm, 3μm, 4μm, 5μm, 6μm, 7μm, 8μm, 9μm, 10μm, 12μm, 14μm, 16μm, 18μm, 20μm, and all thickness values between these thicknesses.
[0096] Also like Figure 1 As shown in , the outer layered film 120 includes a plurality of layers (130A, 130B). In one or more embodiments, the outer layered film 120 may include a period 132 comprising two or more layers. In one or more embodiments, the two or more layers are characterized by having different refractive indices from each other. In one embodiment, the period 132 includes a first low RI layer 130A and a second high RI layer 130B. The difference in refractive index between the first low RI layer and the second high RI layer may be about 0.01 or greater, about 0.05 or greater, about 0.1 or greater, or even about 0.2 or greater.
[0097] In some embodiments, Figure 1 As shown in FIG. 1 , the outer layered film 120 is divided into an anti-reflection region 130 and an interference layer, and an anti-scratch layer 150 is disposed between these structures (described in further detail below). In these embodiments, the anti-reflection region 130 and the interference layer can have the same thickness or different thicknesses, and each includes one or more layers. In other embodiments (not shown), the outer layered film 120 includes an optical interference layer below the anti-scratch layer 150, and there is no optical interference layer that can interact with the anti-reflection region 130 (see FIG. 1 ). Figure 1 ) equivalent structure.
[0098] like Figure 1 (and the following Figures 1A to 1F ) and summarized above, the cover article 100 of the present invention may include an outer layered film 120 having one or more of an anti-reflective region 130 and an interference layer. Each of the anti-reflective region 130 and the interference layer (between the anti-scratch layer 150 and the substrate 110) includes a plurality of alternating low refractive index (RI) layers 130A and high refractive index layers 130B, respectively. According to an embodiment, each of the anti-reflective region 130 and the interference layer includes a period 132 of two or more layers, such as a low RI layer 130A and a high RI layer 130B, or a low RI layer 130A, a high RI layer 130B, and a low RI layer 130A. In addition, each of the anti-reflective region 130 and the interference layer of the outer layered film 120 may include a plurality of periods 132, such as 1 to 30 periods, 1 to 25 periods, 1 to 20 periods, and all periods within the above ranges. Furthermore, the number of periods 132, the number of layers of anti-reflective regions 130 and interference layers, and / or the number of layers within a given period 132 may be different, or they may be the same. Furthermore, in some implementations, the total amount of the plurality of alternating low RI layers 130A and high RI layers 130B and the scratch resistant layer 150 may be in the range of 6 to 50 layers, 6 to 40 layers, 6 to 30 layers, 6 to 28 layers, 6 to 26 layers, 6 to 24 layers, 6 to 22 layers, 6 to 20 layers, 6 to 18 layers, 6 to 16 layers, and 6 to 14 layers, and all ranges and numbers of layers between the above values.
[0099] like Figure 1 , the outer layer film 120 may include a plurality of periods 132. A single period 132 may include a first low RI layer 130A and a second high RI layer 130B, such that when a plurality of periods 132 are provided, the first low RI layers 130A (designated "L" for illustration) and the second high RI layers 130B (designated "H" for illustration) alternate in the following layer sequence: L / H / L / H or H / L / H / L, such that the first low RI layers 130A and the second high RI layers 130B appear to alternate along the physical thickness of the outer layer film 120.
[0100] exist Figure 1 In the example cover article 100 in FIG. 1 , the anti-reflective coating region 130 includes five (5) periods 132 (three periods above the anti-scratch layer 150 and two periods below the anti-scratch layer 150). In some embodiments, the outer layered film 120 may include up to twenty-five (25) periods 132 (also referred to herein as "N" periods, where N is an integer). For example, the outer layered film 120 may include about 2 to about 20 periods 132, about 2 to about 15 periods 132, about 2 to about 12 periods 132, about 2 to about 10 periods 132, about 2 to about 12 periods 132, about 3 to about 8 periods 132, about 3 to about 6 periods 132, or any other period 132 within these ranges. For example, the outer layer film 120 may include 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17, 18, 19, 20, 21, 22, 23, 24, or 25 periods 132.
[0101] exist Figure 1 In the embodiment shown in , the outer layered film 120 may include an additional cap layer 131, which may include a material with a lower refractive index than the second high RI layer 130B. In an embodiment, one of the low refractive index layers of the outer layered film 120 is a cap layer 131.
[0102] As used herein, the terms "low RI" and "high RI" refer to the relative values of the refractive indices of layers 130A and 130B relative to each other (e.g., low RI < high RI). In one or more implementations, when used with a low RI layer 130A, the term "low RI" includes a range of about 1.3 to about 1.7 or 1.75. In one or more embodiments, when used with a high RI layer 130B, the term "high RI" includes a range of about 1.7 to about 2.6 (e.g., about 1.85 or greater). In one or more embodiments, when used with the optional third layer of period 132, the term "medium RI" includes a refractive index range of 1.55 to 1.80, 1.56 to 1.80, 1.6 to 1.75, and all refractive indices within these ranges. In some embodiments, the ranges of the low RI, medium RI, and / or high RI layers may overlap; however, in most cases, the layers of the outer layer film 120 have a general relationship with respect to RI: low RI < medium RI (where "medium RI" applies, for example, to the case of a three-layer period) < high RI. In one or more embodiments, the difference in refractive index of each of the low RI layer 130A (and / or cap layer 131) and the high RI layer 130B (and / or anti-scratch layer 150) may be about 0.01 or greater, about 0.05 or greater, about 0.1 or greater, or even about 0.2 or greater.
[0103] Suitable materials for the outer layer film 120 include: SiO 2 、Al2 O 3 ,GeO 2 、SiO、AlO x N y 、AlN、SiN x 、SiO x N y 、Si u Al v O x N y 、 2 O 5 , Nb 2 O 5 、TiO 2 、ZrO 2 、TiN、MgO、MgF 2 , BaF 2 , CaF 2 SnO 2 , HfO 2 , Y 2 O 3 、MoO 3 ,DyF 3 , YbF 3 , YF 3 , CeF 3 , polymers, fluoropolymers, plasma polymerized polymers, siloxane polymers, silsesquioxanes, polyimides, fluorinated polyimides, polyetherimides, polyethersulfones, polyphenylsulfones, polycarbonates, polyethylene terephthalate, polyethylene naphthalate, acrylic polymers, polyurethane polymers, polymethyl methacrylate, other materials listed below as suitable for the scratch resistant layer, and other materials known in the art. Some examples of materials suitable for the low RI layer 130A include SiO 2 、Al 2 O 3 ,GeO 2 、SiO、AlO x N y 、SiO x N y 、Si u Al v O x N y 、MgO、MgAl 2 O 4 MgF 2 , BaF 2 , CaF 2 ,DyF 3 , YbF 3 , YF 3 and CeF 3The nitrogen content of the material used for the first low RI layer can be minimized (e.g., in materials such as Al 2 O 3 MgAl 2 O 4 Some examples of materials suitable for the middle RI layer 130C include, but are not limited to, SiAl x O y N z 、AlO x N y 、SiO x N y , HfO 2 , Y 2 O 3 and Al 2 O 3 In the case where a material having a medium refractive index is required as the medium RI layer 130C, some embodiments may utilize SiO x N y , for example, having relatively low levels of nitrogen (eg, less than 3%). Some examples of materials suitable for the high RI layer 130B include Si u Al v O x N y 、 2 O 5 , Nb 2 O 5 、AlN、Si 3 N 4 、AlO x N y 、SiO x N y 、SiN x 、SiN x :Hy、HfO 2 、TiO 2 、ZrO 2 , Y 2 O 3 、Al 2 O 3 、MoO 3 According to some implementations, each high RI layer 130B in the outer layered film 120 includes a silicon-containing nitride or a silicon-containing oxynitride (e.g., Si 3 N 4 、SiN y or SiO x N y ). In one or more embodiments, each of the high RI layers 130B may have a high hardness (eg, a hardness greater than 8 GPa), and the high RI materials listed above may include high hardness and / or scratch resistance.
[0104] In an example, the high RI layer 130B may also be a high hardness layer or a scratch resistant layer (e.g., Figure 1 ), and the high RI materials listed above may also include high hardness or scratch resistance. In some implementations, the oxygen content of the materials used for the high RI layer 130B and / or the scratch resistant layer 150 may be minimized, especially in SiN x or AlN x In addition, the exemplary SiO x N y The high RI material may contain about 0 atomic % to about 20 atomic % oxygen, or about 5 atomic % to about 15 atomic % oxygen, and 30 atomic % to about 50 atomic % nitrogen. The above materials may be hydrogenated up to about 30% by weight. In the case where a medium refractive index material is required as a medium RI layer, some embodiments may utilize AlN and / or SiO x N y In other embodiments, each of the high RI layer 130B and / or the anti-scratch layer 150 comprises SiN x or SiO x N y In some embodiments, AlO x N y The material can be considered as oxygen-doped AlN x That is, these oxygen-doped AlN x The material may have AlN x The crystalline structure (eg, wurtzite) need not have an AlON crystalline structure. It should be understood that the scratch resistant layer 150 may include any of the materials disclosed as suitable for use in the high RI layer 130B.
[0105] The hardness of the high RI layer 130B and / or the anti-scratch layer 150 may be specifically characterized. In some embodiments, the maximum hardness of the high RI layer 130B and / or the anti-scratch layer 150 may be about 8 GPa or more, about 10 GPa or more, about 12 GPa or more, about 15 GPa or more, about 18 GPa or more, or about 20 GPa or more, as measured by the Berkovich indenter hardness test at an indentation depth of about 100 nm or more.
[0106] In some cases, the high RI layer 130B material may be deposited as a single layer and may be characterized as a scratch resistant layer (e.g., scratch resistant layer 150), and this single layer may have a thickness between about 200 nm and 10,000 nm for repeatable hardness determinations. In other embodiments where the high RI layer 130B is deposited as a single layer, this layer may have a thickness of about 200 nm to about 10,000 nm, about 200 nm to about 5,000 nm, about 500 nm to about 5,000 nm, about 1,000 nm to about 4,000 nm, about 1,500 nm to about 4,000 nm, about 1,500 nm to about 3,000 nm, and all thickness values between these thicknesses.
[0107] Reference again Figure 1C to Figure 1F In the cover product 100 shown in , according to some embodiments, each of the mid-RI layers 130C may have a hardness greater than 10 GPa (or greater than 15 GPa, or greater than 17 GPa) as measured by the Berkovich hardness test at an indentation depth of 125 nm. Without being bound by theory, the use of the mid-RI layer 130C helps to produce high hardness at shallow depths by two mechanisms: 1) reducing the amount of low RI, low hardness material in the outer structure 130a of the optical film structure 120 (e.g., minimizing the volume of the low RI layer 130A); and 2) including a relatively higher hardness mid-RI material employed in the mid-RI layer 130C compared to the low RI material of the low RI layer 130A replaced by the mid-RI material in the optical film structure 120. In general, the inventors have found that the hardness measured at an indentation depth of 125 nm correlates well with abrasion resistance and wear resistance in certain wear tests, particularly those that use lower loads and a large number of wear cycles to simulate repeated real-world wear events common to consumer electronic devices. About Figure 1C to Figure 1F For additional details and embodiments of the cover product shown in , please refer to the commonly assigned U.S. Provisional Application No. 63 / 337,846, filed on May 3, 2022, entitled "Transparent Glass-Ceramic Product with High Shallow Hardness and Display Device Having the Same," which is incorporated herein by reference in its entirety.
[0108] according to Figure 1 The embodiment of the cover article 100 shown in FIG. Figures 1A to 1F), each of the high RI layers 130B of the outer layer film 120 may have a physical thickness ranging from about 5 nm to 2000 nm, about 5 nm to 1500 nm, about 5 nm to 1000 nm, and all thicknesses and thickness ranges between these values. For example, each of the high RI layers 130B may have a physical thickness of 5 nm, 10 nm, 20 nm, 30 nm, 40 nm, 50 nm, 60 nm, 70 nm, 80 nm, 90 nm, 100 nm, 250 nm, 500 nm, 750 nm, 1000 nm, 1250 nm, 1500 nm, 1750 nm, 2000 nm, and all thickness values between these levels. In addition, each of the high RI layers 130B may have a physical thickness ranging from about 5 nm to 500 nm, about 5 nm to 400 nm, about 5 nm to 300 nm, and all thicknesses and thickness ranges between these values. As examples, each of these high RI layers 130B may have a physical thickness of 5 nm, 10 nm, 20 nm, 30 nm, 40 nm, 50 nm, 60 nm, 70 nm, 80 nm, 90 nm, 100 nm, 200 nm, 300 nm, 400 nm, 500 nm, and all thickness values between these levels.
[0109] In addition, according to Figure 1 (and the following Figures 1A to 1F ), each of the low RI layers 130A of the outer layer film 120 may have a physical thickness of about 5 nm to 300 nm, about 5 nm to 250 nm, about 5 nm to 200 nm, and all thicknesses and thickness ranges between these values. For example, each of these low RI layers 130A may have a physical thickness of 5 nm, 10 nm, 20 nm, 30 nm, 40 nm, 50 nm, 60 nm, 70 nm, 80 nm, 90 nm, 100 nm, 150 nm, 200 nm, 250 nm, 300 nm, and all thickness values between these levels.
[0110] according to Figure 1C to Figure 1F In the embodiment of the cover article 100 shown in , each of the mid RI layers 130C can have a physical thickness of about 5 nm to 300 nm, about 5 nm to 250 nm, about 5 nm to 200 nm, and all thicknesses and thickness ranges between these values. For example, each of these mid RI layers 130C can have a physical thickness of 5 nm, 10 nm, 20 nm, 30 nm, 40 nm, 50 nm, 60 nm, 70 nm, 80 nm, 90 nm, 100 nm, 150 nm, 200 nm, 250 nm, 300 nm, and all thickness values between these levels.
[0111] In one or more embodiments, at least one of the layers of the outer layered film 120 may include a specific optical thickness range. As used herein, the term "optical thickness" is determined by the product of the physical thickness (d) of the layer and the refractive index (n). In one or more embodiments, at least one of the layers of the outer layered film 120 may include an optical thickness ranging from about 2nm to about 200nm, from about 10nm to about 100nm, from about 15nm to about 100nm, from about 15 to about 500nm, or from about 15 to about 5000nm. In some embodiments, all of the layers of the outer layered film 120 may each have an optical thickness ranging from about 2nm to about 200nm, from about 10nm to about 100nm, from about 15nm to about 100nm, from about 15nm to about 500nm, or from about 15nm to about 5000nm. In some cases, at least one layer of the outer layered film 120 has an optical thickness of about 50nm or greater. In some cases, each of the low RI layer 130A and / or the medium RI layer 130C has an optical thickness ranging from about 2 nm to about 200 nm, about 10 nm to about 100 nm, about 15 nm to about 100 nm, about 15 nm to about 500 nm, or about 15 nm to about 5000 nm. In other cases, each of the high RI layers 130B has an optical thickness ranging from about 2 nm to about 200 nm, about 10 nm to about 100 nm, about 15 nm to about 100 nm, about 15 nm to about 500 nm, or about 15 nm to about 5000 nm. In some embodiments, the anti-scratch layer 150 is the thickest layer in the outer layered film 120 and / or has a refractive index higher than the refractive index of any other layer in the film structure.
[0112] In some embodiments, the topmost air-side layer of the outer layer film 120 may include a high RI layer 130B (not shown) that also exhibits high hardness. In some embodiments, an additional coating (not shown) may be disposed on top of this topmost air-side high RI layer 130B or cap layer 131 (e.g., the additional coating may include a low friction coating, an oil repellent coating, or an easy-to-clean coating). When added to the topmost air-side layer including the high RI layer 130B, the addition of a low RI layer 130A and / or cap layer 131 having a very low thickness (e.g., about 10 nm or less, about 5 nm or less, or about 2 nm or less) has minimal impact on optical performance. The low RI layer 130A having a very low thickness may include SiO 2 , oil repellent or low friction layer or SiO 2 Combination with oil repellent material. Exemplary low friction layers may include diamond-like carbon. Such materials (or one or more layers of the outer layered film 120) may exhibit a coefficient of friction of less than 0.4, less than 0.3, less than 0.2, or even less than 0.1.
[0113] In one or more embodiments, the combined physical thickness of the high RI layers 130B may be characterized. For example, in some embodiments, the combined thickness of the high RI layers 130B may be about 100 nm or more, about 150 nm or more, about 200 nm or more, about 250 nm or more, about 300 nm or more, about 350 nm or more, about 400 nm or more, about 450 nm or more, about 500 nm or more, about 550 nm or more, about 600 nm or more, about 650 nm or more, about 700 nm or more, about 750 nm or more, about 800 nm or more, about 850 nm or more, about 900 nm or more, about 950 nm or more, or even about 1000 nm or more. The combined thickness is the calculated combination of the thicknesses of the individual high RI layers 130B in the outer layered film 120, even when there is an intervening low RI layer 130A or other layers. In some embodiments, the combined physical thickness of the high RI layer 130B, which may also include a high hardness material (e.g., a nitride or oxynitride material), may be greater than 30% of the total physical thickness of the outer layer film 120. For example, the combined physical thickness of the high RI layer 130B may be about 25% or more, 30% or more, 35% or more, 40% or more, about 50% or more, or even about 60% or more of the total physical thickness of the outer layer film 120.
[0114] The cover article 100 may include one or more additional coatings disposed on the outer layered film 120. In one or more embodiments, the additional coating may include an easy-to-clean coating. Examples of suitable easy-to-clean coatings are described in U.S. Patent Application No. 13 / 690,904, entitled "Methods for Making Glass Articles with Optical and Easy-to-Clean Coatings," filed on November 30, 2012 and published on April 24, 2014 as U.S. Patent Application Publication No. 2014 / 0113083, the core portion of which is incorporated herein by reference in its entirety. The easy-to-clean coating may have a thickness ranging from about 5 nm to about 50 nm and may include known materials, such as fluorinated silanes. The easy-to-clean coating may alternatively or additionally include a low-friction coating or surface treatment. Exemplary low-friction coating materials may include diamond-like carbon, silanes (e.g., fluorosilanes), phosphonates, olefins, and alkynes. In some embodiments, the easy-to-clean coating may have a thickness ranging from about 1 nm to about 40 nm, about 1 nm to about 30 nm, about 1 nm to about 25 nm, about 1 nm to about 20 nm, about 1 nm to about 15 nm, about 1 nm to about 10 nm, about 5 nm to about 50 nm, about 10 nm to about 50 nm, about 15 nm to about 50 nm, about 7 nm to about 20 nm, about 7 nm to about 15 nm, about 7 nm to about 12 nm, or about 7 nm to about 10 nm, and all ranges and sub-ranges therebetween.
[0115] The additional coating may include one or more anti-scratch layers (e.g., having a composition similar to that of the anti-scratch layer 150). In some embodiments, the additional coating includes a combination of an easy-to-clean material and an anti-scratch material. In one example, the combination includes an easy-to-clean material and diamond-like carbon. Such additional coatings may have a thickness ranging from about 5 nm to about 20 nm. The components of the additional coating may be provided in separate layers. For example, diamond-like carbon may be provided as a first layer, and the easy-to-clean material may be provided as a second layer on the first layer of diamond-like carbon. The thickness of the first layer and the second layer may be within the range provided above for the additional coating. For example, the first layer of diamond-like carbon may have a thickness of about 1 nm to about 20 nm or about 4 nm to about 15 nm (or more specifically about 10 nm), and the second layer of the easy-to-clean material may have a thickness of about 1 nm to about 10 nm (or more specifically about 6 nm). The diamond-like coating may include tetrahedral amorphous carbon (Ta-C), Ta-C:H and / or aCH.
[0116] As described herein, the outer layer film 120 includes a scratch resistant layer 150, which may be disposed within the outer layer film 120 (eg, Figures 1 to 1B ), directly disposed on the substrate 110 (not shown) or at the outermost surface 122 (not shown) of the outer layer film 120. In some embodiments, as Figures 1 to 1B As shown in FIG. 1 , the anti-scratch layer 150 is disposed between the layers of the outer layered film 120, such that the anti-reflection region 130 is located above the anti-scratch layer 150, and another portion of the outer layered film 120 is below the layer 150 and above the substrate 110. In an embodiment, the portion of the outer layered film 120 below the layer 150 serves as an optical interference layer, which can be used to bridge the refractive index difference between the substrate 110 and the anti-scratch layer 150, and includes alternating high refractive index layers 130B and low refractive index layers 130A. The two portions of the outer layered film 120 (i.e., the first portion disposed between the anti-scratch layer 150 and the substrate 110, and the anti-reflection region 130 disposed on the anti-scratch layer 150) may have different thicknesses from each other, or may have substantially the same thickness as each other. The layers of the two portions of the outer layered film 120 may be the same in composition, order, thickness, and / or configuration, or may be different from each other. Furthermore, the layers of the two portions of the outer layered film 120 may contain the same number of periods 132 (N), or the number of periods 132 in each of these portions may be different from each other (see Figures 1 to 1B 132).
[0117] Exemplary materials used in the anti-scratch layer 150 (or the anti-scratch layer used as an additional coating as described above) may include inorganic carbides, nitrides, oxides, diamond-like materials, or combinations of these materials. Examples of materials suitable for use in the anti-scratch layer 150 include metal oxides, metal nitrides, metal oxynitrides, metal carbides, metal oxycarbides, and / or combinations thereof. Exemplary metals include B, Al, Si, Ti, V, Cr, Y, Zr, Nb, Mo, Sn, Hf, Ta, and W. Specific examples of materials that can be utilized in the anti-scratch layer 150 or coating may include Si u Al v O x N y 、 2 O 5 , Nb 2 O 5 、AlN、AlN x 、SiAl x N y 、AlN x / SiAl x N y 、Si 3 N 4 、AlO x N y 、SiO x N y 、SiN y 、SiN x :Hy、HfO 2 、TiO 2 、ZrO 2 , Y 2 O 3 、Al 2 O 3 、MoO 3 , diamond, diamond-like carbon, Si x C y 、Si x O y C z 、TiO x N y and combinations thereof. Examples of materials suitable for use in the anti-scratch layer 150 include metal oxides, metal nitrides, metal oxynitrides, metal carbides, metal oxycarbides, and / or combinations thereof. Exemplary metals include B, Al, Si, Ti, V, Cr, Y, Zr, Nb, Mo, Sn, Hf, Ta, and W. Specific examples of materials that may be utilized in the anti-scratch layer 150 may include Al 2 O 3 、AlN、AlO x N y 、Si 3 N 4、SiO x N y 、Si u Al v O x N y , diamond, diamond-like carbon, Si x C y 、Si x O y C z 、ZrO 2 、TiO x N y In some implementations, the anti-scratch layer 150 may include Si 3 N 4 、SiN y 、SiO x N y In an embodiment, each of the anti-scratch layers 150 employed in the cover article 100 exhibits a fracture toughness value greater than about 1 MPa√m while exhibiting a hardness value greater than about 10 GPa as measured by the Berkovich hardness test.
[0118] The scratch resistant layer 150 may also include a nanocomposite material, or a material with a controlled microstructure to improve hardness, toughness, or wear / abrasion resistance. For example, the scratch resistant layer 150 may include nanocrystals ranging in size from about 5 nm to about 30 nm. In an embodiment, the scratch resistant layer 150 may include conversion toughened zirconia, partially stabilized zirconia, or zirconia toughened alumina. In an embodiment, the scratch resistant layer 150 exhibits a fracture toughness value greater than about 1 MPa√m, while exhibiting a hardness value greater than about 8 GPa.
[0119] The anti-scratch layer 150 may include a single layer (e.g. Figures 1 to 1C ), or multiple sub-layers or a single layer exhibiting a refractive index gradient. In the case of using multiple layers, such layers form a scratch-resistant coating. For example, the scratch-resistant layer 150 may include Si u Al v O x N y A composition gradient of Si, Al, O, and N, wherein the concentration of any one or more of Si, Al, O, and N varies to increase or decrease the refractive index. Refractive index gradients can also be formed using porosity. Such gradients are more fully described in U.S. Patent Application No. 14 / 262,224, entitled “Scratch Resistant Articles Having Gradient Layers,” filed on April 25, 2014 and now published as U.S. Patent No. 9,703,011 on July 11, 2017, the core portion of which is incorporated herein by reference in its entirety.
[0120] In other embodiments, the anti-scratch layer 150 may include a single layer (eg, Figures 1 to 1C ), or a plurality of sub-layers or a single layer, exhibits a refractive index gradient, or exhibits a thick high hardness portion in addition to a refractive gradient portion. The gradient portion is characterized by a gradual change in the refractive index. For example, some or all of the refractive index transitions in the layer structure are characterized by an absolute (positive or negative) value of the refractive index "slope" of 0.1 / nm or less (meaning that the refractive index change per nm coating thickness is less than 0.1), 0.05 / nm or less (or less than about 0.5 per 10 nm), 0.02 / nm or less (or less than 0.2 per 10 nm), 0.016 / nm or less, 0.012 / nm or less, or even 0.01 / nm or less (less than about 0.1 per 10 nm). In some embodiments, the refractive index slope of the gradient portion is 0.001 or greater, 0.002 or greater, or 0.005 or greater. The refractive index gradient can be implemented as a continuous change in the refractive index, or as a series of small steps in the refractive index. For example, the refractive index slope discussed herein is measured and calculated over a refractive index interval of 0.04. In other words, the refractive index slope is 0.04 divided by the distance over which the refractive index changes by 0.04. This approach results in the distance between the refractive index steps being taken into account when calculating the refractive index slope for step sizes of 0.04 or less. In some embodiments, the refractive index interval for calculating the refractive index slope may be 0.02, 0.03, 0.04, 0.05, or 0.06. For example, the scratch resistant layer 150 may include Si u Al v O x N y A composition gradient of wherein the concentration of at least two of Si, Al, O, and N varies to increase or decrease the refractive index. The refractive index gradient may be a gradient selected from at least one of a porosity gradient, a density gradient, and an elastic modulus gradient. Such gradients are more fully described in U.S. Patent Application No. 16 / 643,339, filed on February 28, 2020, entitled “Hybrid Gradient Interference Hard Coating,” the contents of which are incorporated herein by reference in their entirety.
[0121] According to some embodiments, the anti-scratch layer 150 may have a thickness of about 200 nm to about 5000 nm. Figures 1 to 1CAs shown in exemplary form in the cover article 100 shown in , each of the scratch resistant layers 150 may be relatively thick, such as greater than or equal to about 50 nm, 60 nm, 70 nm, 75 nm, 80 nm, 90 nm, 100 nm, 150 nm, 200 nm, 250 nm, 300 nm, 325 nm, 350 nm, 375 nm, 400 nm, 425 nm, 450 nm, 475 nm, 500 nm, 525 nm, 550 nm, 575 nm, 600 nm, 700 nm, 800 nm, 900 nm, 1 micron, 2 microns, 3 microns, 4 microns, 5 microns, 6 microns, 7 microns, or even 8 microns, compared to other layers (e.g., low RI layer 130A, high RI layer 130B, cap layer 131, etc.). In some implementations, the scratch resistant layer 150 has a thickness of about 50 nm to about 10,000 nm, about 80 nm to about 10,000 nm, about 100 nm to about 10,000 nm, about 200 nm to about 10,000 nm, about 200 nm to about 7,500 nm, about 200 nm to about 5,000 nm, about 200 nm to about 3,000 nm, about 500 nm to about 5,000 nm, about 500 nm to about 3,000 nm, about 500 nm to about 2,500 nm, about 1,000 nm to about 4,000 nm, about 1,500 nm to about 4,000 nm, about 1,500 nm to about 3,000 nm, and all thickness values between these thicknesses. For example, the thickness of the scratch resistant layer 150 may be 200 nm, 300 nm, 400 nm, 500 nm, 600 nm, 700 nm, 800 nm, 900 nm, 1000 nm, 1100 nm, 1200 nm, 1300 nm, 1400 nm, 1500 nm, 1600 nm, 1700 nm, 1800 nm, 1900 nm, 2000 nm, 2100 nm, 2200 nm, 2300 nm, 2400 nm, 2500 nm, 2600 nm, 2700 nm, 2800 nm, 2900 nm, 3000 nm, 3500 nm, 4000 nm, 4500 nm, 5000 nm, 7500 nm, 10000 nm, and all thickness subranges and thickness values therebetween.
[0122] In an exemplary embodiment of the cover product 100 of the present invention, Figure 1As shown in , the outer layer film 120 may include an anti-scratch layer 150 of the same composition as the high RI layer 130B, and one or more low RI layers 130A and high RI layers 130B may be positioned above the anti-scratch layer 150, respectively and alternately, with an optional cap layer 131 positioned above the low RI layer 130A and the high RI layer 130B, wherein the cap layer 131 comprises a low RI material. In this configuration, the low RI layer 130A, the high RI layer 130B, and the cap layer 131 define the anti-reflective region 130. The anti-scratch layer 150 may be alternately defined as the thickest hard layer or the thickest high RI layer in the entire outer layer film 120 or in the entire cover product 100. Without being bound by theory, it is believed that when a relatively small amount of material is deposited above the anti-scratch layer 150, the cover product 100 may exhibit increased hardness at the indentation depth. However, including a low RI layer and a high RI layer above the anti-scratch layer 150 may enhance the optical properties of the cover product 100.
[0123] exist Figure 1 In some embodiments of the cover article 100, relatively few layers (e.g., only 1, 2, 3, 4, or 5 layers) may be positioned above the anti-scratch layer 150 in the anti-reflective region 130, and each of these layers may be relatively thin (e.g., less than 100 nm, less than 75 nm, less than 50 nm, or even less than 25 nm). In other embodiments, a greater number of layers (e.g., 3 to 15 layers) may be positioned above the anti-scratch layer 150 in the anti-reflective region 130, and each of these layers may also be relatively thin (e.g., less than 200 nm, less than 175 nm, less than 150 nm, less than 125 nm, less than 100 nm, less than 75 nm, less than 50 nm, or even less than 25 nm).
[0124] exist Figure 1 In one implementation of the embodiment of the cover article 100 shown in , the anti-reflective region 130 may include three (3) periods 132 and a cap layer 131 above the scratch resistant layer 150. In addition, there are two (2) periods 132 below the scratch resistant layer 150, and the additional low RI layer 130A below the scratch resistant layer 150 and the scratch resistant layer 150 itself constitute additional periods 132. Therefore, in this configuration, the outer layered film 120 has six periods 132 (i.e., N=6) and a cap layer 131. Figure 1 In another implementation of the embodiment shown in , the region of the outer layer film 120 below the anti-scratch layer 150 includes six periods 132 (as described in detail in Examples 1 and 3, discussed in detail below). Thus, the outer layer film 120 in this configuration has ten periods 132 (i.e., N=10). Figure 1In a further implementation of the embodiment shown in , the region of the outer layer film 120 beneath the anti-scratch layer 150 includes five (5) periods 132 (as described in detail in Examples 2 and 4, discussed in detail below). Thus, the outer layer film 120 in this configuration has nine periods 132 (i.e., N=9).
[0125] In another exemplary implementation of the cover product 100 of the present invention, Figure 1A As shown in , the anti-reflective region 130 may include one (1) period 132 and a cap layer 131 above the scratch resistant layer 150. In addition, there are two (2) periods 132 below the scratch resistant layer 150, and the additional low RI layer 130A below the scratch resistant layer 150 and the scratch resistant layer 150 itself constitute additional periods 132. Therefore, in this configuration, the outer layered film 120 has four periods 132 (i.e., N=4) and a cap layer 131.
[0126] In another exemplary implementation of the cover product 100 of the present invention, Figure 1B As shown in , the outer layer film 120 may include an anti-scratch layer 150 having the same composition as the high RI layer 130B, and one or more high RI layers 130B and low RI layers 130A may be positioned above the anti-scratch layer 150 respectively and alternately, and an optional cap layer 131 is positioned above the high RI layer 130B, wherein the cap layer 131 includes a low RI material. In this configuration, the low RI layer 130A, the high RI layer 130B and the cap layer 131 define the anti-reflection area 130. Figure 1B In the exemplary embodiment shown in , the anti-reflective region 130 may include four (4) periods 132 above the scratch resistant layer 150 (i.e., each period 132 is a high RI layer 130B and a low RI layer 130A or cap layer 131). In addition, there are two (2) periods 132 below the scratch resistant layer 150, and the additional low RI layer 130A below the scratch resistant layer 150 and the scratch resistant layer 150 itself constitute additional periods 132. Therefore, in this configuration, the outer layer film 120 has seven periods 132 (i.e., N=7). Figure 1B In another implementation of the embodiment shown in (as described in detail in Examples 5 and 6, discussed in detail below), the region of the outer layered film 120 below the scratch resistant layer 150 includes five (5) periods 132; the additional low RI layer 130A below the scratch resistant layer 150 and the scratch resistant layer 150 itself constitute additional periods 132; and the anti-reflective region 130 includes five (5) periods 132. Thus, in this configuration the outer layered film 120 has eleven periods 132 (i.e., N=11).
[0127] In another exemplary implementation of the cover product 100 of the present invention, Figure 1C to Figure 1FAs shown in FIG. 1 , the cover article 100 may include a substrate 110 and an outer layered film 120 defining an outer surface 120a and an inner surface 120b disposed on the substrate 110. The substrate 110 includes opposing major surfaces 112, 114 and opposing minor surfaces 116, 118. The outer layered film 120 is Figure 1C to Figure 1F , the inner surface 120b is disposed on the first opposing major surface 112, and the outer layered film is shown as being disposed on the second opposing major surface 114. However, in some embodiments, one or more of the outer layered films 120 may be disposed on the opposing second major surface 114 and / or on one or both of the opposing minor surfaces 116, 118. Figure 1C to Figure 1F As shown in and as summarized above, the cover article 100 of the present invention includes an outer layered film 120 having one or more of an outer structure 130a and an inner structure 130b. The outer layered film 120 includes a plurality of alternating low RI layers and high RI layers, 130A and 130B, respectively. In an embodiment, each or one of the outer structure 130a and the inner structure 130b includes a plurality of alternating low RI layers and high RI layers, 130A and 130B, respectively. In an embodiment, each or one of the outer structure 130a and the inner structure 130b includes a plurality of alternating medium RI layers and high RI layers, 130C and 130B, respectively. In some preferred implementations, the outer structure 130a includes at least one medium RI layer 130C in contact with one of the high RI layer 130B and the anti-scratch layer 150. In some preferred implementations, the outer structure 130a includes at least one outermost cap layer 131, such as Figure 1C to Figure 1F shown in exemplary form.
[0128] As an example, in Figure 1C to Figure 1F In the embodiment, the period 132 of the outer structure 130a or the inner structure 130b includes a low RI layer 130A and a high RI layer 130B or a medium RI layer 130C and a high RI layer 130B. When multiple periods are included in either or both of the outer structure 130a and the inner structure 130b, the low RI layer 130A (designated as "L"), the medium RI layer 130C (designated as "M"), and the high RI layer 130B (designated as "H") may be alternated in the following layer sequence: L / H / L / H..., H / L / H / L..., M / H / M / H..., H / M / H / M..., so that the low RI layer 130A and the high RI layer 130B or the medium RI layer 130C and the high RI layer 130B alternate along the physical thickness of the outer structure 130a and the inner structure 130b of the outer layered film 120. In a preferred implementation, as Figure 1C to Figure 1F As shown in , the period 132 in the outer structure 130a is configured as H / M / H / M... above the anti-scratch layer 150; and the period 132 in the inner structure 130b is configured as L / H / L / H... above the substrate 110 and below the anti-scratch layer 150.
[0129] In the implementation of the cover article 100, as Figure 1C As shown in , the number of periods 132 of the outer structure 130a and the inner structure 130b can be configured so that the outer structure 130a includes a total of six (6) alternating layers (e.g., alternating medium RI layers 130C and high RI layers 130B); and the inner structure 130b includes at least fifteen (15) layers (e.g., alternating low RI layers and high RI layers, 130A and 130B, respectively). In addition, in this implementation, the outer structure 130a of the outer layer film 120 includes a cap layer 131 (similar in structure and thickness to the low RI layer 130A) above the outer structure 130a; and an anti-scratch layer 150 between the outer structure 130a and the inner structure 130b.
[0130] In the implementation of the cover article 100, as Figure 1D As shown in , the number of periods 132 of the outer structure 130a and the inner structure 130b can be configured so that the outer structure 130a includes a total of ten (10) alternating layers (e.g., alternating medium RI layers 130C and high RI layers 130B); and the inner structure 130b includes at least fifteen (15) layers (e.g., alternating low RI layers and high RI layers, 130A and 130B, respectively). In addition, in this implementation, the outer structure 130a of the outer layer film 120 includes a cap layer 131 (similar in structure and thickness to the low RI layer 130A) above the outer structure 130a; and an anti-scratch layer 150 between the outer structure 130a and the inner structure 130b.
[0131] In the implementation of the cover article 100, as Figure 1E As shown in , the number of periods 132 of the outer structure 130a and the inner structure 130b can be configured so that the outer structure 130a includes a total of six (6) alternating layers (e.g., alternating medium RI layers and high RI layers, 130C and 130B, respectively) and an additional medium RI layer 130C repeated adjacent to another medium RI layer 130C; and the inner structure 130b includes at least fifteen (15) layers (e.g., alternating low RI layers and high RI layers, 130A and 130B, respectively). In addition, in this implementation, the outer structure 130a of the outer layered film 120 includes a cap layer 131 (similar in structure and thickness to the low RI layer 130A) above the outer structure 130a; and an anti-scratch layer 150 between the outer structure 130a and the inner structure 130b.
[0132] In the implementation of the cover article 100, as Figure 1FAs shown in , the number of periods 132 of the outer structure 130a and the inner structure 130b can be configured so that the outer structure 130a includes a total of four (4) alternating layers (e.g., alternating medium RI layers and high RI layers, 130C and 130B, respectively); and the inner structure 130b includes at least eleven (11) layers (e.g., alternating low RI layers and high RI layers, 130A and 130B, respectively). In addition, in this implementation, the outer structure 130a of the outer layer film 120 includes a cap layer 131 (similar in structure and thickness to the low RI layer 130A) above the outer structure 130a; and an anti-scratch layer 150 between the outer structure 130a and the inner structure 130b.
[0133] According to another embodiment of the cover article 100 of the present invention (not shown), the number of periods 132 of the interference layer below the anti-reflective zone 130 and the anti-scratch layer 150 can be configured so that the anti-reflective zone 130 includes at least two (2) layers (e.g., alternating low RI layers 130A and high RI layers 130B), and the interference layer includes at least seven (7) layers (e.g., two periods 132 of alternating low RI layers 130A and high RI layers 130B, and an additional period 132 of three (3) layers (alternating low RI layers 130A / high RI layers 130B / low RI layers 130A)). In addition, in this embodiment, the outer layered film 120 and the anti-reflective zone 130 include a cap layer 131 (similar in structure and thickness to the low RI layer 130A); and an anti-scratch layer 150 between the anti-reflective zone 130 and the interference layer.
[0134] according to Figures 1 to 1B In some embodiments of the cover article 100 shown in FIG. 1 , the outermost cap layer 131 of the outer layer film 120 may not be exposed, but may have a top coating (not shown) disposed thereon. Figure 1C to Figure 1F In some embodiments of the cover article 100 shown in FIG. 1 , the outermost cap layer 131 of the outer layered film 120 may not be exposed, but may have a top coating 140 disposed thereon. In some implementations of the cover article 100, each high RI layer 130B in the outer film layer 120 comprises a nitride, a silicon-containing nitride (e.g., SiN y 、Si 3 N 4 ), oxynitrides or silicon-containing oxynitrides (e.g., SiAl x O y N z or SiO x N y ). In addition, according to some embodiments, each low RI layer 130A in the outer layer film 120 includes an oxide or a silicon-containing oxide (eg, SiO doped with Al, N, or F). 2 、SiO x or SiO 2 ).
[0135] According to an embodiment of the cover product 100, Figures 1 to 1F As shown in exemplary form in FIG. 1 , the cover article can achieve a good combination of low reflectivity in the infrared spectrum or visible and infrared spectrum with high scratch resistance and / or hardness using certain structural features in the anti-reflective region 130 of the outer layer film 120. These structural features include a thickness greater than the typical thickness of the cap layer 131; a thickness less than the typical combined thickness of the low refractive index layers; and / or a specified thickness range of the anti-reflective region 130.
[0136] Therefore, if Figures 1 to 1F As shown in exemplary form in FIG. 1 , embodiments of the cover article 100 are configured such that the cap layer 131 has a thickness of at least 110 nm, 120 nm, 130 nm, 140 nm, or even 150 nm. In some embodiments of the cover article 100, the cap layer 131 has a thickness of about 110 nm to about 200 nm, about 110 nm to about 175 nm, or about 110 nm to about 150 nm. For example, the cap layer 131 may have a thickness of about 110 nm, 115 nm, 120 nm, 125 nm, 130 nm, 140 nm, 150 nm, 160 nm, 170 nm, 180 nm, 190 nm, 200 nm, and all thickness values between the above ranges and sub-ranges. Additionally or alternatively, the cover article 100 may be configured such that the low refractive index layers 130A of the anti-reflective zone 130 have a combined thickness of less than 295 nm, 285 nm, 275 nm, 250 nm, 240 nm, 230 nm, 220 nm, or 210 nm. In some embodiments, the combined thickness of the low RI layers 130A in the anti-reflective zone 130 may be in the range of about 200 nm to about 295 nm, about 200 nm to about 275 nm, or about 200 nm to about 250 nm, and all combined thickness values between the above ranges. Additionally or alternatively, the cover article 100 may be configured with an anti-reflective zone 130 having a thickness ranging from about 100 nm to about 525 nm, about 150 nm to about 525 nm, or about 200 nm to about 525 nm. In some embodiments of the cover article 100, the thickness of the anti-reflective region 130 may be approximately 100 nm, 125 nm, 150 nm, 175 nm, 200 nm, 225 nm, 250 nm, 275 nm, 300 nm, 325 nm, 350 nm, 375 nm, 400 nm, 425 nm, 450 nm, 475 nm, 500 nm, 525 nm, and all thickness values between the above ranges and sub-ranges.
[0137] The outer layer film 120 and / or the cover article 100 can be described in terms of hardness as measured by the Berkovich indenter hardness test. As previously described, the Berkovich indenter hardness test involves pressing a diamond Berkovich indenter into the outermost surface 122 of the cover article 100 (see Figures 1 to 1F ) or the surface of any one or more of the layers in the outer layered film 120 to form an indentation with an indentation depth in the range of about 50 nm to about 1000 nm (or the entire thickness of the outer layered film 120 or its layers, whichever is smaller), and measuring the maximum hardness from this indentation along the entire indentation depth range or a section of this indentation depth (e.g., in the range of about 100 nm to about 600 nm, for example, at an indentation depth of 100 nm or greater, etc.).
[0138] In some embodiments, the cover article 100 (e.g., as shown in FIG. 1 ) has a hardness of 0.0407 W when measured at the outermost surface 122 by the Berkovich indenter hardness test at an indentation depth of about 100 nm to about 500 nm or at an indentation depth of about 100 nm to 900 nm. Figures 1 to 1F ) may exhibit a maximum hardness of about 8 GPa or greater, about 10 GPa or greater, about 11 GPa or greater, about 12 GPa or greater, about 13 GPa or greater, about 14 GPa or greater, about 16 GPa or greater, about 18 GPa or greater, or even about 20 GPa or greater. The hardness of the cover article 100 may even be as high as about 20 GPa or 30 GPa. Such measured hardness values may be exhibited by the outer layer film 120 and / or the cover article 100 along an indentation depth of about 50 nm or greater, or about 100 nm or greater (e.g., about 50 nm to about 300 nm, about 50 nm to about 400 nm, about 50 nm to about 500 nm, about 50 nm to about 600 nm, about 100 nm to about 300 nm, about 100 nm to about 400 nm, about 100 nm to about 500 nm, about 100 nm to about 600 nm, about 200 nm to about 300 nm, about 200 nm to about 400 nm, about 200 nm to about 500 nm, or about 200 nm to about 600 nm). Such hardness values may also be measured from the outermost surface 122 of the outer layer film 120 to a depth of 200 nm. In one or more embodiments, the cover article 100 exhibits a hardness greater than the hardness of the substrate 110 (which may be measured on a surface opposite the outermost surface 122).
[0139] According to some embodiments of the cover article 100, the cover article 100 may exhibit a maximum hardness of 8 GPa, 9 GPa, 10 GPa, 11 GPa, 12 GPa, 13 GPa, 14 GPa, 15 GPa, 16 GPa, 17 GPa, 18 GPa, 19 GPa, 20 GPa, or more, as measured by a Berkovich indenter hardness test at an indentation depth of about 100 nm to about 500 nm from the outermost surface 122 of the outer layered film 120. In some implementations, the maximum hardness of the cover article 100 at an indentation depth of 100 nm is greater than 8 GPa, 9 GPa, 10 GPa, 11 GPa, 12 GPa, 13 GPa, 14 GPa, 15 GPa, 16 GPa, 17 GPa, 18 GPa, or 19 GPa. In some implementations, the maximum hardness of the cover article 100 at an indentation depth of 500 nm is greater than 8 GPa, 9 GPa, 10 GPa, 11 GPa, 12 GPa, 13 GPa, 14 GPa, 16 GPa, 17 GPa, 18 GPa, or 19 GPa. In addition, according to some implementations, the cover article 100 may exhibit a maximum hardness of about 8 GPa or more, 10 GPa or more, about 12 GPa or more, or about 14 GPa or more, 15 GPa or more, 16 GPa or more, 17 GPa or more, or even 18 GPa or more, as measured from the outermost surface 122 of the outer layered film 120 by the Berkovich indenter hardness test over an indentation depth range of about 100 nm to 500 nm, about 100 nm to about 900 nm, or about 200 nm to about 900 nm.
[0140] Further with respect to the residual compressive stress and elastic modulus level (and hardness level) of the outer layer film 120, these properties may be controlled by adjusting the stoichiometry and / or thickness of the low RI layer 130A, the high RI layer 130B, the cap layer 131, and the anti-scratch layer 150. In embodiments, the residual compressive stress (e.g., greater than or equal to 700 MPa, 700 MPa to 1100 MPa, etc.) and elastic modulus level (e.g., greater than 140 GPa, 140 GPa to 200 GPa, 140 GPa to 180 GPa, etc.) (and hardness level) exhibited by the outer layer film 120 may be controlled by adjusting the processing conditions used to sputter the layers of the outer layer film 120, particularly the high RI layer 130B and the anti-scratch layer 150 thereof. In some implementations, for example, a reactive sputtering process may be employed to deposit the high RI layer 130B comprising a silicon-containing nitride or a silicon-containing oxynitride. Furthermore, these high RI layers 130B can be deposited by applying power to a silicon sputtering target in a reactive gas environment containing argon (e.g., at a flow rate of 50 to 150 sccm), nitrogen (e.g., at a flow rate of 200 to 250 sccm), and oxygen, wherein the residual compressive stress and elastic modulus levels are largely determined by the selected oxygen flow rate. For example, based on the aforementioned argon and nitrogen flow conditions, a relatively low oxygen flow rate (e.g., 45 sccm) can be used to produce a SiO x N y The stoichiometric high RI layer 130B makes the outer layer film 120 exhibit a residual compressive stress of about 942 MPa, a hardness of 17.8 GPa, and an elastic modulus of 162.6 GPa. As another example, according to the aforementioned argon and nitrogen flow conditions, a relatively high oxygen flow rate (e.g., 65 sccm) can be used to produce a SiO x N y The stoichiometric high RI layer 130B causes the outer layer film 120 to exhibit a residual compressive stress of about 913 MPa, a hardness of 16.4 GPa, and an elastic modulus of 148.4 GPa. Therefore, the stoichiometry of the outer layer film 120, particularly the high RI layer 130B and the anti-scratch layer 150 thereof, can be controlled to achieve target residual compressive stress and elastic modulus levels, which unexpectedly correlate to a favorable high average failure stress level (e.g., greater than or equal to 700 MPa) in the cover article 100.
[0141] According to an embodiment of the cover product 100 of the present invention, Figures 1 to 1FAs shown in exemplary form in FIG. 1 , the cover article 100 exhibits a first surface average light reflectance of less than 2% at a near normal angle of incidence of 8°. In embodiments, the cover article 100 may exhibit a first surface average light reflectance of less than 2%, less than 1.75%, less than 1.5%, less than 1.25%, or even less than 1.2% at a near normal angle of incidence of 8°. For example, the cover article 100 may exhibit a first surface average light reflectance of 1.9%, 1.8%, 1.7%, 1.6%, 1.5%, 1.4%, 1.3%, 1.2%, 1.1%, 1.0%, 0.9%, 0.8%, 0.7%, 0.6%, 0.5%, 0.4%, 0.3% at a near normal angle of incidence of 8°, and all reflectance values between the above ranges and sub-ranges.
[0142] According to an embodiment of the cover product 100 of the present invention, Figures 1 to 1F As shown in exemplary form in FIG. 1 , the cover article 100 exhibits a first surface average reflectivity of less than 10% for infrared wavelengths of 1000 to 1700 nm (or for visible wavelengths of 420 nm to 1000 nm, and these infrared wavelengths) at an incident angle of 8° to 40°, or 8° to 60°. In embodiments, the cover article 100 may exhibit a first surface average reflectivity of less than 10%, less than 8%, less than 6%, less than 5%, or even less than 4.5% for infrared wavelengths of 1000 to 1700 nm (or for visible wavelengths of 420 nm to 1000 nm, and these infrared wavelengths) at an incident angle of 8° to 40°, or 8° to 60°. For example, the cover article 100 may exhibit a first surface average reflectivity of 9%, 8%, 7%, 6%, 5%, 4.5%, 4%, 3.5%, 3%, 2.5%, 2%, 1%, 0.5% at an infrared wavelength of 1000 to 1700 nm (or at a visible wavelength of 420 nm to 1000 nm, as well as these infrared wavelengths) at an incident angle of 8° to 40°, or 8° to 60°, and all reflectivity values between the above ranges and sub-ranges.
[0143] According to an embodiment of the cover product 100 of the present invention, Figures 1 to 1FAs shown in the exemplary form in FIG. 1 , the cover article 100 exhibits a first surface average reflectivity of less than 15% for infrared wavelengths of 1000 to 1700 nm at an incident angle of 60°. In embodiments, the cover article 100 may exhibit a first surface average reflectivity of less than 15%, less than 12%, less than 10%, or even less than 9% for infrared wavelengths of 1000 to 1700 nm at an incident angle of 60°. For example, the cover article 100 may exhibit a first surface average reflectivity of 14%, 13%, 12%, 11%, 10%, 9%, 8%, 7%, 6%, 5%, 2.5% for infrared wavelengths of 1000 to 1700 nm at an incident angle of 60°, and all reflectivity values between the above ranges and sub-ranges.
[0144] According to an embodiment of the cover product 100 of the present invention, Figures 1 to 1F As shown in exemplary form in FIG. 1 , the cover article 100 exhibits a first surface maximum reflectivity of less than 15% for infrared wavelengths of 1000 to 1700 nm at a near normal angle of incidence of 8°. In embodiments, the cover article 100 may exhibit a first surface maximum reflectivity of less than 15%, less than 10%, less than 8%, less than 6%, or even less than 5% for infrared wavelengths of 1000 to 1700 nm at a near normal angle of incidence of 8°. For example, the cover article 100 may exhibit a first surface maximum reflectivity of 14%, 13%, 12%, 11%, 10%, 9%, 8%, 7%, 6%, 5%, 4%, 3%, 2.5%, 2% for infrared wavelengths of 1000 to 1700 nm at a near normal angle of incidence of 8°, and all maximum reflectivity values between the above ranges and sub-ranges.
[0145] According to an embodiment of the cover product 100 of the present invention, Figures 1 to 1F As shown in exemplary form in FIG. 1 , the cover article 100 exhibits a dual-surface average light transmittance of greater than 94% at a near-normal angle of incidence of 8°. In embodiments, the cover article 100 may exhibit a dual-surface average light transmittance of greater than 94%, greater than 94.5%, or even greater than 95% at a near-normal angle of incidence of 8° (recognizing that the maximum achievable value is about 96% due to the effect of the uncoated surface of the substrate 110). For example, the cover article 100 may exhibit a dual-surface average light transmittance of approximately 94%, 94.25%, 94.5%, 94.75%, 95%, 95.25%, 95.5%, 95.75%, 96% at a near-normal angle of incidence of 8°, and all transmittance values between the above ranges and sub-ranges.
[0146] According to an embodiment of the cover product 100 of the present invention, Figures 1 to 1FAs shown in exemplary form in FIG. 1 , the cover article 100 exhibits a dual-surface average transmittance of greater than 85% for infrared wavelengths of 1000 to 1700 nm at an incident angle of 0° to 30°, or 0° to 40°. In embodiments, the cover article 100 may exhibit a dual-surface average transmittance of greater than 85%, greater than 88%, greater than 90%, greater than 91%, or even greater than 92% for infrared wavelengths of 1000 to 1700 nm at an incident angle of 0° to 30°, or 0° to 40°. For example, the cover article 100 may exhibit a dual-surface average transmittance of about 85%, 86%, 87%, 88%, 89%, 90%, 91%, 92%, 93%, 94%, 95% for infrared wavelengths of 1000 to 1700 nm at an incident angle of 0° to 30°, or 0° to 40°, and all transmittance values between the above ranges and sub-ranges.
[0147] According to an embodiment of the cover product 100 of the present invention, Figures 1 to 1F As shown in exemplary form in FIG. 1 , the cover article 100 exhibits a dual-surface average transmittance of greater than 75% for infrared wavelengths of 1000 to 1700 nm at an incident angle of about 60°. In embodiments, the cover article 100 may exhibit a dual-surface average transmittance of greater than 75%, greater than 80%, greater than 81%, greater than 82%, or even greater than 83% for infrared wavelengths of 1000 to 1700 nm at an incident angle of about 60°. For example, the cover article 100 may exhibit a dual-surface average transmittance of about 75%, 76%, 77%, 78%, 79%, 80%, 81%, 82%, 83%, 84%, 85% for infrared wavelengths of 1000 to 1700 nm at an incident angle of about 60°, and all transmittance values between the above ranges and sub-ranges.
[0148] According to an embodiment of the cover product 100 of the present invention, Figures 1 to 1F As shown in exemplary form in FIG. 1 , the cover article 100 exhibits a dual surface minimum transmittance of greater than 80% for infrared wavelengths of 1000 to 1700 nm at a normal angle of incidence of about 0°. In embodiments, the cover article 100 may exhibit a dual surface minimum transmittance of greater than 80%, greater than 85%, greater than 88%, greater than 90%, or even greater than 91% for infrared wavelengths of 1000 to 1700 nm at a normal angle of incidence of about 0°. For example, the cover article 100 may exhibit a dual surface minimum transmittance of about 80%, 81%, 82%, 83%, 84%, 85%, 86%, 87%, 88%, 89%, 90%, 92%, 93%, 94%, 95% for infrared wavelengths of 1000 to 1700 nm at a normal angle of incidence of about 0°, and all minimum transmittance values between the above ranges and sub-ranges.
[0149] According to an embodiment of the cover product 100 of the present invention, Figures 1 to 1F As shown in an exemplary form in FIG. 1 , the cover article 100 exhibits a first surface reflected color (CIE coordinates under illumination with a D65 light source) at all incident angles from 0° to 90°, wherein a* is from -10 to +10 and b* is from -12 to +5. In some implementations of the cover article 100 of the present invention, the first surface reflected color at all incident angles from 0° to 90° is: a* is from -4 to +4, or -3 to +3, or even -2 to +2; and b* is from -8 to +3, or -7 to +2.5, or -6 to +2.
[0150] According to some implementations, Figures 1 to 1F The cover product 100 shown in FIG. 1 can exhibit a first surface (i.e., through one of the major surfaces 112, 114 of the substrate 110) reflected color of less than 10, less than 8, less than 6, less than 4, less than 3, or even less than 2 with a D65 light source as given by √(a*2+b*2), as measured at normal incidence, all angles of incidence from 0 to 10 degrees, or even from 0 to 90 degrees. For example, the cover product 100 can exhibit a reflected color of less than 10, 9, 8, 7, 6, 5, 4, 3.75, 3.5, 3.25, 3, 2.75, 2.5, 2.25, 2, 1.9, 1.8, 1.7, 1.6, 1.5, 1.4, 1.3, 1.2, 1.1, 1, or even lower, as measured at normal incidence, all angles of incidence from 0 to 10 degrees, or even from 0 to 90 degrees.
[0151] According to an embodiment of the cover product 100 of the present invention, Figures 1 to 1F As shown in an exemplary form in FIG. 1 , the cover article 100 exhibits a dual surface transmission color (CIE coordinates under illumination with a D65 light source) at all incident angles from 0° to 90°, wherein a* is from -4 to +4 and b* is from -4 to +4. In some implementations of the cover article 100 of the present invention, the dual surface transmission color at all incident angles from 0° to 90° is: a* is from -2 to +2, -1.5 to +1.5, or -1 to +1; and b* is from -2 to +2, -1 to +2, or 0 to +2.
[0152] Substrate 110 may include inorganic materials, and may include amorphous substrates, crystalline substrates, glass ceramic substrates or combinations thereof. In some implementations, substrate 110 may include inorganic materials having an amorphous portion and a crystalline portion. Substrate 110 may be formed of artificial materials and / or naturally occurring materials (e.g., quartz and polymers). For example, in some cases, substrate 110 is characterized by being organic, and specifically polymeric. Examples of suitable polymers include, but are not limited to, thermoplastics, including polystyrene (PS) (including styrene copolymers and mixtures), polycarbonate (PC) (including copolymers and mixtures), polyesters (including copolymers or mixtures, including polyethylene terephthalate and polyethylene terephthalate copolymers), polyolefins (PO) and cyclic polyolefins (cyclic PO), polyvinyl chloride (PVC), acrylic polymers including polymethyl methacrylate (PMMA) (including copolymers and mixtures), thermoplastic polyurethanes (TPU), polyetherimide (PEI) and mixtures of these polymers. Other exemplary polymers include epoxy resins, styrene resins, phenolic resins, melamine resins, and silicone resins.
[0153] In some embodiments, the substrate 110 may specifically exclude polymers, plastics, and / or metal materials. The substrate 110 is characterized as a base-containing substrate (i.e., the substrate includes one or more bases). In one or more embodiments, the substrate 110 exhibits a refractive index ranging from about 1.45 to about 1.55. In embodiments, the substrate 110 may exhibit an average stress-to-failure at a surface on one or more opposing major surfaces of 0.5% or greater, 0.6% or greater, 0.7% or greater, 0.8% or greater, 0.9% or greater, 1% or greater, 1.1% or greater, 1.2% or greater, 1.3% or greater, 1.4% or greater, 1.5% or greater, or even 2% or greater, as measured using a ROR test, using at least 5, at least 10, at least 15, or at least 20 samples to determine the average stress-to-failure value. In specific embodiments, the substrate 110 may exhibit an average stress-to-failure of about 1.2%, about 1.4%, about 1.6%, about 1.8%, about 2.2%, about 2.4%, about 2.6%, about 2.8%, or about 3% or more at its surface on one or more opposing major surfaces thereof.
[0154] Suitable substrates 110 may exhibit an elastic modulus (or Young's modulus) ranging from about 30 GPa to about 120 GPa. In some cases, the elastic modulus of the substrate may be in the range of about 30 GPa to about 110 GPa, about 30 GPa to about 100 GPa, about 30 GPa to about 90 GPa, about 30 GPa to about 80 GPa, about 30 GPa to about 70 GPa, about 40 GPa to about 120 GPa, about 50 GPa to about 120 GPa, about 60 GPa to about 120 MPa, about 70 GPa to about 120 GPa, and all ranges and sub-ranges therebetween. In some embodiments, the substrate 110 may exhibit an elastic modulus greater than 85 GPa.
[0155] In one or more embodiments, the amorphous substrate may include glass, which may be strengthened or non-strengthened. Examples of suitable glasses include soda-lime glass, alkali-aluminosilicate glass, alkali-containing borosilicate glass, and alkali-aluminoborosilicate glass. In some variants, the glass may not contain lithium. In one or more alternative embodiments, the substrate 110 may include a crystalline substrate, such as a glass-ceramic substrate (which may be strengthened or non-strengthened), or may include a single crystal structure, such as sapphire. In one or more specific embodiments, the substrate 110 includes an amorphous base (e.g., glass) and a crystalline coating (e.g., a sapphire layer, a polycrystalline alumina layer, and / or a spinel (MgAl 2 O 4 )layer).
[0156] In one or more embodiments, the substrate 110 includes one or more glass-ceramic materials and may be strengthened or non-strengthened. In one or more embodiments, the substrate 110 may include one or more crystalline phases, such as lithium disilicate, lithium metasilicate, petalite, beta-type quartz and / or beta-type spodumene, as may be combined with the remaining glass in the structure. In an embodiment, the substrate 110 includes a disilicate phase. In another embodiment, the substrate 110 includes a disilicate phase and a petalite phase. According to an embodiment, the substrate 110 has a crystallinity of at least 40% by weight. In some implementations, the substrate 110 has a crystallinity of at least about 40%, 45%, 50%, 55%, 60%, 65%, 70%, 75%, 80%, 85% or more (by weight), wherein the remainder is a glass phase. Furthermore, according to some embodiments, each of the crystalline phases of the substrate 110 has an average crystallite size of less than 100 nm, less than 75 nm, less than 50 nm, less than 40 nm, less than 30 nm, and all crystallite sizes are within or less than these levels. According to an exemplary embodiment, the substrate 110 includes lithium disilicate and petalite phases, wherein lithium disilicate is 40 wt%, petalite is 45 wt%, and the remainder is residual glass (i.e., about 85% crystalline, about 15% residual amorphous / glass); each crystalline phase has a majority of crystals with an average crystallite size in the range of 10 nm to 50 nm.
[0157] The substrate 110 of one or more embodiments may have a hardness that is less than the hardness of the entire cover article 100 (as measured by the Berkovich Indenter Hardness Test described herein). The hardness of the substrate 110 may be measured using methods known in the art, including but not limited to the Berkovich Indenter Hardness Test or the Vickers Hardness Test.
[0158] The substrate 110 may be a substantially optically clear, transparent component without light scattering. In such embodiments, the substrate may exhibit an average light transmittance of about 85% or greater, about 86% or greater, about 87% or greater, about 88% or greater, about 89% or greater, about 90% or greater, about 91% or greater, or about 92% or greater over an optical wavelength range. In one or more alternative embodiments, the substrate 110 may be opaque or exhibit an average light transmittance of less than about 10%, less than about 9%, less than about 8%, less than about 7%, less than about 6%, less than about 5%, less than about 4%, less than about 3%, less than about 2%, less than about 1%, or less than about 0.5% over an optical wavelength range. In some embodiments, these light reflectance and transmittance values may be total reflectance or total transmittance (considering the reflectance or transmittance on both major surfaces of the substrate), or may be observed on a single side of the substrate (i.e., only on the outermost surface 122 of the outer layered film 120, without considering the opposite surface). Unless otherwise specified, the average reflectivity or transmittance of the substrate alone is measured at an incident illumination angle of 0 degrees relative to the substrate major surface 112 (however, such measurements may be provided at incident illumination angles of 45 degrees or 60 degrees). The substrate 110 may selectively present a color such as white, black, red, blue, green, yellow, orange, etc.
[0159] Additionally or additionally, for aesthetic and / or functional reasons, the physical thickness of the substrate 110 may vary along one or more of its dimensions. For example, the edges of the substrate 110 may be thicker than more central areas of the substrate 110. The length, width, and physical thickness dimensions of the substrate 110 may also vary depending on the application or use of the cover article 100.
[0160] A variety of different processes may be used to provide the substrate 110. For example, where the substrate 110 comprises an amorphous substrate such as glass, various formation methods may include a float glass process and down-draw processes such as fusion drawing and channel drawing.
[0161] Once the substrate 110 is formed, it may be strengthened to form a strengthened substrate. As used herein, the term "strengthened substrate" may refer to a substrate that has been chemically strengthened (e.g., by ion exchange of larger ions for smaller ions in the surface of the substrate). However, other strengthening methods known in the art may be used, such as thermal tempering, or using the mismatch in thermal expansion coefficients between portions of the substrate to create compressive stress and a central tension region to form a strengthened substrate.
[0162] When the substrate 110 is chemically strengthened by an ion exchange process, the ions in the surface layer of the substrate are replaced or exchanged with larger ions having the same valence or oxidation state. The ion exchange process is generally performed by immersing the substrate in a molten salt bath containing larger ions to be exchanged with smaller ions in the substrate. Those skilled in the art will appreciate that the parameters of the ion exchange process, including but not limited to the composition and temperature of the salt bath, the immersion time, the number of immersions of the substrate in one or more salt baths, the use of multiple salt baths, additional steps such as annealing, washing, and the like, are generally determined by the composition of the substrate and the desired compressive stress (CS) of the substrate resulting from the strengthening operation, the depth of the compressive stress layer (or layer depth DOL, or compression depth DOC). For example, ion exchange of an alkali-containing glass substrate can be achieved by immersing in at least one molten bath containing a salt such as, but not limited to, nitrates, sulfates, and chlorides of larger alkali metal ions. The temperature of the molten salt bath is generally in the range of about 380° C. to a maximum of about 450° C., and the immersion time is in the range of about 15 minutes to a maximum of about 40 hours. However, temperatures and immersion times different from those described above may also be used.
[0163] Additionally, non-limiting examples of ion exchange processes in which a substrate is immersed in multiple ion exchange baths with washing and / or annealing steps between immersions are described in U.S. Patent Application No. 12 / 500,650, filed July 10, 2009 by Douglas C. Allan et al. and in U.S. Patent Application No. 12 / 500,650, filed July 10, 2009 by Christopher M. Lee et al. are described in U.S. Patent No. 8,312,739, issued November 20, 2012, wherein U.S. Patent Application No. 12 / 500,650 is entitled "Glass with Compressed Surface for Consumer Applications" and claims priority to U.S. Provisional Patent Application No. 61 / 079,995 filed on July 11, 2008, in which a substrate is strengthened by immersion in multiple, sequential ion exchange treatments in salt baths of varying concentrations; U.S. Patent No. 8,312,739 is entitled "Dual-Stage Ion Exchange for Chemical Strengthening of Glass" and claims priority to U.S. Provisional Patent Application No. 61 / 084,398 filed on July 29, 2008, in which a substrate is strengthened by ion exchange in a first bath diluted with effluent ions, followed by immersion in a second bath having a lower effluent ion concentration than the first bath. The contents of U.S. Patent Application No. 12 / 500,650 and U.S. Patent No. 8,312,739 are incorporated herein by reference in their entirety.
[0164] The degree of chemical strengthening achieved by ion exchange can be quantified based on the parameters of central tension (CT), surface CS and depth of compression (DOC) (i.e., the point at which the stress state in the substrate changes from compressive stress to tensile stress), and depth of layer (DOL). Compressive stress (including surface CS) is measured by a surface stress meter (FSM), using commercially available instruments such as FSM-6000, manufactured by Orihara Industrial Co., Ltd. (Japan). Surface stress measurement relies on the accurate measurement of the stress optical coefficient (SOC), which is related to the birefringence of the glass. SOC is further measured according to Procedure C (Glass Disk Method) described in ASTM Standard C770-16 entitled "Standard Test Method for Measuring Stress Optical Coefficient of Glass", the contents of which are incorporated herein by reference in their entirety. The maximum CT value is measured using a scattered light polariscope (SCALP) technique known in the art. As used herein, DOC means the depth at which stress in the chemically strengthened alkali-aluminosilicate glass articles described herein changes from compressive stress to tensile stress. DOC can be measured by FSM or SCALP based on the ion exchange treatment. When the stress in the cover article is generated by exchanging potassium ions into the glass article, FSM is used to measure DOC. When the stress is generated by exchanging sodium ions into the article, SCALP is used to measure DOC. Since it is believed that the exchange depth of sodium indicates DOC and the exchange depth of potassium ions indicates a quantitative change in compressive stress (rather than a change in stress from compressive stress to tensile stress), DOC is measured by SCALP when the stress in the article is generated by exchanging potassium ions and sodium ions into the substrate; the exchange depth of potassium ions in such glass articles is measured by FSM.
[0165] In one embodiment, the substrate 110 may have a surface CS (also referred to as "residual surface compressive stress") of 200 MPa or greater, 250 MPa or greater, 300 MPa or greater, for example, 400 MPa or greater, 450 MPa or greater, 500 MPa or greater, 550 MPa or greater, 600 MPa or greater, 650 MPa or greater, 700 MPa or greater, 750 MPa or greater, or 800 MPa or greater. In another embodiment, the strengthening substrate 110 may exhibit a surface compressive stress (CS) of about 200 MPa to about 1200 MPa, about 200 MPa to about 1000 MPa, about 200 MPa to about 800 MPa, about 200 MPa to about 600 MPa, about 200 MPa to about 500 MPa, about 200 MPa to about 400 MPa, about 225 MPa to about 400 MPa, about 250 MPa to about 400 MPa, and all CS sub-ranges and values within the above ranges. The strengthening substrate 110 may have a DOC of 10 μm or more, 15 μm or more, 20 μm or more, 25 μm or more, or 50 μm or more (e.g., 25 μm, 30 μm, 35 μm, 40 μm, 45 μm, 50 μm or more; and about 5 μm to about 150 μm), a DOL of about 1 μm to 5 μm, 1 μm to 10 μm, or 1 μm to about 15 μm, and / or a pressure of 10 MPa or more, 2 In some embodiments, the CT of the cover article 100 is about 0 MPa or more, 30 MPa or more, 40 MPa or more, 50 MPa or more, 75 MPa or more, 100 MPa or more, 125 MPa or more (e.g., 80 MPa, 90 MPa, or 100 MPa or more; and 80 MPa to 200 MPa, etc.) but less than 250 MPa (e.g., 200 MPa or less, 175 MPa or less, 150 MPa or less, etc.). In such implementations of the cover article 100 with a substrate 110 having a CT of about 50 MPa to about 200 MPa or 80 MPa to about 200 MPa, the thickness of the substrate 110 should be limited to about 0.6 mm or less to ensure that the substrate is not brittle. For implementations with thicker substrates, e.g., having thicknesses up to 0.8 mm, 0.9 mm, 1.0 mm, 1.25 mm, or even up to about 1.5 mm, the upper limit of CT should be kept below 200 MPa to ensure that the substrate is not brittle (e.g., 150 MPa for a thickness of 0.8 mm).
[0166] The depth of compression (DOC) of the substrate 110 may be 0.1·(thickness of the substrate (t)) to about 0.25·t, for example, about 0.15·t to about 0.25·t, about 0.15·t to about 0.25·t, or about 0.15·t to about 0.20·t, and all DOC values between the above ranges. For example, the substrate 110 may have a DOC of 20% of the substrate thickness, compared to 15% or less for an ion-exchanged glass substrate. In an embodiment, the depth of compression of the substrate material may be about 8% to about 20% of the thickness of the substrate 110. Note that the above DOC values are measured from one of the major surfaces 112 or 114 of the substrate 110. Thus, for a substrate 110 having a thickness of 600 μm, the DOC may be 20% of the substrate thickness, about 120 μm from each of the major surfaces 112, 114 of the substrate 110, or a total of 240 μm for the entire substrate. In one or more embodiments, the strengthening substrate 110 can exhibit one or more of the following mechanical properties: surface CS of about 200 MPa to about 400 MPa, DOL greater than 30 μm, DOC of about 0.08·t to about 0.25·t, and CT of about 80 MPa to about 200 MPa.
[0167] Example glasses that can be used in substrate 110 can include an alkali-aluminosilicate glass composition or an alkali-aluminoborosilicate glass composition, although other glass compositions are also contemplated. Such glass compositions can be chemically strengthened by an ion exchange process. An example glass composition includes SiO 2 , B 2 O 3 And Na 2 O, among which (SiO 2 +B 2 O 3 )≥66mol%.Na 2 O≥9 mol.%. In an embodiment, the glass composition includes at least 6 wt.% aluminum oxide. In a further embodiment, the substrate includes a glass composition having one or more alkaline earth oxides, such that the alkaline earth oxide content is at least 5 wt.%. In some embodiments, a suitable glass composition further includes K 2 At least one of O, MgO and CaO. In a specific embodiment, the glass composition used in the substrate may include 61-75 mol.% SiO 2 ; 7-15 mol.% Al 2 O 3 ; 0-12 mol.% B 2 O 3 ; 9-21 mol.% Na 2 O; 0-4 mol.% K 2O; 0-7 mol.% MgO; and 0-3 mol.% CaO.
[0168] Further example glass compositions suitable for use in substrate 110 include: 60-70 mol.% SiO 2 ; 6-14 mol.% Al 2 O 3 ; 0-15 mol.% B 2 O 3 ; 0-15 mol.% Li 2 O; 0-20 mol.% Na 2 O; 0-10 mol.% K 2 O; 0-8 mol.% MgO; 0-10 mol.% CaO; 0-5 mol.% ZrO 2 ; 0-1 mol.% SnO 2 ; 0-1 mol.% CeO 2 ; Less than 50ppm As 2 O 3 ; and less than 50ppm Sb 2 O 3 ; Among them 12mol.%≤(Li 2 O+Na 2 O+K 2 O)≦20mol%. 0mol%≦(MgO+CaO)≦10mol%.
[0169] Still further example glass compositions suitable for substrate 110 include: 63.5-66.5 mol. % SiO 2 ; 8-12 mol.% Al 2 O 3 ; 0-3 mol.% B 2 O 3 ; 0-5 mol.% Li 2 O; 8-18 mol.% Na 2 O; 0-5 mol.% K 2 O; 1-7 mol.% MgO; 0-2.5 mol.% CaO; 0-3 mol.% ZrO 2 ; 0.05-0.25 mol.% SnO 2 ; 0.05-0.5 mol.% CeO 2 ; Less than 50ppm As 2 O 3 ; and less than 50ppm Sb 2 O 3 ; Among them 14mol.%≤(Li 2 O+Na2 O+K 2 O)≦18mol.% and 2mol.%≦(MgO+CaO)≦7mol.%.
[0170] In certain embodiments, an alkali-aluminosilicate glass composition suitable for use in substrate 110 includes aluminum oxide, at least one alkali metal, and in some embodiments, greater than 50 mol.% SiO 2 , while in other embodiments, contains at least 58 mol.% SiO 2 , and in still other embodiments, comprises at least 60 mol.% SiO 2 , where (Al 2 O 3 +B 2 O 3 ) / ∑ modifier (i.e., the sum of modifiers) is greater than 1, wherein the components in the ratio are expressed in mol.%, and the modifiers are alkali metal oxides. In a specific embodiment, this glass composition comprises: 58-72 mol.% SiO 2 ; 9-17 mol.% Al 2 O 3 ; 2-12 mol.% B 2 O 3 ; 8-16 mol.% Na 2 O; and 0-4 mol.% K 2 O, where (Al 2 O 3 +B 2 O 3 ) / ∑ modifier (i.e., the sum of the modifiers) is greater than 1.
[0171] In still another embodiment, the substrate 110 may include an alkali-aluminosilicate glass composition comprising: 64-68 mol.% SiO 2 ; 12-16 mol.% Na 2 O; 8-12 mol.% Al 2 O 3 ; 0-3 mol.% B 2 O 3 ; 2-5 mol.% K 2 O; 4-6 mol.% MgO; and 0-5 mol.% CaO, of which: 66 mol.% ≤ SiO 2 +B 2 O 3 +CaO≦69mol.%;Na 2 O+K 2 O+B 2 O 3+MgO+CaO+SrO>10 mol.%; 5 mol.% ≤ MgO+CaO+SrO ≤ 8 mol.%; (Na 2 O + B 2 O 3 ) - Al 2 O 3 ≤ 2 mol.%; 2 mol.% ≤ Na 2 O - Al 2 O 3 ≤ 6 mol.%; and 4 mol.% ≤ (Na 2 O + K 2 O) - Al 2 O 3 ≤ 10 mol.%.
[0172] In an alternative embodiment, the substrate 110 may comprise an alkali aluminosilicate glass composition comprising: 2 mol.% or greater of Al 2 O 3 and / or ZrO 2 , or 4 mol.% or greater of Al 2 O 3 or ZrO 2 .
[0173] In the case where the substrate 110 comprises a crystalline substrate, the substrate may comprise a single crystal, which may comprise Al 2 O 3 . Such single crystal substrates are referred to as sapphire. Other suitable materials for crystalline substrates include polycrystalline alumina layers and / or spinel (MgAl 2 O 4 ).
[0174] Optionally, the substrate 110 may be crystalline and comprise a glass-ceramic substrate, which may be strengthened or unstrengthened and have a suitable composition to support strengthening. Examples of suitable glass-ceramics may include Li 2 O - Al 2 O 3 -SiO 2 systems (i.e., LAS-systems) glass-ceramics, MgO - Al 2 O 3 -SiO 2 systems (i.e., MAS-systems) glass-ceramics, and / or glass-ceramics comprising a major crystalline phase including β-quartz solid solution, β-spodumene ss, cordierite, and lithium disilicate. The glass-ceramic substrate may be strengthened using the chemical strengthening process disclosed herein. In one or more embodiments, the MAS-system glass-ceramic substrate may be strengthened in a Li 2 SO 4 molten salt, whereby 2Li + may be exchanged for Mg2+ exchange.
[0175] According to some embodiments of the cover product 100 of the present invention, the substrate 110 may be a glass-ceramic material of the LAS system, having the following composition: 70-80% SiO 2 5-10% Al 2 O 3 10-15% Li 2 O, 0.01-1% Na 2 O, 0.01-1% K 2 O, 0.1-5% P 2 O 5 , and 0.1-7% ZrO 2 (in wt. %, calculated as oxide). In some implementations of the cover article 100 of the present invention, the substrate 110 may be a LAS system having the following composition: 70-80% SiO 2 5-10% Al 2 O 3 10-15% Li 2 O, 0.01-1% Na 2 O, 0.01-1% K 2 O, 0.1-5% P 2 O 5 , and 0.1-5% ZrO 2 (in wt.%, calculated as oxide). According to another embodiment, the substrate 110 may be a LAS system having the following composition: 70-75% SiO 2 5-10% Al 2 O 3 10-15% Li 2 O, 0.05-1% Na 2 O, 0.1-1% K 2 O, 1-5% P 2 O 5 2-7% ZrO 2 , and 0.1-2% CaO (in wt.%, calculated as oxide). According to a further embodiment, the substrate 110 may have the following composition: 71-72% SiO 2 , 6-8% Al 2 O 3 10-13% Li 2 O, 0.05-0.5% Na 2 O, 0.1-0.5% K 2 O, 1.5-4% P 2 O 5 4-7% ZrO 2, and 0.5-1.5% CaO (in wt.%, calculated as oxide). More generally, these compositions of substrate 110 are advantageous for the cap product 100 of the present invention because it exhibits low haze levels, high transparency, high fracture toughness (e.g., greater than 0.8 MPa·√m), and high elastic modulus, and is ion exchangeable.
[0176] The substrate 110 according to one or more embodiments may have a physical thickness ranging from about 50 μm to about 5 mm in various portions of the substrate 110. The physical thickness of the example substrate 110 ranges from about 50 μm to about 500 μm (e.g., 50, 75, 100, 200, 300, 400, or 500 μm). Further example substrates 110 have a physical thickness ranging from about 50 μm to about 2000 μm (e.g., 50, 75, 100, 250, 500, 600, 700, 800, 900, 1000, 1250, 1500, 1750, or 2000 μm). The substrate 110 may have a physical thickness greater than about 1 mm (e.g., about 2, 3, 4, or 5 mm). In one or more specific embodiments, the substrate 110 may have a physical thickness of 2 mm or less, or less than 1 mm. The substrate 110 may be acid polished or otherwise treated to remove or reduce the effects of surface defects.
[0177] like Figures 1 to 1F The cover product 100 illustrated in exemplary form in the accompanying drawings and disclosed herein may be incorporated into an apparatus article, for example, an apparatus article having a display (or display article) (e.g., consumer electronics, including mobile phones, tablet computers, computers, navigation systems, wearable devices (e.g., watches), and the like), an augmented reality display, a head-up display, a glass-based display, an architectural apparatus article, a transportation apparatus article (e.g., a car, a train, an airplane, a marine vessel, etc.), an electrical apparatus article, or any article that benefits from transparency, scratch resistance, abrasion resistance, damage resistance, or a combination thereof. Figure 2A and Figure 2B An exemplary article incorporating any of the cover articles disclosed herein is shown in FIG. Specifically, Figure 2A and Figure 2BA consumer electronic product 200 is shown, which includes a housing 202 having a front surface 204, a rear surface 206, and side surfaces 208; an electronic component (not shown) at least partially within the housing 202 or completely within the housing 202 and including at least one of a display 210 and a sensor 220. In addition, the display 210 is at or adjacent to the front surface 204 of the housing 202, and the sensor 220 is at or adjacent to the front surface 204 or the rear surface 206 of the housing 202. In addition, a cover 212 is disposed at or above at least one of the display 210 and the sensor 220. In some embodiments, at least one of the cover 212 or a portion of the housing 202 may include any of the cover articles 100 disclosed herein.
[0178] Examples
[0179] Various embodiments are further illustrated by the following modeling examples (Examples 1-10). The optical properties of the examples (e.g., light reflectance and transmittance) are modeled using computational techniques, particularly transmission matrix modeling techniques, to model thin film properties as understood by those skilled in the art. x high RI layers), laboratory experiments, and thin film properties (e.g., refractive index values) obtained by larger volume sputtering fabrication.
[0180] In the previous experiments, the refractive index (as a function of wavelength) of each of the formed layers and the glass substrate was measured using a spectroscopic ellipsometer. The refractive index thus measured was then used to calculate the reflectance spectrum of the example. For convenience, the example uses a single refractive index value in its descriptive table, which corresponds to a point selected from the dispersion curve at a wavelength of about 550nm.
[0181] Comparative modeling examples (i.e., Comparative Example 1 and Comparative Example 2) are also provided as a comparison of the performance of the cover articles of the present invention, and these comparative examples may have inferior optical performance when deposited on a substrate. In many of the examples described herein, the substrate used is Glass 3( Glass 3) (available from Corning, Inc.). Examples of glass 3 compositions are described in US Pat. Nos. 7,666,511, 4,483,700, and 5,674,790, the core contents of which are hereby incorporated by reference into the present invention.
[0182] In the following example cover products, the total thickness of the outer layered film 120 depends largely on the thickness of the thickest hard coating (e.g., the thickest anti-scratch layer 150). In each design, this thickest layer can vary its thickness in the range of about 200nm to 10000+nm, while the change in optical performance is minimal. In general, a thicker anti-scratch layer 150 will result in higher scratch resistance or damage resistance. The thickness of the anti-scratch layer selected for these designs here (about 500-2000nm) has been selected as a better combination of manufacturability and high scratch resistance for consumer electronics applications. In some cases, it is desirable to minimize the thickness of the layer of the anti-reflective zone 130 above the thickest anti-scratch layer 150 to optimize hardness and scratch resistance. This may be a challenge for optical coatings with extended bandwidths, because the extended bandwidth of anti-reflective coatings is typically associated with thicker anti-reflective coating stacks. It may also be particularly desirable to minimize the amount of low RI material (having an RI of less than 1.55 or less than 1.5 at a wavelength of 550 nm, such as SiO in the example) in the anti-reflective region 130 above the thickest anti-scratch layer 150. 2 ), for example, less than 280 nm, or in the range of 80-280 nm. Here, the bottom cover article design exhibits an optimized combination of low visible light reflectance, high visible light transmittance, and an extended infrared bandwidth of low reflectance and high transmittance, while also optimizing visible light color, achievable hardness, and relatively low anti-reflective region stack thickness.
[0183] Comparative Example 1
[0184] A strengthened glass substrate was coated with the comparative outer layer film of Table 1 below, designated as Comparative Example 1. Specifically, the outer layer film of Comparative Example 1 had 19 layers, of which layer 10 was the thickest (500 nm).
[0185] FIG. 3A to FIG. 3C The optical properties of Comparative Example 1 are shown. Specifically, Figure 3A 2 is a graph of the first surface reflectivity versus wavelength for this comparative cover product at 8°, 30°, 40°, and 60° incident angles. Comparative Example 1 has an antireflective (AR) bandwidth (defined herein as <3% first surface or single-side reflectivity) of about 410-1010 nm. However, as shown in the various figures, the first surface reflectivity rises rapidly at near normal (8 degree) incidence to above 4% at wavelengths of about 1050-1700 nm (which is the approximate reflectivity of an uncoated glass surface), to above 6% at wavelengths of about 1100-1700 nm, and even exceeds 22% at 1550 nm. At higher angles of incidence, such as 60 degrees, the reflectivity is even higher, reaching a peak of about 27% near 1450 nm.
[0186] Figure 3Bis a graph of the first surface reflected color of this comparative cover product at all viewing angles from 0 degrees to 90 degrees using a D65 light source. Figure 3B It can be seen that the reflected color of this comparative example ranges from about -2.4 to +1 in a* and about -3.5 to +2.3 in b*.
[0187] also, Figure 3C is a graph of dual surface transmission color of this comparative cover product at all viewing angles from 0 degrees to 90 degrees with a D65 illuminant. Figure 3C The results shown in are from modeling of this comparative cover product having an outer layered film on one major surface of a glass substrate and an uncoated glass substrate forming a second major surface. Figure 3C As shown in , the transmission color ranges from about -0.2 to +0.2 in a* and about -0 to +2.5 in b*.
[0188] Table 1 - Comparative Example 1, Optical Films on Strengthened Glass Articles
[0189]
[0190]
[0191] Example 1
[0192] A strengthened glass substrate was coated with the outer layer film of Table 2 below, designated as Example 1. Specifically, the outer layer film of Example 1 has 21 layers, of which layer 8 is the thickest (500 nm). Note that the thickness of layer 8 can be adjusted between about 200-10000+ nm without substantially changing the optical performance. In addition, the thickness of the substrate can be varied, for example, from about 0.05 mm to about 5 mm, without departing from the spirit of the present invention. For the first surface modeling calculations, the presence of air medium was not included.
[0193] The optical properties of Example 1 are as follows FIG. 4A to FIG. 4C Specifically, Figure 4A : is a graph of the first surface reflectivity versus wavelength for this example cover article at 8°, 30°, 40°, and 60° incident angles. Example 1 has a first surface reflectivity that remains below 5% for an extended IR bandwidth of 800-1700nm at a viewing (light incident) angle of 0-40 degrees, and below 9.5% for 800-1700nm at 60 degrees of incidence.
[0194] Figure 4B This is a graph of the first surface reflected color of the cover product of this example at all viewing angles from 0 degrees to 90 degrees using a D65 light source. Figure 4B It can be seen that the reflected color ranges from about -1.1 to +7.1 in a* and about -10.5 to +2.9 in b*.
[0195] also, Figure 4C : is a graph of the dual surface transmission color of this example cover article at all viewing angles from 0 degrees to 90 degrees using a D65 light source. Figure 4C The results shown in derive from modeling of a cover article having an outer layered film on one major surface of a glass substrate and an uncoated glass substrate forming a second major surface. Figure 4C As shown in , the transmission color ranges from about -0.8 to +0 in a* and about -0 to +1.9 in b*.
[0196] Table 2 - Example 1, Cover Article for Sensor
[0197]
[0198]
[0199] Example 2
[0200] A strengthened glass substrate was coated with the outer layer film of Table 3 below, designated as Example 2. Specifically, the outer layer film of Example 2 had 19 layers, of which layer 8 was the thickest (600 nm). Note that the thickness of layer 8 can be adjusted between about 200-10000+ nm without substantially changing the optical performance. Additionally, the thickness of the substrate can vary, for example, from about 0.05 mm to about 5 mm, without departing from the spirit of the present invention. For the first surface modeling calculations, the presence of air medium was not included.
[0201] The optical properties of Example 2 are as follows FIG. 5A to FIG. 5C Specifically, Figure 5A : is a graph of the first surface reflectance versus wavelength for this example cover article at 8°, 30°, 40°, and 60° incident angles. Example 2 has a first surface reflectance of less than 2% in the visible range of 450-750 nm at near normal (8 degree) incidence. In addition, the first surface reflectance remains less than 5% for an extended IR bandwidth of 800-1700 nm at viewing (light incident) angles of 0-30 degrees, less than 6% at 0-40 degree incident angles, and less than 10.5% at 60 degree incidence.
[0202] Figure 5B This is a graph of the first surface reflected color of the cover product of this example at all viewing angles from 0 degrees to 90 degrees using a D65 light source. Figure 5B It can be seen that the reflected color ranges from about -0 to +1.9 in a* and about -5.8 to +1.8 in b*.
[0203] also, Figure 5C : is a graph of the dual surface transmission color of this example cover article at all viewing angles from 0 degrees to 90 degrees using a D65 light source. Figure 5CThe results shown in are from modeling of a cover article having an outer layered film on one major surface of a glass substrate and an uncoated glass substrate forming a second major surface. Figure 5C As shown in , the transmission color ranges from about -0.4 to +0 in a* and about -0 to +1.7 in b*.
[0204] Table 3 - Example 2, Cover Article for Sensor
[0205]
[0206]
[0207] Example 3
[0208] A strengthened glass substrate was coated with the outer layer film of Table 4 below, designated as Example 3. Specifically, the outer layer film of Example 3 has 21 layers, of which layer 8 is the thickest (500 nm). Note that the thickness of layer 8 can be adjusted between about 200-10000+ nm without substantially changing the optical performance. In addition, the thickness of the substrate can be varied, for example, from about 0.05 mm to about 5 mm, without departing from the spirit of the present invention. For the first surface modeling calculations, the presence of air medium was not included.
[0209] The optical properties of Example 3 are as follows FIG. 6A to FIG. 6C Specifically, Fig. 6A : is a graph of the first surface reflectivity versus wavelength for this example cover article at 8°, 30°, 40°, and 60° incident angles. Example 3 has a first surface reflectivity of less than 2% in the visible light range of 450-700 nm at near normal (8 degree) incidence. In addition, the first surface reflectivity remains less than 4% for an extended IR bandwidth of 800-1700 nm at a viewing (light incident) angle of 0-30 degrees, less than 5% at an incident angle of 0-40 degrees, and less than 9% at 60 degrees of incidence.
[0210] Figure 6B This is a graph of the first surface reflected color of the cover product of this example at all viewing angles from 0 degrees to 90 degrees using a D65 light source. Figure 6B It can be seen that the reflected color ranges from about -0.6 to +4.0 in a* and about -7.5 to +2.3 in b*.
[0211] also, Figure 6C : is a graph of the dual surface transmission color of this example cover article at all viewing angles from 0 degrees to 90 degrees using a D65 light source. Figure 6C The results shown in are from modeling of a cover article having an outer layered film on one major surface of a glass substrate and an uncoated glass substrate forming a second major surface. Figure 6CAs shown in , the transmission color ranges from about -0.6 to +0 in a* and about -0 to +1.6 in b*.
[0212] Table 4 - Example 3, Cover Article for Sensor
[0213]
[0214]
[0215] Example 4
[0216] A strengthened glass substrate was coated with the outer layer film of Table 5 below, designated as Example 4. Specifically, the outer layer film of Example 4 has 19 layers, of which layer 8 is the thickest (600 nm). Note that the thickness of layer 8 can be adjusted between about 200-10000+ nm without substantially changing the optical performance. In addition, the thickness of the substrate can be varied, for example, from about 0.05 mm to about 5 mm, without departing from the spirit of the present invention. For the first surface modeling calculations, the presence of air medium was not included.
[0217] The optical properties of Example 4 are as follows FIG. 7A to FIG. 7C Specifically, Fig. 7A : is a graph of the first surface reflectivity versus wavelength for this example cover article at 8°, 30°, 40°, and 60° incident angles. Example 4 has a first surface reflectivity of less than 2% in the visible light range of 450-700 nm at near normal (8 degree) incidence. In addition, the first surface reflectivity remains below 4.5% for an extended IR bandwidth of 800-1700 nm at a viewing (light incident) angle of 0-30 degrees, below 5% for 800-1700 nm at 0-40 degrees, and below 10% for 800-1700 nm at 60 degrees of incidence.
[0218] Figure 7B This is the first surface reflection color graph of the cover article of this example at all viewing angles from 0 degrees to 90 degrees using a D65 light source. Figure 7B It can be seen that the reflected color ranges from about -0 to +1.4 in a* and about -4.4 to +1.4 in b*.
[0219] also, Figure 7C : is a graph of the dual surface transmission color of this example cover article at all viewing angles from 0 degrees to 90 degrees using a D65 light source. Figure 7C The results shown in are from modeling of a cover article having an outer layered film on one major surface of a glass substrate and an uncoated glass substrate forming a second major surface. Figure 7C As shown in , the transmission color ranges from about -0.4 to +0 in a* and about -0 to +1.6 in b*.
[0220] Table 5 - Example 4, Cover Article for Sensor
[0221]
[0222]
[0223] Example 5
[0224] A strengthened glass substrate was coated with the outer layer film of Table 6 below, designated as Example 5. Specifically, the outer layer film of Example 5 had 22 layers, of which layer 11 was the thickest (1960 nm). Note that the thickness of layer 11 can be adjusted between about 200-10000+ nm without substantially changing the optical performance. In addition, the thickness of the substrate can be varied, for example, from about 0.05 mm to about 5 mm, without departing from the spirit of the present invention. For the first surface modeling calculations, the presence of air medium was not included.
[0225] Example 5 Using different SiO x N y The thickest layer of the material (compared to Examples 1-4) is used for impedance matching and anti-reflection areas of the outer layer film. x N y The material has a refractive index of 1.829, an elastic modulus of about 160 GPa, a compressive stress of about -940 MPa, and a hardness of about 17.8 GPa. This combination of hardness, modulus, and compressive stress has been shown to improve or optimize the scratch resistance and flexural strength of this combination of cover products including a chemically strengthened glass substrate.
[0226] The optical properties of Example 5 are as follows FIG. 8A to FIG. 8C Specifically, Fig. 8A : is a graph of the first surface reflectance versus wavelength for this example cover article at 8°, 30°, 40°, and 60° incident angles. Example 5 has a first surface reflectance of less than 2% in the visible light range of 450-700 nm at near normal (8 degree) incidence. In addition, the first surface reflectance remains below 5.1% for an extended IR bandwidth of 800-1700 nm at a viewing (light incident) angle of 0-30 degrees, below 6% for 800-1700 nm at 0-40 degrees, and below 11% for 800-1700 nm at 60 degrees of incidence.
[0227] Figure 8B This is a graph of the first surface reflected color of the cover product of this example at all viewing angles from 0 degrees to 90 degrees using a D65 light source. Figure 8B It can be seen that the reflected color ranges from about -0.1 to +0.8 in a* and about -5.4 to +1.7 in b*.
[0228] also, Figure 8C: is a graph of the dual surface transmission color of this example cover article at all viewing angles from 0 degrees to 90 degrees using a D65 light source. Figure 8C The results shown in are from modeling of a cover article having an outer layered film on one major surface of a glass substrate and an uncoated glass substrate forming a second major surface. Figure 8C As shown in , the transmission color ranges from about -0.25 to +0.1 in a* and about -0 to +1.2 in b*.
[0229] Table 6 - Example 5, Cover Article for Sensor
[0230]
[0231]
[0232] Example 6
[0233] A strengthened glass ceramic substrate was coated with the outer layered film of Table 7 below, designated as Example 6. Specifically, the outer layered film of Example 6 had 22 layers, of which layer 11 was the thickest (1960 nm). Note that the thickness of layer 11 can be adjusted between about 200-10000+ nm without substantially changing the optical properties. In addition, the thickness of the substrate can be varied, for example, from about 0.05 mm to about 5 mm, without departing from the spirit of the present invention. For the first surface modeling calculations, the presence of air medium was not included.
[0234] Example 6 is a design similar to Example 5, in which the substrate is changed to a chemically strengthened glass-ceramic composition. In addition, the impedance matching layer (i.e., the layer between the substrate and the scratch resistant layer, layer 11) has been modified to account for the different refractive index of the glass-ceramic substrate. Example 6 also uses the same optimized SiO x N y material for impedance matching and the thickest anti-scratch layer. x N y The material has a refractive index of 1.829, an elastic modulus of about 160 GPa, a compressive stress of about -940 MPa, and a hardness of about 17.8 GPa. This combination of hardness, modulus, and compressive stress has been shown to improve or optimize the combined scratch resistance and flexural strength of this cover article.
[0235] The optical properties of Example 6 are as follows 9A to 9C Specifically, Fig.9A: is a graph of the first surface reflectance versus wavelength for this example cover article at 8°, 30°, 40°, and 60° incident angles. Example 6 has a first surface reflectance of less than 2% in the visible range of 450-700 nm at near normal (8 degree) incidence. In addition, the first surface reflectance remains below 5% for an extended IR bandwidth of 800-1700 nm at viewing (light incident) angles of 0-30 degrees, below 5.5% for 800-1700 nm at 0-40 degrees, below 10.1% for 800-1670 nm at 60 degrees incidence, and below 11.5% for 800-1700 nm at 60 degrees incidence.
[0236] Fig. 9B This is a graph of the first surface reflected color of the cover product of this example at all viewing angles from 0 degrees to 90 degrees using a D65 light source. Fig. 9B It can be seen that the reflected color ranges from about -0.1 to +0.8 in a* and about -5.4 to +1.7 in b*.
[0237] also, Fig. 9C : is a graph of the dual surface transmission color of this example cover article at all viewing angles from 0 degrees to 90 degrees using a D65 light source. Fig. 9C The results shown in are from modeling of a cover article having an outer layered film on one major surface of a glass-ceramic substrate and an uncoated glass-ceramic substrate forming a second major surface. Fig. 9C As shown in , the transmission color ranges from about -0.4 to +0.1 in a* and about -0 to +1.6 in b*.
[0238] Table 7 - Example 6, Cover Article for Sensor
[0239]
[0240]
[0241] Example 7
[0242] A strengthened glass substrate was coated with the outer layer film of Table 8 below, designated as Example 7. Specifically, the outer layer film of Example 7 has 22 layers, of which layer 11 is the thickest (600 nm). Note that the thickness of layer 11 can be adjusted between about 200-10000+ nm without substantially changing the optical performance. In addition, the thickness of the substrate can be varied, for example, from about 0.05 mm to about 5 mm, without departing from the spirit of the present invention. For the first surface modeling calculations, the presence of air medium was not included.
[0243] The optical properties of Example 7 are as follows FIG. 10A to FIG. 10C Specifically, Fig. 10A: is a graph of the first surface reflectance versus wavelength for this example cover article at 8°, 30°, 40°, and 60° incident angles. Example 7 has a first surface reflectance of less than 2% in the visible light range of 450-700 nm at near normal (8 degree) incidence. In addition, the first surface reflectance remains below 5.5% for an extended IR bandwidth of 800-1700 nm at a viewing (light incident) angle of 0-30 degrees, below 6% for 800-1700 nm at 0-40 degrees, and below 11% for 800-1700 nm at 60 degree incidence.
[0244] Fig. 10B This is a graph of the first surface reflected color of the cover product of this example at all viewing angles from 0 degrees to 90 degrees using a D65 light source. Fig. 10B It can be seen that the reflected color ranges from about -0 to +1.1 in a* and about -5.7 to +1.2 in b*.
[0245] also, Fig. 10C : is a graph of the dual surface transmission color of this example cover article at all viewing angles from 0 degrees to 90 degrees using a D65 light source. Fig. 10C The results shown in are from modeling of a cover article having an outer layered film on one major surface of a glass substrate and an uncoated glass substrate forming a second major surface. Fig. 10C As shown in , the transmission color ranges from about -0.5 to +0 in a* and about -0 to +2.0 in b*.
[0246] Table 8 - Example 7, Cover Article for Sensor
[0247]
[0248]
[0249]
[0250] Table 9 below provides a summary of selected properties of a comparative example (Comparative Example 1) and examples from the present invention (Examples 1-7). Reflection and transmission at infrared wavelengths of 1000-1700 nm are significantly differentiated between the comparative example and the examples of the present invention (Examples 1-7) at various light incidence angles (angle of incidence, AOI). The bold values in Table 9 highlight that the performance of Comparative Example 1 is not as good as these ranges of the examples of the present invention, Examples 1-7. Visible light metrics (light reflectance and transmittance, color metrics a* and b*) and hardness are also important for the intended application. Hardness is estimated based on an empirical model derived from experimental multilayer films, from SiO 2 、SiN x and SiO x Ny Start with a separate layer.
[0251] Table 9 - Summary of properties of cover articles for sensors (Examples 1-7, Comparative Example 1)
[0252]
[0253]
[0254]
[0255] Example 8
[0256] In this example, a cover product including a strengthened glass ceramic substrate was prepared, the structure of which is described in Table 10 below and as described in U.S. Provisional Application No. 63 / 337,846, filed on May 3, 2022, entitled "Transparent Glass Ceramic Article with High Shallow Hardness and Display Device Having the Same", which is incorporated herein by reference in its entirety. The glass ceramic substrate is an ion-exchanged LAS glass ceramic substrate having a thickness of 600 μm and a refractive index of 1.533. In addition, the glass ceramic substrate has the following composition: 74.5% SiO 2 ; 7.53% Al 2 O 3 ; 2.1% P 2 O 5 11.3% Li 2 O; 0.06% Na 2 O; 0.12% K 2 O; 4.31% ZrO 2 ; 0.06% Fe 2 O 3 ; and 0.02% SnO 2 (wt. % by oxide). In addition, the glass ceramic substrate was ceramized according to the following schedule: (a) ramping from room temperature to 580°C at 5°C / min; (b) holding at 580°C for 2.75 hours; (c) ramping to 755°C at 2.5°C / min; (d) holding at 755°C for 0.75 hours; and (e) cooling to room temperature at furnace speed. After ceramization, the glass ceramic substrate was heated in 60% KNO 3 / 40% NaNO 3 +0.12% LiNO 3 (wt.%) molten salt bath at 500°C for 6 hours. In addition, the outer layer membrane layer was deposited according to the vapor deposition conditions described in U.S. Patent Application Publication No. 2020 / 0158916, the core part of which is incorporated herein by reference.
[0257] Referring again to the cover article of this example, the layers of the outer layered film (e.g., layers 17-23 in Table 10) above the scratch resistant layer (e.g., layer 16 in Table 10) are configured to achieve high shallow layer hardness while not negatively affecting the optical properties of the article, including reflectivity in the visible, infrared, and near infrared spectra. As can be seen from the outer layered film design in Table 10, the medium refractive index layer (SiO x N y Layers 18, 20 and 22) are adjacent to the high refractive index layer (SiN y Layers 17, 19 and 21) are provided, which drives a shallow high hardness level in the product. Similarly, it can be seen from Table 10 that the low refractive index layer (e.g., SiO 2 The total thickness of the layer 23) is minimized to a level of less than 25 nm, which also helps drive a shallow high hardness level in the article. In at least some embodiments, this shallow high hardness level as described above can be understood as a hardness of the cover article greater than 15 GPa, or greater than 17 GPa, as measured by the Berkovich hardness test at an indentation depth of 125 nm (e.g., see Fig. 15B and Fig. 15C ).
[0258] refer to Fig.11A , provides a graph of the first surface reflectivity versus wavelength for this example of the present invention measured at a near-normal incidence angle of 8°. Notably, this example exhibits low maximum and minimum reflectivity oscillations of less than 6% in the 1000 to 1700 nm band. Fig.11A It can also be seen that this example exhibits a maximum reflectivity of less than 12% in the near infrared spectrum from 1000 to 1700 nm.
[0259] refer to Fig. 11B , provides a graph of the single-side reflected color measured for this example of the invention at various outer layer film thickness ratio factors at incident angles of 0° to 90°. Fig. 11B It can be seen that this inventive example exhibits a color shift that is fairly consistent and less than 4 over a wide range of outer layer film thickness scaling factors from about 70% to 100%.
[0260] Table 10 - Example 8 Lid Product Design with Strengthened Glass Ceramic Substrate
[0261]
[0262]
[0263] Total thickness(nm): 2903.7
[0264] AR layer thickness (nm): 270.0
[0265] AR low RI thickness (nm): 14
[0266] Example 9
[0267] In this example, a cover article including a strengthened glass ceramic substrate was prepared, the structure of which is described in Table 11 below and as described in U.S. Provisional Application No. 63 / 337,846, filed on May 3, 2022, entitled "Transparent Glass Ceramic Article with High Shallow Hardness and Display Device Having the Same", which is incorporated herein by reference in its entirety. The glass ceramic substrate is an ion-exchanged LAS glass ceramic substrate having a thickness of 600 μm and a refractive index of 1.533. The glass ceramic substrate has the following composition: 74.5% SiO 2 ; 7.53% Al 2 O 3 ; 2.1% P 2 O 5 11.3% Li 2 O; 0.06% Na 2 O; 0.12% K 2 O; 4.31% ZrO 2 ; 0.06% Fe 2 O 3 ; and 0.02% SnO 2 (wt. % by oxide). In addition, the glass ceramic substrate was ceramized according to the following schedule: (a) ramping from room temperature to 580°C at 5°C / min; (b) holding at 580°C for 2.75 hours; (c) ramping to 755°C at 2.5°C / min; (d) holding at 755°C for 0.75 hours; and (e) cooling to room temperature at furnace speed. After ceramization, the glass ceramic substrate was heated in 60% KNO 3 / 40% NaNO 3 +0.12% LiNO 3 (wt.%) was ion exchange strengthened at 500° C. for 6 hours in a molten salt bath of 1% MgO (wt.%). The layers of the outer layer membrane were deposited according to the vapor deposition conditions described in U.S. Patent Application Publication No. 2020 / 0158916, the core portion of which is incorporated herein by reference.
[0268] Referring again to the cover article of this example, the layers of the outer layered film (e.g., layers 17-27 in Table 11) above the scratch resistant layer (e.g., layer 16 in Table 11) are configured to achieve high shallow layer hardness without negatively affecting the optical properties of the article, including reflectivity in the visible, infrared, and near infrared spectra. As can be seen from the outer layered film design in Table 11, the medium refractive index layer (SiO x N yLayers 18, 20, 22, 24 and 26) are adjacent to the high refractive index layer (SiN y Layers 17, 19, 21, 23 and 25) are provided, which drives a shallow high hardness level in the product. Similarly, it can be seen from Table 11 that the low refractive index layer (e.g., SiO 2 The total thickness of the layer 27 is minimized to a level of less than 25 nm, which also helps drive a shallow high hardness level in the article. In at least some embodiments, this shallow high hardness level as described above can be understood as a hardness of the cover article greater than 15 GPa, or greater than 17 GPa, as measured by the Berkovich hardness test at an indentation depth of 125 nm (e.g., see Fig. 15B and Fig. 15C ).
[0269] refer to Fig. 12A , provides a graph of the first surface reflectivity versus wavelength for this example of the present invention measured at a near-normal incidence angle of 8°. Notably, this example exhibits low maximum and minimum reflectivity oscillations of less than 2.5% in the wavelength band of 1000 to 1700 nm. Fig. 12A It can also be seen that this example exhibits a low maximum reflectivity of less than 6% in the near infrared spectrum from 1000 to 1700 nm.
[0270] refer to Fig. 12B , provides a graph of the single-side reflected color measured for this example of the invention at various outer layer film thickness ratio factors at incident angles of 0° to 90°. Fig. 12B It can be seen that the color shift exhibited by this inventive example is fairly consistent and is less than 4 over the entire range of the outer layer film thickness scaling factor from about 50% to 100% shown in this figure.
[0271] Table 11 - Example 9 Lid Product Design with Strengthened Glass Ceramic Substrate
[0272]
[0273]
[0274] Total thickness(nm): 3096.6
[0275] AR layer thickness (nm): 462.9
[0276] AR low RI thickness (nm): 14
[0277] Example 10
[0278] In this example, a cover product including a strengthened glass ceramic substrate was prepared, the structure of which is described in Table 12 below and as described in U.S. Provisional Application No. 63 / 337,846, filed on May 3, 2022, entitled "Transparent Glass Ceramic Article with High Shallow Hardness and Display Device Having the Same", which is incorporated herein by reference in its entirety. The glass ceramic substrate is an ion-exchanged LAS glass ceramic substrate having a thickness of 600 μm and a refractive index of 1.528. In addition, the glass ceramic substrate has the following composition: 74.5% SiO 2 ; 7.53% Al 2 O 3 ; 2.1% P 2 O 5 11.3% Li 2 O; 0.06% Na 2 O; 0.12% K 2 O; 4.31% ZrO 2 ; 0.06% Fe 2 O 3 ; and 0.02% SnO 2 (wt. % as oxide). The glass ceramic substrate was ceramized according to the following schedule: (a) ramping from room temperature to 580°C at 5°C / min; (b) holding at 580°C for 2.75 hours; (c) ramping to 755°C at 2.5°C / min; (d) holding at 755°C for 0.75 hours; and (e) cooling to room temperature at furnace speed. After ceramization, the glass ceramic substrate was heated in 60% KNO 3 / 40% NaNO 3 +0.12% LiNO 3 (wt.%) was ion exchange strengthened at 500° C. for 6 hours in a molten salt bath of 1% MgO (wt.%). The layers of the outer layer membrane were deposited according to the vapor deposition conditions described in U.S. Patent Application Publication No. 2020 / 0158916, the core portion of which is incorporated herein by reference.
[0279] Referring again to the cover article of this example, the layers of the outer layered film (e.g., layers 17-23 in Table 12) above the scratch resistant layer (e.g., layer 16 in Table 12) are configured to achieve high shallow layer hardness without negatively affecting the optical properties of the article, including reflectivity in the visible, IR, and near IR spectra. As can be seen from the outer layered film design in Table 12, the medium refractive index layer (SiO x N y Layers 18, 20 and 22) are adjacent to the high refractive index layer (SiN yLayers 17, 19 and 21) are provided, which drives a shallow high hardness level in the product. Similarly, as shown in Table 12, the low refractive index layer (e.g., SiO 2 The total thickness of the layer 24 is minimized to a level of less than 25 nm, which also helps drive a shallow high hardness level in the article. In at least some embodiments, this shallow high hardness level as described above can be understood as a hardness of the cover article greater than 15 GPa, or greater than 17 GPa, as measured by the Berkovich hardness test at an indentation depth of 125 nm (e.g., see Fig. 15B and Fig. 15C ). In addition, it can also be seen from Table 12 that the outer structure of this example includes a medium refractive index layer (e.g., layer 23) repeated adjacent to another medium refractive index layer (e.g., layer 22), which can also positively affect the hardness level of the article at shallow indentation depths.
[0280] refer to Fig.13A , provides a graph of the first surface reflectivity versus wavelength for this inventive example measured at a near-normal incidence angle of 8°. Notably, this example exhibits low maximum and minimum reflectivity oscillations of less than 2% in the wavelength band of 1000 to 1700 nm. Fig.13A It can also be seen that this example exhibits a low maximum reflectivity of less than 5.5% in the near infrared spectrum from 1000 to 1700 nm.
[0281] refer to Fig. 13B , provides a graph of the single-side reflected color measured for this inventive example at various outer layer film thickness ratio factors at incident angles of 0° to 90°. Fig. 13B It can be seen that this inventive example exhibits a fairly consistent color shift and is less than 4 over the entire range of outer layer film thickness scaling factors from about 40% to 100% shown in this figure.
[0282] Table 12 - Example 10 Lid Product Design with Strengthened Glass Ceramic Substrate
[0283]
[0284]
[0285] Total thickness(nm): 2949.4
[0286] AR layer thickness (nm): 388.2
[0287] AR low RI thickness (nm): 14
[0288] Comparative Example 2
[0289] In this example, a comparative cover article was prepared that included a strengthened glass substrate, the structure of which is described in Table 13 below. The glass substrate was an ion-exchanged aluminosilicate glass substrate having a thickness of 550 μm and a refractive index of 1.51. The substrate had the following composition: 61.81% SiO 2 ; 3.9% B 2 O 3 ; 19.69% Al 2 O 3 ;12.91% Na 2 O; 0.018% K 2 O; 1.43% MgO; 0.019% Fe 2 O 3 ; and 0.223% SnO 2 (wt. % calculated as oxide). The substrate was strengthened using a molten salt bath to achieve a maximum compressive stress (CS) of 850 MPa with a depth-of-layer (DOL) of 40 μm. In addition, the layers of the outer layer membrane were deposited according to the vapor deposition conditions described in U.S. Patent Application Publication No. 2020 / 0158916, the core portion of which is incorporated herein by reference.
[0290] refer to Fig.14A , provides a graph of the first surface reflectivity versus wavelength for this comparative example measured at a near-normal incident angle of 8°. Notably, this comparative example exhibits high maximum and minimum reflectivity oscillations greater than 8% in the wavelength band of 1000 to 1700 nm. Fig.14A It can also be seen that this comparative example exhibits high reflectivity in the near infrared spectrum, for example, greater than 7% at 940 nm, greater than 12% at 1200 nm, greater than 13% at 1350 nm, and greater than 11% at 1500 nm.
[0291] refer to Fig. 14B , provides a graph of the single-sided reflected color measured for this comparative example at various optical film structure thickness ratio factors at incident angles of 0° to 90°. Fig. 14B It can be seen that the color shift exhibited by this comparative example is less than 4 only within a narrow range of the optical film structure thickness proportionality factor from about 95% to 100%.
[0292] Table 13 - Comparative Example 2 Coated Product Design with Strengthened Glass Substrate
[0293]
[0294]
[0295] Total thickness(nm): 2510.8
[0296] AR layer thickness (nm): 312.6
[0297] AR low RI thickness (nm): 116.1
[0298] Mechanical properties of Examples 8-10
[0299] Reference now Fig.15A , providing a box plot of the average product failure stress measured in the ring-on-ring test for the cover products of Examples 8-10, Comparative Example 2, and a control glass-ceramic substrate without an outer delamination film. Fig.15A It can be seen that the examples of the present invention exhibit an average failure stress level of at least 800 MPa, which is comparable to the bare glass ceramic substrate without an outer delamination film ( Fig.15A In contrast, the average fracture stress level of the comparative example (Comparative Example 2) is less than 600 MPa, which is much lower than the average fracture stress level of the inventive examples (Examples 8-10).
[0300] Reference now Fig. 15B and Fig. 15C , provides a graph of hardness and elastic modulus versus displacement, as measured in the Berkovich hardness test of the outer layer film of the cover articles of Examples 8-10. Fig. 15B It can be seen that each of the examples of the present invention (Examples 8-10) exhibits a hardness of about 15 GPa or more at a shallow indentation depth of 100 to 125 nm. Fig. 15C It can be seen that each of the inventive examples (Examples 8-10) exhibits a maximum elastic modulus in the range of 160-200 GPa, and the elastic modulus at 15% of the total thickness of the outer layered film (about 450 nm for these examples) is 120-160 GPa.
[0301] The various features described in this specification may be combined in any and all combinations, for example as listed in the following examples.
[0302] Embodiment 1. Provided is a cover product for a sensor, comprising: a substrate comprising a thickness of 50 μm to 5000 μm, an outer major surface and an inner major surface, wherein the outer major surface and the inner major surface are opposite to each other, and the substrate is a chemically strengthened glass substrate or a glass ceramic substrate; and an outer layered film, the outer layered film is disposed on the outer major surface of the substrate, and wherein the cover product exhibits a first surface average reflectivity of less than 10% for a wavelength of 1000 nm to 1700 nm at at least one incident angle of 8° to 60°.
[0303] Embodiment 2. The cover product according to embodiment 1, wherein the outer layer film comprises an anti-scratch layer, the anti-scratch layer comprises a nitride or an oxynitride and has a thickness of about 80 nm to 10000 nm.
[0304] Embodiment 3. The cover article of embodiment 2, wherein the outer layer film comprises a refractive index gradient.
[0305] Embodiment 4. The cover product of embodiment 2, wherein the outer layered film comprises a plurality of alternating high and low refractive index layers, and wherein each of the high refractive index layers comprises a nitride or an oxynitride and has a refractive index greater than that of each of the low refractive index layers.
[0306] Embodiment 5. A cover product according to embodiment 4, wherein one of the low refractive index layers is a cap layer defining the outermost surface of the outer layered film, the cap layer having a thickness of at least 110 nm, and further wherein the outer layered film comprises an anti-reflective zone above the anti-scratch layer, the low refractive index layer of the anti-reflective zone comprising a total thickness of less than 275 nm.
[0307] Embodiment 6. The cover article of any of embodiments 1-5, wherein the cover article further exhibits a dual surface average transmittance greater than 85% for infrared wavelengths of 1000 nm to 1700 nm at at least one incident angle of 8° to 40°.
[0308] Embodiment 7. The cover article of any of embodiments 1-6, wherein the cover article exhibits a first surface average reflectivity of less than 5% at at least one incident angle of 8° to 40° for infrared wavelengths of 1000 nm to 1700 nm.
[0309] Embodiment 8. The cover article of any of embodiments 1-7, wherein the cover article further exhibits a first surface average reflectivity of 2% to 5% at a wavelength of 800 nm to 1000 nm at an incident angle of 8°.
[0310] Embodiment 9. The cover article of any one of embodiments 1-8, wherein the cover article further exhibits a first surface reflectance CIE color for all incident angles from 0° to 90°, wherein a* is from -10 to +10 and b* is from -12 to +5 (CIE coordinates b*), as measured under D65 light source illumination.
[0311] Embodiment 10. The cover article of any of embodiments 1-9, wherein the cover article exhibits a first surface average light reflectance of less than 2% at an incident angle of about 8°.
[0312] Embodiment 11. The cover product according to any one of embodiments 2 and embodiments 4-10, wherein each of the anti-scratch layer and the high refractive index layer comprises SiN xor SiO x N y .
[0313] Embodiment 12. The cover article of any one of embodiments 2 and embodiments 4-11, wherein the outer layered film comprises an anti-reflective zone above the scratch resistant layer, and the anti-reflective zone comprises at least five alternating high and low refractive index layers.
[0314] Embodiment 13. The cover article according to any one of embodiments 2 and embodiments 4-12, wherein the outer layered film comprises an optical interference layer between the anti-scratch layer and the substrate, the optical interference layer comprising alternating high refractive index layers and low refractive index layers.
[0315] Embodiment 14. The cover article of any of embodiments 5-13, wherein the cap layer has a thickness of 110 nm to about 200 nm.
[0316] Embodiment 15. The cover article of any of embodiments 5-14, wherein the high refractive index layer adjacent to the cap layer has a thickness of about 10 nm to less than 150 nm.
[0317] Embodiment 16. The lid article of any of Embodiments 1-15, wherein the outer layered film exhibits a residual compressive stress greater than or equal to 700 MPa and an elastic modulus greater than or equal to 140 GPa.
[0318] Embodiment 17. The cover article according to any one of embodiments 1-16, wherein the substrate is a glass ceramic comprising an elastic modulus greater than 85 GPa and a fracture toughness greater than 0.8 MPa·√m.
[0319] Embodiment 18. The lid article of any of Embodiments 1-17, wherein the outer layer film exhibits a residual compressive stress of 700 MPa to 1100 MPa and an elastic modulus of 140 GPa to 200 GPa.
[0320] Embodiment 19. The lid article of any of Embodiments 1-18, wherein the outer layer film exhibits an elastic modulus of 140 GPa to 180 GPa.
[0321] Embodiment 20. The cover article of any of embodiments 1-19, wherein the substrate has a residual surface compressive stress of 200 MPa to 1200 MPa and a depth of compression (DOC) of 5 μm to 150 μm.
[0322] Embodiment 21. The cover article of any of Embodiments 1-20, wherein the substrate further exhibits a maximum central tension (CT) value of 80 MPa to 200 MPa, and further wherein the substrate has a thickness of about 1.5 mm or less.
[0323] Embodiment 22. The cover article of any of embodiments 1-21, wherein the substrate has a residual surface compressive stress of 200 MPa to 400 MPa.
[0324] Embodiment 23. The lid article of any of embodiments 1-22, wherein the lid article exhibits an average stress at failure of 800 MPa or greater in a ring-on-ring test with the outer surface of the outer layered film under tension.
[0325] Embodiment 24. A glass screen protector for a smart phone, comprising: a cover glass; and an adhesive backing disposed on the cover glass,
[0326] wherein the adhesive backing is for attachment to a smartphone, and further wherein at least a portion of the cover glass comprises the cover article of any one of Examples 1-23.
[0327] Embodiment 25. A consumer electronic product comprising: a housing comprising a front surface, a rear surface, and a side surface; an electronic component at least partially within the housing, the electronic component comprising at least one of a display and a sensor, the display being at or adjacent to the front surface of the housing, and the sensor being at or adjacent to the front surface or the rear surface of the housing; and a cover disposed above at least one of the display and the sensor, wherein at least a portion of the cover comprises the cover product described in any one of Embodiments 1-23.
[0328] Embodiment 26. Provides a cover product for a sensor, comprising: a substrate comprising a thickness of 50 μm to 5000 μm, an outer major surface and an inner major surface, wherein the outer major surface and the inner major surface are opposite to each other, and the substrate is a chemically strengthened glass substrate or a glass ceramic substrate; and an outer layered film disposed on the outer major surface of the substrate, wherein the outer layered film exhibits a hardness of at least 8 GPa, as measured by a Berkovich indenter hardness test from the outermost surface of the outer layered film to a depth of about 100 nm to about 500 nm, and further wherein the cover product exhibits a first surface average reflectivity of less than 10% for a wavelength of 1000 nm to 1700 nm at at least one incident angle of 8° to 60°.
[0329] Embodiment 27. The cover article of embodiment 26, wherein the outer layer film comprises a refractive index gradient.
[0330] Embodiment 28. The cover product of embodiment 26, wherein the outer layered film comprises a plurality of alternating high refractive index layers and low refractive index layers, and wherein each of the high refractive index films comprises a nitride or an oxynitride and has a refractive index greater than the refractive index of each of the low refractive index layers,
[0331] Embodiment 29. The cover article of embodiment 28, wherein the outer layered film comprises an anti-scratch layer having a thickness of about 80 nm to 10000 nm, and further wherein the outer layered film comprises an anti-reflective region above the anti-scratch layer, the anti-reflective region comprising a thickness of about 100 nm to about 525 nm.
[0332] Embodiment 30. The cover article of any of Embodiments 26-29, wherein the cover article further exhibits a dual surface average transmittance greater than 85% for infrared wavelengths from 1000 nm to 1700 nm at at least one incident angle from 8° to 40°.
[0333] Embodiment 31. The cover article of any of Embodiments 26-30, wherein the cover article exhibits a first surface average reflectivity of less than 5% for infrared wavelengths of 1000 nm to 1700 nm at at least one incident angle of 8° to 40°.
[0334] Embodiment 32. The cover article of any of Embodiments 26-31, wherein the cover article exhibits a first surface average light reflectance of less than 2% at an incident angle of about 8°.
[0335] Embodiment 33. The cover article of any of Embodiments 26-32, wherein the cover article further exhibits a first surface average reflectivity of 2% to 5% at an incident angle of 8° for wavelengths of 800 nm to 1000 nm.
[0336] Embodiment 34. The cover article of any of Embodiments 26-33, wherein the cover article further exhibits a first surface reflectance CIE color for all incident angles from 0° to 90°, wherein a* is from -10 to +10 and b* is from -12 to +5 (CIE coordinates b*), as measured under illumination with a D65 light source.
[0337] Embodiment 35. The cover article of any one of embodiments 29-34, wherein each of the anti-scratch layer and the high refractive index layer comprises SiN x or SiO x N y .
[0338] Embodiment 36. The cover article of any of Embodiments 28-35, wherein the anti-reflective zone comprises at least five alternating high and low refractive index layers.
[0339] Embodiment 37. The lid article of any of Embodiments 26-36, wherein the outer layered film exhibits a residual compressive stress greater than or equal to 700 MPa and an elastic modulus greater than or equal to 140 GPa.
[0340] Embodiment 38. The cover article of any one of embodiments 26-37, wherein the substrate is a glass ceramic comprising an elastic modulus greater than 85 GPa and a fracture toughness greater than 0.8 MPa·√m.
[0341] Embodiment 39. The lid article of any of Embodiments 26-38, wherein the outer layer film exhibits a residual compressive stress of 700 MPa to 1100 MPa and an elastic modulus of 140 GPa to 200 GPa.
[0342] Embodiment 40. The lid article of any of Embodiments 26-39, wherein the outer layer film exhibits an elastic modulus of 140 GPa to 180 GPa.
[0343] Embodiment 41. The cover article of any of Embodiments 26-40, wherein the substrate has a residual surface compressive stress of 200 MPa to 1200 MPa and a depth of compression (DOC) of 5 μm to 150 μm.
[0344] Embodiment 42. The cover article of any of Embodiments 26-41, wherein the substrate further exhibits a maximum central tension (CT) value of 80 MPa to 200 MPa, and further wherein the substrate has a thickness of about 1.5 mm or less.
[0345] Embodiment 43. The cover article of any of Embodiments 26-42, wherein the substrate has a residual surface compressive stress of 200 MPa to 400 MPa.
[0346] Embodiment 44. The lid article of any of Embodiments 26-43, wherein the lid article exhibits an average stress at failure of 800 MPa or greater in a Ring-on-Ring test with the outer surface of the outer layered film under tension.
[0347] Embodiment 45. The cover article of any of Embodiments 26-44, wherein the cover article exhibits a first surface average light reflectance of less than 2% at an incident angle of about 8°.
[0348] Embodiment 46. A glass screen protector for a smartphone, comprising: a cover glass; and an adhesive backing disposed on the cover glass, wherein the adhesive backing is used to attach to the smartphone, and further wherein at least a portion of the cover glass comprises the cover product described in any one of Embodiments 26-45.
[0349] Embodiment 47. A consumer electronic product, comprising: a housing comprising a front surface, a rear surface, and a side surface; an electronic component at least partially within the housing, the electronic component comprising at least one of a display and a sensor, the display being at or adjacent to the front surface of the housing, and the sensor being at or adjacent to the front surface or the rear surface of the housing; and a cover disposed above at least one of the display and the sensor, wherein at least a portion of the cover comprises the cover product described in any one of Embodiments 26-45.
[0350] Embodiment 48. Provided is a cover product for a sensor, comprising: a substrate comprising a thickness of 50 μm to 5000 μm, an outer major surface and an inner major surface, wherein the outer major surface and the inner major surface are opposite to each other, and the substrate is a chemically strengthened glass substrate or a glass ceramic substrate; and an outer layered film disposed on the outer major surface of the substrate, wherein the outer layered film comprises a plurality of alternating high refractive index layers and low refractive index layers, wherein each of the high refractive index layers comprises a nitride or an oxynitride, and has a refractive index greater than that of each of the low refractive index layers, wherein the outer layered film comprises an anti-scratch layer having a thickness of about 80 nm to 10000 nm, wherein one of the low refractive index layers is a layer defining an outer A cap layer at the outermost surface of a layered film, and the cap layer has a thickness of at least 110 nm, wherein the outer layered film comprises an anti-reflective zone above the scratch resistant layer, and the anti-reflective zone comprises a thickness of about 100 nm to about 525 nm, wherein the low refractive index layers of the anti-refractive zone comprise a total thickness of less than 275 nm, wherein the outer layered film exhibits a hardness of at least 8 GPa, as measured by a Berkovich indenter hardness test from the outermost surface of the outer layered film to a depth of about 100 nm to about 500 nm, and further wherein the cover article exhibits a first surface average reflectivity of less than 10% for wavelengths of 1000 nm to 1700 nm at at least one incident angle of 8° to 60°.
[0351] Embodiment 49. The cover article of embodiment 48, wherein the cover article further exhibits a dual surface average transmittance greater than 85% for infrared wavelengths from 1000 nm to 1700 nm at at least one incident angle from 8° to 40°.
[0352] Embodiment 50. The cover article of embodiment 48 or embodiment 49, wherein the cover article further exhibits a dual surface average transmittance greater than 75% at an incident angle of 60° for infrared wavelengths between 1000 nm and 1700 nm.
[0353] Embodiment 51. The cover article of any of Embodiments 48-50, wherein the cover article exhibits a first surface average reflectivity of less than 5% for infrared wavelengths of 1000 nm to 1700 nm at at least one incident angle of 8° to 40°.
[0354] Embodiment 52. The cover article of any of Embodiments 48-51, wherein the cover article further exhibits a first surface average reflectivity of 2% to 5% at a wavelength of 800 nm to 1000 nm at an incident angle of 8°.
[0355] Embodiment 53. The cover article of any one of Embodiments 48-52, wherein the cover article further exhibits a first surface reflectance CIE color for all incident angles from 0° to 90°, wherein a* is from -10 to +10 and b* is from -12 to +5 (CIE coordinates b*) as measured under D65 light source illumination.
[0356] Embodiment 54. The cover article of any one of embodiments 48-53, wherein each of the anti-scratch layer and the high refractive index layer comprises SiN x or SiO x N y .
[0357] Embodiment 55. The cover article of any of Embodiments 48-54, wherein the cover article exhibits a first surface average light reflectance of less than 2% at an incident angle of about 8°.
[0358] Embodiment 56. The cover article of any of Embodiments 48-55, wherein the cap layer has a thickness of 110 nm to about 200 nm.
[0359] Embodiment 57. The cover article of any of Embodiments 48-56, wherein the high refractive index layer adjacent to the cap layer has a thickness of about 10 nm to less than 150 nm.
[0360] Embodiment 58. The lid article of any of Embodiments 48-57, wherein the outer layer film exhibits a residual compressive stress greater than or equal to 700 MPa and an elastic modulus greater than or equal to 140 GPa.
[0361] Embodiment 59. The cover article of any one of embodiments 48-58, wherein the substrate is a glass ceramic comprising an elastic modulus greater than 85 GPa and a fracture toughness greater than 0.8 MPa·√m.
[0362] Embodiment 60. The lid article of any of Embodiments 48-59, wherein the outer layer film exhibits a residual compressive stress of 700 MPa to 1100 MPa and an elastic modulus of 140 GPa to 200 GPa.
[0363] Embodiment 61. The lid article of any of Embodiments 48-60, wherein the outer layer film exhibits an elastic modulus of 140 GPa to 180 GPa.
[0364] Embodiment 62. The cover article of any of Embodiments 48-61, wherein the substrate has a residual surface compressive stress of 200 MPa to 1200 MPa and a depth of compression (DOC) of 5 μm to 150 μm.
[0365] Embodiment 63. The cover article of any of Embodiments 48-62, wherein the substrate further exhibits a maximum central tension (CT) value of 80 MPa to 200 MPa, and further wherein the substrate has a thickness of about 1.5 mm or less.
[0366] Embodiment 64. The cover article of any of Embodiments 48-63, wherein the substrate has a residual surface compressive stress of 200 MPa to 400 MPa.
[0367] Embodiment 65. The lid article of any of Embodiments 48-64, wherein the lid article exhibits an average stress at failure of 800 MPa or greater in a Ring-on-Ring test with the outer surface of the outer layered film under tension.
[0368] Embodiment 66. A glass screen protector for a smartphone, comprising: a cover glass; and an adhesive backing disposed on the cover glass, wherein the adhesive backing is used to attach to the smartphone, and further wherein at least a portion of the cover glass comprises the cover product described in any one of Embodiments 48-65.
[0369] Embodiment 67. A consumer electronic product, comprising: a housing comprising a front surface, a rear surface, and a side surface; an electronic component at least partially within the housing, the electronic component comprising at least one of a display and a sensor, the display being at or adjacent to the front surface of the housing, and the sensor being at or adjacent to the front surface or the rear surface of the housing; and a cover disposed over at least one of the display and the sensor, wherein at least a portion of the cover comprises the cover product described in any one of Embodiments 48-65.
[0370] Embodiment 68. Provides a cover product for a sensor, comprising: a substrate comprising a thickness of 50 μm to 5000 μm, an outer major surface and an inner major surface, wherein the outer major surface and the inner major surface are opposite to each other, and the substrate is a chemically strengthened glass substrate or a glass ceramic substrate; and an outer layered film disposed on the outer major surface of the substrate, wherein the cover product exhibits a first surface average reflectivity of less than 10% for a wavelength of 1000 nm to 1700 nm at at least one incident angle of 8° to 60°, and wherein the outer layered film exhibits a residual compressive stress greater than or equal to 700 MPa and an elastic modulus greater than or equal to 140 GPa.
[0371] Embodiment 69. The cover article according to embodiment 68, wherein the outer layered film comprises an anti-scratch layer, the anti-scratch layer comprises a nitride or an oxynitride and has a thickness of about 80 nm to 10000 nm.
[0372] Embodiment 70. The cover article of embodiment 69, wherein the outer layered film comprises a refractive index gradient.
[0373] Embodiment 71. The cover product of embodiment 69, wherein the outer layered film comprises a plurality of alternating high refractive index layers and low refractive index layers, and wherein each of the high refractive index layers comprises a nitride or an oxynitride and has a refractive index greater than that of each of the low refractive index layers.
[0374] Embodiment 72. The lid article of any of Embodiments 68-71, wherein the outer layer film exhibits a residual compressive stress of 700 MPa to 1100 MPa and an elastic modulus of 140 GPa to 200 GPa.
[0375] Embodiment 73. The lid article of any of Embodiments 68-72, wherein the outer layer film exhibits an elastic modulus of 140 GPa to 180 GPa.
[0376] Embodiment 74. The cover article of any of embodiments 68-73, wherein the substrate has a residual surface compressive stress of 200 MPa to 1200 MPa and a depth of compression (DOC) of 5 μm to 150 μm.
[0377] Embodiment 75. The cover article of any of Embodiments 68-74, wherein the substrate further exhibits a maximum central tension (CT) value of 80 MPa to 200 MPa, and further wherein the substrate has a thickness of about 1.5 mm or less.
[0378] Embodiment 76. The cover article of any of Embodiments 68-75, wherein the substrate has a residual surface compressive stress of 200 MPa to 400 MPa.
[0379] Embodiment 77. The lid article of any of Embodiments 68-76, wherein the lid article exhibits an average stress at failure of 800 MPa or greater in a Ring-on-Ring test with the outer surface of the outer layered film under tension.
[0380] Embodiment 78. The cover article of any one of embodiments 68-77, wherein the substrate is a glass ceramic comprising an elastic modulus greater than 85 GPa and a fracture toughness greater than 0.8 MPa·√m.
[0381] Embodiment 79. A glass screen protector for a smartphone, comprising: a cover glass; and an adhesive backing disposed on the cover glass, wherein the adhesive backing is used to attach to the smartphone, and further wherein at least a portion of the cover glass comprises the cover product of any one of Embodiments 68-78.
[0382] Embodiment 80. A consumer electronic product, comprising: a housing comprising a front surface, a rear surface, and a side surface; an electronic component at least partially within the housing, the electronic component comprising at least one of a display and a sensor, the display being at or adjacent to the front surface of the housing, and the sensor being at or adjacent to the front surface or the rear surface of the housing; and a cover disposed above at least one of the display and the sensor, wherein at least a portion of the cover comprises the cover product described in any one of Embodiments 68-78.
[0383] Embodiment 81. Provides a cover product for a sensor, comprising: a glass ceramic substrate comprising a first major surface and a second major surface, the major surfaces being opposite to each other; and an outer layered film defining an outer surface, the outer layered film being disposed on the first major surface, wherein the cover product exhibits a hardness greater than 15 GPa, as measured by a Berkovich hardness test at an indentation depth of approximately 125 nm from the outer surface of the outer layered film, and further wherein the cover product exhibits a first surface average reflectivity of less than 10% for wavelengths of 1000 nm to 1700 nm at at least one incident angle of 8° to 60°.
[0384] Embodiment 82. A cover product according to embodiment 81, wherein: the outer layered film comprises a scratch-resistant layer and a plurality of alternating high refractive index layers and low refractive index layers, the outer layered film further comprises an outer structure and an inner structure, the scratch-resistant layer is disposed between the outer structure and the inner structure, the outer structure comprises at least one medium RI layer in contact with one of the high RI layer and the scratch-resistant layer, the medium RI layer comprises a refractive index of 1.55 to 1.80, each of the high RI layers comprises a refractive index greater than 1.80, and each of the low RI layers comprises a refractive index less than 1.55, and the glass-ceramic substrate comprises an elastic modulus greater than 85 GPa and a fracture toughness greater than 0.8 MPa·√m.
[0385] Embodiment 83. The lid article of Embodiment 81 or Embodiment 82, wherein the outer layer film exhibits a residual compressive stress greater than or equal to 700 MPa and an elastic modulus greater than or equal to 140 GPa.
[0386] Embodiment 84. The lid article of any of Embodiments 81-83, wherein the outer layer film exhibits a residual compressive stress of 700 MPa to 1100 MPa and an elastic modulus of 140 GPa to 200 GPa.
[0387] Embodiment 85. The lid article of any of Embodiments 81-84, wherein the outer layer film exhibits an elastic modulus of 140 GPa to 180 GPa.
[0388] Embodiment 86. The cover article of any one of embodiments 81-85, wherein the glass ceramic substrate has a residual surface compressive stress of 200 MPa to 1200 MPa and a depth of compression (DOC) of 5 μm to 150 μm.
[0389] Embodiment 87. The cover article of any of Embodiments 81-86, wherein the glass-ceramic substrate further exhibits a maximum central tension (CT) value of 80 MPa to 200 MPa, and further wherein the glass-ceramic substrate has a thickness of about 1.5 mm or less.
[0390] Embodiment 88. The cover article of any one of Embodiments 81-87, wherein the glass ceramic substrate has a residual surface compressive stress of 200 MPa to 400 MPa.
[0391] Embodiment 89. The lid article of any of Embodiments 81-88, wherein the lid article exhibits an average stress at failure of 700 MPa or greater in a Ring-on-Ring test with the outer surface of the outer layered film under tension.
[0392] Embodiment 90. The lid article of any of Embodiments 81-89, wherein the lid article exhibits an average stress at failure of 500 MPa or greater in a four-point bend test with the outer surface of the outer layered film under tension.
[0393] Embodiment 91. The lid article of any of Embodiments 81-90, wherein the lid article exhibits a hardness greater than 17 GPa as measured by a Berkovich hardness test at an indentation depth of about 125 nm from the outer surface of the outer layered film.
[0394] Embodiment 92. A glass screen protector for a smartphone, comprising: a cover glass; and an adhesive backing disposed on the cover glass, wherein the adhesive backing is used to attach to the smartphone, and further wherein at least a portion of the cover glass comprises the cover product described in any one of Embodiments 81-91.
[0395] Embodiment 93. A consumer electronic product, comprising: a housing comprising a front surface, a rear surface, and a side surface; an electronic component at least partially within the housing, the electronic component comprising at least one of a display and a sensor, the display being at or adjacent to the front surface of the housing, and the sensor being at or adjacent to the front surface or the rear surface of the housing; and a cover disposed over at least one of the display and the sensor, wherein at least a portion of the cover comprises the cover product described in any one of Embodiments 81-91.
[0396] Many changes and modifications may be made to the above-described embodiments of the present invention without departing substantially from the spirit and various principles of the present invention. All such modifications and variations are intended to be included within the scope of the present invention herein and protected by the following claims.
Claims
1. A cover product for a sensor, comprising: A substrate, comprising a thickness of 50 μm to 5000 μm, an outer major surface and an inner major surface, wherein the outer major surface and the inner major surface are opposite to each other, and the substrate is a chemically strengthened glass substrate or a glass ceramic substrate; and an outer layer film disposed on the outer major surface of the substrate, and Wherein the cover article exhibits a first surface average reflectivity of less than 10% at a wavelength of 1000 nm to 1700 nm at at least one incident angle of 8° to 60°. 2 . The cover article according to claim 1 , wherein the outer layered film comprises an anti-scratch layer comprising a nitride or an oxynitride and having a thickness of about 80 nm to 10,000 nm.
3. The cover article of claim 2 wherein the outer layer film comprises a refractive index gradient.
4. The cover product of claim 2, wherein the outer layered film comprises a plurality of alternating high refractive index layers and low refractive index layers, and wherein each of the high refractive index layers comprises a nitride or an oxynitride and has a refractive index greater than that of each of the low refractive index layers.
5. The cover article of claim 4, wherein one of the low refractive index layers is a cap layer defining an outermost surface of the outer layered film, the cap layer having a thickness of at least 110 nm, and further wherein the outer layered film comprises an anti-reflective zone above the anti-scratch layer, the low refractive index layers of the anti-reflective zone comprising a total thickness of less than 275 nm.
6. The cover article of any one of claims 1-5, wherein the cover article further exhibits a dual surface average transmittance greater than 85% for infrared wavelengths from 1000 nm to 1700 nm at at least one incident angle from 8° to 40°.
7. The cover article of any one of claims 1-6, wherein the cover article exhibits a first surface average reflectivity of less than 5% for infrared wavelengths from 1000 nm to 1700 nm at at least one incident angle from 8° to 40°.
8. The cover product of any one of claims 1-7, wherein the cover product further exhibits a first surface average reflectivity of 2% to 5% at an incident angle of 8° for wavelengths of 800 nm to 1000 nm.
9. The cover product of any one of claims 1-2, wherein the cover product further exhibits a first surface reflectance CIE color for all angles of incidence from 0° to 90°, wherein a* is from -10 to +10 and b* is from -12 to +5 (CIE coordinates b*) as measured under illumination with a D65 illuminant.
10. The cover article of any one of claims 1-9, wherein the cover article exhibits a first surface average light reflectance of less than 2% at an incident angle of about 8°.
11. The cover product according to any one of claims 2 and 4-10, wherein each of the anti-scratch layer and the high refractive index layer comprises SiN x or SiO x N y .
12. The cover article of any one of claims 2 and 4, wherein the outer layer film comprises an anti-reflection zone above the scratch resistant layer, and the anti-reflection zone comprises at least five alternating high and low refractive index layers.
13. The cover article of any one of claims 2 and 4-12, wherein the outer layer film comprises an optical interference layer between the scratch resistant layer and the substrate, the optical interference layer comprising alternating high and low refractive index layers.
14. The lid article of claims 5-13, wherein the thickness of the cap layer is from 110 nm to about 200 nm.
15. The cover article of claims 5-14, wherein the high refractive index layer adjacent to the cap layer has a thickness of about 10 nm to less than 150 nm.
16. The lid article of any one of claims 1-15, wherein the outer layer film exhibits a residual compressive stress greater than or equal to 700 MPa and an elastic modulus greater than or equal to 140 GPa.
17. The cover article of any one of claims 1-16, wherein the substrate is a glass ceramic comprising an elastic modulus greater than 85 GPa and a fracture toughness greater than 0.8 MPa·√m.
18. The lid article of any one of claims 1-17, wherein the outer layer film exhibits a residual compressive stress of 700 MPa to 1100 MPa and an elastic modulus of 140 GPa to 200 GPa.
19. The lid article of any one of claims 1-18, wherein the outer layer film exhibits an elastic modulus of 140 GPa to 180 GPa.
20. The cover article of any one of claims 1-19, wherein the substrate has a residual surface compressive stress of 200 MPa to 1200 MPa and a depth of compression (DOC) of 5 μm to 150 μm.
21. The cover article of any one of claims 1-20, wherein the substrate further exhibits a maximum central tension (CT) value of 80 MPa to 200 MPa, and further wherein the substrate has a thickness of about 1.5 mm or less.
22. The cover article of any one of claims 1-21, wherein the substrate has a residual surface compressive stress of 200 MPa to 400 MPa.
23. The lid article of any one of claims 1-22, wherein the lid article exhibits an average stress at failure of 800 MPa or greater in a ring-on-ring test with the outer surface of the outer layered film under tension.
24. A glass screen protector for a smart phone, comprising: cover glass; and an adhesive backing disposed on the cover glass, wherein the adhesive backing is for attachment to the smartphone, and Further wherein at least a portion of the cover glass comprises a cover product according to any one of claims 1-23.
25. A consumer electronic product comprising: A housing, the housing comprising a front surface, a rear surface, and a plurality of side surfaces; a plurality of electronic components at least partially within the housing, the electronic components including at least one of a display at or adjacent to the front surface of the housing and a sensor at or adjacent to the front surface or the rear surface of the housing; and a cover disposed over at least one of the display and the sensor, Wherein at least a portion of the cover comprises a cover article according to any one of claims 1-23.
26. A cover product for a sensor, comprising: a substrate comprising a thickness of 50 μm to 5000 μm, an outer major surface and an inner major surface, wherein the outer major surface and the inner major surface are opposite to each other, and the substrate is a chemically strengthened glass substrate or a glass ceramic substrate; and an outer layer film disposed on the outer major surface of the substrate, wherein the outer layer film exhibits a hardness of at least 8 GPa as measured by a Berkovich indenter hardness test at a depth of about 100 nm to about 500 nm from the outermost surface of the outer layer film, and Further wherein the cover article exhibits a first surface average reflectivity of less than 10% at a wavelength of 1000 nm to 1700 nm at at least one incident angle of 8° to 60°.
27. The cover article of claim 26 wherein the outer layer film comprises a refractive index gradient.
28. The cover product of claim 26, wherein the outer layered film comprises a plurality of alternating high refractive index layers and low refractive index layers, and wherein each high refractive index layer comprises a nitride or an oxynitride, and wherein the refractive index of each high refractive index layer is greater than the refractive index of each low refractive index layer.
29. The cover article of claim 28, wherein the outer layer film comprises an anti-scratch layer having a thickness of about 80 nm to 10,000 nm, and further wherein the outer layer film comprises an anti-reflective region above the anti-scratch layer, and the anti-reflective region has a thickness of about 100 nm to about 525 nm.
30. The cover article of any one of claims 26 to 29, wherein the cover article further exhibits a dual surface average transmittance greater than 85% for infrared wavelengths from 1000 nm to 1700 nm at at least one incident angle from 8° to 40°.
31. The cover article of any one of claims 26 to 30, wherein the cover article exhibits a first surface average reflectivity of less than 5% at at least one incident angle of 8° to 40° for infrared wavelengths of 1000 nm to 1700 nm.
32. The cover article of any one of claims 26 to 31, wherein the cover article exhibits a first surface average light reflectance of less than 2% at an incident angle of about 8°.
33. The cover article of any one of claims 26 to 32, wherein the cover article further exhibits a first surface average reflectivity of 2% to 5% at a wavelength of 800 nm to 1000 nm at an incident angle of 8°.
34. The cover product of any one of claims 26 to 33, wherein the cover product further exhibits a first surface reflectance CIE color for all angles of incidence from 0° to 90°, wherein a* is from -10 to +10 and b* is from -12 to +5 (CIE coordinates b*) as measured under illumination with a D65 illuminant.
35. The cover article according to any one of claims 29 to 34, wherein the anti-scratch layer and each of the high refractive index layers comprise SiN x or SiO x N y .
36. The cover article of any one of claims 28 to 35, wherein the anti-reflective zone comprises at least five alternating high and low refractive index layers.
37. The lid article of any one of claims 26 to 36, wherein the outer layer film exhibits a residual compressive stress greater than or equal to 700 MPa and an elastic modulus greater than or equal to 140 GPa.
38. The cover article of any one of claims 26 to 37, wherein the substrate is a glass-ceramic comprising an elastic modulus greater than 85 GPa and a fracture toughness greater than 0.8 MPa·m.
39. The lid article of any one of claims 26 to 38, wherein the outer layer film exhibits a residual compressive stress of 700 MPa to 1100 MPa and an elastic modulus of 140 GPa to 200 GPa.
40. The lid article of any one of claims 26 to 39, wherein the outer layer film exhibits an elastic modulus of 140 GPa to 180 GPa.
41. The cover article of any one of claims 26 to 40, wherein the substrate has a residual surface compressive stress of 200 MPa to 1200 MPa and a depth of compression (DOC) of 5 microns to 150 microns.
42. The cover article of any one of claims 26 to 41, wherein the substrate further exhibits a maximum central tension (CT) value of 80 MPa to 200 MPa, and further wherein the substrate has a thickness of about 1.5 mm or less.
43. The cover article of any one of claims 26 to 42, wherein the substrate has a residual surface compressive stress of 200 MPa to 400 MPa.
44. The lid article of any one of claims 26 to 43, wherein the lid article exhibits an average stress at failure of 800 MPa or greater in a ring-on-ring test with the outer surface of the outer layered film under tension.
45. The cover article of any one of claims 26 to 44, wherein the cover article exhibits a first surface average light reflectance of less than 2% at an incident angle of about 8°.
46. A glass screen protector for a smart phone, comprising: cover glass; and an adhesive backing disposed on the cover glass, wherein the adhesive backing is for attachment to the smartphone, and Further wherein at least a portion of the cover glass comprises a cover product according to any one of claims 26 to 45.
47. A consumer electronic product comprising: A housing, the housing comprising a front surface, a rear surface, and a plurality of side surfaces; a plurality of electronic components at least partially within the housing, the electronic components including at least one of a display at or adjacent to the front surface of the housing and a sensor at or adjacent to the front surface or the rear surface of the housing; and a cover disposed over at least one of the display and the sensor, Wherein at least a portion of the lid comprises a lid article according to any one of claims 26 to 45.
48. A cover product for a sensor, comprising: a substrate comprising a thickness of 50 μm to 5000 μm, an outer major surface and an inner major surface, wherein the outer major surface and the inner major surface are opposite to each other, and the substrate is a chemically strengthened glass substrate or a glass ceramic substrate; and an outer layer film disposed on an outer major surface of the substrate, wherein the outer layer film comprises a plurality of alternating high refractive index layers and low refractive index layers, wherein each high refractive index layer comprises nitride or oxynitride and has a refractive index greater than that of each low refractive index layer, wherein the outer layer film comprises an anti-scratch layer having a thickness of about 80 nm to 10,000 nm, wherein one of the low refractive index layers is a cap layer defining the outermost surface of the outer layer film, and the thickness of the cap layer is at least 110 nm, wherein the outer layer film comprises an anti-reflection region above the anti-scratch layer, and the thickness of the anti-reflection region is about 100 nm to about 525 nm, The total thickness of the low refractive index layer in the anti-reflection zone is less than 275 nm, wherein the outer layer film exhibits a hardness of at least 8 GPa as measured by a Berkovich indentation hardness test to a depth of about 100 nm to about 500 nm from the outermost surface of the outer layer film, and Further wherein the cover article exhibits a first surface average reflectivity of less than 10% at a wavelength of 1000 nm to 1700 nm at at least one incident angle of 8° to 60°.
49. The lid article of claim 48, wherein the lid article further exhibits a dual surface average transmittance greater than 85% for infrared wavelengths from 1000 nm to 1700 nm at at least one incident angle from 8° to 40°.
50. The lid article of claim 48 or 49, wherein the lid article further exhibits a dual surface average transmittance greater than 75% at an incident angle of 60° for infrared wavelengths between 1000 nm and 1700 nm.
51. The cover article of any one of claims 48 to 50, wherein the cover article exhibits a first surface average reflectivity of less than 5% for infrared wavelengths from 1000 nm to 1700 nm at at least one incident angle from 8° to 40°.
52. The cover article of any one of claims 48 to 51, wherein the cover article further exhibits a first surface average reflectivity of 2% to 5% at an incident angle of 8° for wavelengths of 800 nm to 1000 nm.
53. The cover product of any one of claims 48 to 52, wherein the cover product further exhibits a first surface reflectance CIE color at all angles of incidence from 0° to 90°, wherein a* is from -10 to +10 and b* is from -12 to +5 (CIE coordinates b*), as measured under illumination with a D65 illuminant.
54. The cover article according to any one of claims 48 to 53, wherein the anti-scratch layer and each high refractive index layer comprises SiN x or SiO x N y .
55. The cover article of any one of claims 48 to 54, wherein the cover article exhibits a first surface average light reflectance of less than 2% at an incident angle of about 8°.
56. The lid article of any one of claims 48 to 55, wherein the cap layer has a thickness of 110 nm to about 200 nm.
57. The cover article of any one of claims 48 to 56, wherein the high refractive index layer adjacent to the cap layer has a thickness of about 10 nm to less than 150 nm.
58. The lid article of any one of claims 48 to 57, wherein the outer layer film exhibits a residual compressive stress greater than or equal to 700 MPa and an elastic modulus greater than or equal to 140 GPa.
59. The cover article of any one of claims 48 to 58, wherein the substrate is a glass-ceramic comprising an elastic modulus greater than 85 GPa and a fracture toughness greater than 0.8 MPa·√m.
60. The lid article of any one of claims 48 to 59, wherein the outer layer film exhibits a residual compressive stress of 700 MPa to 1100 MPa and an elastic modulus of 140 GPa to 200 GPa.
61. The lid article of any one of claims 48 to 60, wherein the outer layer film exhibits an elastic modulus of 140 GPa to 180 GPa.
62. The cover article of any one of claims 48 to 61, wherein the substrate has a residual surface compressive stress of 200 MPa to 1200 MPa and a depth of compression (DOC) of 5 microns to 150 microns.
63. The cover article of any one of claims 48 to 62, wherein the substrate further exhibits a maximum central tension (CT) value of 80 MPa to 200 MPa, and further wherein the substrate has a thickness of about 1.5 mm or less.
64. The cover article of any one of claims 48 to 63, wherein the substrate has a residual surface compressive stress of 200 MPa to 400 MPa.
65. The lid article of any one of claims 48 to 64, wherein the lid article exhibits an average stress at failure of 800 MPa or greater in a Ring-on-Ring test with the outer surface of the outer layered film under tension.
66. A glass screen protector for a smartphone, comprising: cover glass; and an adhesive backing disposed on the cover glass, wherein the adhesive backing is for attachment to a smartphone, and Further wherein at least a portion of the cover glass comprises a cover product according to any one of claims 48 to 65.
67. A consumer electronic product comprising: A housing, the housing comprising a front surface, a rear surface and a side surface; an electronic assembly at least partially located within the housing, the electronic assembly comprising at least one of a display and a sensor, the display being located at or proximate to a front surface of the housing, the sensor being located at or proximate to a front surface or a rear surface of the housing; and a cover disposed over at least one of the display and the sensor, Wherein at least a portion of the lid comprises a lid article according to any one of claims 48 to 65.
68. A cover product for a sensor, comprising: a substrate comprising a thickness of 50 μm to 5000 μm, an outer major surface and an inner major surface, wherein the outer major surface and the inner major surface are opposite to each other, and the substrate is a chemically strengthened glass substrate or a glass ceramic substrate; and an outer layer film disposed on an outer major surface of the substrate, wherein the cover article exhibits a first surface average reflectivity of less than 10% at at least one incident angle of 8° to 60° for wavelengths of 1000 nm to 1700 nm, and Further wherein the outer layer membrane exhibits a residual compressive stress greater than or equal to 700 MPa and an elastic modulus greater than or equal to 140 GPa.
69. The cover article of claim 68, wherein the outer layer film comprises an anti-scratch layer having a thickness of about 80 nm to 10,000 nm, the anti-scratch layer comprising a nitride or an oxynitride.
70. The cover article of claim 69 wherein the outer layer film comprises a refractive index gradient.
71. The cover product of claim 69, wherein the outer layered film comprises a plurality of alternating high refractive index layers and low refractive index layers, wherein each high refractive index layer comprises a nitride or an oxynitride, and wherein the refractive index of each high refractive index layer is greater than the refractive index of each low refractive index layer.
72. The lid article of any one of claims 68 to 71, wherein the outer layer film exhibits a residual compressive stress of 700 MPa to 1100 MPa and an elastic modulus of 140 GPa to 200 GPa.
73. The lid article of any one of claims 68 to 72, wherein the outer layer film exhibits an elastic modulus of 140 GPa to 180 GPa.
74. The cover article of any one of claims 68 to 73, wherein the substrate has a residual surface compressive stress of 200 MPa to 1200 MPa and a depth of compression (DOC) of 5 microns to 150 microns.
75. The cover article of any one of claims 68 to 74, wherein the substrate further exhibits a maximum central tension (CT) value of 80 MPa to 200 MPa, and further wherein the substrate has a thickness of about 1.5 mm or less.
76. The cover article of any one of claims 68 to 75, wherein the substrate has a residual surface compressive stress of 200 MPa to 400 MPa.
77. The lid article of any one of claims 68 to 76, wherein the lid article exhibits an average stress at failure of 800 MPa or greater in a ring-on-ring test with the outer surface of the outer layered film under tension.
78. The cover article of any one of claims 68 to 77, wherein the substrate is a glass-ceramic comprising an elastic modulus greater than 85 GPa and a fracture toughness greater than 0.8 MPa·√m.
79. A glass screen protector for a smart phone, comprising: cover glass; and an adhesive backing disposed on the cover glass, wherein the adhesive backing is for attachment to the smartphone, and Further wherein at least a portion of the cover glass comprises a cover product according to any one of claims 68 to 78.
80. A consumer electronic product comprising: A housing, the housing comprising a front surface, a rear surface, and a plurality of side surfaces; a plurality of electronic components at least partially within the housing, the electronic components including at least one of a display at or adjacent to the front surface of the housing and a sensor at or adjacent to the front surface or the rear surface of the housing; and a cover disposed over at least one of the display and the sensor, Wherein at least a portion of the cover comprises a cover article according to any one of claims 68 to 78.
81. A cover product for a sensor, comprising: a glass-ceramic substrate comprising a first major surface and a second major surface, the major surfaces being opposite to each other; and an outer layer membrane, the outer layer membrane defining an outer surface, the outer layer membrane being disposed on the first major surface, wherein the lid article exhibits a hardness greater than 15 GPa as measured by the Berkovich Hardness Test at an indentation depth of about 125 nanometers into the outer surface of the outer layer film, and Further wherein the cover article exhibits a first surface average reflectivity of less than 10% at at least one incident angle of 8° to 60° for wavelengths of 1000 nanometers to 1700 nanometers.
82. The lid product according to claim 81, in: The outer layer film comprises a scratch resistant layer and a plurality of alternating high refractive index (RI) layers and low RI layers, The outer layered film further comprises an outer structure and an inner structure, wherein the anti-scratch layer is disposed between the outer structure and the inner structure. The outer structure comprises at least one medium RI layer in contact with the high RI layer and the anti-scratch layer, The refractive index of the medium RI layer is between 1.55 and 1.80, the refractive index of each high RI layer is greater than 1.80, and the refractive index of each low RI layer is less than 1.55, and The glass-ceramic substrate comprises an elastic modulus greater than 85 GPa and a fracture toughness greater than 0.8 MPa·√m.
83. The lid article of claim 81 or 82, wherein the outer layer film exhibits a residual compressive stress greater than or equal to 700 MPa and an elastic modulus greater than or equal to 140 GPa.
84. The lid article of any one of claims 81 to 83, wherein the outer layer film exhibits a residual compressive stress of 700 MPa to 1100 MPa and an elastic modulus of 140 GPa to 200 GPa.
85. The lid article of any one of claims 81 to 84, wherein the outer layer film exhibits an elastic modulus of 140 GPa to 180 GPa.
86. The cover article of any one of claims 81 to 85, wherein the glass ceramic substrate has a residual surface compressive stress of 200 MPa to 1200 MPa and a depth of compression (DOC) of 5 microns to 150 microns.
87. The cover article of any one of claims 81 to 86, wherein the glass-ceramic substrate further exhibits a maximum central tension (CT) value of 80 MPa to 200 MPa, and further wherein the glass-ceramic substrate has a thickness of about 1.5 mm or less.
88. The cover article of any one of claims 81 to 87, wherein the glass ceramic substrate has a residual surface compressive stress of 200 MPa to 400 MPa.
89. The lid article of any one of claims 81 to 88, wherein the lid article exhibits an average stress at failure of 700 MPa or greater in a ring-on-ring test with the outer surface of the outer layered film under tension.
90. The lid article of any one of claims 81 to 89, wherein the lid article exhibits an average stress at failure of 500 MPa or greater in a four point bend test with the outer surface of the outer layered film under tension.
91. The lid article of any one of claims 81 to 90, wherein the lid article exhibits a hardness greater than 17 GPa as measured by the Berkovich Hardness Test at an indentation depth of about 125 nm into the outer surface of the outer layered film.
92. A glass screen protector for a smart phone, comprising: cover glass; and an adhesive backing disposed on the cover glass, wherein the adhesive backing is used to attach to the smartphone, and Further wherein at least a portion of the cover glass comprises a cover product according to any one of claims 81 to 91.
93. A consumer electronic product comprising: A housing, the housing comprising a front surface, a rear surface, and a plurality of side surfaces; a plurality of electronic components at least partially within the housing, the electronic components including at least one of a display at or adjacent to the front surface of the housing and a sensor at or adjacent to the front surface or the rear surface of the housing; and a cover disposed over at least one of the display and the sensor, Wherein at least a portion of the cover comprises a cover product according to any one of claims 81 to 91.
Citation Information
Cited By
Optical film and application thereof
CN122018055A
Optical film and applications thereof
CN122018055B