Expansion control for bonding

By vertically oriented growth of copper grains at the bonding interface of semiconductor devices and low-temperature annealing, combined with surface activation treatment and alloying elements to form an alloy, the problem of insufficient bonding strength without gaps or binders in semiconductor devices is solved, achieving efficient and reliable metal-to-metal bonding.

CN118922933APending Publication Date: 2024-11-08ADEIA SEMICONDUCTOR BONDING TECHNOLOGIES INC
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380027629.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-16
Filing Date
2023-03-14
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

In the existing technology, the bonding method of conductive pads of semiconductor components is difficult to achieve efficient and reliable adhesive-free bonding, resulting in gaps at the bonding interface and insufficient bonding strength.

Method used

The direct metal-to-metal bonding technology is employed, which involves vertically oriented growth of copper grains at the bonding interface, low-temperature annealing of copper material with 111 crystal planes, activation and termination treatment of the bonding surface, formation of alloying elements to increase bonding strength, and full metal-to-metal bonding achieved by controlling cell size and thermal expansion coefficient.

Benefits of technology

It achieves efficient, seamless, adhesive-free metal-to-metal bonding at low temperatures, improving bonding strength and reliability while reducing thermal budget consumption.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118922933A_ABST
    Figure CN118922933A_ABST
Patent Text Reader

Abstract

Disclosed are an element and a bonding structure including the element. The element may include: a non-conductive region having a cavity extending at least partially through a thickness of the non-conductive region from a contact surface; and a contact feature formed in the cavity. The non-conductive region is configured to be directly bonded to the non-conductive region of the second element. The contact pad of the element is configured to be directly bonded to the contact pad of the second element. The contact pad may include a first conductive material and a second conductive material. The first conductive material may have a cell size larger than a cell size of the second conductive material. The first conductive material may be a metal alloyed material. The first conductive material may be a metal silicide, and the second conductive material may be a metal. The bonded conductive contact may include a conductive material and an alloying element, and an amount of the alloying element may vary with a thickness of the bonded conductive contact.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] CROSS-REFERENCE TO RELATED APPLICATIONS

[0002] This application claims priority to U.S. Provisional Patent Application No. 63 / 320,525, filed on March 16, 2022, entitled “EXPANSION CONTROL FOR BONDING,” which is incorporated herein by reference in its entirety. Technical Field

[0003] The field relates to conductive features with controllable expansion rates. Background Art

[0004] Semiconductor elements (such as integrated device dies or chips) can be mounted or stacked on other elements. For example, semiconductor elements can be mounted to a carrier (such as a package substrate, an interposer, a reconstituted wafer or element, etc.). As another example, a semiconductor element can be stacked on top of another semiconductor element, for example, a first integrated device die can be stacked on a second integrated device die. Each of the semiconductor elements can have a conductive pad for mechanically and electrically bonding the semiconductor elements to each other. There is a continuing need for improved methods for forming conductive pads for reliable bonding. BRIEF DESCRIPTION OF THE DRAWINGS

[0005] The detailed description is set forth with reference to the accompanying drawings.In the drawings, the use of the same reference numerals in different drawings indicates similar or equivalent items.

[0006] For this discussion, the devices and systems illustrated in the drawings are shown as having multiple components. As described herein, various embodiments of the devices and / or systems may include fewer components and remain within the scope of the present disclosure. Alternatively, other embodiments of the devices and / or systems may include additional components or various combinations of the described components and remain within the scope of the present disclosure.

[0007] Figure 1A is a schematic cross-sectional side view of a structure including two elements before annealing according to an embodiment.

[0008] Figure 1B is a schematic cross-sectional side view of a bonded structure after annealing according to an embodiment.

[0009] FIG. 2A to FIG. 2E The formation according to the embodiment is shown Figure 1B Schematic cross-sectional views of the various steps in the process of bonding structures.

[0010] Figure 3 and Figure 4 Shown can be used for Figure 1A and Figure 1BMaterial properties of various materials for the contact pads shown in FIG.

[0011] Figure 5 is a schematic cross-sectional side view of a structure according to an embodiment.

[0012] Figure 6 According to the embodiment, the annealing Figure 5 Schematic cross-sectional side view of the combined structure after the structure of .

[0013] Figure 7 Shows the material properties of various metals combined with copper.

[0014] Fig. 8A is a schematic cross-sectional side view of an element according to an embodiment.

[0015] Figure 8B It is annealing Fig. 8A Schematic cross-sectional side view of an element following an element of .

[0016] 9A to 9F Schematic cross-sectional views showing various steps in a process of forming a bonding structure according to an embodiment. DETAILED DESCRIPTION

[0017] The present disclosure describes methods for controlling the growth and expansion of metal grains of conductive pads in components (such as microelectronic components). Various embodiments disclosed herein may be advantageous for direct metal bonding (such as direct hybrid bonding). For example, two or more semiconductor components (such as integrated device dies, wafers, etc.) may be stacked or combined with each other to form a combined structure. The conductive contact pads of one component may be electrically connected to the corresponding conductive contact pads of another component. Any suitable number of components may be stacked in the combined structure. The methods and bonding pad structures described herein may also be useful in other contexts.

[0018] In some embodiments, the elements are directly bonded to each other without an adhesive. In various embodiments, the non-conductive (e.g., semiconductor or inorganic dielectric) material of the first element can be directly bonded to the corresponding non-conductive (e.g., semiconductor or inorganic dielectric) field region of the second element without an adhesive. In various embodiments, the conductive region (e.g., metal pad) of the first element can be directly bonded to the corresponding conductive region (e.g., metal pad) of the second element without an adhesive. The non-conductive material can be referred to as a non-conductive bonding region or bonding layer of the first element. In some embodiments, the non-conductive material of the first element can be directly bonded to the corresponding non-conductive material of the second element using a bonding technique without an adhesive, using at least the direct bonding techniques disclosed in U.S. Patent Nos. 9,564,414; 9,391,143; and 10,434,749, the entire contents of each of which are incorporated herein by reference in their entirety and for all purposes. In other applications, in a bonding structure, the non-conductive material of the first element can be directly bonded to the conductive material of the second element so that the conductive material of the first element is tightly matched with the non-conductive material of the second element.

[0019] In various embodiments, direct bonding can be formed without an intervening adhesive. For example, the semiconductor or dielectric bonding surface can be polished to a high degree of smoothness. The bonding surface can be cleaned and exposed to a plasma and / or an etchant to activate the surface. In some embodiments, the surface can be terminated with a substance after or during activation (e.g., during a plasma and / or etching process). Without being limited by theory, in some embodiments, an activation process can be performed to break chemical bonds at the bonding surface, and a termination process can provide additional chemicals at the bonding surface, thereby increasing the bonding energy during direct bonding. In some embodiments, activation and termination are provided in the same step, for example, activating and terminating the surface with a plasma or a wet etchant. In other embodiments, the bonding surface can be terminated in a separate process to provide additional substances for direct bonding. In various embodiments, the termination substance can include nitrogen. In addition, in some embodiments, the bonding surface can be exposed to fluorine. For example, there may be one or more fluorine peaks near the layer and / or bonding interface. Therefore, in a directly bonded structure, the bonding interface between the two non-conductive materials can include a very smooth interface with a higher nitrogen content and / or fluorine peak at the bonding interface. Additional examples of activation and / or termination treatments can be found in U.S. Patent Nos. 9,564,414; 9,391,143; and 10,434,749, the entire contents of each of which are incorporated herein by reference in their entirety and for all purposes.

[0020] In various embodiments, the conductive contact pads of the first element may also be directly bonded to the corresponding conductive contact pads of the second element. For example, direct hybrid bonding techniques may be used to provide conductor-to-conductor direct bonding along a bonding interface comprising a covalently directly bonded dielectric-to-dielectric surface prepared as described above. In various embodiments, direct bonding of conductors to conductors (e.g., contact pads to contact pads) and hybrid bonding of dielectrics to dielectrics may be formed using direct bonding techniques disclosed at least in U.S. Patents Nos. 9,716,033 and 9,852,988, the entire contents of each of which are incorporated herein by reference in their entirety and for all purposes. The bonding structures described herein may also be used for direct metal bonding without bonding to non-conductive regions, or for other bonding techniques.

[0021] In some embodiments, as described above, inorganic dielectric bonding surfaces can be prepared and directly bonded to each other without an intervening adhesive. Conductive contact pads (which can be surrounded by non-conductive dielectric field regions) can also be directly bonded to each other without an intervening adhesive. In some embodiments, the corresponding contact pads can be recessed below the outer (e.g., upper) surface of the dielectric field or non-conductive bonding region, for example, recessed less than 30nm, less than 20nm, less than 15nm, or less than 10nm, for example, recessed in the range of 2nm to 20nm or in the range of 4nm to 10nm. In some embodiments, the non-conductive bonding regions can be directly bonded to each other at room temperature without an adhesive, and then the bonded structure can be annealed. During annealing, the contact pads can expand relative to the non-conductive bonding regions and contact each other to form a metal-to-metal direct bond. It is beneficial to use a hybrid bonding technique, such as a direct bonding interconnect or a hybrid bonding technique available from Adeia, Inc. of San Jose, California. A high density of pads (eg, a regular array of small or fine pitch) connected across a direct bonding interface can be achieved. In various embodiments, the contact pads may include copper, although other metals may also be suitable.

[0022] Thus, in a direct bonding process, a first element may be directly bonded to a second element without an intervening adhesive. In some arrangements, the first element may include a singulated element (such as a singulated integrated device die). In other arrangements, the first element may include a carrier or substrate (e.g., a wafer) that includes a plurality of (e.g., tens, hundreds, or more) device regions that, when singulated, form a plurality of integrated device dies. Similarly, the second element may include a singulated element (such as a singulated integrated device die). In other arrangements, the second element may include a carrier or substrate (e.g., a wafer).

[0023] As described herein, the first element and the second element can be directly bonded to each other without an adhesive, which is different from a deposition process. The first element and the second element can include non-deposition elements accordingly. In addition, unlike the deposition layer, the direct bonding structure can include a defective region along the bonding interface, in which there is a nanovoid. The nanovoid may be formed due to the activation of the bonding surface (e.g., exposure to plasma). As described above, the bonding interface can include material concentrations from activation and / or the last chemical treatment process. For example, in an embodiment activated by nitrogen plasma, a nitrogen peak can be formed at the bonding interface. In an embodiment activated by oxygen plasma, an oxygen peak can be formed at the bonding interface. In some embodiments, the bonding interface can include silicon oxynitride, silicon oxycarbonitride, or silicon carbonitride, wherein the nitrogen level present at the bonding interface indicates that the nitrogen of at least one element in the element before direct bonding is terminated. In some embodiments, nitrogen and nitrogen-related parts may not be present at the bonding interface. As described herein, direct bonding can include a covalent bond, which is stronger than a van der Waals bond. The bonding layer can also include a polished surface that is flattened to a high degree of smoothness.

[0024] In various embodiments, the metal-to-metal bond between the contact pads may be bonded so that the copper grains grow into each other across the bonding interface. In some embodiments, the copper may have grains vertically oriented along the 111 crystal planes for improving copper diffusion across the bonding interface. In some embodiments, the orientation error of the 111 crystal planes in the conductive material may be within a range of ±30° relative to the vertical direction of the surface of the conductive material. In some embodiments, the crystal orientation error may be within a range of ±20°, or within a range of ±15° relative to the vertical direction. The bonding interface may extend substantially completely to at least a portion of the bonding contact pads so that there is substantially no gap between the non-conductive bonding areas at or near the bonding contact pads. In some embodiments, a barrier layer may be provided under the contact pads (e.g., which may include copper). However, in other embodiments, there may be no barrier layer under the contact pads, for example, as described in U.S. Pat. No. 11,195,748, which is incorporated herein by reference in its entirety and for all purposes.

[0025] The annealing temperature and annealing duration used to form a metal-to-metal direct bond may affect the consumption of the thermal budget by the annealing. It may be desirable to reduce the annealing temperature and / or reduce the annealing duration to minimize the consumption of the thermal (energy) budget. <111> ) can be 3 to 4 orders of magnitude faster than surface diffusion along 100 or 110 crystal planes. In addition, a metal (e.g., Cu) having grains oriented along 111 crystal planes can have a higher surface mobility than conventional back-end-of-line (BEOL) copper. In addition, low-temperature direct metal-to-metal bonding is achieved by higher creep rates on the 111 faces of Cu and reconstruction of the surface of the conductive pad. Therefore, in order to shorten the annealing time and / or reduce the annealing temperature for direct bonding (e.g., direct hybrid bonding), it may be advantageous to have 111 crystal planes on the bonding surface. The advantages of having 111 crystal planes may be particularly evident at lower temperatures because metal surface diffusion (e.g., Cu surface diffusion) is also slowed down when the annealing temperature is reduced. Accordingly, in various embodiments disclosed herein, the crystal structure may have grains with a 111 texture that are preferentially oriented vertically or parallel to the bonding surface to enhance metal diffusion (e.g., copper diffusion) during direct bonding. In some embodiments, the orientation error of the 111 crystal plane in the conductive material can be within a range of ±30° relative to the vertical direction of the surface of the conductive material. In some embodiments, the crystal orientation error can be within a range of ±20°, or within a range of ±15° relative to the vertical direction.

[0026] The metal layer can be formed using a process selected to electroplate a copper (Cu) layer having Cu in a 111 crystal orientation. For example, the Cu layer can be deposited from a non-superfilled or superfilled electroplating bath using an electroplating chemistry selected to optimize the effective filling of voids (e.g., vias, trenches) in the substrate rather than optimizing the direct metal-to-metal bonding that occurs during direct hybrid bonding. The subsequent metal treatment described below can facilitate subsequent bonding, so that any desired electroplating chemistry can be adopted to optimize for other considerations (such as the above-mentioned filling). For example, the microstructure (e.g., grain size) of the deposited or applied metal layer can be stabilized by an annealing step that is separate from the annealing step of the direct hybrid bonding that occurs subsequently.

[0027] As described above, the contact pads can expand relative to the non-conductive bonding area and contact each other to form a metal-to-metal direct bond. Adequate expansion during annealing can facilitate successful metal-to-metal bonding. For example, the expansion of the contact pad can be primarily caused by thermal expansion of the material of the contact pad (e.g., copper) relative to the non-conductive bonding area. In some embodiments, by judiciously utilizing a material having a relatively larger atomic unit cell than, for example, a unit cell of copper to form the contact pad, the bonding temperature (e.g., annealing temperature) for bonding the contact pad can be reduced. The increase in the unit cell size of the contact pad can at least partially cause the contact pad to expand. The unit cell size can be referred to as the volume of an atomic unit cell of a material at room temperature at sea level or at atmospheric pressure. Room temperature can be about 25°C, and sea level or atmospheric pressure can be about 101325 Pa or 760 mm Hg. The unit cell is the smallest part of the crystal lattice that shows the three-dimensional pattern of the entire crystal. For example, at room temperature at atmospheric pressure, cobalt has The unit cell size of titanium is The unit cell size of nickel is The unit cell size of silicon is The unit cell size of the contact pad may be 100%. Some contact pad materials may have a lower thermal expansion rate than other materials, and some contact pad materials may be more expensive or unsuitable for direct bonding than other materials. Various embodiments disclosed herein use two or more different types of conductive materials to form contact pads, thereby providing sufficient direct bonding between contact pads at a relatively low material cost and a relatively low thermal budget. For example, the contact pad may include two or more types of conductive materials that provide greater thermal expansion than one type of conductive material to provide such sufficient direct bonding.

[0028] Figure 1A is a schematic cross-sectional side view of a structure 1 including two elements (eg, a first element 2 and a second element 3 ) before annealing according to an embodiment. Figure 1B The bonding structure 1' (after annealing) according to the embodiment Figure 1A Schematic cross-sectional side view of the structure 1).

[0029] The first element 2 may include a non-conductive region 10 (e.g., a non-conductive or dielectric field region), a barrier layer 12, and a contact pad or conductive feature 14. The contact pad 14 may include a first conductive material 16 and a second conductive material 18. Similarly, the second element 3 may include a non-conductive region 20 (e.g., a non-conductive or dielectric field region), a barrier layer 22, and a contact pad or conductive feature 24. The contact pad 24 may include a first conductive material 26 and a second conductive material 28. The first element 2 and the second element 3 may be bonded to each other along a bonding interface 30. In some embodiments, the non-conductive region 10 and the non-conductive region 20 may be directly bonded to each other without an intervening adhesive. In some embodiments, the second conductive material 18 of the first element 2 and the second conductive material 28 of the second element 3 may be directly bonded to each other without an intervening adhesive. Although in the illustrated embodiment, the structure 1 and the bonded structure 1' include the same elements 2, 3, in some embodiments, the structures 1, 1' may have different elements that are bonded together.

[0030] The barrier layer 12 may be disposed between the non-conductive material 10 and the contact pads 14. In some embodiments, the barrier layer 12 may isolate the non-conductive material 10, 20 and the contact pads 14, 24 to prevent or mitigate diffusion of the conductive material 16, 18, 26, 28 into the non-conductive material 10, 20. In some embodiments, the barrier layer 12 may include a sputtered cobalt layer.

[0031] In some embodiments, the thermal expansion rate, volume growth rate, and / or unit cell size of the first conductive material 16 may be greater than the thermal expansion rate, volume growth rate, and / or unit cell size of the second conductive material 18. Certain material properties of the first conductive material 16 and the second conductive material 18 (such as thermal expansion rate, volume growth rate, and unit cell size) may change depending on ambient conditions. For example, the material properties of the first conductive material 16 and the second conductive material 18 may change depending on temperature or pressure. Those skilled in the art will understand that when conditions are not specified, the ambient conditions are at sea level at room temperature. When the properties of two or more materials are compared herein, the properties of the materials under the same conditions are compared.

[0032] In some embodiments, the first conductive material 16 has a volume growth rate of at least 10% relative to a volume growth rate of a material of the second conductive material 18 or a back-end of line (BEOL) layer (not shown) below the first conductive material 16 and the second conductive material 18. For example, the first conductive material 16 may have a volume growth rate in a range between 10% and 500%, between 10% and 275%, between 50% and 500%, or between 50% and 275% relative to a volume growth rate of a material of the second conductive material 18 or a back-end of line (BEOL) layer (not shown) below the first conductive material 16 and the second conductive material 18. In some embodiments, a unit cell size of the first conductive material 16 may be at least 1.3 times larger than a unit cell size of the second conductive material 18. For example, a unit cell size of the first conductive material 16 may be at least 1.5 times, 2 times, 3 times, or 5 times larger than a unit cell size of the second conductive material 18. In some embodiments, the first conductive material 16 may include a metal silicide or an alloy-forming metal. For example, some example materials for the first conductive material 16 may be at least 1.5 times, 2 times, 3 times, or 5 times larger than a unit cell size of the second conductive material 18. Figure 3 to Figure 4 Found in. In some embodiments, when annealed at a specific temperature, the volume expansion of the alloy formed between the first conductive material 16 and the second conductive material 18 can be at least 10% higher than the volume expansion of the first conductive material 16 or the second conductive material 18. Additionally, other embodiments may have an element including one or more BEOL layers. The BEOL layer may include a metallization layer (conductive traces embedded in an insulating layer) formed (e.g., deposited) over the back side of the barrier layer of the element 1, 2. For example, the metallization layer may be formed directly over the back side of the barrier layer so as to contact the barrier layer. In some embodiments, the BEOL layer may include multiple layers, and the uppermost layer of the BEOL layer may include a bonding layer. The volume expansion of the bonding layer (conductive material 18, 28) of the first conductive feature or the second conductive feature is at least 10% higher than the volume expansion of the BEOL layer below the bonding layer. As disclosed herein, selecting the materials of the first conductive material 16 and the second conductive material 18 may be critical to providing sufficient direct bonding between the contact pads 14, 24 at a relatively low material cost and a relatively low thermal budget.

[0033] In some embodiments, the first conductive material 16 can be buried under the second conductive material 18 (e.g., at least partially disposed under the second conductive material 18). For example, the first conductive material 16 can be completely buried under the second conductive material 18. Figure 1BAs shown, the second conductive material 18 can be completely enclosed in the space between the barrier layer 12 and the overlying second conductive material 18. In some embodiments, the first conductive material 16 and the second conductive material 18 can be combined with each other to form an alloy. The thermal expansion rate or unit cell size of the formed alloy can be greater than the thermal expansion or unit cell size of the precursor material (first conductive material 16 or 18). In some other embodiments, the first conductive material 16 and the second conductive material 18 may not be combined with each other.

[0034] In some embodiments, the first conductive material 16 may be exposed on the contact surface of the contact pad 14. In some embodiments, it may be beneficial to select a material for the second conductive material 18, 28 that is compatible with a chemical mechanical polishing (CMP) process in preparation for direct bonding. A material having a hardness that does not cause over-smearing or dishing during the polishing process may be a CMP compatible material. Because the first conductive material 16, 26 is embedded below the second conductive material 18, 28, the first conductive material 16, 26 may or may not be compatible with the CMP process.

[0035] The thickness of the first conductive material 16 can be thinner than the thickness of the second conductive material 18. The thickness of the first conductive material 16, 26 can be determined at least in part by the expansion rate of the material of the first conductive material 16, 26 and the gap between the contact pads 14, 24 before annealing. In some embodiments, depending on the depth of the cavity, the thickness of the first conductive material 16, 26 can be in a range of, for example, 20nm to 20000nm, 30nm to 17500nm, 40nm to 15000nm, 50nm to 10000nm, 50nm to 7000nm, or 50nm to 500nm. Selecting the thickness of the first conductive material 16, 26 from these ranges can help provide sufficient direct bonding between the contact pads 14, 24 with relatively low material cost and relatively low thermal budget.

[0036] FIG. 2A to FIG. 2E Schematic cross-sectional views of various steps in the process of forming a bonding structure 1' according to an embodiment are shown. Figure 2A , a cavity 19 may be formed in the non-conductive material 10. In some embodiments, the cavity 19 may be formed by selectively etching the non-conductive material 10. Figure 2B, a barrier layer 12 and a first conductive material 16 may be provided in the cavity 19. The first conductive material 16 may include a plurality of constituent elements 16a, 16b. For example, the barrier layer 12 and the first conductive material 16 may be provided by atomic layer deposition (ALD), sputtering and electroplating or a combination thereof. The electroplating step may include electroless deposition or electrolytic deposition. At least a portion of the first conductive material 16 may be removed by, for example, an etching (e.g., dry or wet etching) process and / or a photolithography process. Figure 2C In some embodiments, the second barrier layer 13 may be provided in the cavity above the first conductive material 16. In some embodiments, the first conductive material 16 may be enclosed between the first barrier layer 12 and the second barrier layer 13. In other embodiments, the second barrier layer 13 may not be provided (see Figure 1A ).exist Figure 2D , a second conductive material 18 can be provided. The surface of the non-conductive material 10 and / or the surface of the second conductive material 18 can be polished, for example, by CMP, to prepare the element for direct bonding to another element. In some embodiments, after polishing the surface of the non-conductive material 10 and / or the surface of the second conductive material 18, the surface of the second conductive material 18 can be recessed relative to the surface of the non-conductive material 10. Figure 2E , the element can be directly bonded (e.g., directly mixed and bonded) to another element. After cleaning and activating the bonding surface of one or two elements by known methods, the element can be directly bonded. For example, the activation process can include at least one bonding surface in the bonding surface of the cleaning element to remove unwanted particles, and / or expose the bonding surface to one or more plasma treatments, rinse and dry the bonding surface. The rinse solvent used for rinsing can include deionized (DI) water or low molecular weight alcohol. The non-conductive material of the element can be directly bonded to the non-conductive material of another element. After combining the non-conductive materials of the two elements, the structure can be annealed at a higher temperature to bond the second conductive material to the contact pad of another element. In some embodiments, the first conductive material 16 can, for example, form an alloy with the first barrier layer 12 and / or the second barrier layer 13, and the alloy has a unit cell size larger than the unit cell size of the second conductive material 18. For example, the alloy can include a copper-zinc alloy, a magnesium alloy, or a cobalt silicide alloy.

[0037] Figure 3 and Figure 4 Shown can be used Figure 1A and Figure 1B Material properties of the various materials of the contact pads 14 , 24 are illustrated. Figure 3 The volume growth of the alloy shown in Figure 3 The alloy volume growth rate of each of the silicide alloys listed in compared to copper. Figure 3The silicide alloys listed in may be examples of the first conductive materials 16 , 26 . Figure 4 The materials listed in may be examples of first conductive materials 16, 26. In some embodiments, brass, bronze, or cadmium copper alloy may be electroplated into the inlay cavity from an alkaline bath including a suitable complexing agent. Figure 3 As shown, the first conductive material 16, 26 may include copper, titanium, nickel, brass, magnesium, manganese, zinc, tin, bronze, or cadmium. Beneficially, the incorporation of the embedded first conductive materials 16, 26 may reduce the annealing temperature sufficiently to cause metal expansion and direct electrical contact between opposing pads (e.g., between opposing second conductive materials 18, 28). The increased expansion properties of the first conductive materials 16, 26 compared to the second conductive materials 18, 28 may help improve direct bonding yields at lower temperatures while also providing a surface of the second conductive materials 18, 28 that is compatible with CMP used to prepare for direct bonding.

[0038] In some embodiments where the first conductive material 16, 26 includes nickel (Ni) and the second conductive material 18, 28 includes silicon (Si), a nickel silicide (Ni2Si) layer may be formed. For an element having a 2 μm thickness and a 20 nm contact recess before bonding, the thickness of the nickel silicide layer may be 27 nm or greater to compensate for the recess without thermal expansion coefficient (CTE) expansion, based on the 533% volume expansion of nickel silicide. The relationship between the change in recess (ΔL), volume expansion (V1), and layer thickness (L1) may be represented by the following equation (Equation 1) and is shown in the following table (Table 1).

[0039]

[0040] Material V1 L1 ΔL Ni2Si 533% 27nm 20nm

[0041] Table 1

[0042] In some embodiments, the first conductive material 16, 26 may include copper (Cu), and the second conductive material 18, 28 may include magnesium (Mg). Including a combination of copper and magnesium in the contact pad can reduce the annealing temperature for bonding the contact pad to a corresponding pad of another component compared to including only copper in the contact pad. For example, under some conditions, the annealing temperature can be reduced by about 125°C. The following table (Table 2) shows a comparison between some parameters of a copper pad (both the first conductive material and the second conductive material include copper) and a multilayer pad including 50% copper and 50% magnesium (the first conductive material includes magnesium, and the second conductive material includes copper).

[0043] parameter Cu Cu+Mg <![CDATA[α Cu ]]> 17 17 <![CDATA[α1]]> 17(Cu) 26(Mg) <![CDATA[L Cu ]]> 1um 1um <![CDATA[L1]]> 1um 1um ΔT 600C 475C ΔL 20nm 20nm

[0044] Table 2

[0045] In Table 2, α Cu represents the CTE of copper, α1 represents the CTE of the first conductive material, and L Cu represents the thickness of the copper layer (second conductive material), L1 represents the thickness of the second conductive material, ΔT represents the temperature change relative to the initial temperature of 25°C, and ΔL represents the concavity change before and after annealing. The relationship between these parameters can be expressed by the following equation (Equation 2):

[0046] ΔL=(α Cu L Cu +α1L1)ΔT (Equation 2.

[0047] Figure 5 is a schematic cross-sectional side view of a structure 4 including a first element 5 and a second element 6 before annealing according to an embodiment. Figure 6 The bonding structure 4' according to the embodiment (after annealing Figure 5 4). Unless otherwise stated, Figure 5 and Figure 6 The components shown can be used with Figure 1A and Figure 1B Similar components are identical or substantially similar.

[0048] The first element 5 may include a non-conductive region 10, a barrier layer 12, and a contact pad or conductive feature 44. The contact pad 44 may include a first conductive material 46, a first layer 48a of a second conductive material, and a second layer 48b of a second conductive material. In some embodiments, the first conductive material 46 may be vertically sandwiched between the first layer 48a and the second layer 48b. Similarly, the second element 6 may include a non-conductive region 20, a barrier layer 22, and a contact pad or conductive feature 54. The contact pad 54 may include a first conductive material 56, a first layer 58a of a second conductive material, and a second layer 58b of a second conductive material. The first element 5 and the second element 6 may be bonded to each other along the bonding interface 30 (e.g., directly mixed). In some embodiments, the non-conductive region 10 and the non-conductive region 20 may be directly bonded to each other without an intervening adhesive. In various embodiments, the first conductive materials 46, 56 may include alloying elements (e.g., alloying metals) that form a metal alloy with the second conductive material when annealed. For example, the first conductive material 46, 56 may include zinc (Zn), beryllium (Be), palladium (Pd), aluminum (Al), or a similar material. The annealing process may form the contact pads 44, 54 into different forms, thereby defining the contact pads 44', 54'. For example, the first conductive material 46, 56, the first layer 48a, 58a, and the second layer 48b, 58b may at least partially form the alloy 60, 62. During the annealing process, the first conductive material 46, 56, the first layer 48a, 58a, and the second layer 48b, 58b may at least partially form the alloy 60, 62. Figure 5After the structure 4 is formed, the contact pad 44' and the contact pad 54' can expand so as to contact each other and also form a metal alloy. When the alloys 60, 62 are formed before the annealing for bonding the contact pad 44' and the contact pad 54', the alloys 60, 62 can be compatible with the CMP process used to prepare for direct bonding. In some embodiments, the contact pad 44' and the contact pad 54' can be directly bonded to each other without an intervening adhesive. In some embodiments, the contact pad 44' and the contact pad 54' can include a gradient of alloying elements (e.g., a gradient of the first conductive material 46, 56). In the illustrated embodiment, the structure 4 and the bonded structure 4' include identical elements 5, 6, but in other embodiments, the structure 4 can have different elements bonded together. In some embodiments, the resistivity of the alloys 60, 62 formed by bonding elements 5 and 6 can be less than 20 times, less than 15 times, less than 10 times, or less than 5 times higher than the resistivity of the material of the BEOL layer below the bonding layer. For example, the alloys 60 , 62 may include a lower resistivity metal (eg, nickel), and the material of the BEOL layers may include a higher resistivity metal (eg, copper).

[0049] Figure 7 Example materials for the first conductive element are shown. Figure 7 The material properties of various metals combined with copper are also shown. The volume expansion of the pad can be calculated by the following equation (Equation 3):

[0050]

[0051] For example, when copper-zinc alloy (Cu3Zn) is applied to Equation 3, it can be expressed as follows:

[0052]

[0053] Fig. 8A is a schematic cross-sectional side view of an element 7 according to an embodiment. Figure 8B It is annealing Fig. 8A Schematic cross-sectional side view of element 7' following element 7. Unless otherwise stated, Fig. 8A and Figure 6 The components shown can be used with Figure 1A , Figure 1B , Figure 5 and Figure 6 Similar components are identical or substantially similar.

[0054] Element 7 may include non-conductive region 10, barrier layer 12, and contact pad or conductive feature 64. Contact pad 64 may include first conductive material 66, first layer 68a of second conductive material, and second layer 68b of second conductive material. In some embodiments, second layer 68b may be omitted. First conductive material 66 and second conductive material (first layer 68a and second layer 68b) may be selected to increase the roughness of the surface of alloyed conductive feature 70 during annealing. First conductive material 66 may be located at or near the contact surface of contact pad 64. In some embodiments, first conductive material 66 may be located within 25% of the thickness of contact pad 64 from its contact surface.

[0055] In some embodiments, the first conductive material 66 may include an alloyed material. In some embodiments, the first conductive material 66 may include a hexagonal crystal structure, and the second conductive material (the first layer 68a and the second layer 68b) may include a face-centered cubic structure. For example, the first conductive material 66 may include titanium, and the second conductive material (the first layer 68a and the second layer 68b) may include copper. After annealing the element 7, the contact pad 64 may form an orthorhombic crystal structure. When the orthorhombic crystal structure is formed, the surface roughness of the contact pad 64 may increase. Due to the formation of the orthorhombic crystal structure, the contact pad 64' may include spikes or whiskers. The surface roughness of the surface of the alloyed conductive feature 70 of the element 7 may be between 3nm and 100nm or between 3nm and 50nm. The surface roughness of the alloyed conductive feature 70 may be higher than the roughness of the bonding surface of the non-conductive region (which may be less than 1nm and preferably less than 0.5nm). The alloyed conductive feature 70 with a relatively rough surface morphology combined at an elevated temperature induces the corresponding conductive feature to more effectively bridge the recess between the conductive features. The bridging of the recesses induces physical contact (at lower temperatures) between metallic conductive features on opposing components to promote metallurgical bonding at lower temperatures.

[0056] 9A to 9F Schematic cross-sectional views of various steps in the process of forming a bonding structure 9 according to an embodiment are shown. Fig. 9A , a cavity 19 may be formed in the non-conductive material 10. In some embodiments, the cavity 19 may be formed by selective etching. Fig. 9B , the barrier layer 12, the first conductive material 66 and the second conductive material (e.g., the first layer 68a and the second layer 68b) may be provided in the cavity 19 and at least partially provided above the surface of the non-conductive material 10. For example, the first conductive material 66 and the second conductive material (the first layer 68a and the second layer 68b) may be provided by sputtering, electroplating, or a combination thereof. Fig. 9C, the surface of the non-conductive material 10 and / or the second layer 68b of the second conductive material may be polished by, for example, CMP to define an element (e.g., the first element 7). In some embodiments, the second layer 68b may be recessed relative to the surface of the non-conductive material 10. Fig.9D , after fully preparing at least one of the surfaces of the first element 7 and the second element 8 for bonding (e.g., direct hybrid bonding), the element (first element 7) can be bonded to another element (second element 8). The non-conductive material 10 of the first element 7' can be directly bonded to the non-conductive material 82 of the second element 8. After bonding the non-conductive materials 10, 82 of the two elements 7, 8, the structure can be annealed to bond the second conductive material 68b to the contact pad 80 of the second element 8. During the bonding process, the first conductive material 66 and the second conductive material (first layer 68a and second layer 68b) can at least partially form an alloy to define an alloyed conductive feature 70. Fig.9D , nano-roughened surfaces, spikes, protrusions or whiskers may be formed on the contact surfaces of the alloyed conductive features 70 and / or the contact pads 80 of the elements 7, 8. As described above, the nano-roughened bonding surface of the conductive material of the first element 7 or the second element 8 may be formed by judiciously selecting materials with different lattice symmetries for the first material 66 and the second material (the first layer 68a and the second layer 68b). Other known methods, for example, apply a dry or wet etchant to selectively and very slightly etch away a portion of the grain boundaries of the conductive material of the first element 7 or the second element 8. Fig.9E shows the first time period after combining the first element 7 and the second element 8 at an elevated temperature. Fig.9D The bonding structure 9. The contact pads of the elements 7, 8 may diffuse into each other over time. In some embodiments, in a first time period, a nano-scale roughened surface, spikes, protrusions or whiskers may be observed. Fig.9F The second time period after the combination of the first element 7 and the second element 8 is shown. Fig.9E The second time period is greater than the first time period. After the second time period, in some embodiments, the nano-roughened surface, spikes, protrusions, or whiskers may not be visible. In some other embodiments, after the second time period, the nano-roughened surface, spikes, protrusions, or whiskers may be observed.

[0057] In some embodiments, the bonded structures disclosed herein may include a void between a contact pad of one component and a contact pad of another component. The gas in the void may expand to push the material of the contact pad toward the inner surface.

[0058] In one aspect, a component having a contact surface is disclosed. The component may include: a non-conductive region, a cavity having a thickness extending at least partially from the contact surface through the non-conductive region; and a contact pad formed in the cavity. The contact pad includes a first conductive material and a second conductive material. The first conductive material has a unit cell size that is larger than a unit cell size of the second conductive material. The first conductive material is a metal alloy material. The non-conductive region is configured to be directly bonded to the non-conductive region of the second component, and the contact pad of the component is configured to be directly bonded to the contact pad of the second component.

[0059] In one embodiment, the unit cell size of the first conductive material is at least 1.3 times larger than the unit cell size of the second conductive material.

[0060] In one embodiment, the component further comprises a barrier layer conformally disposed along a surface of the cavity.

[0061] In one embodiment, the first conductive material is disposed between the bottom surface of the cavity and the second conductive material.

[0062] In one embodiment, the first conductive material is completely buried under the second conductive material.

[0063] In one embodiment, the first conductive material is not exposed.

[0064] In one embodiment, the second conductive material is copper.

[0065] In one embodiment, the first conductive material has a characteristic formation temperature below 230° C. The first conductive material may have a characteristic formation temperature below 130° C.

[0066] In one embodiment, the first conductive material is a metal silicide, which may include nickel, titanium or cobalt.

[0067] In one embodiment, the first conductive material includes zinc, titanium or nickel.

[0068] In one embodiment, the second conductive material includes a face-centered cubic structure, and the first conductive material includes a hexagonal crystal structure. The second conductive material may include copper, and the first conductive material may include titanium. The resistivity of the first conductive material may be greater than the resistivity of the second conductive material. The resistivity of the first conductive material may be less than 40 times the resistivity of the second conductive material. The resistivity of the first conductive material may be less than 20 times the resistivity of the second conductive material. The thickness of the second conductive material may be greater than the thickness of the first conductive material.

[0069] In one embodiment, the first conductive material is a chemical mechanical polishing compatible material.

[0070] In one aspect, a first element having a contact surface is disclosed. The first element may include: a non-conductive region, a cavity having a thickness extending at least partially from the contact surface through the non-conductive region; and a contact pad formed in the cavity. The contact pad includes a metal and a metal silicide. The metal silicide has a unit cell size that is larger than a unit cell size of the metal. The non-conductive region is configured to be directly bonded to the non-conductive region of a second element, and the metal is configured to be directly bonded to the contact pad of the second element.

[0071] In one embodiment, the first element further comprises a barrier layer conformally disposed along a surface of the cavity.

[0072] In one embodiment, the metal silicide is disposed between the bottom surface of the cavity and the metal.

[0073] In one embodiment, the metal silicide is completely buried under the metal.

[0074] In one embodiment, the metal is not exposed.

[0075] In one embodiment, the metal is copper.

[0076] In one embodiment, the metal silicide is a metal alloy material.

[0077] In one embodiment, the metal silicide has a characteristic formation temperature below 230°C.

[0078] In one embodiment, the metal silicide includes nickel, titanium, or copper.

[0079] In one embodiment, the resistivity of the metal silicide is greater than the resistivity of the metal. The resistivity of the metal silicide may be less than 40 times the resistivity of the metal. The resistivity of the metal silicide may be less than 20 times the resistivity of the metal.

[0080] In one embodiment, the thickness of the metal is greater than the thickness of the metal silicide.

[0081] In one embodiment, the metal and the metal silicide are non-reactive with each other.

[0082] In one embodiment, the metal includes copper and the metal silicide includes zinc.

[0083] In one embodiment, the metal silicide is a chemical mechanical polishing compatible material.

[0084] In one aspect, a bonded structure is disclosed. The bonded structure may include: a first element having a first non-conductive region and a first conductive feature; and a second element having a second non-conductive region and a second conductive feature, the second non-conductive region being directly bonded to the first non-conductive region, and the second conductive feature being directly bonded to the first conductive feature to define a bonded conductive contact. The bonded conductive contact includes a first conductive material and a second conductive material. The first conductive material has a unit cell size that is larger than a unit cell size of the second conductive material. The first conductive material is an alloy including the second conductive material.

[0085] In one embodiment, the bonded conductive contact includes a gradient of alloying elements.

[0086] In one aspect, a bonded structure is disclosed. The bonded structure may include: a first element having a first non-conductive region and a first conductive feature; and a second element having a second non-conductive region and a second conductive feature, the second non-conductive region being directly bonded to the first non-conductive region, and the second conductive feature being directly bonded to the first conductive feature to define a bonded conductive contact. The bonded conductive contact includes a first conductive material and a second conductive material. The first conductive material has a unit cell size that is larger than a unit cell size of the second conductive material. The first conductive feature includes a metal silicide.

[0087] In one embodiment, the first component further includes a barrier layer between the first non-conductive region and the first conductive feature.

[0088] In one embodiment, the metal silicide includes nickel, titanium, or copper.

[0089] In one aspect, a bonded structure is disclosed. The bonded structure may include: a first element having a first non-conductive region and a first conductive feature; and a second element having a second non-conductive region and a second conductive feature, the second non-conductive region being directly bonded to the first non-conductive region, the second conductive feature being directly bonded to the first conductive feature to define a bonded conductive contact. The bonded conductive contact includes a conductive material and an alloying element. The amount of the alloying element varies with the thickness of the bonded conductive contact.

[0090] In one embodiment, the first component further includes a barrier layer between the first non-conductive region and the first conductive feature.

[0091] In one embodiment, the first conductive feature comprises a metal silicide. The metal silicide may comprise nickel, titanium or copper.

[0092] In one embodiment, the bonded conductive contact comprises an orthorhombic crystal structure.

[0093] In one embodiment, the bonded conductive contact has a unit cell size that is larger than a unit cell size of the conductive material.

[0094] In one aspect, a bonded structure is disclosed. The bonded structure may include: a first element having a first non-conductive region and a first conductive feature; and a second element having a second non-conductive region and a second conductive feature, the second non-conductive region being directly bonded to the first non-conductive region, the second conductive feature being directly bonded to the first conductive feature to define a bonded conductive contact. The bonded conductive contact includes a crystal structure of lower symmetry than the first conductive feature.

[0095] In one embodiment, the bonded conductive contact includes an orthorhombic crystal structure or a hexagonal crystal structure.

[0096] In one embodiment, the bonded conductive contact includes a gradient of alloying elements.

[0097] In one embodiment, the first component further includes a barrier layer between the first non-conductive region and the first conductive feature.

[0098] In one embodiment, the bonded conductive contact comprises copper titanium.

[0099] In one aspect, a bonding structure is disclosed. The bonding structure may include a first element having a first contact surface. The first element includes: a first non-conductive region, a first cavity having a thickness extending at least partially from the first contact surface through the non-conductive region; and a first contact pad formed in the first cavity. The contact pad includes a first conductive material and a second conductive material. The first conductive material has a unit cell size larger than a unit cell size of the second conductive material. The first conductive material is a metal alloy material. The bonding structure may include a second element having a second contact surface directly bonded to the first contact surface. The second element includes a second non-conductive region directly bonded to the first non-conductive region and a second contact pad directly bonded to the first contact pad.

[0100] In one embodiment, the bonding structure further includes a barrier layer conformally disposed along a surface of the first cavity.

[0101] In one embodiment, the first conductive material is disposed between the bottom surface of the first cavity and the second conductive material. The first conductive material may be completely buried under the second conductive material. The directly bonded first contact pad and the directly bonded second contact pad may define a bonded conductive contact including an orthorhombic crystal structure. The directly bonded contact pad may include copper titanium.

[0102] In one embodiment, the directly bonded first and second contact pads define a bonded conductive contact including a gradient of alloying elements.

[0103] In one aspect, a method of forming an element is disclosed. The method may include: forming a cavity in a non-conductive material; providing a first conductive material having a first unit cell size in the cavity; providing a second conductive material having a second unit cell size in the cavity above the first conductive material; and polishing a surface of the non-conductive material and a surface of the second conductive material. The first unit cell size is larger than the second unit cell size.

[0104] In one embodiment, forming the cavity includes etching a portion of the non-conductive material.

[0105] In one embodiment, the method further comprises providing a barrier layer conformally along a surface of the cavity.

[0106] In one embodiment, providing the first conductive material includes electroplating the first conductive material.

[0107] In one embodiment, the second conductive material is copper.

[0108] In one embodiment, the first conductive material is a metal alloy material.

[0109] In one embodiment, the first conductive material has a characteristic formation temperature below 230°C.

[0110] In one embodiment, the first conductive material is a metal silicide, which may include nickel, titanium or copper.

[0111] In one embodiment, the first conductive material includes aluminum, zinc, titanium, or nickel.

[0112] In one embodiment, the second conductive material comprises a face-centered cubic structure, and the first conductive material comprises a hexagonal crystal structure.

[0113] In one embodiment, the second conductive material comprises copper and the first conductive material comprises titanium.

[0114] In one embodiment, the resistivity of the first conductive material is greater than the resistivity of the second conductive material. The resistivity of the first conductive material may be less than 40 times the resistivity of the second conductive material. The resistivity of the first conductive material may be less than 20 times the resistivity of the second conductive material.

[0115] In one embodiment, the thickness of the second conductive material is greater than the thickness of the first conductive material.

[0116] In one embodiment, polishing includes polishing a surface of the non-conductive material and a surface of the second conductive material by a chemical mechanical polishing compatible material.

[0117] In one embodiment, the component is formed without annealing. A method of forming a bonded structure including a component and a second component having a contact pad may include annealing a first conductive material, a second conductive material, and the contact pad, thereby expanding the first conductive material, the second conductive material, and the contact pad to form a bonded conductive contact. Annealing may form an alloy between the first material and the second material.

[0118] In one aspect, a method of forming an element is disclosed. The method may include: forming a cavity in a non-conductive material; providing a first barrier layer in the cavity; providing a first conductive material having a first unit cell size in the cavity above the first barrier layer; providing a second barrier layer in the cavity above the first conductive material; providing a second conductive material having a second unit cell size in the cavity above the second barrier layer; polishing a surface of the non-conductive material and a surface of the second conductive material. The first unit cell size is larger than the second unit cell size.

[0119] In one embodiment, forming the cavity includes etching a portion of the non-conductive material.

[0120] In one embodiment, providing the first conductive material includes electroplating the first conductive material.

[0121] In one embodiment, the second conductive material is copper.

[0122] In one embodiment, the first conductive material is a metal alloy material.

[0123] In one embodiment, the first conductive material has a characteristic formation temperature below 230°C.

[0124] In one embodiment, the first conductive material is a metal silicide.

[0125] In one embodiment, the second conductive material comprises a face-centered cubic structure and the first conductive material comprises a hexagonal crystal structure.The second conductive material may comprise copper and the first conductive material may comprise titanium.

[0126] In one embodiment, the resistivity of the first conductive material is greater than the resistivity of the second conductive material. The resistivity of the first conductive material may be less than 40 times the resistivity of the second conductive material. The resistivity of the second conductive material may be less than 20 times the resistivity of the first conductive material.

[0127] In one embodiment, the thickness of the second conductive material is greater than the thickness of the first conductive material.

[0128] In one embodiment, polishing includes polishing a surface of the non-conductive material and a surface of the second conductive material by a chemical mechanical polishing compatible material.

[0129] In one embodiment, the component is formed without annealing.

[0130] In one aspect, a method of forming a component is disclosed. The method may include: forming a cavity in a non-conductive material; providing a first conductive material having a hexagonal crystal structure; providing a second conductive material having a face-centered cubic structure; and polishing a surface of the non-conductive material and a surface of the first conductive material.

[0131] In one embodiment, forming the cavity includes etching a portion of the non-conductive material.

[0132] In one embodiment, providing the first conductive material includes electroplating the first conductive material.

[0133] In one embodiment, the second conductive material is copper.

[0134] In one embodiment, the first conductive material has a characteristic formation temperature below 230°C.

[0135] In one embodiment, the second conductive material comprises copper and the first conductive material comprises titanium.

[0136] In one embodiment, the resistivity of the first conductive material is greater than the resistivity of the second conductive material.

[0137] In one embodiment, the thickness of the second conductive material is greater than the thickness of the first conductive material.

[0138] In one embodiment, polishing includes polishing a surface of the non-conductive material and a surface of the second conductive material by a chemical mechanical polishing compatible material.

[0139] In one embodiment, the component is formed without annealing. A method of forming a bonded structure including a component and a second component having a contact pad may include: annealing a first conductive material, a second conductive material, and the contact pad, thereby expanding the first conductive material, the second conductive material, and the contact pad to form a bonded conductive contact. Annealing may form an alloy between the first conductive material and the second conductive material.

[0140] In one aspect, a method of forming a bonded structure is disclosed. The method may include providing a first element having a first non-conductive region and a first conductive feature. The first conductive feature includes a first conductive material and a second conductive material. The first conductive material has a unit cell size that is larger than a unit cell size of the second conductive material. The first conductive material is a metal alloy material. The method may include providing a second element having a second non-conductive region and a second conductive feature. The method may include: directly bonding the first non-conductive region and the second non-conductive region; and annealing the first conductive feature and the second conductive feature to bond the first conductive material and the second conductive feature of the first conductive feature.

[0141] In one embodiment, providing the first element includes forming a cavity in the first non-conductive region and at least partially filling the cavity with a first conductive feature. Forming the cavity may include etching a portion of the non-conductive material. The method may also include conformally providing a barrier layer along a surface of the cavity. Providing the first conductive feature may include electroplating the first conductive feature.

[0142] In one embodiment, the first conductive material is copper.

[0143] In one embodiment, the second conductive material has a characteristic formation temperature below 230°C.

[0144] In one embodiment, the second conductive material is a metal silicide, which may include nickel, titanium or copper.

[0145] In one embodiment, the second conductive material includes aluminum, zinc, titanium, or nickel.

[0146] In one embodiment, the first conductive material comprises a face-centered cubic structure and the second conductive material comprises a hexagonal crystal structure.The first conductive material may comprise copper and the second conductive material may comprise titanium.

[0147] In one embodiment, the resistivity of the second conductive material is greater than the resistivity of the first conductive material. The resistivity of the second conductive material may be less than 40 times the resistivity of the first conductive material. The resistivity of the second conductive material may be less than 20 times the resistivity of the first conductive material.

[0148] In one embodiment, the thickness of the first conductive material is greater than the thickness of the second conductive material.

[0149] In one embodiment, the method further includes polishing the surface of the non-conductive material and the surface of the first conductive material by a chemical mechanical polishing compatible material.

[0150] In one embodiment, annealing includes annealing the first conductive feature and the second conductive feature at a temperature between 100°C and 200°C.

[0151] In one embodiment, annealing includes annealing the first conductive feature and the second conductive feature at a temperature between 100°C and 150°C.

[0152] In one embodiment, annealing forms an alloy between the first conductive material and the second conductive material.

[0153] In one aspect, a method of forming a bonded structure is disclosed. The method may include providing a first element having a first non-conductive region and a first conductive feature. The first conductive feature includes a first conductive material and a second conductive material. The method may include: providing a second element having a second non-conductive region and a second conductive feature; directly bonding the first non-conductive region and the second non-conductive region; and annealing the first conductive feature and the second conductive feature to bond the first conductive material of the first conductive feature and the second conductive feature and to form an alloy between the first conductive material and the second conductive material.

[0154] In one aspect, a component having a contact surface is disclosed. The component may include: a non-conductive region, a cavity having a thickness extending at least partially from the contact surface through the non-conductive region; and a contact pad formed in the cavity, the contact pad including a first conductive material and a second conductive material. The first conductive material is a metal alloying material configured to form an alloy with the second material. The alloy has a unit cell size that is larger than the unit cell size of the second conductive material. The non-conductive region is configured to be directly bonded to the non-conductive region of the second component. The contact pad of the component is configured to be directly bonded to the contact pad of the second component.

[0155] In one aspect, a component having a contact surface is disclosed. The component may include: a non-conductive region, a cavity having a thickness extending at least partially from the contact surface through the non-conductive region; and a contact pad formed in the cavity. The contact pad includes a first conductive material and a second conductive material. The first conductive material has a unit cell size that is larger than a unit cell size of the second conductive material. The first conductive material has a thermal expansion coefficient that is larger than a thermal expansion coefficient of the second conductive material. The non-conductive region is configured to be directly bonded to the non-conductive region of the second component. The contact pad of the component is configured to be directly bonded to the contact pad of the second component.

[0156] In one aspect, a component having a contact surface is disclosed. The component may include: a non-conductive region, a cavity having a thickness extending at least partially through the non-conductive region from the contact surface; and a contact pad formed in the cavity, the contact pad including a roughened contact surface. The non-conductive region is configured to be directly bonded to the non-conductive region of a second component, and the contact pad of the component is configured to be directly bonded to the contact pad of the second component.

[0157] In one embodiment, the roughened contact surface includes spikes.

[0158] In one embodiment, the contact pad comprises an orthorhombic crystal structure.

[0159] In one embodiment, the surface roughness of the contact surface ranges between 3 nm and 100 nm.

[0160] In one embodiment, the surface roughness of the contact surface ranges between 3 nm and 50 nm.

[0161] In one embodiment, the contact surface has a higher surface roughness than the bonding surface of the non-conductive region.

[0162] In one aspect, a bonded structure is disclosed. The bonded structure may include a first element including a first non-conductive region having a cavity and a conductive contact feature disposed in the cavity. The conductive contact feature includes a first conductive material and a second conductive material. The bonded structure may include a second element directly bonded to the non-conductive region of the first element. The conductive contact feature includes a unit cell that is larger than a unit cell of the first conductive material or the second conductive material.

[0163] In one embodiment, the conductive contact feature includes an alloy of a first conductive material and a second conductive material.

[0164] In one embodiment, the conductive contact feature is directly bonded to a second conductive contact feature of the second component without an intervening adhesive.

[0165] Unless the context clearly requires otherwise, throughout the specification and claims, the words "comprise", "comprising", "include", "including", etc. should be interpreted in an inclusive sense, rather than in an exclusive or exhaustive sense; that is, interpreted as "including but not limited to". The word "coupled" as generally used herein refers to two or more elements that can be directly connected or connected through one or more intermediate elements. Similarly, the word "connected" as generally used herein refers to two or more elements that can be directly connected or connected through one or more intermediate elements. Additionally, when used in this application, the words "herein", "above", "below" and words of similar meaning should refer to the entirety of this application, rather than to any particular part of this application. In addition, as used herein, when a first element is described as being "on" or "above" a second element, the first element can be directly on or above the second element, so that the first element and the second element are in direct contact, or the first element can be indirectly on or above the second element, so that one or more elements are between the first element and the second element. Where the context permits, words in the above detailed description using the singular or plural may also include the plural or singular, respectively. The word "or" when referring to a list of two or more items encompasses all of the following interpretations of the word: any item in the list, all items in the list, and any combination of items in the list.

[0166] Furthermore, unless otherwise specifically stated or understood in the context as used, conditional language used herein, such as “can,” “could,” “might,” “may,” “eg,” “for example,” “such as,” etc., is generally intended to convey that certain embodiments include and other embodiments do not include certain features, elements, and / or states. Thus, such conditional language is generally not intended to imply that these features, elements, and / or states are in any way essential to one or more embodiments.

[0167] Although certain embodiments have been described, these embodiments are presented only by way of example and are not intended to limit the scope of the present disclosure. In fact, the novel devices, methods, and systems described herein can be implemented in various other forms; in addition, without departing from the spirit of the present disclosure, various omissions, replacements, and changes can be made to the form of the methods and systems described herein. For example, although the blocks are presented in a given arrangement, alternative embodiments can utilize different components and / or circuit topologies to perform similar functionality, and some blocks can be deleted, moved, added, subdivided, combined, and / or modified. Each of these blocks can be implemented in a variety of different ways. Any suitable combination of the elements and actions of the various embodiments described above can be combined to provide other embodiments. The attached claims and their equivalents are intended to cover such forms or modifications that fall within the scope and spirit of the present disclosure.

Claims

1. A component having a contact surface, the component comprising: a non-conductive region having a cavity extending from the contact surface at least partially through the thickness of the non-conductive region; as well as a contact pad formed in the cavity, the contact pad comprising a first conductive material and a second conductive material, the first conductive material having a unit cell size larger than a unit cell size of the second conductive material, the first conductive material being a metal alloy material, Wherein the non-conductive region is configured to be directly bonded to a non-conductive region of a second element, and the contact pad of the element is configured to be directly bonded to a contact pad of the second element. 2 . The element of claim 1 , wherein the unit cell size of the first conductive material is at least 1.3 times larger than the unit cell size of the second conductive material. 3 . The element of claim 1 , further comprising a barrier layer conformally disposed along a surface of the cavity. The element according to claim 1 , wherein the first conductive material is disposed between a bottom surface of the cavity and the second conductive material. The element of claim 1 , wherein the first conductive material is completely buried under the second conductive material. The element of claim 1 , wherein the first conductive material is not exposed. The element of claim 1 , wherein the second conductive material is copper.

8. The element of claim 1, wherein the first conductive material has a characteristic forming temperature lower than 230°C.

9. The element of claim 8, wherein the first conductive material has a characteristic forming temperature lower than 130°C.

10. The element according to claim 1, wherein the first conductive material is a metal silicide.

11. The element of claim 10, wherein the metal silicide comprises nickel, titanium or cobalt.

12. The element of claim 1, wherein the first conductive material comprises zinc, titanium, or nickel. 13 . The element according to claim 1 , wherein the second conductive material comprises a face-centered cubic structure, and the first conductive material comprises a hexagonal crystal structure.

14. The element of claim 13, wherein the second conductive material comprises copper and the first conductive material comprises titanium.

15. The element of claim 14, wherein the first conductive material has a resistivity greater than that of the second conductive material.

16. The element of claim 15, wherein the resistivity of the first conductive material is less than 40 times the resistivity of the second conductive material.

17. The element of claim 16, wherein the resistivity of the first conductive material is less than 20 times the resistivity of the second conductive material.

18. The element according to claim 1, wherein a thickness of the second conductive material is greater than a thickness of the first conductive material.

19. The element of claim 1, wherein the first conductive material is a chemical mechanical polishing compatible material.

20. A first element having a contact surface, the first element comprising: a non-conductive region having a cavity extending from the contact surface at least partially through the thickness of the non-conductive region; as well as a contact pad formed in the cavity, the contact pad comprising a metal and a metal silicide, the metal silicide having a unit cell size larger than a unit cell size of the metal, Wherein the non-conductive region is configured to be directly bonded to a non-conductive region of a second component, and the metal is configured to be directly bonded to a contact pad of the second component.

21. The first element of claim 20, further comprising a barrier layer conformally disposed along a surface of the cavity.

22. The first element of claim 20, wherein the metal silicide is disposed between a bottom surface of the cavity and the metal.

23. The first element of claim 20, wherein the metal silicide is completely buried under the metal.

24. The first component of claim 20, wherein the metal is not exposed.

25. The first element of claim 20, wherein the metal is copper.

26. The first component of claim 20, wherein the metal silicide is a metal alloy material.

27. The first element of claim 20, wherein the metal silicide has a characteristic formation temperature lower than 230°C.

28. The first element according to claim 20, wherein the metal silicide comprises nickel, titanium or copper.

29. The first element according to claim 20, wherein the resistivity of the metal silicide is greater than the resistivity of the metal.

30. The first element according to claim 29, wherein the resistivity of the metal silicide is smaller than 40 times the resistivity of the metal.

31. The first element according to claim 30, wherein the resistivity of the metal silicide is smaller than 20 times the resistivity of the metal.

32. The first element according to claim 20, wherein a thickness of the metal is greater than a thickness of the metal silicide.

33. The first element according to claim 20, wherein the metal and the metal silicide do not react with each other.

34. The first element of claim 20, wherein the metal comprises copper and the metal silicide comprises zinc.

35. The first element of claim 20, wherein the metal silicide is a chemical mechanical polishing compatible material.

36. A combined structure comprising: a first element having a first non-conductive region and a first conductive feature; as well as a second element having a second non-conductive region and a second conductive feature, the second non-conductive region being directly bonded to the first non-conductive region and the second conductive feature being directly bonded to the first conductive feature to define a bonded conductive contact, The combined conductive contact includes a first conductive material and a second conductive material, the first conductive material has a unit cell size larger than a unit cell size of the second conductive material, and the first conductive material is an alloy including the second conductive material.

37. The bonded structure of claim 36, wherein the bonded conductive contact comprises a gradient of alloying elements.

38. A combined structure comprising: a first element having a first non-conductive region and a first conductive feature; as well as a second element having a second non-conductive region and a second conductive feature, the second non-conductive region being directly bonded to the first non-conductive region and the second conductive feature being directly bonded to the first conductive feature to define a bonded conductive contact, Wherein the bonded conductive contact comprises a first conductive material and a second conductive material, the first conductive material having a unit cell size that is larger than a unit cell size of the second conductive material, wherein the first conductive feature comprises a metal silicide.

39. The bonded structure of claim 38, wherein the first element further comprises a barrier layer between the first non-conductive region and the first conductive feature.

40. The bonded structure of claim 38, wherein the metal silicide comprises nickel, titanium or copper.

41. A combined structure comprising: a first element having a first non-conductive region and a first conductive feature; as well as a second element having a second non-conductive region and a second conductive feature, the second non-conductive region being directly bonded to the first non-conductive region and the second conductive feature being directly bonded to the first conductive feature to define a bonded conductive contact, Wherein the bonded conductive contact comprises a conductive material and an alloying element, and wherein an amount of the alloying element varies with a thickness of the bonded conductive contact.

42. The bonded structure of claim 41, wherein the first element further comprises a barrier layer between the first non-conductive region and the first conductive feature.

43. The bonded structure of claim 41, wherein the first conductive feature comprises a metal silicide.

44. The bonded structure of claim 43, wherein the metal silicide comprises nickel, titanium or copper.

45. The bonded structure of claim 41, wherein the bonded conductive contact comprises an orthorhombic crystal structure.

46. ​​The bonded structure of claim 41, wherein the bonded conductive contact has a unit cell size that is larger than a unit cell size of the conductive material.

47. A bonding structure comprising: a first element having a first non-conductive region and a first conductive feature; as well as a second element having a second non-conductive region and a second conductive feature, the second non-conductive region being directly bonded to the first non-conductive region and the second conductive feature being directly bonded to the first conductive feature to define a bonded conductive contact, Wherein the bonded conductive contact comprises a crystal structure of lower symmetry than the first conductive feature.

48. The bonded structure of claim 47, wherein the bonded conductive contact comprises an orthorhombic crystal structure or a hexagonal crystal structure.

49. The bonded structure of claim 47, wherein the bonded conductive contact comprises a gradient of alloying elements.

50. The bonded structure of claim 47, wherein the first component further comprises a barrier layer between the first non-conductive region and the first conductive feature.

51. The bonded structure of claim 47, wherein the bonded conductive contact comprises copper titanium.

52. A combined structure comprising: A first element having a first contact surface, the first element comprising: a first non-conductive region having a first cavity extending from the first contact surface at least partially through the thickness of the non-conductive region; and a first contact pad formed in the first cavity, the contact pad comprising a first conductive material and a second conductive material, the first conductive material having a unit cell size larger than a unit cell size of the second conductive material, the first conductive material being a metal alloy material; and A second element having a second contact surface directly bonded to the first contact surface, the second element comprising: a second non-conductive region directly bonded to the first non-conductive region; and The second contact pad is directly bonded to the first contact pad.

53. The bonding structure of claim 52, further comprising a barrier layer conformally disposed along a surface of the first cavity.

54. The bonding structure of claim 52, wherein the first conductive material is disposed between a bottom surface of the first cavity and the second conductive material.

55. The bonded structure of claim 54, wherein the first conductive material is completely buried under the second conductive material.

56. The bonded structure of claim 54, wherein the directly bonded first and second contact pads define a bonded conductive contact comprising an orthorhombic crystal structure.

57. The bonded structure of claim 56, wherein the directly bonded contact pad comprises copper titanium.

58. The bonded structure of claim 54, wherein the directly bonded first and second contact pads define a bonded conductive contact comprising a gradient of alloying elements.

59. A method of forming a component: forming a cavity in a non-conductive material; providing a first conductive material having a first unit cell size in the cavity; providing a second conductive material having a second unit cell size in the cavity above the first conductive material, the first unit cell size being larger than the second unit cell size; and The surface of the non-conductive material and the surface of the second conductive material are polished.

60. The method of claim 59, wherein forming the cavity comprises etching a portion of the non-conductive material.

61. The method of claim 59, further comprising providing a barrier layer conformally along a surface of the cavity.

62. The method of claim 59, wherein providing the first conductive material comprises electroplating the first conductive material.

63. The method of claim 59, wherein the second conductive material is copper.

64. The method of claim 59, wherein the first conductive material is a metal alloy material.

65. The method of claim 59, wherein the first conductive material has a characteristic formation temperature below 230°C.

66. The method of claim 59, wherein the first conductive material is a metal silicide.

67. The method of claim 66, wherein the metal silicide comprises nickel, titanium, or copper.

68. The method of claim 59, wherein the first conductive material comprises aluminum, zinc, titanium, or nickel.

69. The method of claim 59, wherein the second conductive material comprises a face-centered cubic structure and the first conductive material comprises a hexagonal crystal structure.

70. The method of claim 69, wherein the second conductive material comprises copper and the first conductive material comprises titanium.

71. The method of claim 59, wherein the resistivity of the first conductive material is greater than the resistivity of the second conductive material.

72. The method of claim 71, wherein the resistivity of the first conductive material is less than 40 times the resistivity of the second conductive material.

73. The method of claim 72, wherein the resistivity of the first conductive material is less than 20 times the resistivity of the second conductive material.

74. The method of claim 59, wherein the second conductive material has a thickness greater than a thickness of the first conductive material.

75. The method of claim 59, wherein the polishing comprises polishing the surface of the non-conductive material and the surface of the second conductive material by a chemical mechanical polishing compatible material.

76. The method of claim 59, wherein the element is formed without annealing.

77. A method for forming a combined structure, the combined structure comprising an element according to claim 0 and a second element having a contact pad, the method comprising annealing the first conductive material, the second conductive material and the contact pad, thereby causing the first conductive material, the second conductive material and the contact pad to expand to form a combined conductive contact.

78. The method of claim 77, wherein the annealing forms an alloy between the first material and the second material.

79. A method of forming a component: forming a cavity in a non-conductive material; providing a first barrier layer in the cavity; providing a first conductive material having a first unit cell size in the cavity above the first barrier layer; providing a second barrier layer in the cavity above the first conductive material; providing a second conductive material having a second unit cell size in the cavity above the second barrier layer, the first unit cell size being larger than the second unit cell size; and The surface of the non-conductive material and the surface of the second conductive material are polished.

80. The method of claim 79, wherein forming the cavity comprises etching a portion of the non-conductive material.

81. The method of claim 79, wherein providing the first conductive material comprises electroplating the first conductive material.

82. The method of claim 79, wherein the second conductive material is copper.

83. The method of claim 79, wherein the first conductive material is a metal alloy material.

84. The method of claim 79, wherein the first conductive material has a characteristic formation temperature below 230°C.

85. The method of claim 79, wherein the first conductive material is a metal silicide.

86. The method of claim 79, wherein the second conductive material comprises a face-centered cubic structure and the first conductive material comprises a hexagonal crystal structure.

87. The method of claim 86, wherein the second conductive material comprises copper and the first conductive material comprises titanium.

88. The method of claim 79, wherein the resistivity of the first conductive material is greater than the resistivity of the second conductive material.

89. The method of claim 88, wherein the resistivity of the first conductive material is less than 40 times the resistivity of the second conductive material.

90. The method of claim 89, wherein the resistivity of the second conductive material is less than 20 times the resistivity of the first conductive material.

91. The method of claim 79, wherein the second conductive material has a thickness greater than a thickness of the first conductive material.

92. The method of claim 79, wherein the polishing comprises polishing the surface of the non-conductive material and the surface of the second conductive material by a chemical mechanical polishing compatible material.

93. The method of claim 79, wherein the element is formed without annealing.

94. A method of forming a component: forming a cavity in a non-conductive material; providing a first conductive material having a hexagonal crystal structure; providing a second conductive material having a face-centered cubic structure; as well as The surface of the non-conductive material and the surface of the first conductive material are polished.

95. The method of claim 94, wherein forming the cavity comprises etching a portion of the non-conductive material.

96. The method of claim 94, wherein providing the first conductive material comprises electroplating the first conductive material.

97. The method of claim 94, wherein the second conductive material is copper.

98. The method of claim 94, wherein the first conductive material has a characteristic formation temperature below 230°C.

99. The method of claim 94, wherein the second conductive material comprises copper and the first conductive material comprises titanium.

100. The method of claim 94, wherein the resistivity of the first conductive material is greater than the resistivity of the second conductive material.

101. The method of claim 94, wherein the thickness of the second conductive material is greater than the thickness of the first conductive material.

102. The method of claim 94, wherein the polishing comprises polishing the surface of the non-conductive material and the surface of the second conductive material by a chemical mechanical polishing compatible material.

103. The method of claim 94, wherein the element is formed without annealing.

104. A method for forming a combined structure, the combined structure comprising an element according to claim 0 and a second element having a contact pad, the method comprising annealing the first conductive material, the second conductive material and the contact pad, thereby causing the first conductive material, the second conductive material and the contact pad to expand to form a combined conductive contact.

105. The method of claim 104, wherein the annealing forms an alloy between the first conductive material and the second conductive material.

106. A method of forming a bonded structure, the method comprising: providing a first element having a first non-conductive region and a first conductive feature, the first conductive feature comprising a first conductive material and a second conductive material, the first conductive material having a unit cell size larger than a unit cell size of the second conductive material, the first conductive material being a metal alloyed material; providing a second element having a second non-conductive region and a second conductive feature; directly bonding the first non-conductive region and the second non-conductive region; as well as The first conductive feature and the second conductive feature are annealed to combine the first conductive material of the first conductive feature and the second conductive feature.

107. The method of claim 106, wherein providing the first element comprises forming a cavity in the first non-conductive region and at least partially filling the cavity with the first conductive feature.

108. The method of claim 107, wherein forming the cavity comprises etching a portion of the non-conductive material.

109. The method of claim 108, further comprising providing a barrier layer conformally along a surface of the cavity.

110. The method of claim 107, wherein providing the first conductive feature comprises electroplating the first conductive feature.

111. The method of claim 106, wherein the first conductive material is copper.

112. The method of claim 106, wherein the second conductive material has a characteristic formation temperature below 230°C.

113. The method of claim 106, wherein the second conductive material is a metal silicide.

114. The method of claim 113, wherein the metal silicide comprises nickel, titanium, or copper.

115. The method of claim 106, wherein the second conductive material comprises aluminum, zinc, titanium, or nickel.

116. The method of claim 106, wherein the first conductive material comprises a face-centered cubic structure and the second conductive material comprises a hexagonal crystal structure.

117. The method of claim 116, wherein the first conductive material comprises copper and the second conductive material comprises titanium.

118. The method of claim 106, wherein the second conductive material has a resistivity greater than the resistivity of the first conductive material.

119. The method of claim 118, wherein the resistivity of the second conductive material is less than 40 times the resistivity of the first conductive material.

120. The method of claim 119, wherein the resistivity of the second conductive material is less than 20 times the resistivity of the first conductive material.

121. The method of claim 106, wherein the thickness of the first conductive material is greater than the thickness of the second conductive material.

122. The method of claim 106, further comprising polishing a surface of the non-conductive material and a surface of the first conductive material by a chemical mechanical polishing compatible material.

123. The method of claim 106 wherein the annealing comprises annealing the first conductive feature and the second conductive feature at a temperature between 100°C and 200°C.

124. The method of claim 106, wherein the annealing comprises annealing the first conductive feature and the second conductive feature at a temperature between 100°C and 150°C.

125. The method of claim 106, wherein the annealing forms an alloy between the first conductive material and the second conductive material.

126. A method of forming a bonded structure, the method comprising: providing a first element having a first non-conductive region and a first conductive feature, the first conductive feature comprising a first conductive material and a second conductive material; providing a second element having a second non-conductive region and a second conductive feature; directly bonding the first non-conductive region and the second non-conductive region; as well as The first conductive feature and the second conductive feature are annealed to combine the first conductive material of the first conductive feature and the second conductive feature and to form an alloy between the first conductive material and the second conductive material.

127. A component having a contact surface, the component comprising: a non-conductive region having a cavity extending from the contact surface at least partially through the thickness of the non-conductive region; as well as a contact pad formed in the cavity, the contact pad comprising a first conductive material and a second conductive material, the first conductive material being a metal alloying material configured to form an alloy with the second material, the alloy having a unit cell size larger than a unit cell size of the second conductive material, Wherein the non-conductive region is configured to be directly bonded to a non-conductive region of a second element, and the contact pad of the element is configured to be directly bonded to a contact pad of the second element.

128. A component having a contact surface, the component comprising: a non-conductive region having a cavity extending from the contact surface at least partially through the thickness of the non-conductive region; as well as a contact pad formed in the cavity, the contact pad comprising a first conductive material and a second conductive material, the first conductive material having a unit cell size larger than a unit cell size of the second conductive material, the first conductive material having a thermal expansion coefficient larger than a thermal expansion coefficient of the second conductive material, Wherein the non-conductive region is configured to be directly bonded to a non-conductive region of a second element, and the contact pad of the element is configured to be directly bonded to a contact pad of the second element.

129. A component having a contact surface, the component comprising: a non-conductive region having a cavity extending from the contact surface at least partially through the thickness of the non-conductive region; as well as a contact pad formed in the cavity, the contact pad comprising a roughened contact surface, Wherein the non-conductive region is configured to be directly bonded to a non-conductive region of a second element, and the contact pad of the element is configured to be directly bonded to a contact pad of the second element.

130. The element of claim 130, wherein the roughened contact surface comprises spikes.

131. The element of claim 129, wherein the contact pad comprises an orthorhombic crystal structure.

132. The element of claim 129, wherein the surface roughness of the contact surface ranges between 3 nm and 100 nm.

133. The element of claim 129, wherein the surface roughness of the contact surface ranges between 3 nm and 50 nm.

134. The element of claim 129, wherein the surface roughness of the contact surface is higher than the roughness of the bonding surface of the non-conductive region.

135. A combined structure comprising: a first element including a first non-conductive region having a cavity and a conductive contact feature disposed in the cavity, the conductive contact feature including a first conductive material and a second conductive material; as well as a second element directly bonded to the non-conductive region of the first element; Wherein the conductive contact feature comprises a unit cell that is larger than a unit cell of the first conductive material or the second conductive material.

136. The bonded structure of claim 135, wherein the conductive contact feature comprises an alloy of the first conductive material and the second conductive material.

137. The bonded structure of claim 135, wherein the conductive contact feature is directly bonded to a second conductive contact feature of the second element without an intervening adhesive.