Solvent-free process for preparing lithium ion batteries

By using multifunctional carbon black instead of activated carbon in the dry manufacturing of lithium-ion battery electrodes, the impurities and water absorption problems of fibrillator are solved, the energy density and life of the electrode are improved, and more efficient electrochemical performance is achieved and environmentally friendly production.

CN118922953APending Publication Date: 2024-11-08CABOT CORP
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202380028554.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-21
Filing Date
2023-03-17
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

In the existing dry-process technology for manufacturing lithium-ion battery electrodes, fibrillators such as activated carbon used have high impurities and strong water absorption, which affects battery performance and requires a higher load, which limits the content and conductivity of the active material.

Method used

Multifunctional carbon black is used as a replacement for the binder, providing conductivity and mechanical enhancement in dry manufacturing through its selected morphology and surface chemistry, reducing dependence on conductive additives and increasing the load capacity of the active material.

Benefits of technology

It improves the energy density and life of the electrode, reduces in-plane resistivity, reduces cost and environmental impact during the manufacturing process, and eliminates the need for harmful solvents.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005049077090000171
    Figure BDA0005049077090000171
  • Figure BDA0005049077090000181
    Figure BDA0005049077090000181
  • Figure BDA0005049077090000441
    Figure BDA0005049077090000441
Patent Text Reader

Abstract

A solvent-free process employs multifunctional carbon black to prepare compositions and electrodes for lithium ion batteries. The multifunctional carbon black provides two or more desirable properties, e.g., as a conductive carbon additive, as a fibrillating agent, and / or as a mechanical reinforcement. In one example, an electroactive material (e.g., graphite or a lithium transition metal compound), a binder, and a multifunctional carbon black are combined in one or more steps. High shear mixing is used to treat the binder in the presence of multifunctional carbon black. The resulting composition can be formed into a film which can be applied to a suitable substrate to create an electrode.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] Government support

[0002] This invention was made with government support under Award No. DE-EE0009109.0000 awarded by the Office of Energy Efficiency and Renewable Energy (EERE) of the U.S. Department of Energy. The government has certain rights in this invention.

[0003] Related Applications

[0004] This application claims the benefit of U.S. Provisional Application No. 63 / 322,074, filed on March 21, 2022, under 35 USC 119(e), the entire contents of which are incorporated herein by reference. Background Art

[0005] Lithium-ion batteries (LIBs) are a common source of electrical energy for many applications from electronic devices to electric vehicles. Lithium-ion batteries typically include a negative electrode and a positive electrode in an arrangement that allows lithium ions and electrons to move to and from the electrodes during charge and discharge. The electrolyte solution in contact with the electrodes provides a conductive medium in which the ions can move. To prevent direct reaction between the electrodes, a separator that is permeable to ions is used to physically and electrically isolate the electrodes. During operation, electrical contact is made with the electrodes, allowing electrons to flow through the device to provide power, and allowing lithium ions to move from one electrode to another through the electrolyte.

[0006] Most commercially available lithium-ion batteries have anodes containing graphite, a material capable of incorporating lithium via an intercalation mechanism. Typically, lithium is added to the graphite anode during the charging cycle and removed as the battery is used. Other anode materials used in addition to or in place of graphite include lithium titanate, tin oxide, silicon (Si), and SiO x (where x is typically 1.04, 1.06, etc.).

[0007] The cathode typically includes a conductive substrate that supports a mixture containing a binder and at least one electrochemically active material. The electroactive material (e.g., lithium transition metal oxide) is capable of receiving and releasing lithium ions. As with the anode, the binder is used to provide mechanical integrity and stability to the electrode.

[0008] Since the electroactive materials and binders often exhibit poor electrically conducting or even insulating properties, the cathode often includes additive components for enhancing the electrical conductivity of the electrode. For example, conductivity additives, carbon conductivity additives can also be found in LIB anode compositions.

[0009] To make electrodes, the active electrode material (e.g., graphite) is mixed with a binder (typically a polymeric or resinous material). Many existing manufacturing methods employ casting techniques based on wet slurries that contain not only a binder but also solvents, plasticizers, conductivity additives, etc. During manufacturing, the slurry is coated or extruded onto a conductive substrate. Since the solvent is detrimental to the final product, it is removed by drying.

[0010] However, drying operations (especially those intended to remove solvents) take time, slowing down the overall production process. In addition, they may cause cost and environmental issues, typically due to the toxicity of solvents (e.g., NMP). In terms of the final product, removing the solvent during the drying process often results in the migration of the binder to the electrode surface. Although minimal migration is acceptable in some cases, it is problematic in other cases. For example, for high loads (thick, >4.5 mAh / cm 2 ) electrodes, migration is aggravated, leading to delamination and poor electrode performance.

[0011] Therefore, "dry" alternatives are being developed that aim to reduce or eliminate the drying steps associated with slurry techniques.While dry processes also produce electrodes that typically contain electroactive material, binder, and conductivity additive components, they do not require the use of solvents.

[0012] Dry approaches that have been proposed include high shear mixing involving a fibrillable binder, use of a sacrificial binder that is removed during electrode treatment, dry powder spraying, electrostatic spray deposition, cold plasma deposition, sputtering deposition, powder printing, etc. In some embodiments, a fibrillation promoter is incorporated into the binder, and the resulting formulation is subjected to high shear mixing to fibrillate the binder, thereby creating a network structure that can better hold the material together and carry the active material.

[0013] By far, the most common additive used to promote the fibrillation of adhesives is activated carbon (AC). Typically, AC is derived from carbonaceous source materials such as bamboo, coconut shells, willow peat, wood, coir, lignite, coal, and petroleum asphalt. Activation is achieved by physical or chemical methods known in the art. For many applications, AC powder is ground to a particle size of tens of microns (μm) before activation. Summary of the invention

[0014] While dry manufacturing methods have the potential to eliminate many of the challenges posed by the addition and / or removal of (often harmful) solvents, problems still exist.

[0015] For example, current "dry" manufacturing techniques utilize not only active electrode materials, but also many other ingredients, such as fibrillation promoters, conductivity additives, and binders. Since many of these components do not participate in the electrochemical reactions that produce electrical energy, they can negatively impact certain performance characteristics of the battery (e.g., capacity and energy density) because they effectively reduce the amount of active material that can be contained in a given volume.

[0016] Prior art fibrillation agents such as AC often contain high impurity levels. In addition, the high surface area and surface oxygen-containing groups typical of AC tend to promote significant water absorption. These features can lead to irreversible capacity loss, thereby reducing battery performance. In addition, AC cannot increase sufficient conductivity, resulting in the need to increase the amount of conductivity additives in the overall formulation. Even as a simple fibrillation promoter, AC often requires a relatively high loading (5 to 10 wt % in many cases), and this itself also limits the amount of active material that can be included.

[0017]

[0006] Therefore, there is a need for compositions and processes that address at least some of the problems associated with existing approaches.

[0018] In general, the present invention relates to the use of certain carbon blacks to make desired improvements to manufacturing processes, product electrodes and / or assembled batteries. More specifically, the present invention relates to the use of these materials in dry or solvent-free electrode manufacturing processes.

[0019] The carbon black has a selected morphology and / or surface chemistry and can provide two or more functions in the case of dry (solvent-free) electrode manufacturing methods. For example, the multifunctional carbon black described herein can act as a fibrillating agent as a replacement for AC; act as a conductive carbon additive; and / or act as a mechanical reinforcement (or in other words, act as an adhesion aid, adding mechanical strength and flexibility to the product electrode).

[0020] In general, a "multifunctional" carbon black (CB) can be defined as a CB that effectively deforms or fibrillates a binder used in a solvent-free process; contributes to the conductivity of electrons / ions of an electrode; and / or provides a mechanical benefit. In a specific implementation, a multifunctional CB can be considered to be capable of fibrillating a binder capable of fibrillation at a loading of no more than 5 weight percent (wt%). At this loading, the multifunctional CB also acts as a carbon conductivity additive, reducing the in-plane resistivity of the electrode. In many cases, mechanical benefits are also obtained.

[0021] For many dry processes, the BET of the multifunctional CB is no greater than about 1600 m 2 / g, for example, about 35 to about 1600 m 2 / g, and the OAN is not greater than about 650 ml / 100 g, for example, in the range of 120 to about 650 ml / 100 g.

[0022] Other desirable CB attributes may include high surface roughness (with macroporosity close to the particle surface), good electronic conductivity (with a powder resistivity of about 1.0 Ω·cm or less at 0.5 g / cm 3 Measured at a compressed density of 1.5 %.

[0023] In addition to the BET and OAN properties described above, many multifunctional CBs that can be used are characterized by one or more of the following: about 15 mJ / m 2 or lower surface energy; at least about Raman crystallite plane size (La); at least about 0.1 cm 3 / g of mesopore volume; and, at least about 0.2 cm 3 The total volume of mesopores and macropores can be at least about 1 cm 3 / g.

[0024] For some anode applications, solvent-free processes use BET values ​​of about 35 to about 1600 m 2 / g, for example, between about 55 and about 200 m 2 / g, and OAN is about 120 to about 650 ml / 100 g, such as CB in the range of about 130 to about 240 ml / 100 g. In further examples, CB has one or more of the following properties: about 15 mJ / m 2 or lower surface energy; at least about Raman crystallite plane size (La); at least about 0.1 cm 3 / g (e.g., about 0.1 to about 0.25 cm 3 / g) of mesopore volume; and, at least about 0.1 cm 3 / g (e.g., about 0.1 to about 0.4 cm 3 The total volume of mesopores and macropores may be at least about 0.2 cm 3 / g (e.g., about 0.2 to about 0.8 cm 3 / g).

[0025] For some cathode applications, solvent-free processes use BET values ​​of about 35 to about 1600 m 2 / g, such as in the range of about 500 to about 1600, and OAN is about 120 to about 650 ml / 100 g, such as in the range of about 250 to about 650 ml / 100 g. In a further example, the CB has one or more of the following properties: about 15 mJ / m 2 or lower surface energy; at least about Raman crystallite plane size (La); at least about 0.1 cm 3 / g (e.g., at least about 0.35 cm 3 / g) of mesopore volume; and, at least about 0.2 cm 3 / g (e.g., at least about 0.4 cm 3 The total volume of mesopores and macropores may be at least about 1 cm 3 / g.

[0026] In many embodiments, the methods described herein are performed without adding any liquid (typically any solvent). The ingredients are provided as loose particulate materials, such as flowable or pourable powders, flakes, beads, granules, pellets, etc.

[0027] However, in some cases, a small amount of liquid (e.g., solvent) can be used to carry out the methods described herein, typically a step different from the fibrillation step. Typically, if liquid is added, the amount is no more than about 10% by weight of the total amount of the ingredients used. In many cases, liquid (e.g., solvent) is added in an amount no more than 1% by weight.

[0028] One aspect of the present invention is characterized by a method for preparing an electrode composition. The method includes combining an active electrode material, a binder and a multifunctional carbon black (e.g., a multifunctional carbon black described herein), and treating the binder in the presence of the multifunctional carbon black. Many implementations of the method are performed without the addition of a liquid (typically a solvent).

[0029] In general, the binder can be any semi-crystalline polymer. Thus, the method can be carried out with binders conventionally considered "capable of fibrillation" as well as binders conventionally considered "not capable of fibrillation"; combinations thereof can also be used.

[0030] In one example, a method for preparing an electrode composition includes: mixing an active electrode material, a binder capable of fibrillation, and a multifunctional carbon black (e.g., a carbon black having a BET of not greater than about 1600 m 2 / g and OAN is not greater than about 650ml / 100g) in combination, and subjecting the adhesive to a fibrillation operation in the presence of the multifunctional carbon black.

[0031] Another aspect of the invention is characterized by a method for preparing an electrode composition. The method includes treating a binder in the presence of a multifunctional carbon black having properties as described above (e.g., subjecting the binder to high shear conditions), and adding an electrode active material before, during, or after the binder treatment. The binder can be a binder capable of fibrillation, a binder that is not capable of fibrillation, or any combination thereof.

[0032] In a specific implementation, the method described herein is carried out without adding any fibrillating aids other than the multifunctional carbon. In this case, the carbon black used provides the function of the entire adhesive treatment (e.g., fibrillation), completely replacing conventional fibrillating agents, such as activated carbon. In addition to using an adhesive treatment (e.g., fibrillation) component composed of multifunctional carbon black as described herein, an adhesive treatment component consisting essentially of or comprising multifunctional carbon black can also be used. Therefore, in some instances, multifunctional carbon black is used in combination with various amounts of conventional fibrillating aids (e.g., activated carbon). Multifunctional CB can also be combined with another multifunctional CB and / or with conventional conductive carbon additives (CCA).

[0033] The electroactive material, adhesive (e.g., adhesive capable of fibrillation) and multifunctional CB can be combined in a single step, with the adhesive treatment, fibrillation operation, for example, being performed subsequently. In other embodiments, the components are combined sequentially. For example, in the presence of a multifunctional additive, the adhesive is first treated (e.g., fibrillated), which step is followed by mixing with the electroactive material. Other sequences are possible. A uniform distribution of the components can be obtained using conditions different from those used in the adhesive treatment (e.g., fibrillation) (usually milder). Low shear mixing techniques can also prevent particle fragmentation and maintain particle size.

[0034] The resulting electrode composition can be further processed, typically a loose granular material, such as a flowing powder, which contains an electroactive material, a treated (e.g., fibrillated) binder, a multifunctional CB, and optional other ingredients. For example, the composition can be formed into a free-standing film, which can be applied to an electrically conductive substrate or carrier to form an electrode. In one method, the composition is calendered and laminated onto a conductive foil substrate. The calendering operation can be performed at room temperature or above room temperature, for example at a temperature similar to or close to the glass transition temperature of the polymer. The lamination step can be performed during or after the calendering of the composition. The resulting product electrodes can be assembled into LIB cells, in which one or both electrodes are prepared by a solvent-free process. In one example, two electrodes are prepared according to the technology described herein.

[0035] In another aspect, the invention features a dry processed film comprising: an active electrode material; a binder, typically treated, such as fibrillated; and a multifunctional carbon black. Prior to any drying operation, the dry processed film has a weight that is the same as its theoretical weight or that differs from its theoretical weight by no more than 1 weight percent. The multifunctional carbon black has a mass not greater than about 1600 m 2 / g BET and OAN no greater than about 650 ml / 100 g. In some examples, the multifunctional carbon black also has at least one of the following properties: 15 mJ / m 2 or lower surface energy; at least Raman crystallite plane size (La); at least 0.35cm 3 / g of mesopore volume; and, at least 0.2 cm 3 The total volume of mesopores and macropores can be at least about 1 cm 3 / g.

[0036] In one implementation, the in-plane resistivity of an electrode prepared by the techniques described herein is no greater than the in-plane resistivity characteristic of a reference electrode prepared using AC.

[0037] Practical embodiments of the present invention have many advantages. For example, the use of multifunctional CB can reduce the amount of adhesive and / or conventional processing additives required in the manufacturing process, increase the potential loading of active materials and lead to electrodes with higher energy density and thus batteries. The method described herein can reduce or eliminate the need for AC. In many cases, a smaller amount of additives is required, increasing the available content allowed by the active electrode material, resulting in batteries with higher energy density and longer life. CB multifunctional additives can improve binder fibrillation and the distribution of materials on the electrode. Enhanced adhesion and mechanical stability represent other potential benefits. Dry electrodes prepared using carbon black described herein show good charge transfer. The reduction in electrode impedance expected using multifunctional CB additives can improve the rate capacity and charging performance of the unit cell, opening up opportunities for thicker electrodes with fast charging capabilities and batteries with higher energy density.

[0038] While binder migration is often observed in slurry prepared electrodes, the methods and compositions described herein appear to produce a uniform distribution throughout the electrode. The fibrillated binder holds the electroactive particles (along with the conductivity additive) together (cohesion) while also keeping the electrode film layer attached to the metal substrate (adhesion).

[0039] The solvent-free technology described herein reduces or eliminates the use of hazardous solvents such as N-methyl-2-pyrrolidone (NMP) and the like. Being able to bypass the drying step associated with slurry (or other "wet" methods) can simplify, speed up manufacturing and reduce the footprint of the electrode production line. These benefits, as well as reducing or eliminating the need for solvent recycling or emission reduction measures, can contribute to overall cost reduction.

[0040] In some embodiments, dry processes can be performed using binders that are not typically considered to be binders capable of fibrillation, thereby expanding production options.

[0041] The above and other features of the present invention, including various details of structure and combinations of parts and other advantages, will now be described in more detail with reference to the accompanying drawings and pointed out in the claims. It should be understood that the specific methods and devices embodying the present invention are shown by way of illustration and not as limitations of the present invention. The principles and features of the present invention can be used in various and many embodiments without departing from the scope of the present invention. BRIEF DESCRIPTION OF THE DRAWINGS

[0042] In the drawings, reference numerals refer to the same parts throughout the different views. The drawings are not necessarily drawn to scale; emphasis is instead placed upon illustrating the principles of the invention. In the drawings:

[0043] 1A and 1B are SEM images (low and high magnification) of a cross section of a reference (comparative) electrode prepared by a dry process using activated carbon (AC);

[0044] FIG1C is a graph of elemental fluorine across the electrodes of FIG1A ;

[0045] 1D and 1E are SEM images (low and high magnification) of a cross section of an electrode prepared by a dry process using an unmodified CB additive;

[0046] FIG1F is a graph of elemental fluorine across the electrodes of FIG1D ;

[0047] 1G and 1H are SEM images (low and high magnification) of a cross section of an electrode prepared by a dry process, wherein the CB used is a heat-treated version of the CB of FIGS. 1C and 1D ;

[0048] FIG. 1I is a graph of elemental fluorine across the electrodes of FIG. 1G ;

[0049] Figure 2 The in-plane resistivity of the electrodes of FIGS. 1A and 1B (reference), FIGS. 1D and 1E (unmodified CB), and FIGS. 1G and 1H (heat-treated CB) are shown;

[0050] Figure 3 The tensile strength of the self-supporting graphite electrode films and the in-plane resistivity of the reference graphite electrode prepared by dry process using activated carbon and the graphite electrodes prepared by dry process using several CB specifications classified by BET surface area parameters are compared;

[0051] Figure 4 The tensile strength and elastic modulus of a reference free-standing NCM electrode membrane prepared by dry process using activated carbon and NCM electrode membranes prepared by dry process using several CB specifications at 5 wt% loading in the formulation were compared;

[0052] Figure 5 The tensile strength and elastic modulus of free-standing NCM electrode films prepared by dry process using several CB specifications at 2 wt % loading in the formulation were compared;

[0053] Figure 6 The in-plane resistivities of the reference NCM electrode prepared by dry process using activated carbon and the NCM electrodes prepared by dry process using the selected CBs were compared.

[0054] Figure 7The tensile strength and elastic modulus of free-standing NCM electrode films prepared by dry process using CB specifications at 1 wt% loading in the formulation were compared, wherein the CB material was in fluffy and pelletized forms.

[0055] Figure 8 is a graph showing the 0.2C, 0.5C, 1C, 2C, and 3C discharge capacities of complete button cell cells with NCM622 cathodes using the conductivity additives disclosed herein.

[0056] Fig. 9 is a graph showing the C / 20 discharge capacity of a complete button cell battery with a NCM622 cathode using the conductivity additive disclosed herein.

[0057] Fig.10 is a graph showing the first cycle irreversible capacity of a complete coin cell battery with a NCM622 cathode using the conductivity additive disclosed herein.

[0058] Fig.11 is a graph showing the discharge capacity cycles of half coin cell batteries with NCM622 cathodes using the conductivity additives disclosed herein. DETAILED DESCRIPTION

[0059] The present invention will now be described more fully hereinafter with reference to the accompanying drawings, in which illustrative embodiments of the present invention are shown. However, the present invention may be implemented in many different forms and should not be construed as limited to the embodiments set forth herein; on the contrary, these embodiments are provided so that this disclosure will be thorough and complete, and will fully convey the scope of the present invention to those skilled in the art.

[0060] As used herein, the term "and / or" includes any and all combinations of one or more associated listed items. In addition, all conjunctions used should be understood in the most inclusive sense. Therefore, the word "or" should be understood to have the definition of a logical "or", rather than a logical "exclusive or", unless the context clearly requires otherwise. In addition, the singular form and the articles "a", "one (kind)" and "the" are intended to also include plural forms, unless otherwise clearly stated. It will be further understood that when used in this specification, the terms include, comprise, include and / or include specify the presence of the features, integers, steps, operations, elements and / or components, but do not exclude the presence or addition of one or more other features, integers, steps, operations, elements, components and / or groups thereof. In addition, it should be understood that when an element including a component or subsystem is referred to and / or shown as being connected or coupled to another element, it can be directly connected or coupled to another element, or there may be intermediate elements.

[0061] It should be understood that although terms such as "first" and "second" are used herein to describe various elements, these elements should not be limited by these terms. These terms are only used to distinguish one element from another element. Therefore, without departing from the teachings of the present invention, the element discussed below can be referred to as a second element, and similarly, the second element can be referred to as a first element.

[0062] Unless otherwise defined, all terms (including technical and scientific terms) used herein have the same meaning as commonly understood by one of ordinary skill in the art to which the invention belongs. It will be further understood that terms such as those defined in commonly used dictionaries should be interpreted as having a meaning consistent with their meaning in the context of the relevant art, and will not be interpreted in an idealized or overly formal sense unless explicitly defined as such in this article.

[0063] The present invention generally relates to the manufacture of electrodes for electrochemical cells, in many cases for batteries (eg, LIBs). In one example, the battery of interest is a rechargeable LIB.

[0064] Typically, LIB batteries are named according to the acronym of the electroactive material used to form the cathode, usually an intercalation compound. The embodiments described herein can be practiced or applied to various types of lithium-ion batteries currently known in the art (e.g., LCO, LMO, NCM, NCA, LCP, LFP, LFMP, LFSF, or LTS, etc.) or future developed LIBs.

[0065] Many electrode manufacturing techniques for electrochemical cell applications involve forming an electrode (anode or cathode) composition that can be applied (coated, extruded, laminated, etc.) to a conductive substrate. In the composition, the active electrode material is mixed (blended) with a binder (e.g., a polymer, a resin, etc.) that is used to associate and hold the active material together. A liquid is typically included to dissolve or entrain the binder material, plasticizer, and / or other additives.

[0066] Typically, in conventional solvent-based methods, the polymer binder and other components are mixed with a suitable liquid to form a slurry, which can then be applied to a substrate. The typical amount of liquid used is at least about 40% based on the total weight of the ingredients used; many wet processes require even higher amounts of solvent. As the solvent is removed (e.g., during drying), the binder becomes increasingly viscous and adheres to the particles and / or substrate present.

[0067] In contrast to slurry-based techniques, the embodiments described herein relate to a "solvent-free", also referred to as a "dry" process. In this solvent-free method, some and typically all of the ingredients required to prepare the electrode composition (e.g., active materials, binders, additives, etc.) are provided as loose granular materials, such as free-flowing powders, flakes, pellets, beads, etc. The implementations described herein may include one or more operations designed to mix these ingredients (using, for example, equipment designed to blend loose granular materials) and at least one operation designed to handle the binder. Subjecting the binder to certain shear conditions, for example, can result in deformation of the binder, such as elongation of the binder, formation of binder strands, entanglement, etc. For certain types of binders, this is referred to as "fibrillation" of the binder.

[0068] In many aspects of the invention, the ingredients are combined and the adhesive is processed (eg, fibrillated) without the addition of any liquid (eg, solvent).

[0069] Although most embodiments relate to methods that are carried out without liquid addition and are completely solvent-free, a small amount of liquid (e.g., solvent) can be used in some cases to wet, for example, at least some of the particles being mixed. For example, this can occur when forming a pre-blend, which is then completely dried before subsequent operations. In an implementation, any solvent used to form a pre-blend, for example, is removed by drying before the adhesive is deformed. The processing (e.g., fibrillation) of the adhesive is then carried out with loose, free-flowing or pourable particles under completely solvent-free conditions.

[0070] Suitable solvents can be selected from solvents typically encountered in LIB production, and include, but are not limited to, N-methylpyrrolidone (NMP), acetone, alcohols, and water. The solvent can be removed by standard drying techniques. It is expected that such low solvent levels can be completely or nearly completely removed.

[0071] For many applications, the amount of solvent employed is no greater than about 1 wt % and typically less than 1 wt % of the total product electrode composition (e.g., a composition containing electroactive material, treated (e.g., fibrillated) binder, and other ingredients, additive components). In illustrative examples, the amount of solvent employed is in the range of about 0 to up to 1 wt %, such as about 0 to about 0.2, to about 0.4, to about 0.6, to about 0.8 wt %; or about 0.2 to about 0.4, to about 0.6, to about 0.8, to about 1 wt %; or about 0.2 to about 0.4, to about 0.6, to about 0.8, to about 1 wt %; or about 0.4 to about 0.6, to about 0.8, to about 1 wt %; or about 0.4 to about 0.6, to about 0.8, to about 1 wt %; or about 0.6 to about 0.8, to about 1.0 wt %; or about 0.8 to about 1 wt %.

[0072] In other cases, the amount of solvent added can be in the range of about 0 to about 10 weight %, for example, in the range of about 0 to about 2, to about 4, to about 6, to about 8 weight %; or about 2 to about 4, to about 6, to about 8, to about 10 weight %; or about 4 to about 6, to about 8, to about 10 weight %; or about 6 to about 8, to about 10 weight %; or about 8 to about 10 weight %.

[0073] Although it is possible to mix the ingredients and process (e.g., fibrillate) the binder entirely in the absence of solvent, some electrode production schemes use small amounts of solvent in subsequent operations (operations performed after the dry electrode composition has been formed) to "wet" the product film, for example, during calendering. Such processes are also referred to herein as "dry" processes.

[0074] Finished products (e.g., electrodes, self-supporting films, or films laminated on current collectors) prepared by solvent-free or dry processes as described herein can be identified by the absence of detectable processing solvents or processing solvent residues. In contrast, products obtained by wet (slurry) techniques typically contain detectable processing solvents and / or processing solvent residues. In different methods, it is expected that electrode products or films prepared according to embodiments of the present invention show uniform or substantially uniform adhesive distribution over the electrode or film thickness; typically, less uniformity is observed with wet techniques, which typically results in migration of the adhesive toward the film surface.

[0075] As for the ingredients used, the solvent-free process described herein involves: an electroactive component (a material or combination of materials that participates in the electrochemical charge / discharge reaction of an electrochemical cell, such as by absorbing or desorbing lithium); a binder, which may be a fibrillating binder or a non-fibrillating binder; and multifunctional carbon black (CB). Additional ingredients may be included in some cases.

[0076] For many LIB anodes, the electroactive material (also referred to herein as "active electrode material" or simply "active material" or "AM") is graphite, such as natural graphite, artificial graphite (e.g., massive artificial graphite (MAG)), or a blend of the two. Mesocarbon microbeads (MCMB), mesophase pitch-based carbon fiber (MCF), vapor grown carbon fiber (VGCF) may also be used. In other embodiments, the active anode compound comprises, consists essentially of, or consists of silicon, such as a silicon-graphite composite, a nano-silicon (Si) or SiO-containing carbon fiber. x Particles of graphite.

[0077] The principles described herein can also be used with other active anode materials (e.g., those known or currently explored, or those developed in the future). Examples include, but are not limited to: (a) intercalation / deintercalation materials (e.g., carbon-based materials, porous carbon, graphene, TiO2, Li4Ti5O 12 (b) alloying / dealloying materials (e.g., Si, SiO x , doped Si, Ge, Sn, Al, Bi, SnO2, etc.); and (c) conversion materials (such as transition metal oxides (Mn x O y 、NiO、Fe x O y, CuO, Cu2O, MoO2, etc.), by formula M x X y Metal sulfides, metal phosphides and metal nitrides represented by X=S, P, N)).

[0078] The amount of active anode material can vary depending on the specific type of energy storage device. In an illustrative example, the amount of active anode material (e.g., graphite) is at least 80% by weight, such as at least 85% by weight, at least 90% by weight, at least 95% by weight, or at least 99% by weight, relative to the total weight of the (dry) electrode composition. The amount of anode active material (e.g., graphite) can be about 80% by weight to about 85% by weight, 90% by weight, 93% by weight, 96% by weight, 99% by weight; or about 85% by weight to about 90% by weight, 93% by weight, 96% by weight, 99% by weight; or about 90% to about 93, 96, 99% by weight; or about 93% to about 96, 99% by weight; or about 96% to about 99% by weight.

[0079] Dry processes for preparing LIB cathodes can use LCO (lithium cobalt oxide), LMO (lithium manganese oxide), NCM (lithium nickel cobalt manganese oxide), NCA (lithium nickel cobalt aluminum oxide), LCP (lithium cobalt phosphate), LFP (lithium iron phosphate), LMFP (lithium manganese iron phosphate), LFSF (lithium iron fluorosulfate), LTS (lithium titanium sulfide). Materials such as these are generally referred to herein as "lithium transition metal compounds", such as "lithium transition metal oxides". In addition to cathode materials based on intercalation chemistry (e.g., chemical reactions typically involving the transfer of a single electron), other types of cathode materials (e.g., with lithium ions inserted into FeF3) can transfer multiple electrons through more complex reaction mechanisms (called conversion reactions). Other active cathode materials known in the art or developed in the future can be used.

[0080] In some embodiments, the dry process described herein utilizes NCM (also referred to as "NMC") or NCA cathode compositions. These materials are generally known to those skilled in the art. In addition, many battery-grade formulations (e.g., NCM622) are commercially available in powder form.

[0081] In more detail, NCM can be represented by the formula Li 1+x (Ni y Co 1-y-z Mn z ) 1-x O2 represents, wherein x is in the range of 0 to 1, y is in the range of 0 to 1 (e.g., 0.3-0.8), and z is in the range of 0 to 1 (e.g., 0.1-0.3). Examples of NCMs include Li 1+x (Ni 0.33 Co 0.33 Mn0.33 ) 1-x O2、Li 1+x (Ni 0.4 Co 0.3 Mn 0.3 ) 1-x O2、Li 1+x (Ni 0.4 Co 0.2 Mn 0.4 ) 1-x O2、Li 1+x (Ni 0.4 Co 0.1 Mn 0.5 ) 1-x O2、Li 1+x (Ni 0.5 Co 0.1 Mn 0.4 ) 1-x O2、Li 1+x (Ni 0.5 Co 0.3 Mn 0.2 ) 1-x O2、Li 1+x (Ni 0.5 Co 0.2 Mn 0.3 ) 1-x O2、Li 1+x (Ni 0.6 Co 0.2 Mn 0.2 ) 1-x O2、Li 1+x (Ni 0.8 Co 0.1 Mn 0.1 ) 1-x O2 and Li 1+x (Ni 0.9 C 0.05 Mn 0.05 ) 1-x O2.

[0082] NCA can be composed of the formula Li 1+x (Ni y Co 1-y-z Al z ) 1-x O2 represents, wherein x is in the range of 0 to 1, y is in the range of 0 to 1, and z is in the range of 0 to 1. An example of NCA is Li 1+x (Ni 0.8 Co 0.15 Al 0.05 ) 1-x O2.

[0083] The amount of electroactive cathode material employed may vary depending on the specific type of energy storage device. In illustrative examples, the amount of NCM or NCA is at least 90 wt %, such as at least 93 wt %, at least 96 wt %, at least 98 wt %, or at least 99 wt %, relative to the total weight of the (dry) electrode composition. NCM or NCA may be about 90 wt % to about 93 wt %, 96 wt %, 99 wt %; or about 93 to about 96, 99 wt %; or about 96 to about 99 wt %.

[0084] In addition to the active material, the dry process described herein employs a binder. Generally, the binder can be any semi-crystalline polymer.

[0085] In some embodiments, the binder is a fibrillating binder.The fibrillating binder may be provided in an adhesive component that consists of, consists essentially of, or comprises a fibrillating binder.

[0086] Under certain processing conditions, such as high shear mixing in the presence of a fibrillating agent, a binder capable of fibrillation can produce fibrils, forming a network that can connect and carry other particles present in the formulation. In more detail, it is believed that the fibrillation of the binder produces a matrix, lattice or network of fibrils that impart mechanical structure to the electrode. In the product electrode, the fibrillated binder can be detected in the SEM image, which will show the presence of fibrils wrapped around at least a portion of at least some of the particles (e.g., active material particles) present. Other indirect techniques that can be used to assess the relative degree of binder fibrillation include, for example, energy dispersive X-ray spectroscopy (EDX), powder rheology, and tensile strength. EDX allows the distribution of fluorine elements in the entire dry electrode to be mapped and the effectiveness of binder fibrillation to be assessed. Powder rheology measures the cohesive interactions between particles in a free-flowing electrode powder mixture, while the tensile strength test measures the strength of a self-supporting electrode film, both of which represent the degree of binder fibrillation. In some cases, poor or no fibrillation can be inferred for dried product electrode films that crumble or peel away from the substrate.

[0087] In some implementations, the binder capable of fibrillation is a fibrillation-capable fluoropolymer, such as polytetrafluoroethylene or PTFE.Other binders that are considered capable of fibrillation include, but are not limited to, ultra-high molecular weight polypropylene, polyethylene, and copolymers, and any combination thereof.

[0088] The binder capable of fibrillation (alone or as a component of a binder component (e.g., in a polymer blend)) can be provided in an amount of about 1 to about 10 wt%, such as about 1-2, 2-3, 3-4, 4-5, 5-6, 6-7, 7-8, 8-9, 9-10 wt%. In one example, the binder capable of fibrillation is provided in an amount of about 5 wt%. In other examples, the binder capable of fibrillation is present in an amount of about 1 to about 2, about 3, about 4, about 5, about 6, about 7, about 8, about 9 weight %; or about 2 weight % to about 3 weight %, about 4 weight %, about 5 weight %, about 6 weight %, about 7 weight %, about 8 weight %, about 9 weight %, about 10 weight %; or about 3 weight % to about 4 weight %, about 5 weight %, about 6 weight %, about 7 weight %, about 8 weight %, about 9 weight %, about 10 weight %; or about 4 to about 5, about 6, about 7, about 8, about 9, about 10 weight %; or about 5 to about 6, about 7, about 8, about 9, about 10; or about 6 to about 7, about 8, about 9, about 10 weight %; or about 7 to about 8, about 9, about 10 weight %; or about 8 weight % to about 9 weight %, about 10 weight %.

[0089] However, not all situations use adhesives that can fibrillate. Therefore, some embodiments of the present invention use adhesive components that are composed of one or more adhesives that cannot fibrillate, are essentially composed of one or more adhesives that cannot fibrillate, or contain one or more adhesives that cannot fibrillate. As used herein, the term "non-fibrillable" adhesive refers to an adhesive that is difficult to fibrillate under the same conditions that are sufficient to fibrillate the "fibrillable" adhesive. However, even if complete fibrillation is not achieved, aspects of the present invention (under the same or substantially the same processing conditions for the counterpart that can fibrillate) can still cause the adhesive that cannot fibrillate to deform, such as stretching, elongation, entanglement, etc., usually to a significant extent.

[0090] Without wishing to be bound by a particular explanation or mechanism, it is believed that fibrillation can be considered an extreme phenomenon in which the adhesive polymer (which may start out as a colloidal particle) becomes very thinly stretched, forming very long (high aspect ratio) strands (ribbons) that can bridge more than two electroactive particles, thereby holding them together. Practicing the embodiments described herein can also result in stretching (elongation) and / or entanglement of the adhesive that is not capable of fibrillation, forming a CB-adhesive composite and / or becoming coated with CB. Even if fully fibrillated, this "treated" adhesive that is not capable of fibrillation can still be used as a glue to connect, bond together and provide connectivity and adhesion to the current collector for the electroactive particles. Deformation of the adhesive that is not capable of fibrillation can be observed by at least some of the above-mentioned techniques.

[0091] In an example, the adhesive that can not be fibrillated is a fluoropolymer, such as polyvinylidene fluoride (PVDF). Other examples that can be considered as the adhesive that can not be fibrillated include poly (vinyl difluoride-to-hexafluoropropylene) (PVDF-HFP), polyimide and water-soluble adhesive, such as poly (ethylene oxide), polyvinyl alcohol (PVA), polyvinyl pyrrolidone (PVP), polyvinyl acetate, polyethylene-to-vinyl acetate, some polyolefins, cellulose, cellulose derivatives etc. Other possible adhesives that can not be fibrillated include polyethylene and polypropylene, ethylene-propylene-diene terpolymer (EPDM), sulfonated EPDM, styrene-butadiene rubber (SBR) and fluororubber except ultra-high molecular weight type, and their copolymers and mixtures. In an example, the adhesive that can not be fibrillated is cellulose ester, cellulose ether, nitrocellulose, carboxyalkyl cellulose, cellulose salt and cellulose salt derivatives. In some embodiments, the particulate non-fibrillating binder is selected from at least one of cellulose, cellulose acetate, methyl cellulose, ethyl cellulose, hydroxypropyl cellulose (HPC), hydroxyethyl cellulose (HEC), nitrocellulose, carboxymethyl cellulose (CMC), carboxyethyl cellulose, carboxypropyl cellulose, carboxyisopropyl cellulose, sodium cellulose, sodium nitrate cellulose, and sodium carboxyalkyl cellulose. Other examples use a combination of a non-fibrillating binder (e.g., PVDF) and a non-fibrillating binder (e.g., PTFE).

[0092] The same or similar amounts of binder that are not capable of fibrillation may be used as those used for the binder capable of fibrillation.Other suitable amounts may be determined, for example, by routine experimentation.

[0093] It is also possible to use a combination of a binder that is capable of fibrillating and a binder that is not capable of fibrillating.

[0094] Electrode compositions typically include ingredients such as conductivity additives (eg, conductive carbon additives or CCA), plasticizers, etc. In the case of solvent-free processes, conventional techniques also require a binder fibrillating (also called "fibrillating") agent or auxiliary, typically an AC.

[0095] It is found that conventional fibrillating additives (e.g., AC) can be supplemented and often completely replaced by CB materials that provide multiple benefits. For example, certain carbon blacks can be used as binder fibrillating (or in some cases, binder deforming) agents, as conductivity additives (creating conductive networks, such as long-range conductivity of electrodes), and as mechanical reinforcement aids (imparting mechanical load-bearing, stability, and / or flexibility to electrode products, usually coatings, layers, or films typically applied to conductive substrates to form battery electrodes).

[0096] Typically, CB is a material that exists in the form of aggregates, which in turn are formed from CB primary particles. In most cases, primary particles do not exist independently of CB aggregates. While primary particles may have an average primary particle diameter in the range of about 10 nanometers (nm) to about 50 nm, for example, about 10 nm to about 15 nm; about 10 nm to about 20 nm; about 10 nm to about 25 nm; about 10 nm to about 30 nm; or about 10 nm to about 40 nm, aggregates may be quite large. CB aggregates have a fractal geometry and are generally referred to in the art as CB "particles" (not to be confused with the "primary particles" described above).

[0097] Many types of CB are produced in a furnace-type reactor by pyrolyzing a hydrocarbon feedstock (FS) with hot combustion gases to produce a combustion product containing particulate CB. The properties of a given CB generally depend on the manufacturing conditions and can be changed or modified, for example, by changes in temperature, pressure, FS, residence time, quench temperature, throughput, and / or other parameters.

[0098] As is known in the art, CBs can be described by certain properties determined according to procedures well known in the art (usually standardized protocols). For example, CBs can be characterized by: their Brunauer-Emmett-Teller (BET) surface area, measured, for example, according to ASTM D6556-10; their oil absorption number (OAN), determined, for example, according to ASTM D 2414-16; their statistical thickness surface area (STSA), a property that can be determined by ASTM D 6556-10.

[0099] For a given CB, it may also be of interest in some cases to specify the ratio of its STSA to its BET surface area (STSA:BET ratio).

[0100] The crystalline domains of CB can be characterized by the La crystallite size as determined by Raman spectroscopy. La is defined as 43.5×(area of ​​the G band / area of ​​the D band). The crystallite size can give an indication of the degree of graphitization, with higher La values ​​associated with higher degrees of graphitization. Raman measurements of La are based on "Raman studies of heat-treated carbon blacks" by Gruber et al., Carbon, Vol. 32(7), pp. 1377-1382, 1994, which is incorporated herein by reference. The Raman spectrum of carbon includes a wavelength of about 1340 cm -1 and 1580cm -1 There are two main "resonance" bands at , denoted as "D" and "G" bands. The D band is usually attributed to the disordered sp 2carbon, and the G band is attributed to graphitic or "ordered" sp 2 Carbon. Using an empirical method, the ratio of the G / D band is highly correlated with La measured by X-ray diffraction (XRD), and regression analysis gives the empirical relationship:

[0101] L a =43.5×(area of ​​G band / area of ​​D band),

[0102] Where L a Measured in angstroms. Therefore, higher L a Values ​​correspond to more ordered crystal structures.

[0103] The crystallization domain can be obtained by L c The L was determined by X-ray diffraction using an X-ray diffractometer (PANalytical X'Pert Pro, PANalytical BV) with a copper tube, a tube voltage of 45 kV and a tube current of 40 mA. c Crystallite size. A sample of carbon black particles was loaded into a sample holder (accessory of the diffractometer) and measured at a speed of 0.14° / min in an angle range of 10° to 80° (2q). The peak position and the full width at half maximum value were calculated by the diffractometer software. For the measurement angle calibration, lanthanum hexaboride (LaB6) was used as an X-ray standard. Based on the obtained measurement results, the Scherrer equation was used. To determine L c crystallite size, where K is the shape factor constant (0.9); λ is the Cu K α1 The wavelength of the characteristic X-rays β is the peak width at half maximum in radians; and q is determined by taking half the measured angular peak position (2q).

[0104] Surface cleanliness can be described by the surface energy (SEP) of the CB, which is a property that can be determined by dynamic vapor (water) adsorption (DVS) or water diffusion pressure (as described, for example, in U.S. Patent No. 10,886,535 B2, issued to Korchev et al. on January 5, 2021, and incorporated herein by reference).

[0105] Average pore diameter and pore volume can be determined according to the technique described in EP Barrett, LG Joyner, PP Halenda, J. Am. Chem. Soc. 1951, 73, 373-380 (BJH method).

[0106] Other techniques that can be used to study CBs include Fourier transform infrared (FTIR) spectroscopy, thermogravimetric analysis (TGA), X-ray photoelectron spectroscopy (XPS), scanning electron microscopy (SEM), and transmission electron microscopy (TEM). FTIR spectroscopy is particularly useful for determining the nature of surface functional groups, while SEM / TEM techniques help visualize the size and morphology of particles. XPS is often used to determine the elemental composition of a material, and TGA can provide information about the decomposition and oxidation characteristics of carbon.

[0107] Tables 1A and 1B below present physical properties that characterize illustrative CBs (ie, CB1 through CB17).

[0108] Table 1A

[0109]

[0110] Table 1B

[0111]

[0112] Various CBs have been and continue to be developed for carbon conductivity additive (CCA) applications. Attractive electrical conductivity is generally combined with high specific surface and extensively developed structure (arrangement of primary CB particles within the aggregate) and porosity. CBs that can be added to anode and / or cathode compositions for LIBs prepared by a slurry process are described, for example, in International Publication No. WO2020 / 197670 of Cabot Corp., published on October 1, 2020, and WO2020 / 197673 of Cabot Corp., published on October 1, 2020. Both are incorporated herein by reference in their entirety.

[0113] Examples of commercially available CBs that are effective as CCAs include the CCAs available from Cabot Corporation. 50. 63. 66. 200, 300, HP and MAX 90 carbon black pellets; C-NERGY from Imerys TM C45, C-NERGY TM C65 and SUPER products; Li-400, Li-250, Li-100 and Li-435 products from Denka; and EC300 and EC600 products from Ketjen.

[0114] Further to exhibiting the electrical conductivity required for LIB applications, other properties that may contribute to the multifunctionality of CBs relate to one, more, or all of the following: surface roughness; surface chemistry (surface energy); particle strength; and particle size.

[0115] Typically, CB surface roughness is related to the porosity of the particle, such as described by pore volume or pore size distribution. For example, it is known that RMS surface roughness (calculated as the root mean square of the measured microscopic peaks and valleys of the surface) is related to the surface pore size (e.g., of similar order of magnitude). For example, 2 nm pores may indicate an approximate RMS surface roughness of 1 nm.

[0116] Broadly speaking, CB porosity can belong to one or more of the following categories: microporosity, defined by pores with diameters less than 2 nm; mesoporosity, defined by pores with diameters ranging from 2 to 50 nm; and macroporosity, defined by pores with diameters greater than 50 nm.

[0117] The pore size distribution and pore volume in carbon black can be determined by gas physical adsorption techniques such as nitrogen adsorption porosimetry, by measuring nitrogen adsorption using BET analysis, and then fitting the adsorption isotherm with different models (e.g., DFT (density functional theory) and BJH (Barrett-Joyner-Halenda) model) according to the pore size region of interest. The BJH adsorption model is relied upon to fit the N2 adsorption isotherm and calculate the mesopore and macropore volumes provided herein.

[0118] Without wishing to be bound by a particular explanation, it is believed that the fibrillating nature in the multifunctional CB may be driven at least in part by the macroporosity of the particles, where the macropores serve as anchor points for interlocking the binder on the CB surface and stretching the binder into fibrils when high shear forces are applied.

[0119] While some carbon blacks are primarily microporous materials, techniques exist for increasing the porosity level and / or producing CBs with tailored porosity types.

[0120] For example, contacting the CB starting material with an oxidant stream can enhance the porosity, particularly the mesoporous properties, of the CB product. Increasing the porosity of furnace black can be achieved by extending the residence time in the carbon black reactor, allowing the tail gas extra time to erode and etch the carbon surface. Another method relies on adding alkaline earth metal ions to the carbon black feedstock, because these ions are known to catalyze the etching of carbon black by the tail gas. Both techniques involve "in situ" etching of the CB, i.e., etching the CB in the furnace reactor during production to produce a carbon black with internal porosity. Some methods that can be used to modify carbon black are described in, for example, U.S. Patent No. 8,895,142B2 to Kyrlidis et al. and U.S. Patent No. 10,087,330B2 to Green et al., both of which are incorporated herein by reference. Commercially, the modified carbon black that can be used is available from Cabot Corporation. In Tables 1A and 1B above, CB 15 is a steam-etched form of CB4.

[0121] It is also found that fibrillation properties depend on surface chemistry or surface activity, which is a function generally associated with the manufacturing and / or heating processes used in preparing a particular CB. In many cases, surface chemistry or surface activity is associated with oxygen-containing groups found on the CB surface. In some embodiments, good fibrillation CB candidates lack or are depleted of oxygen-containing surface groups, tending to be less hydrophilic (more hydrophobic).

[0122] For example, it is believed that effective fibrillation is driven at least in part by the affinity (adhesion) of the CB and the adhesive (e.g., an adhesive capable of fibrillation). Therefore, in one implementation, a preferred multifunctional CB for successfully fibrillating an adhesive such as PTFE is a hydrophobic CB (i.e., a CB lacking oxygen-containing surface groups) and / or a low surface energy CB. The oxygen content can be measured by inert gas fusion. The oxygen content of the low surface chemistry CB is in the range of about 10ppm to about 5000ppm, for example, about 100ppm to about 1000ppm.

[0123] The presence of oxygen-containing surface groups can be reduced or minimized by techniques known in the art or to be developed in the future, such as heat treatment or other surface modification methods. Surface-modified (e.g., heat-treated) CBs can be compared and differentiated from conventional carbon blacks by X-ray scattering, Raman spectroscopy, surface energy measurements by gas adsorption, or other techniques known in the art. In some cases, heat-treated and other surface-modified CBs also tend to show reduced moisture absorption during treatment. In Tables 1A and 1B, CB9 is a heat-treated form of CB11, while CB3 is a heat-treated form of CB4.

[0124] Other CB properties to be considered in multifunctional CB candidates relate to their physical form. For example, CB particle size is a property that can be determined by particle size distribution (PSD) technology and / or scanning electrode microscopy (SEM). It is also believed that the particle strength (shown as particle hardness and / or particle cohesion) of the CB plays a role in the multifunctional properties of the selected CB. Particle strength allows the CB to effectively stretch the polymer adhesive; this, together with particle roughness, can represent a very important mechanical property for achieving desired adhesive fibrillation. Particle strength can be measured by single pellet collision testing, oscillatory viscoelasticity measurements, or other techniques known in the art.

[0125] Initially (before the CB undergoes mixing (particularly high shear mixing)), the D50 particle size of the multifunctional CB used may be in the range of about 0.5 to about 20 μm, for example, in the range of about 1 to about 10 μm, for example, in the range of about 2 to about 5 μm. As a result of the binder treatment, such as fibrillation (usually under high shear conditions), the starting multifunctional CB particles may be broken into smaller particles, whose particle size is, for example, in the range of about 0.05 to about 1 μm, for example, about 0.1 to about 0.3 μm.

[0126] For example, a multifunctional CB may be combined with a second CB (which may or may not be multifunctional) in a CB blend.

[0127] The CB granular material may be provided in any number of forms. For example, it has been found that a truly fluffy CB-containing powder performs particularly well in some of the dry processes tested. Such powdered materials may be characterized by their particle size, BET and / or other properties. In many cases, the density of the powder used is no greater than about 100 g / cm 3 .

[0128] For example, less fluffy CB particles in the form of jet-milled pellets can also be used. Powdered CB can be granulated using techniques and equipment known in the art. In one example, CB is granulated together with an emulsion solution of a binder for forming an electrode composition as described herein. Other methods use emulsion solutions of different binders, such as binders belonging to the same chemical family group or having similar functional active groups, which can be combined with or otherwise interact with the binder for performing a dry process. Therefore, it is believed that the energy interaction between the granulated CB and the binder for preparing the electrode composition is increased.

[0129] Suitable pellet sizes for pure CB may range from about 0.1 mm to about 5 mm. In one example, the particle size is from about 0.1 to about 0.5, 1, 1.5, 2, 2.5, 3, 3.5, 4, 4.5 mm, or from about 0.5 to about 1, 1.5, 2, 2.5, 3, 3.5, 4, 4.5, 5 mm; or from about 1 to about 1.5, 2, 2.5, 3, 3.5, 4, 4.5, 5 mm; or from about 1.5 to about 2, 2.5, 3, 3.5, 4, 4.5, 5 mm; or from about 2 to about 2.5, 3, 3.5, 4, 4.5, 5 mm; or from about 2.5 to about 3, 3.5, 4, 4.5, 5 mm; or from about 3 to about 3.5, 4, 4.5, 5 mm; or from about 3.5 to about 4, 4.5, 5 mm; or from about 4 to about 4.5, 5 mm; or from about 4.5 to about 5 mm.

[0130] Carbon black pellets are also useful in some cases. In many cases, CB pellets are a densified form of CB, with no polymer present in the final product. Typically, CB pellets can be formed by conventional pelletizing processes associated with CB production. CB pellets can also be formed by dispersing fluffy CB in water and then spray drying.

[0131] In some embodiments, the particles used change their form and / or function during the solvent-free technology described herein. Therefore, the initial CB granular material can be relied upon to process (e.g., fibrillate) the polymer binder. The size crushing that occurs during this operation can release smaller CB units. In the presence of electroactive materials, the fragmentation of the particles can enhance the distribution of smaller CB units throughout the electrode composition, resulting in an electrode film with improved conductivity and / or mechanical strength.

[0132] The surface roughness and / or surface energy of the particles is usually controlled by selecting the particles that make up the particles. For example, the surface roughness can be selected based on the surface texture produced by the primary particles and / or aggregates that make up the secondary particles. Such a surface is rough on a dimensional scale, where the roughness is provided by the nanometer / micrometer scale of the hills and valleys on the surface of the CB particles.

[0133] The multifunctional CB in the form of particles can have a particle size in the micrometer range, such as 1-10 μm, for example: about 1 to about 2, 3, 4, 5, 6, 7, 8, 9 μm; or about 2 to about 3 μm, 4 μm, 5 μm, 6 μm, 7 μm, 8 μm, 9 μm, 10 μm; or about 3 to about 4 μm, 5 μm, 6 μm, 7 μm, 8 μm, 9 μm, 10 μm; or about 4 to about 5, 6, 7, 8, 9, 10 μm; or about 5 to about 6, 7, 8, 9, 10 μm; or about 6 to about 7, 8, 9, 10 μm; or about 7 to about 8, 9, 10 μm; or about 8 to about 9, 10 μm; or about 9 to about 10 μm. For some particles, the initial size can be reduced by grinding to various degrees, for example from approximately 10 μm to less than 1 μm. Some implementations utilize a combination of sizes.

[0134] The strength of the pellets may also be considered. This may be minimized by forming the pellets in the absence of (or with minimal content of) a binder during pellet formation; increased strength of the pellets may be achieved by using different concentrations of binder and / or different types of binders. In some implementations, the binder used to form the CB pellets is the same or similar binder as used in the dry process, such as a binder capable of fibrillation.

[0135] Some embodiments employ particulates that are fragile under processing conditions such as fibrillation. In this case, the strength of the particulates can be controlled so that the strength is high enough to fibrillate or deform the polymer binder and low enough to separate the particulates and release conductive and reinforcing carbon units, such as aggregates.

[0136] Particulate CB can be used as a multifunctional additive alone or in combination with another form of CB, which in some cases may also be multifunctional.

[0137] The CB used in the dry process described herein is selected or customized to perform two or more functions. In a specific embodiment, various CB attributes are balanced to achieve the best possible combination of electrical conductivity, adhesive fibrillation and / or mechanical properties. For example, the CB that is considered to be an excellent CCA additive may not necessarily be proven to be a good or even enough fibrillation aid. Therefore, when using CB, it may be necessary to select a process and sometimes compromise, which brings good electrical conductivity and good fibrillation properties. The multifunctional properties of realizing or optimizing CB can rely on the experimental evaluation of the performance of the film and / or electrode produced by the solvent-free process. Suitable CB can also be selected by considering their properties, for example, relevant to specific dry process scheme or conditions.

[0138] In one example, the CB is selected to combine sufficient surface area (e.g., as measured by BET N2 adsorption) for optimal adhesive processing, such as fibrillation, while ensuring that the specific CB aggregates used (e.g., CB pellets or jet-milled CB particles) can be broken down into sufficiently small particles, such as less than 2 microns (μm), to maximize surface interactions between the CB particles and the adhesive to effectively process (e.g., fibrillate) the adhesive.

[0139] The CB used in the dry process described herein may have a thickness of not greater than about 1600 m 2 / g, for example, not more than about 1500, 1400, 1300, 1200, 1100, 1000, 900, 800, 700, 600, 500, 400, 300, 200, 100 or 35 m 2 / g BET. BET can be in the range of about 35 to about 1600, for example, about 35 to about 100, 200, 300, 400, 500, 600, 700, 800, 900, 1000, 1100, 1200, 1300, 1400, 1500; or about 100 to about 200, 300, 400, 500, 600, 700, 800, 900, 1000, 1100, 1200, 1300, 1400, 1500, 1600; or about 200 to about 300, 400, 500, 600, 700, 800, 900, 1000, 1100, 1200, 1300, 1400, 1500, 1600; or about 300 to about 400, 500, 600, 700, 800, 900, 1000, 1100, 1200, 1300, 1400, 1500, 1600; or about 400 to about 500, 600, 700, 800, 900, 1000, 1100, 1200, 1300, 1400, 1500, 1600; or about 500 to about 60 0, 700, 800, 900, 1000, 1100, 1200, 1300, 1400, 1500, 1600; or about 600 to about 700, 800, 900, 1000, 1100, 1200, 1300, 1400, 1500, 1600; or about 700 to about 800, 900, 1000, 1100, 1200, 1300, 1400, 1500, 1600; or about 800 to about 900, 1000, 1100, 1200, 1300, 1400 , 1500, 1600; or about 900 to about 1000, 1100, 1200, 1300, 1400, 1500, 1600; or about 1000 to about 1100, 1200, 1300, 1400, 1500, 1600; or about 1100 to about 1200, 1300, 1400, 1500, 1600; or about 1200 to about 1300, 1400, 1500, 1600; or about 1300 to about 1400, 1500, 1600; or about 1400 to about 1500m 2 / g、1600m 2 / g; or about 1500 to about 1600.

[0140] The CB used in the dry process described herein may have an OAN of not greater than about 650 ml / 100 g, e.g., not greater than about 600, not greater than about 500, not greater than about 400, not greater than about 300, not greater than about 250, not greater than about 200, not greater than about 150, not greater than about 120 ml / 100 g. The OAN of the multifunctional CB can be in the range of about 120 to about 650 ml / 100 g, for example, about 120 to about 200, to about 300, to about 400, to about 500, to about 600, to about 650 ml / 100 g; or about 200 to about 300, to about 400, to about 500, to about 600, to about 650 ml / 100 g; or about 300 to about 400, to about 500, to about 600, to about 650 ml / 100 g; or about 400 to about 500, or to about 600, to about 650 ml / 100 g; or about 500 to about 600, to about 650 ml / 100 g; or about 600 to about 650 ml / 100 g.

[0141] LIB anodes can be prepared by a dry process using a BET of no greater than about 1600 m 2 / g, for example, not more than about 1500, not more than about 1200, not more than about 1000, not more than about 700, not more than about 500, not more than about 200, not more than about 100, or not more than about 35 m 2 / g of CB. BET can be from about 35 to about 1600 m 2 / g. For example, BET can be from about 35 to about 50, to about 75, to about 100, to about 150, to about 200; or from about 50 to about 75, to about 100, to about 150, to about 200; or from about 75 to about 100, to about 150, to about 200; or from about 100 to about 150, to about 200; or from about 150 to about 200m 2 In one example, the BET of the selected CB is about 55 m 2 / g to about 200m 2 / g range.

[0142] For anode applications, the CB used in the solvent-free process described herein can have an OAN of not greater than about 650 ml / 100 g, e.g., not greater than about 500, not greater than about 400, not greater than about 300, not greater than about 240, not greater than about 200, not greater than about 150, not greater than about 120 ml / 100 g. In one implementation, the OAN of the CB selected for preparing the LIB anode by the dry process is in the range of about 120 to about 650 ml / 100 g, such as about 120 to about 150, about 200, about 240, about 300 ml / 100 g; or about 120 to about 150, about 200, about 240, about 300 ml / 100 g; or about 120 to about 150, about 200, about 240, about 300 ml / 100 g; or about 150 to about 200, about 240, about 300 ml / 100 g; or about 200 to about 240, about 300 ml / 100 g; or about 200 to about 240, about 300 ml / 100 g; or about 240 to about 300 ml / 100 g. In one example, the selected CB has an OAN in the range of about 130 to about 240 ml / 100 g.

[0143] The LIB cathode can be prepared by a dry process using a BET of at least about 90 m 2 / g, for example at least about at least: 90, 100, 200, 300, 400, 500, 600, 700, 800, 900, 1000, 1100, 1200, 1300, 1400, 1500, up to about 1600m 2 / g CB. BET can be between about 500 and about 1600m 2 / g, for example, in the range of about 800 to about 900, 1000, 1100, 1200, 1300, 1400, 1500; or about 900 to about 1000, 1100, 1200, 1300, 1400, 1500, 1600; or about 1000 to about 1100, 1200, 1300, 1400, 1500, 1600; or about 1100 to about 1200, 1300, 1400, 1500, 1600; or about 1200 to about 1300, 1400, 1500, 1600; or about 1300 to about 1400, 1500, 1600; or about 1400 to about 1500, 1600m 2 / g, or about 1500 to about 1600m 2 In one example, the BET of the selected CB is about 1350 m 2 / g to about 1600m 2 In another example, the BET of the selected CB is between about 50 and about 190 m 2 / g, for example, about 90 to about 100 m2 In another example, the BET of the CB is 500-650 m 2 / g.

[0144] For cathode applications, the CB used in the solventless process described herein can have an OAN of no greater than about 650 ml / 100 g, such as less than about 600, less than about 500, less than about 500, less than about 400, less than about 300, less than about 250, less than about 200, as low as about 120 ml / 100 g. The OAN of the CB can be in the range of about 120 to about 250, to about 350, to about 450, to about 550; or about 250 to about 350, to about 450, to about 550, to about 650; or about 350 to about 450, to about 550, to about 650; or about 450 to about 550, to about 650 ml / 100 g; or about 550 to about 650 ml / 100 g. In one example, the selected CB has an OAN in the range of about 250 to about 650 ml / 100 g.

[0145] In many cases, the CBs useful for preparing LIB cathodes by the dry methods described herein have a relative humidity of about 80 to about 1600 m 2 The BET surface area of ​​the LIB cathode is about 1350 to about 1600 m / 100 g and the OAN surface area of ​​the LIB cathode is about 120 to about 650 m / 100 g. 2 / g range), and relatively low OAN (e.g., in the range of about 120 to about 220 ml / 100 g). Another exemplary CB that can be used to prepare a LIB cathode has a BET surface area of ​​about 80 to about 200 m 2 / g, OAN is between about 140 and about 280 m 2 / g range, such as about 240 or less, in the range of about 140 to about 180 ml / 100 g. Another exemplary CB has a range of about 500 to about 1600 ml / 100 g. 2 / g and an OAN in the range of about 180 to about 650 ml / 100 g. Another exemplary CB that can be used to prepare a LIB cathode has a BET below 650 m / 100 g. 2 / g (e.g., between about 500 and about 650 m 2 / g) and a BET surface area in the range of about 180 to about 260 ml / 100 g.

[0146] In many cases, the CBs useful for preparing LIB anodes by the dry methods described herein have a relative humidity of about 35 to about 1600 m 2The BET surface area of ​​the LIB anode is about 50 to about 200 m / 100 g, and the OAN surface area of ​​the LIB anode is about 120 to about 650 m / 100 g. 2 / g range) and OAN in the range of about 130 to about 240 ml / 100 g.

[0147] In many implementations, the L a The crystallite size is at least For example to For example, L of CB a The crystallite size can be about to about 20, about 30, about or about to about 30, to about 40, to about or about to about 40, about or about 40 to about

[0148] The surface energy (SEP) of the multifunctional CB described herein may be less than or equal to 15 mJ / m 2 , for example, about 1 to about 10 mJ / m 2 , for example, about 1 to about 3, about 5, about 7, about 9 mJ / m 2 ; or about 3mJ / m 2 About 5mJ / m 2 , about 7mJ / m 2 , about 9mJ / m 2 , about 10mJ / m 2 ; or about 5mJ / m 2 About 7mJ / m 2 , about 9mJ / m 2 , about 10mJ / m 2 ; or about 7mJ / m 2 About 9mJ / m 2 , about 10mJ / m 2 ; or about 9mJ / m 2 About 10mJ / m 2 .

[0149] Regarding porosity, the multifunctional CB may have a porosity of at least 0.35 cm 3 / g of mesopore volume, for example, from about 0.35 to about 2 cm 3 / g, and at least 1cm 3 / g of the total volume of mesopores and macropores, for example, from about 1 to about 3 cm 3 In some implementations, for high surface area CBs (e.g., BET greater than about 800 m 2 / g), for example, the mesopore volume is about 0.35 to about 0.5, about 1, about 1.5; about 0.5 cm 3 / g to about 1cm 3 / g, about 1.5cm 3 / g, about 2cm 3 / g; or about 1 to about 1.5, about 2; or about 1.5cm 3 / g to about 2cm 3 / g.

[0150] The total volume of mesopores and macropores used to characterize the multifunctional CB can be at least 0.2 cm 3 / g, typically higher. In one example, the multifunctional CB used to prepare the anode composition has a thickness of about 0.2 to about 0.8 cm 3 The total volume of mesopores and macropores in the range of 1 / g. Multifunctional CBs suitable for preparing cathode compositions generally have a volume of at least 1 cm 3 / g of total mesopore and macropore porosity.

[0151] The total volume of the mesopores and macropores may be from about 1 to about 1.5, about 2, about 2.5 cm 3 / g; or about 1.5 to about 2.0, about 2.5, about 3 cm 3 / g; or about 2 to about 2.5, about 3cm 3 / g; or about 2.5 to about 3 cm 3 / g.

[0152] In many implementations, the multifunctional CB has a % crystallinity of at least 22%, such as 23% to 50%, such as between about 23 and about 30, 35, 40, 45%; or between about 30 and about 35, 40, 45, 50%; or between about 35 and about 40, 45, 50%; or between about 40 and about 45, 50%; or between about 45 and about 50%.

[0153] Examples of suitable CB materials that may be used include commercially available specifications such as: Series CB (e.g. XCmax 22), Black Series CB (e.g. BP2000 carbon black), Series CB (e.g. PBX 51), Series CB (e.g. LITX HP).

[0154] Electrode compositions prepared by solvent-free processes as described herein typically include multifunctional CBs (as described herein), active electrode materials, and "treated" binders. Some product electrode compositions, particularly those prepared with binders capable of fibrillation, will include fibrillated binders (also referred to herein as "fibrillated binders") that typically exhibit fibrils of high aspect ratio. Compositions prepared with binders that are not capable of fibrillation will still present "treated" binders, i.e., "deformed" (elongated, tangled, etc.) but may be less than the degree observed with binders capable of fibrillation under the same or substantially the same fibrillation conditions. Treated (e.g., fibrillated) binders can be detected by the above-mentioned techniques. Successful binder treatment (e.g., fibrillation) is generally reflected by the quality of the resulting product (e.g., electrode film). In some cases, electrode compositions prepared with binders that are not capable of fibrillation will include "undeformed" (spherical, round, spherical, etc.) binders. Even in this case, the multifunctional CB can be used as a binder and mechanical reinforcement for the electrode while also imparting desired electrical properties.

[0155] The electrode composition can be used to form an anode, a cathode, or both an anode and a cathode, for example, for assembly in a device such as a LIB. One, more or all of the properties that characterize the multifunctional CB can be evaluated in a product electrode composition (wherein the binder has been treated, such as fibrillated), a product electrode (such as a film), typically obtained by further processing the product electrode composition, an assembled electrode (wherein the product electrode, such as a film, has been applied to a suitable substrate), and / or a battery as described herein. For example, the electrode can be tested for adhesion (assessing the attachment of the electrode film to the substrate), cohesion (assessing the degree to which the particles are bonded together), electrode resistivity, and / or other properties by techniques known in the art.

[0156] Based on the total weight of the electrode composition, the multifunctional CB can be provided in an amount ranging from about 0.1 to about 10 wt %, such as about 0.3 to about 5.0 wt %, such as about 0.3 to about 3 wt %. Therefore, in one implementation, the multifunctional CB is present in the composition in an amount of about 0.3 to about 0.5, about 1.0, about 1.5, about 2.0, about 2.5; or about 0.5 to about 1.0, about 1.5, about 2.0, about 2.5, about 3; or about 1.0 to about 1.5, about 2.0, about 2.5, about 3.0; or about 1.5 to about 2.0, about 2.5, about 3.0; or about 2.0 to about 2.5, about 3.0; or about 2.5 to about 3.0. Some implementations utilize CB in an amount greater than about 3 wt %, for example, between 3% and 5% by weight of the product electrode composition, such as between 3 and less: 3.5, 4, or 4.5 wt %; between 3.5 and less: 4, 4.5, or 5 wt %; between 4 and less: 4.5 or 5 wt %; or between 4.5 and 5 wt %. Specific amounts within and outside of these ranges may be selected.

[0157] In many cases, this amount is equal to or preferably less than the amount of AC required to obtain the same or substantially the same electrode performance. In an alternative approach, achieving performance levels established with AC is expected to require smaller amounts of multifunctional CB, freeing up additional volume for the electroactive material.

[0158] For illustrative LIB graphite anode compositions, the loading of the multifunctional CB is no greater than about 5 wt%, typically no greater than about 3 wt%, such as no greater than 1 wt%. In specific examples, the loading of the multifunctional CB is in the range of about 0.1 wt% to about 1.0 wt%, such as in the range of about 0.1 to about 0.5, or about 0.5 to about 1 wt%. Other examples employ higher loadings, such as in the range of about 1 to about 5 wt%, such as at least about 4.5, 4.0, 3.5, 3.0, 2.5, 2.0, or 1.5.

[0159] For illustrative NCM cathode compositions, the loading of the multifunctional CB is no greater than about 5 wt %, typically no greater than about 3 wt %, such as no greater than 1 wt %. In a specific example, the loading of the multifunctional CB is in the range of about 0.1 wt % to about 1.0 wt %, such as in the range of about 0.1 to about 0.5, or about 0.5 to about 1 wt %. Other examples employ higher loadings, such as in the range of about 1 to about 5 wt %, such as at least about 4.5, 4.0, 3.5, 3.0, 2.5, 2.0, or 1.5.

[0160] It has been discovered that, at least in some cases, a multifunctional CB that performs well when added to an anode composition will have properties that differ from the properties exhibited by a multifunctional CB found to perform well in a cathode composition.

[0161] Thus, in some embodiments, graphite anodes are prepared using CBs having relatively clean surfaces (eg, obtained by heat treatment), relatively low surface area and structure, and underdeveloped meso- and macro-porosity.

[0162] In other embodiments, NCM cathodes are prepared using CBs with relatively high surface area and structure, developed meso- and macro-porosity (eg, obtained by vapor etching).

[0163] The relative amount of CB multifunctional additive to the binder capable of fibrillation can be in a ratio of 5:1 to 0.1:10, such as about 1:1 to 0.1:10, 0.5:1 to 0.1:10; 5:1 to 0.5:10, 5:1 to 1:5; 5:1 to 5:10, by weight. In a specific case, the weight ratio of CB multifunctional additive to the binder capable of fibrillation is 1:1.

[0164] In one embodiment, the electrode composition contains an active material in an amount of about 90 wt % to about 99 wt %, e.g., to 98.0 wt %, a fibrillating binder in an amount of about 1 wt % to about 5 wt %, and a CB multifunctional additive in an amount of about 0.3 wt % to about 5 wt %.

[0165] In many cases, the solvent-free processes described herein are carried out in the absence of any fibrillating aids other than the CB multifunctional additive. In other cases, the multifunctional CB may be combined with additional, for example, conventional fibrillating agents such as AC.

[0166] As used herein, the term "fibrillating aid" or "fibrillating agent" refers to a material other than a binder or active electrode material and that promotes fibrillation of a binder capable of fibrillation. "Additional" or "other" fibrillating aids or "additional" or "other" fibrillating agents refer to materials other than (i.e., excluding or not being) the multifunctional CB described above.

[0167] Further implementations utilize a multifunctional CB in combination with a substantially non-fibrillating conductivity additive (e.g., a conventional CCA). As used herein, the term "additional conductivity additive" refers to a material other than (i.e., excluding or not being a multifunctional CB as described above). Typically, the additional conductivity additive lacks or substantially lacks fibrillating functionality.

[0168] Plasticizers and / or other materials conventionally used in electrode compositions may also be included.

[0169] Some illustrative examples employ multifunctional CB and additional (additional) materials, such as conventional fibrillating agents such as AC, hard carbon, graphite, graphene, other non-fibrillating conductive additives, plasticizers, or combinations thereof. In some applications, multifunctional CB is combined with AC in a ratio ranging from about 95:5 to about 50:50.

[0170] Other examples utilize carbon-based additives containing at least two carbon blacks having one or more properties that differ from each other, for example, in terms of their BET. Also possible are blends of carbon blacks having structures-OAN that differ from each other and / or blends of different carbon forms, i.e., blends of activated carbon or graphite with one or more CBs. At least one component in the blend is a multifunctional CB.

[0171] As already indicated, many aspects of the invention relate to methods for producing electrode compositions, electrode products (eg, membranes), electrodes (wherein an electrode product such as a membrane has been applied to a conductive substrate), and / or batteries.

[0172] Turning first to the dry process for preparing the above-mentioned electrode composition, the goal of the process is at least two goals: blending some and typically all of the ingredients, which in most cases are provided in the form of loose (e.g., flowable or pourable) particles; and processing the binder in the presence of the multifunctional CB. In some embodiments, each of these two goals is met by one or more mixing operations performed under specific shear conditions using suitable equipment.

[0173] For example, low shear mixing can be selected to distribute the ingredients as evenly as possible, such as using a roll mill. As used herein, the term "low shear mixing" refers to mixing performed under conditions that are insufficient or substantially insufficient to fibrillate the fibrillating binder. Relying on low shear mixing conditions can also avoid excessive particle fragmentation, which is often a consideration for some electroactive materials.

[0174] In many embodiments, treating the adhesive in the presence of the multifunctional CB is carried out under high shear mixing. As used herein, the term "high shear mixing" refers to shear conditions that are sufficiently severe to deform (e.g., elongate, entangle) the adhesive to a degree sufficient to prepare a membrane electrode by a solvent-free technique. In the case of an adhesive capable of fibrillation, high shear mixing refers to mixing under shear conditions sufficient to fibrillate the adhesive.

[0175] Do not wish to be bound by a specific explanation, it is believed that in the presence of multifunctional CB additives and under high shear conditions, adhesive polymers are deformed, become stretched, elongated and entangled. Surface energy and / or surface roughness attributes for characterizing CB can promote the gripping (grabbing hold) of adhesive polymers, and both (CB and polymer) can become flattened between electroactive particles, causing adhesive polymers to be stretched. In the case where CB particles are dispersed in adhesives or on adhesive surfaces, it is believed that CB particles can keep adjacent polymer domains together. Other factors that work include polymer-polymer interactions (expected increase of elongation of polymers and / or increase with multidirectional shear force), electroactive particles-polymer adhesive interactions (it can be related to surface energy) and / or other factors.

[0176] Under the same or substantially the same high shear conditions, when the adhesive used is an adhesive capable of fibrillation, these performances tend to become more obvious. Surface and other CB properties promote the obstruction (snagging) of polymers everywhere. As all particles move under high shear mixing, polymers become elongated, forming very long, very thin strands (with high aspect ratio). Typically, using adhesives that cannot be fibrillated and processed under the same or substantially the same high shear conditions, these effects will not be too obvious. Or, in other words, adhesives that cannot be fibrillated may need increased high shear conditions to obtain results close to complete fibrillation.

[0177] In addition to the above processing contributions, the multifunctional CB can enhance electrical conductivity and, in many cases, can serve as a mechanical reinforcement by holding together fibrillating and non-fibrillating polymer binders, which are fully or to a lesser extent "deformed" (elongated, entangled, etc.) or "undeformed" (globular, rounded, spherical, etc.).

[0178] In some cases, high shear mixing can also be relied upon to break the particles into smaller fragments. For example, larger particles or particulates of CB (e.g., CB pellets) can be crushed into smaller particles that become evenly distributed throughout the electrode composition, thereby enhancing electrical conductivity and / or mechanical properties.

[0179] The specific shear value may depend on the scale of the operation, the materials involved, the type of mixing equipment, and / or other factors. The low or high mixing setting may be determined or optimized based on prior experience, routine experimentation, and the like.

[0180] The ingredients may be combined in any order designed to obtain a mixture, preferably a well-dispersed mixture, eg, having an even distribution of the ingredients, in other words, a homogeneous mixture. In one example, the CB is homogeneously dispersed on the surface of the binder and the electroactive material.

[0181] Binder treatment (eg, fibrillation) can be performed on any mixture or premix (preblend) that brings together the multifunctional CB additive and the binder.

[0182] Suitable techniques that may be used or adapted for carrying out the mixing and / or binder treatment steps (e.g. fibrillation) include mechanical agitation, shaking, stirring, and the like, and may rely on equipment such as jet mills, tube mills, acoustic mixers, extruders, planetary mixers, other mixing equipment, e.g., laboratory scale mixers, equipment suitable for pilot scale evaluation, equipment suitable for full scale industrial manufacturing, and the like.

[0183] A stepwise sequence may employ one type of equipment for a first operation (eg, making a pre-blend) and another type of equipment for a subsequent operation (eg, fibrillation). The same is true for shear and / or other mixing parameters.

[0184] In one embodiment, the CB multifunctional additive is first combined with the adhesive using a high shear device to treat (e.g., fibrillate) the adhesive. In some cases, this high shear operation also breaks the CB particles (granulated particles or other particles that are easily crushed under high shear conditions) into smaller fragments. The resulting mixture is then combined with an electroactive material (graphite in one example); using low shear conditions during this step is beneficial to maintain the particle size (e.g., of the electroactive material).

[0185] In another embodiment, the multifunctional CB is first combined with the electroactive material in a pre-blending step performed under low shear, for example, to obtain a uniform distribution of the two components. The binder is then added to the pre-blend and processed using high shear conditions, such as fibrillation.

[0186] In further embodiments, the electrochemically active material, binder, and multifunctional CB are all mixed (eg, under low shear conditions); and the mixture is then subjected to high shear conditions to process (eg, fibrillate) the binder.

[0187] Other sequences are possible. For example, the electroactive material may be mixed with the binder first, then the multifunctional CB additive may be added first, and then the binder may be treated (eg, fibrillated) under high shear conditions.

[0188] Low shear mixing and / or high shear treatment (e.g., fibrillation) can be carried out in one or more (two, three, four, five, six, etc.) stages or pulses, which can last for a suitable time period, e.g., in the range of about 10 seconds to about 5 minutes, e.g., in the range of about 30 seconds to about 1 minute, to about 90 seconds, to about 2 minutes, to about 2.5 minutes, to about 3 minutes, to about 4 minutes, to about 5 minutes; about 1 minute to about 90 seconds, to about 2 minutes, to about 3 minutes, to about 4 minutes, to about 5 minutes; about 90 seconds to about 3 minutes, to about 4 minutes, to about 5 minutes; about 2 minutes to about 3 minutes, to about 4 minutes, to about 5 minutes; about 3 minutes to about 4 minutes, to about 5 minutes; about 4 minutes to about 5 minutes. Different time intervals can also be used. The duration of two, more or all pulses can be the same or different.

[0189] The pulse may be followed by a rest period or cooling period. The rest period may be at ambient temperature, such as room temperature. Cooling may be to a temperature below ambient temperature, such as below room temperature, typically at 0°C or lower, such as at a temperature in the range of about -5°C to about 5°C.

[0190] The rest or cooling time may depend on the temperature reached during mixing, the amount processed, etc. In many cases, cooling will last for several minutes, such as 10 minutes to half an hour or more. The cooling time may vary in duration and / or temperature conditions.

[0191] To illustrate, the adhesive-containing composition can be subjected to high shear mixing at about 25,000 rpm to about 10,000 rpm, optionally at about 18,000 rpm, for half a minute, and then cooled to a temperature at or below freezing for 10 minutes, such as at about -10° C. Low shear mixing can be performed at about 2,000 rpm to about 4,000 rpm for 1 minute, and then cooled at about 0° C. for 10 minutes.

[0192] In one example, a pre-blend of the CB multifunctional additive and the electroactive material is prepared using an acoustic mixer, for example, at a force of 100 G for several minutes. The resulting blend is combined with a binder under fibrillation parameters, for example, using a laboratory-scale jet mill at a pressure rate of 100-90-90-10 psi.

[0193] In another example, all components are mixed in a tube mill (eg, IKA TubeMill 100) at 25,000 rpm in a pulsed manner, with blending alternating with rest periods followed by longer duration mixing operations.

[0194] Mixing and / or processing (e.g. fibrillation) steps can be monitored by visual inspection, manual calendering, powder rheology or other suitable techniques. For example, a small amount can be manually processed and sheared or passed through a manual calender. End points can be established based on experience, routine experiments, visual inspection, etc. Whether these operations are successful can also be determined by SEM, performance and / or other techniques usually performed on electrode products (e.g. electrode membranes).

[0195] The resulting electrode composition (containing at least active electrode material, multifunctional CB and deformed, eg, fibrillated, binder) may be in the form of pellets, powder (usually fluffy powder), or other forms of free-flowing or loose particulate material.

[0196] In an optional step, the electrode composition may be screened to remove unwanted agglomerates.

[0197] After mixing and processing (e.g., fibrillation), the optionally screened composition can be formed into a product electrode by any suitable technique known in the art or developed in the future. In one implementation, the composition is formed into a film by calendering, which is an operation that can be performed at room temperature or above room temperature, such as at a temperature similar to or close to the glass transition temperature of the polymer. In a typical calendering operation, the electrode composition is heated and pressurized using an extruder. The softened material is passed through calendering rollers (e.g., vertical) to prepare a product electrode sheet or film. In many embodiments, the film is self-supporting, a property that can be described by a 150 μm thick film, any part of which stands on its own without contacting any type of carrier (e.g., substrate).

[0198] By adjusting the gap between the rollers, and in some cases other process parameters, the desired film thickness can be achieved.

[0199] The roller temperature can be, for example, about room temperature (20°C) to about 200°C. A high roller temperature can produce a thinner self-supporting film at the first pass, while the opposite occurs at a lower temperature. The roller speed can vary. In an illustrative example, the roller speed is set to about 0.17 meters per minute (m / min) to about 1.3 m / min. Slower roller speeds tend to produce thinner self-supporting films at the first pass than faster roller speeds. The hydraulic pressure employed can be in the range of about 1,000 psi to about 7,000 psi. Similarly, higher pressures can produce thinner self-supporting films at the first pass than thicker films obtained at lower pressures.

[0200] Additional passes may be made using a roller mill to reduce the film thickness until the desired thickness and loading is achieved. In a specific implementation, the film thickness is in the range of about 40 μm to about 300 μm, for example, about 50 to about 200 μm, about 100 μm to about 150 μm. It is also possible that the film thickness is in the range of 50 to 100, 50 to 150, 50 to 200, 50 to 250; or 100 to 150, 100 to 200, 100 to 250, 100 to 300; or 150 to 200, 150 to 250, 150 to 300; or 200 to 250, 200 to 300; or 250 to 300 μm. The desired loading may be about 10 mg / cm 2 To about 50mg / cm 2 .

[0201] Self-supporting films prepared using multifunctional CB in a solvent-free process are expected to have good mechanical properties. One mechanical evaluation technique that can be relied upon involves tensile strength testing. For example, graphite anodes are expected to have a tensile strength of at least 100 kPa, while NCM cathode films are expected to have a tensile strength of at least 500 kPa. In an illustrative example, the self-supporting film has a tensile strength of at least 0.1 MPa and a thickness in the range of 80 μm to 500 μm. In many cases, the mechanical properties of the film are at least as good as those of a comparative film made using AC.

[0202] In an optional operation, the film is thermally activated, for example to soften the binder and prepare the electrode product for application to a substrate. In the laboratory, this operation can be performed using, for example, a hot plate at 100 degrees Celsius (° C.). Methods for larger scale processes include temperature controlled roll-to-roll calenders, convection and / or microwave dryers, and the like.

[0203] The membrane (usually self-supporting and containing active electrode material, multifunctional CB and treated, e.g., fibrillated binder) can be applied to a conductive substrate or support (e.g., aluminum or copper current collector). In one embodiment, the membrane is laminated to a carbon-coated copper foil by calendering the two together using, e.g., horizontal hot rollers at appropriate roller temperatures, roller speeds, and hydraulic pressure.

[0204] The roller temperature may range from about 80° C. to about 100° C. Too high a temperature may increase bubble formation and poor adhesion, while too low a temperature may hinder adhesion.

[0205] The roller speed may be about 0.17 m / min to about 1.3 m / min, such as about 0.5 m / min, and the hydraulic pressure may be set to about 500 psi to about 2,000 psi. Other settings may be used. The pressure may be optimized to be high enough to promote adhesion to the substrate without changing the loading, porosity or other properties. In some implementations, lamination is performed before setting the final thickness and / or porosity of the membrane electrode.

[0206] In some cases, the formation of the film and its application to the substrate can be performed in a single step. For example, the powder electrode composition and the substrate foil can be fed together through calendaring rolls under conditions suitable for producing a laminate, where the composition is pressed to form a film of a certain thickness and adhered to the foil. In this method, the formation of a self-supporting film is avoided.

[0207] The shape and / or size of the stacked structure may be designed for a specific application, such as an electrochemical cell, such as a LIB, such as a rechargeable LIB, etc.

[0208] The electrodes prepared as described herein can be incorporated into lithium ion batteries according to methods known in the art, such as those described in Yuping Wu, "Lithium Ion Batteries Fundamentals and Applications", CRC press, (2015). In a specific implementation, the battery is a button-type battery, such as a 2032 button cell battery, a 18650 cylindrical cell battery, a pouch cell, etc.

[0209] In an illustrative example, the LIB includes an anode prepared by a dry process. The anode contains, for example, a multifunctional CB in an amount of not more than 5 wt%, a graphite (e.g., natural graphite, artificial graphite, or a blend of the two, a commercially available type of graphite such as MCMB, MCF, VGCF, MAG, etc.) active anode material and a fibrillating binder. As described above, the graphite active material and the fibrillating binder may be present in the anode in an amount of at least 80 wt% and not more than 5 wt%, respectively.

[0210] The second (counter) electrode in the cell can also be prepared using a solvent-free process. In one implementation, both electrodes in the cell comprise a multifunctional CB as described above.

[0211] The second electrode may also be prepared by conventional dry processes (eg using AC), by slurry, or by another non-dry technique.

[0212] In addition to the two electrodes, a typical LIB includes a suitable electrolyte. Examples include, for example, ethylene carbonate-dimethyl carbonate-ethyl methyl carbonate (EC-DMC-EMC), vinylene carbonate (VC), LiPF6; ethylene carbonate-diethyl carbonate (EC-DEC, LiPF6; or (EC-DMC), LiPF6. In addition, the electrolyte composition may contain SiO x Or special additives for the performance of silicon-containing anodes, such as fluorinated carbonates, such as fluoroethylene carbonate, etc. In the laboratory, the separator that absorbs the electrolyte and prevents electrical contact between the electrodes while allowing Li ion diffusion can be a suitable glass fiber microfilter (e.g., Whatman GF / A). In some cases, membrane separators made of polypropylene / polyethylene (e.g., Celgard 2300) can also be used.

[0213] The composition or morphology of the electrodes and / or batteries described herein can be characterized by various techniques. Examples include, but are not limited to, electron microscopy, such as TEM, SEM, X-ray tomography, Raman spectroscopy, and other suitable qualitative or quantitative analysis methods. In one example, SEM data of a graphite electrode prepared by a dry process using a multifunctional additive described herein revealed the presence of ribbon-like binder fibrils, indicating effective fibrillation.

[0214] The amount of solvent or its absence can be evaluated by weight testing. This involves drying of the wet cast electrode until the electrode weight reaches a value theoretically calculated based on the known solid loading of the slurry, or until the electrode weight stabilizes and does not change for a minimum of 3 minutes. In the case of preparing the electrode in the absence of solvent at all, the weight remains the same during the evaluation. Or, in other words, the weight of the electrode just prepared (before any drying operation) is the same as the theoretical weight (i.e., the weight obtained by adding the weights of the individual components provided in the method) or deviates by no more than 1 weight %.

[0215] Another method that can be used to detect solvents (e.g., NMP) relies on attenuated total reflectance-Fourier transform infrared (ATR-FTIR) spectroscopy (FTIR-ATR) combined with gas chromatography (GC). In many cases, dry electrode films can be distinguished from slurry-based products by very low or undetectable levels of solvent residues. Substantially uniform binder distribution, without binder migration to the film surface, is another feature commonly used to characterize electrode products prepared by solvent-free processes.

[0216] The flexibility property used to characterize the electrode (its resistance to cracking) can be measured by visual inspection when bending the film by hand or using a mandrel bend tester. In a specific implementation, the electrode is evaluated and expected to pass a 10 mm diameter mandrel rod test without visible cracking. In an example, the electrode was found to pass a bend test using an 8 mm diameter pen as the rod.

[0217] Electrode performance can be tested by procedures known in the art or by adapting or developing techniques. Suitable techniques include, for example, in-plane and through-plane electrode conductivity, electrochemical impedance spectroscopy (EIS), constant current charge-discharge, hybrid pulse power capability (HPPC), cycling.

[0218] In many cases, electrodes prepared by solvent-free processes using multifunctional CBs perform at least as well and often better (e.g., as measured by in-plane resistivity, initial capacity, or first cycle efficiency) than comparative (also referred to herein as "reference") electrodes containing the same amount of active electrode material (e.g., graphite), binder, and conventional fibrillating agent such as AC. Alternatively, the amount of multifunctional additive required to achieve the performance obtained with AC is typically lower for electrodes made according to the embodiments described herein.

[0219] In one example, a dry-process graphite anode prepared using a loading of no more than about 1 wt % of the multifunctional CB exhibits performance (measured by in-plane resistivity, rate capability, first cycle efficiency) at least as good as a comparative electrode containing a higher amount (e.g., 5 wt %) of AC.

[0220] Electrodes prepared using multifunctional CB in a solvent-free process are also expected to have good mechanical properties. Mechanical evaluation techniques that can be relied upon include peel tests (e.g., 90°, 180°, T-peel, various clamps), tensile tests, and bending tests (mandrel experiments), etc. In many cases, the performance of electrodes prepared with multifunctional CB is at least as good as that of comparative electrodes made using AC.

[0221] Without wishing to be bound by a particular explanation, it is believed that the use of multifunctional CBs as described herein can produce ribbon-like binder strands or fibrils that can be long enough to wrap around particles of electroactive material and hold them together.

[0222] Thus, even at relatively low levels, the multifunctional CB appears to be able to process (e.g., fibrillate) the binder, creating an effective conductive network in the electrode while also contributing to the desired mechanical properties.

[0223] The compositions and methods described herein can also be used in (e.g., incorporated into) and / or adapted to manufacture other energy storage devices, such as primary alkaline batteries, primary lithium batteries, nickel metal hydride batteries, sodium batteries, lithium sulfur batteries, lithium air batteries, and supercapacitors. Methods for manufacturing such devices are known in the art and are described, for example, in TR Crompton's "Battery Reference Book", Newness (2000).

[0224] The principles described herein may also be implemented or adapted for semi-dry processes. Such methods typically include one step as a wet (or slurry) step. The other steps are performed without adding a liquid (e.g., a solvent).

[0225] An example of a semi-dry process involves a situation where two or more electrode components (e.g., electroactive material and multifunctional CB) can be first mixed together in the presence of a liquid (e.g., solvent), and then subjected to a drying step to remove the solvent. The remaining operations can then be performed without adding a liquid (e.g., solvent). For example, a dried pre-blend (containing an electroactive material and CB) can be combined with a binder, and the binder can be processed (e.g., fibrillated) in the absence of a liquid such as a solvent.

[0226] The present invention is further illustrated by the following non-limiting examples.

[0227] Example

[0228] Materials and methods

[0229] Materials used for the solvent-free electrode process and formulations include graphite BTR 918-2A from Targray; lithium nickel manganese cobalt oxide NCM622 (SNCM03006) from Targray; and a surface area of ​​1500 cm 2 / g of standard activated carbon; conductive CB Ketjenblack EC-600J from Lion Co.; C-NERGY from Imerys TM SUPER C65 carbon black and acetylene black Li-435 from Denka. All other CB specifications are from Cabot Corporation. The fibrillating binder is polytetrafluoroethylene (PTFE). The physical properties of the carbon blacks used in the following examples can be found in Tables 1A and 1B above.

[0230] Typically, graphite electrodes are prepared in several stages. In the first step (S1), the electrode components are combined and mixed (e.g., by high shear mixing) under conditions suitable for fibrillating the binder. The second step (S2) involves passing the powder blend from S1 through a vertical calender preset to an appropriate gap based on the desired film thickness. In the third step (S3), the self-supporting film obtained by S2 is laminated to the collector.

[0231] A cathode electrode was prepared following a similar sequence of steps.

[0232] The thickness of the solvent-free electrode was measured using a manual drop gauge with a 7.14 mm diameter flat gauging contact head.

[0233] The strength and Young's (elastic) modulus of the dry films were measured using a Mecmesin MultiTest-dV motorized force tester with a load of 10N.

[0234] The sheet resistance of the solvent-free electrode was measured using a Signatone Pro4-4400 commercial system (SP4 probe head connected to the back of a Keithley 2410-C source meter). The reported values ​​were normalized by the electrode thickness and reported as electrode resistivity in Ω·cm.

[0235] Example 1

[0236] In this example, a self-supporting graphite anode film was prepared in 2 steps (S1 and S2) using a jet mill as a high shear mixing device in S1, and then laminated on a current collector to form an electrode (S3).

[0237] In S1, the electrode components were pre-blended using a Resodyn acoustic mixer (S1-1) and then mixed using a 4-inch jet mill (S1-2). In more detail, the pre-blending step S1-1 was performed to prepare a uniform distribution of the powder components in the blend, and included a 5-minute pre-blending of the carbon additive and the electrode active material (graphite) in an acoustic mixer at 100% intensity and automatic frequency, followed by the addition of the polymer and blending for another 1 minute at the same settings. The next mixing step S1-2 involved fibrillating the binder and included passing the pre-blended material through a laboratory-scale jet mill at a pressure ratio of 100-90-90-10 psi.

[0238] In S2, the powder blend obtained in S1 was passed through a vertical calender at room temperature to obtain a self-supporting film having a thickness of 110-190 μm.

[0239] In S3, the self-supporting electrode film obtained in S2 was thermally activated on a hot plate set at 100°C and then laminated on a carbon-coated 9 μm thick copper foil (MTI Corporation) by calendering them together using a horizontal hot roll calender preheated to 80°C.

[0240] The compositions of the electrode formulations used (A1 and A2 used CB, while A3 used activated carbon and was used as a reference) are shown in Table A:

[0241] Table A

[0242] Formulation 1D Active Materials Carbon Additives Adhesives A1 90% Graphite 5% CB11 5%PTFE A2 90% Graphite 5% CB9 5%PTFE A3 90% Graphite 5% AC 5%PTFE

[0243] SEM images (low and high magnification) of cross sections of electrode membranes A1, A2 and A3 (90% graphite, 5% PTFE and 5% additives) as a reference and mapping of the fluorine element are presented in FIGS. 1A to 1I .

[0244] In the formulation with activated carbon (AC), the binder fibrils can be easily visualized, SEM pictures 1A and 1B. Fibrils are also easily observed in electrode A2 (see SEM pictures 1G and 1H). This suggests that certain CBs can be used alone as fibrillating additives, similar to the traditionally used AC, and can therefore replace AC in the formulation.

[0245] Some fibrils can also be visualized in SEM images 1D and 1E of electrode A1, but to a lesser extent than in the case of A2. This supports the idea that surface chemistry has an important influence and that PTFE is more likely to interact with the cleaner surface of the heat treated material.

[0246] Figures 1C, 1F and 1I present plots of elemental fluorine, confirming a homogeneous distribution on the electrode. No migration phenomena were detected (which is very common in the case of slurry prepared electrodes).

[0247] Example 2

[0248] The electrical properties of the products of compositions A1 to A3 in Table A were further tested. The electrode membrane was prepared as in Example 1 except that in addition to the combination of acoustic mixer and jet mill in (S1), the blend was further processed using an IKA tube mill 100 at 25,000 rpm for 15 seconds.

[0249] Although the fibrillation capabilities of AC and carbon particle CB9 are similar, as shown in Example 1, CB9 provides the additional benefit of lower electrode resistivity when tested at the same loading. Figure 2As shown, the electrodes containing CB (i.e., A1 and A2) all show improved in-plane resistivity compared to the reference electrode containing AC (i.e., A3).

[0250] Furthermore, since the in-plane resistivity of A2 is nearly as low as that of A1, the improved fibrillation observed with A2 may lead to an overall preference for CB9 (the heat-treated form of CB11) in at least some dry-process applications.

[0251] Example 3

[0252] The graphite electrode in this example was prepared by the same method as in Example 1, except that the jet mill in (S1) was replaced with an IKA tube mill 100, wherein the electrode components were processed at 25,000 rpm, 6×15 sec blending pulses, with a rest period of 45 sec, followed by straight blending at 25,000 rpm for 2 min.

[0253] In S2, the powder blend obtained in S1 was passed through a vertical calender at room temperature to obtain a self-supporting film having a thickness of 120 to 135 μm.

[0254] The electrode formulations employed (labeled B1 to B7, with B8 used as a reference) are listed in Table B below.

[0255] Table B

[0256] Formulation 1D Active Materials Carbon Additives Adhesives B1 90% Graphite 5% CB1 5%PTFE B2 90% Graphite 5% CB3 5%PTFE B3 90% Graphite 5% CB4 5%PTFE B4 90% Graphite 5% CB9 5%PTFE B5 90% Graphite 5% CB11 5%PTFE B6 90% Graphite 5% CB14 5%PTFE B7 90% Graphite 5% CB15 5%PTFE B8 90% Graphite 5% AC 5%PTFE

[0257] Figure 3 The tensile strength of graphite films and the in-plane resistivity of graphite electrodes containing AC (see reference electrode composition B8 in Table B) were compared with electrodes formulated with various CBs, namely additives CB1, CB3, CB4, CB9, CB11, CB14, and CB15 (from Tables 1A and 1B). All electrodes were prepared by a dry process and contained 5 wt% loading of CB additive, graphite (90 wt%), and PTFE (5 wt%). Figure 3 As shown, electrodes prepared by a dry process using CBs believed to provide good binder fibrillating properties (see, for example, carbon blacks CB9, CB11, CB14, and CB15) also exhibit low in-plane resistivity, very comparable to or better than the values ​​observed with good CCA additives such as carbon black CB4 (from Table 1). In addition, electrodes produced using CBs believed to be good fibrillating agents (e.g., carbon blacks CB1, CB3, CB4, CB9, CB11, CB14, and CB15 in Table 1) exhibit lower in-plane resistivity than electrodes observed with AC.

[0258] In one example, a self-supporting graphite film containing CB3 showed modest improvements in tensile strength and in-plane resistivity compared to data observed with CB4 (not heat treated). This supports the idea that chemistry has an important effect and that PTFE is more likely to interact with the cleaner surface of the heat treated material CB3.

[0259] In another example, a self-supporting graphite film containing CB15 (steam etched) showed significant improvements in tensile strength and in-plane resistivity compared to those observed with CB4 (not steam etched). This supports the idea that chemistry and morphology have important effects, and that PTFE is more likely to be fibrillated and more evenly distributed in electrodes with CB15, which has a cleaner surface, higher surface area, higher structure, and forms meso- and macro-porosity of the steam-etched material.

[0260] Furthermore, since relatively low surface area CBs (e.g., carbon blacks CB1 and CB3) may result in less solid electrolyte interface (SEI) formation (the growth of SEI is considered an important factor in LIB capacity fade) compared to relatively high surface area CBs (e.g., carbon blacks CB9, CB11, CB14, CB15), the expected improved cell performance with lower surface area CB particles may lead to an overall preference for this type of performance additive, at least in some dry process applications.

[0261] Example 4

[0262] In this example, a self-supporting NCM622 cathode film was prepared in 2 steps (S1 and S2), where an IKA tube mill 100 was used as a high shear mixing device in S1, and then laminated on a current collector to make an electrode (S3).

[0263] In S1, the electrode components are pre-blended using a Resodyn acoustic mixer (S1-1) and then mixed using an IKA tube mill 100 (S1-2). In more detail, the pre-blending step S1-1 is performed to prepare a uniform distribution of the powder components in the blend, and includes pre-blending the carbon additive and the electrode active material (NCM622) in an acoustic mixer at 100% intensity and automatic frequency for 5 minutes, followed by adding the polymer and blending for another 1 minute at the same settings. The next mixing step S1-2 involves fibrillating the binder and includes passing the pre-blended material through an IKA tube mill 100 at 25,000 rpm, 6×15 second blending pulses, standing for 45 seconds, and then directly blending at 5,000 rpm for 3 minutes.

[0264] In S2, the powder blend obtained in S1 was passed through a vertical calender at 100°C to obtain a self-supporting film with a thickness of 110-170 μm.

[0265] In S3, the self-supporting electrode films obtained in S2 were laminated on a carbon-coated aluminum foil current collector by calendering them together using a vertical hot roll calender preheated to 100°C.

[0266] The electrode formulations used (labeled C1 to C6 and D1 to D6) are listed in Tables C and D, respectively:

[0267] Table C

[0268] Formulation 1D Active Materials Carbon Additives Adhesives Self-supporting electrode membrane C1 90% NCM622 5% CB1 5%PTFE fail C2 90% NCM622 5% CB3 5%PTFE fail C3 90% NCM622 5% CB5 5%PTFE fail C4 90% NCM622 5% CB9 5%PTFE pass C5 90% NCM622 5% CB15 5%PTFE pass C6 90% NCM622 5% AC 5%PTFE fail

[0269] Table D

[0270] Formulation 1D Active Materials Carbon Additives Adhesives Self-supporting electrode membrane D1 94% NCM622 2% CB7 4%PTFE fail D2 94% NCM622 2% CB8 4%PTFE fail D3 94% NCM622 2% CB10 4%PTFE pass D4 94% NCM622 2% CB12 4%PTFE pass D5 94% NCM622 2% CB13 4%PTFE pass D6 94% NCM622 2% CB15 4%PTFE pass

[0271] Figure 4 The tensile strength and elastic modulus of a self-supporting NCM electrode film containing AC (see reference electrode composition C6 in Table C) were compared with electrodes formulated with various CBs, namely additives CB1, CB3, CB5, CB9 and CB15 (from Tables 1A and 1B). All electrodes were prepared by a dry process and contained 5 wt% loading of CB additive, NCM622 (90 wt%) and PTFE (5 wt%). Figure 4 As shown, the electrode films prepared by the dry process using CBs exhibited improved strength compared to the AC-containing reference. In some cases, the formulations containing certain CBs (i.e., CB1, CB3, and CB5) had relatively high elastic moduli (over 400 N / mm 2 ) and appeared to be hard and difficult to further process. In other cases, formulations containing certain forms of CB (i.e., CB9 and CB15) showed tensile strength (over 1000 kPa) and elastic modulus (less than 400 N / mm 2 ) and form a flexible, self-supporting cathode film that passes quality control and can be laminated on a current collector.

[0272] Figure 5 The tensile strength and elastic modulus of NCM electrode films (see electrode compositions in Table D) formulated with various CBs, namely CB7, CB8, CB10, CB12, CB13, and CB15 (from Tables 1A and 1B) were compared. All electrodes were prepared by a dry process and contained 2 wt% loading of CB additive, NCM622 (94 wt%), and PTFE (4 wt%). Figure 4According to the data reported for the formulation of 5 wt% CB, 90 wt% NCM622 and 5 wt% PTFE in , CBs with developed morphology (i.e., CB10, CB12, CB13 and CB15) are able to form flexible, self-supporting electrode membranes compared to membranes obtained with less developed morphology CBs (i.e., CB7 and CB8). The results suggest that relatively high BET, OAN and pore volume types of carbon additives, i.e., CB9, CB10, CB12, CB13 and CB15, are generally preferred for use as processing particles, at least in some dry process applications.

[0273] like Figure 6 As shown, compared with the reference containing AC (i.e., formulation C6), the electrode formulation with carbon black ( Figure 6 Formulation C4) in also showed lower electrode resistivity; lower resistivity is known to be beneficial to battery performance.

[0274] Example 5

[0275] The NCM cathode electrode in this example was prepared in 3 steps by forming a self-supporting dry film using a twin-screw extruder as a high shear mixing device (S1 and S2), which was then laminated on a current collector (S3).

[0276] In S1, a dry electrode powder blend is prepared according to a three-stage operation scheme. In more detail, in S1-1, the three electrode components (NCM622, PTFE and carbon) are first premixed in a drum in powder form for 30 minutes to obtain a more uniform distribution. In S1-2, the pre-blended powder is treated in a twin-screw extruder at a temperature of 100°C, a production volume of 3kg / h and a screw speed of 400rpm to disperse the carbon and fibrillated binder. Finally, the resulting electrode powder blend is in the shape of a flake. In S1-3, the flaky material obtained in S1-2 is post-treated in an IKA grinder at 5000rpm under low shear for 20 seconds to restore its powder form.

[0277] In S2, the powder electrode blend obtained in S1 was passed through a vertical calender at 100°C to obtain a self-supporting film. The final dry electrode film thickness was in the range of 110-120 μm.

[0278] In S3, the self-supporting electrode films obtained in S2 were laminated on a carbon-coated aluminum foil current collector by calendering them together using a vertical hot roll calender preheated to 100°C.

[0279] The electrode formulations employed (labeled E1 and E2) are listed in Table F below.

[0280] Table E

[0281] electrode Active Materials Carbon Additives Adhesives Self-supporting electrode membrane E1 97% NCM622 1% CB2 2%PTFE fail E2 97% NCM622 1% CB12 (fluffy form) 2%PTFE pass E3 97% NCM622 1% CB12 (pelletized form) 2%PTFE pass

[0282] The formulations (i.e., E1, E2, and E3) produced sheets of similar appearance in S1-2. Upon calendering (S2), only formulations E2 and E3 produced self-supporting cathode films. The tensile strength and elastic modulus of these films are shown in Figure 7 Formulation E1 was not able to produce a free-standing film; instead, it broke before reaching the target thickness of 110 μm. Thus, dry electrodes could not be made with Formulation E1. This may indicate that, at least in some dry process applications, it is generally preferred to use carbon additives (e.g., CB12) in fluffy or pelletized form as process particles.

[0283] Example 6

[0284] The graphite electrode in this embodiment is prepared by the same method as in Example 3, except that in step (S2), calendering is performed in two steps at different temperatures. In one case, in order to manufacture a self-supporting film for tensile test testing, the powder blend obtained in S1 is first passed through a vertical calender at room temperature, and then a second time through a calender preheated to 80°C to obtain a self-supporting film with a thickness of 250-280 μm. In another case, in order to prepare a dry electrode for peel strength (adhesion) testing, the powder blend obtained in S1 is passed through a vertical calender preheated to 100°C as a first step, and then at 80°C as a second step, and then the dry film is laminated on the collector by passing them together through a vertical calender preheated to 80°C.

[0285] The electrode formulations employed (labeled F1 to F4) are listed in Table F below.

[0286] Table F

[0287] Formulation 1D Active Materials Carbon Additives Adhesives Tensile Strength Peel strength F1 90% Graphite 5% Carbon 5%PTFE 237kPa 0.035N F2 90% Graphite 5% Carbon 3.75% PTFE, 1.25% PVDF 187kPa Unavailable F3 90% Graphite 5% Carbon 2.5% PTFE, 2.5% PVDF 107kPa 0.089N F4 90% Graphite 5% Carbon 5% PVDF fail fail

[0288] All electrodes are prepared by dry process, and contain carbon additives, graphite (90 weight %) and binder (5 weight %) with a loading of 5 weight %. As shown in Table F, the self-supporting electrode film prepared by the dry process of the binder (see, for example, PTFE) that is expected to be easily stretched and form fibrils also shows a higher tensile strength than the binder that cannot be fibrillated, that is, PVDF partially replaces the PTFE binder that can be fibrillated (see, for example, PTFE / PVDF in formulations F2 and F3, with a ratio of 75:25 and 50:50, respectively). In addition, the formulation containing only the binder that cannot be fibrillated (see, for example, PVDF) does not produce a self-supporting film and fails when the first calender passes. On the other hand, partially replacing PTFE with PVDF in the formulation improves the adhesion of the self-supporting film to the collector (see formulations F3 and F1 in Table F for comparison). This supports the idea that while the presence of a fibrillating binder enables the formation of dry electrodes, a non-fibrillating binder can be used to enhance other electrode properties, such as adhesion of the electrode to the collector, first cycle irreversibility driven by PTFE properties on the anode side of the cell, etc.

[0289] Example 6

[0290] NCM electrodes of two different formulations were prepared by dry and wet (slurry casting) processes and tested in 2032 half-coin cell cells.

[0291] A dry-process NCM cathode, namely G1, was prepared by the same method as in Example 4.

[0292] The wet NCM cathode, G2, was prepared using a two-step mixing process using a Thinky ARE310 planetary centrifugal mixer. The first step included 20 minutes of mixing of the carbon conductivity additive (CCA) / PVDF / NMP millbase with two small tungsten carbide (WC) media for grinding (12 minutes of active mixing). After the NCM622 powder was added to the millbase, the second step included mixing for another 20 minutes without the media (12 minutes of active mixing). Both NCM and CCA powders were pre-dried at 130°C for 20 minutes. The electrode slurry was coated on 15μm thick aluminum foil using an automatic knife coater (MSK-AFA-III model from MTI Corp.). The NMP was evaporated in a convection oven set to 80°C for 20 minutes and finally dried in a vacuum oven at ~100°C. The dry electrode loading on the Al foil was 24.4mg / cm 2 , calendered to a density of 3.4 g / cc using a hand roller press.

[0293] The electrode formulations used (labeled G1 and G2, G2 formulation was prepared by slurry (wet) process) and their properties are listed below in Table F. Electrode G2 employed electrode formulation and exhibited electrode properties as a standard for NCM cathodes in EV applications and, therefore, was used as a baseline.

[0294] Table G

[0295]

[0296] Cathodes G1 and G2 (from Table G) were tested in 2032 half coin cells. Discs with a 15 mm diameter were punched for coin cell preparation and dried at 100°C under vacuum for at least 4 hours. The discs were rolled to the desired density (as shown in Table G) using a manual roller press and assembled into 2032 coin cells in an argon-filled glove box (M-Braun) for testing on lithium foil. A glass fiber microfilter (Whatman GF / A) was used as a separator. The electrolyte was 100 microliters of ethylene carbonate-dimethyl carbonate-ethyl methyl carbonate (EC-DMC-EMC), vinylene carbonate (VC) 1%, LiPF61M (BASF).

[0297] The reported capacities are normalized in mAh / g active cathode mass. The room temperature (25°C) performance of half-coin cells was measured by first forming them using two C / 5-D / 5 charge-discharge cycles, then charging them at 1C rate and discharging them at C / 5, 1C, 2C, and 3C discharge rates. Results ( Figure 8 ) show that the dry process G1 formulation has better or comparable capacity at C-rates up to 1C (0.2C, 0.5C and 1.0C) compared to the slurry process baseline formulation G2.

[0298] Example 7

[0299] Two sets of cathodes were prepared by the same dry and wet (slurry casting) processes as in Example 6. The electrode formulations employed (labeled H1 to H4, where H3 and H4 were used as wet baselines for dry processes H1 and H2, respectively) and the properties of the resulting cathodes are listed in Table H below. All cathodes contained carbon additives at a loading of 1 wt%, NCM622 (96 wt%) and binder (3 wt%), were prepared with two different carbons (i.e., C12 and CB15), and were loaded at 3.9 ± 0.2 mg / cm 2 and 3.8±0.1mg / cm 2 Calendering.

[0300] Table H

[0301]

[0302] The cathodes, i.e. H1, H2, H3 and H4, were tested in 2032 complete coin cell cells. Circular discs with a diameter of 15 mm were punched for coin cell preparation and dried at 100°C under vacuum for at least 4 hours. The discs were rolled with a manual roller press at the desired electrode density and assembled into 2032 coin cell cells in an argon filled glove box (M-Braun) for testing graphite anodes containing 3% CB, 5% PVDF, 92% natural graphite. Celgard filter was used as a separator. The electrolyte was 200 microliters of ethylene carbonate-dimethyl carbonate-ethyl methyl carbonate (EC-DMC-EMC), vinylene carbonate (VC) 1%, LiPF6 1M (BASF).

[0303] Unit cells of each formulation were prepared and the initial C / 20 capacity and first cycle irreversible loss ( Fig. 9 and Fig.10 ). The cathode formulation contained CB12 (from Tables 1A and 1B) and the unit cell group manufactured by the dry process showed comparable discharge capacity and improved (lower) first cycle irreversibility loss compared to the wet cathode. The cathode formulation contained CB15 (from Tables 1A and 1B) and the unit cell group manufactured by the dry process showed discharge capacity and first cycle irreversibility, which were comparable to the wet cathode in both cases. In both cases, the performance of the dry cathode remained comparable or better relative to the wet counterpart, indicating that the dry process can replace the conventional slurry process without affecting the electrochemical performance of the cell.

[0304] Example 8

[0305] A dry NCM cathode containing 2 wt% CB (i.e., CB15 (from Tables 1A and 1B)), NCM622 (94 wt%), and PTFE (4 wt%) was prepared by the same method as in Example 4 and tested in a 2032 half coin cell as described in Example 6. 2 Active material loading and 5.6 mAh / cm 2 A dry cathode was made with a capacity of 1.5 g / cc and rolled at 3.6 g / cc.

[0306] The cycling performance of the half-coin cell was measured by charging it at +25°C using a 1C charge rate and discharging it at +25°C, using a C / 20 discharge rate for the first 5 cycles, then using a C / 10 discharge rate for the next 2 cycles and long term cycling at C / 5. The discharge capacity measured during cycling is close to the theoretical capacity of NCM622, as Fig.11 shown.

[0307] While the invention has been particularly shown and described with reference to preferred embodiments thereof, it will be understood by those skilled in the art that various changes in form and details may be made without departing from the scope of the invention as encompassed by the appended claims.

Claims

1. A method for preparing an electrode composition, the method comprising: combining active electrode materials, binders and multifunctional carbon black; as well as treating the adhesive in the presence of the carbon black, wherein: The method is carried out without the addition of solvent; and The multifunctional carbon black has a thickness of not greater than about 1600 m 2 / g BET and no more than about 650 ml / 100 g OAN.

2. The method of claim 1, wherein the active electrode material is graphite and the multifunctional carbon black has a carbon black content of about 35 to about 1600 m 2 / g range and OAN in the range of about 120 to about 650 ml / 100 g.

3. The method of claim 1, wherein the active electrode material is graphite and the multifunctional carbon black has a carbon black content of about 50 to about 200 m 2 / g range and OAN in the range of about 130 to about 240 ml / 100 g.

4. The method of claim 1, wherein the active electrode material is a lithium transition metal compound and the carbon black has a carbon black content of about 80 to about 1600 m 2 / g range and OAN in the range of about 120 to about 650 ml / 100 g.

5. The method of claim 1, wherein the active electrode material is a lithium transition metal compound and the carbon black has a carbon black content of about 500 to about 1600 m 2 / g range and OAN in the range of about 180 to about 650 ml / 100 g.

6. The method of claim 1, wherein the active electrode material is a lithium transition metal compound and the carbon black has a carbon black content of about 80 to about 200 m 2 / g range and OAN in the range of about 140 to about 280 ml / 100 g.

7. The method of claim 1, wherein the active electrode material is a lithium transition metal compound and the carbon black has a carbon black content of about 1350 to about 1600 m 2 / g range and OAN in the range of about 120 to about 220 ml / 100 g.

8. The method of claim 1, wherein the active electrode material is a lithium transition metal compound and the carbon black has a carbon black content of about 500 to about 650 m 2 / g range and OAN in the range of about 180 to about 260 ml / 100 g.

9. The method according to any one of the preceding claims, wherein the multifunctional carbon black has one or more of the following properties: about 15 mJ / m 2 or lower surface energy; at least about Raman crystallite plane size (La); at least about 0.35 cm 3 / g mesopore volume; at least 1.0cm 3 / g of the total volume of mesopores and macropores; and, a % crystallinity of at least 22%.

10. The method according to any one of the preceding claims, wherein the electrode active material, the binder, the multifunctional carbon black and the electrode composition are loose particulate materials.

11. The method of any one of the preceding claims, wherein the binder is fibrillable, non-fibrillable, or any combination thereof.

12. The method of claim 11, wherein the binder is PTFE, PVDF, or a combination thereof.

13. The method according to any one of the preceding claims, wherein the multifunctional carbon black is provided as a fluffy powder, pellets or granules.

14. The method of any one of the preceding claims, wherein treating the adhesive in the presence of the multifunctional carbon black comprises a high shear operation sufficient to fibrillate the fibrillable adhesive.

15. The method of claim 15, wherein the high shear operation deforms a non-fibrillable binder.

16. The method of any one of the preceding claims, wherein combining the active electrode material, the binder and the carbon black additive is performed under shear conditions that are lower than the shear conditions used to treat the binder in the presence of the carbon black additive.

17. The method according to any one of the preceding claims, wherein the method is carried out in the presence of the multifunctional carbon black as the only fibrillating aid.

18. The process according to any one of claims 1 to 16, wherein the process is carried out in the presence of the multifunctional carbon black and at least one other material selected from activated carbon, another multifunctional carbon black and a conductive carbon additive.

19. A method further comprising applying the electrode composition prepared according to any one of the preceding claims to a conductive substrate to form a battery electrode.

20. The method of any one of claims 1-18, further comprising processing the electrode composition to form a self-supporting film.

21. The method of claim 20, wherein the self-supporting film is prepared by calendering the electrode composition.

22. The method of claim 20, wherein the self-supporting film has a tensile strength of at least 0.1 MPa and a thickness in the range of about 80 to 500 μm.

23. A method for preparing an electrode composition, the method comprising: combining an active electrode material, a binder capable of fibrillation, and multifunctional carbon black; as well as The fibrillating adhesive is subjected to a fibrillating operation in the presence of the multifunctional carbon black, wherein: The method is carried out in the absence of a solvent, and The multifunctional carbon black has a thickness of not greater than about 1600 m 2 / g BET and no more than about 650 ml / 100 g OAN.

24. The method of claim 23, wherein the active electrode material is graphite and the multifunctional carbon black has a carbon black content of about 35 to about 1600 m 2 / g range and OAN in the range of about 120 to about 650 ml / 100 g.

25. The method of claim 23, wherein the active electrode material is graphite and the multifunctional carbon black has a carbon black content of about 50 to about 200 m 2 / g range and OAN in the range of about 130 to about 240 ml / 100 g.

26. The method of claim 23, wherein the active electrode material is a lithium transition metal compound and the carbon black has a carbon black content of about 80 to about 1600 m 2 / g range and OAN in the range of about 120 to about 650 ml / 100 g.

27. The method of claim 23, wherein the active electrode material is a lithium transition metal compound and the carbon black has a carbon black content of about 500 to about 1600 m 2 / g range and OAN in the range of about 180 to about 650 ml / 100 g.

28. The method of claim 23, wherein the active electrode material is a lithium transition metal compound and the carbon black has a carbon black content of about 80 to about 200 m 2 / g range and OAN in the range of about 140 to about 280 ml / 100 g.

29. The method of claim 23, wherein the active electrode material is a lithium transition metal compound and the carbon black has a carbon black content of about 1350 to about 1600 m 2 / g range and OAN in the range of about 120 to about 220 ml / 100 g.

30. The method of claim 23, wherein the active electrode material is a lithium transition metal compound and the carbon black has a carbon black content of about 500 to about 650 m 2 / g range and OAN in the range of about 180 to about 260 ml / 100 g.

31. The method of any one of claims 23-29, wherein the multifunctional carbon black has one or more of the following properties: about 15 mJ / m 2 or lower surface energy; at least about Raman crystallite plane size (La); at least about 0.35 cm 3 / g mesopore volume; at least 1.0cm 3 / g of the total volume of mesopores and macropores; and a % crystallinity of at least 22%.

32. The method according to any one of claims 23 to 30, wherein the method is carried out in the presence of the multifunctional carbon black as the only fibrillating aid.

33. The method according to any one of claims 23 to 30, wherein the method is carried out in the presence of the multifunctional carbon black and at least one other material selected from activated carbon, another multifunctional carbon black and a conductive carbon additive.

34. The method of any one of claims 23 to 32, further comprising a mixing operation conducted under shear conditions lower than the shear conditions employed in the fibrillating operation.

35. The method according to any one of claims 23-33, further comprising premixing the electrode active material and the multifunctional carbon black.

36. The method of any one of claims 23-33, wherein the active electrode material is added before, during or after the binder fibrillation operation.

37. The method of any one of claims 23-35, wherein the fibrillable binder is PTFE.

38. The method of any one of claims 23-36, wherein the electrode composition contains an active electrode material in an amount of about 90 wt % to about 98 wt %, a fibrillating binder in an amount of about 1 wt % to about 5 wt %, and a multifunctional carbon black in an amount of about 0.3 wt % to about 5 wt %.

39. according to the method described in any one of claims 23-37, wherein said multifunctional carbon black is heat-treated or steam-etched.

40. The method of any one of claims 23-38, wherein the multifunctional carbon black is provided as a fluffy powder, in a pelletized form, or as a granular material.

41. The method of any one of claims 23-39, wherein the electrode active material, the fibrillable binder, the multifunctional carbon black and the electrode composition are loose particulate materials.

42. A dry membrane electrode, comprising: an active electrode material, a treated binder and multifunctional carbon black, wherein: Prior to any drying operation, the membrane electrode contains a solvent residue in an amount of no greater than 1 wt % relative to the theoretical weight of the membrane electrode, wherein the multifunctional carbon black has a carbon content of no greater than about 1600 m 2 / g BET and no more than about 650 ml / 100 g OAN.

43. The dry process membrane of claim 41, wherein the active electrode material is graphite and the multifunctional carbon black has a carbon black content of about 35 to about 1600 m 2 / g range and OAN in the range of about 120 to about 650 ml / 100 g.

44. The dry process membrane of claim 41, wherein the active electrode material is graphite and the multifunctional carbon black has a carbon black content of about 50 to about 200 m 2 / g range and OAN in the range of about 130 to about 240 ml / 100 g.

45. The dry process membrane of claim 41, wherein the active electrode material is a lithium transition metal compound and the carbon black has a carbon black content of about 80 to about 1600 m 2 / g range and OAN in the range of about 120 to about 650 ml / 100 g.

46. ​​The dry process membrane of claim 41, wherein the active electrode material is a lithium transition metal compound and the carbon black has a carbon black content of about 500 to about 1600 m 2 / g range and OAN in the range of about 180 to about 650 ml / 100 g.

47. The dry process membrane according to claim 41, wherein the active electrode material is a lithium transition metal compound and the carbon black has a carbon black content of about 80 to about 200 m 2 / g range and OAN in the range of about 140 to about 280 ml / 100 g.

48. The dry process membrane of claim 41, wherein the active electrode material is a lithium transition metal compound and the carbon black has a carbon black content of about 1350 to about 1600 m 2 / g range and OAN in the range of about 120 to about 220 ml / 100 g.

49. The dry process membrane according to claim 41, wherein the active electrode material is a lithium transition metal compound and the carbon black has a carbon black content of about 500 to about 650 m 2 / g range and OAN in the range of about 180 to about 260 ml / 100 g.

50. The dry film according to any one of claims 41 to 48, wherein The multifunctional carbon black has one or more of the following properties: about 15 mJ / m 2 or lower surface energy; at least about Raman crystallite plane size (La); at least about 0.35 cm 3 / g mesopore volume; at least 1.0cm 3 / g of the total volume of mesopores and macropores; and, a % crystallinity of at least 22%.

51. The dry-process membrane electrode according to any one of claims 41 to 49, wherein the multifunctional carbon black is the only fibrillation aid in the membrane electrode.

52. The dry membrane electrode according to any one of claims 41 to 49, further comprising at least one additional material selected from activated carbon, another multifunctional carbon black and a conductive carbon additive.

53. A dry membrane electrode according to any one of claims 41 to 51, wherein the dry membrane electrode is self-supporting or laminated to a substrate.

54. A method for preparing an electrode composition, the method comprising: (a) subjecting the adhesive to high shear conditions in the presence of multifunctional carbon black to treat the adhesive; as well as (b) adding an electrode active material before, during or after step (a), wherein: The multifunctional carbon black has a thickness of not greater than about 1500 m 2 / g BET and no more than about 650 ml / 100 g OAN, and The process is carried out without the addition of solvent.

55. The method of claim 53, wherein the active electrode material is graphite and the multifunctional carbon black has a carbon black content of about 35 to about 1600 m 2 / g range and OAN in the range of about 120 to about 650 ml / 100 g.

56. The method of claim 53, wherein the active electrode material is graphite and the carbon black has a carbon black content of about 50 to about 200 m 2 / g range and OAN in the range of about 130 to about 240 ml / 100 g.

57. The method of claim 53, wherein the active electrode material is a lithium transition metal compound and the carbon black has a carbon black content of about 80 to about 1600 m 2 / g range and OAN in the range of about 120 to about 650 ml / 100 g.

58. The method of claim 53, wherein the active electrode material is a lithium transition metal compound and the carbon black has a carbon black content of about 500 to about 1600 m 2 / g range and OAN in the range of about 180 to about 650 ml / 100 g.

59. The method of claim 53, wherein the active electrode material is a lithium transition metal compound and the carbon black has a carbon black content of about 80 to about 200 m 2 / g range and OAN in the range of about 140 to about 280 ml / 100 g.

60. The method of claim 53, wherein the active electrode material is a lithium transition metal compound and the carbon black has a carbon black content of about 1350 to about 1600 m 2 / g range and OAN in the range of about 120 to about 220 ml / 100 g.

61. The method of claim 53, wherein the active electrode material is a lithium transition metal compound and the carbon black has a carbon black content of about 500 to about 650 m 2 / g range and OAN in the range of about 180 to about 260 ml / 100 g.

62. The method of any one of claims 53-60, wherein the multifunctional carbon black has one or more of the following properties: about 15 mJ / m 2 or lower surface energy; at least about Raman crystallite plane size (La); at least about 0.35 cm 3 / g mesopore volume; at least 1.0cm 3 / g of the total volume of mesopores and macropores; and, a % crystallinity of at least 22%.

63. The method according to any one of claims 53 to 61, wherein the method is carried out in the presence of the multifunctional carbon black as the sole fibrillation aid.

Citation Information

Cited By

  • Dry-method negative electrode, preparation method thereof and battery

    CN120497283A