Method for separating lithium, sodium and potassium from lithium selective membrane extraction material

CN118925506AActive Publication Date: 2024-11-12XI'AN UNIVERSITY OF ARCHITECTURE AND TECHNOLOGY
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202411007293.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-25
Publication Date
2024-11-12
Estimated Expiration
2044-07-25

AI Technical Summary

Technical Problem

The problems of slow lithium mass transfer rate in traditional lithium film extraction systems and the leakage of membrane-based materials in external electric field coupled membrane extraction technology lead to insufficient lithium extraction efficiency and stability.

Method used

The lithium selective extraction film was prepared by adding a specific proportion of polyvinyl chloride, 2-thiophene-formyl trifluoroacetone and a synergistic agent to the solvent, and the electrofilm was extracted under the external electric field, using the synergistic agent and Modifiers improve film stability and lithium transfer rate.

Benefits of technology

The extraction rate of lithium and the stability of the membrane are significantly improved, efficient and fast lithium extraction is achieved, and high circulation stability and selectivity of Li/Na and Li/K are maintained.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118925506A_ABST
    Figure CN118925506A_ABST
Patent Text Reader

Abstract

The invention discloses a method for separating lithium, sodium and potassium by using a lithium selective membrane extraction material, which comprises the following steps of: preparing a lithium selective extraction membrane without adding a modifying agent and preparing a modified lithium extraction membrane by adding a modifying agent: adding polyvinyl chloride, 2-thiophenoyl trifluoroacetone and a synergistic extraction agent into a solvent, stirring to a homogeneous phase, transferring to a flat-bottomed vessel, and carrying out vacuum drying to obtain the lithium sodium potassium separation membrane. And preparing the lithium selective extraction membrane by adopting a solvent evaporation method. A modifier is added when the modified lithium extraction membrane is prepared. A lithium selective extraction membrane or a modified lithium selective extraction membrane is loaded between two liquid pool devices, platinum electrodes connected with an external direct-current stabilized power supply are installed in the two liquid pools respectively, a lithium / sodium / potassium containing mixed solution is injected into the liquid pool on one side of a power supply anode, a desorption solution used for recycling lithium is injected into the liquid pool on one side of the power supply cathode, and the lithium / sodium / potassium containing mixed solution is recycled under the set voltage. And completing extraction when the lithium concentration in the solutions on the two sides does not change any more. According to the method disclosed by the invention, the extraction of lithium is improved, the problem of tolerance loss of the membrane in an electric membrane extraction system is solved, and the prepared membrane has relatively high lithium extraction rate and cycling stability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical fields of material chemistry, separation science, hydrometallurgy, etc., and relates to the preparation of a lithium selective membrane extraction material and its application in lithium extraction under the background of low-concentration liquid lithium resources. Background Art

[0002] With the rapid development of the new energy industry, the market demand for lithium and its compounds is increasing, which has also accelerated the development of liquid lithium resources. Liquid lithium resources, mainly seawater, lithium product processing byproducts and waste lithium product leachate, have large total lithium reserves and low average lithium concentrations, and the coexisting ions are Na(I) and K(I) with similar chemical properties. These characteristics make the selective extraction of Li(I) one of the difficulties in extracting lithium from liquid resources.

[0003] Solvent extraction is an effective method for large-volume water treatment, and it has also shown good treatment effects in lithium / sodium / potassium separation. For example, the 2-thiophenecarboxylic acid trifluoroacetone / trioctylphosphine oxide extraction system can achieve a Li(I) / Na(I) separation factor of 65 and a Li(I) / K(I) separation factor of 133 (Licheng Zhang, Journal of Molecular Liquids, 2019). However, the environmental pollution and economic problems caused by the volatilization and dissolution of a large amount of extractants during the treatment process have made this technology questionable in actual use. Membrane extraction technology is a new type of membrane technology developed on the basis of solvent extraction. Compared with solvent extraction, membrane extraction technology loads the extractant on the base polymer, which requires only a small amount of extractant to complete the selective extraction of metal ions. And by adjusting the membrane components, the treatment effect of solvent extraction technology can also be achieved. For example, in actual research, the separation factor (SF) of Li(I) to Na(I) and K(I) in the 2-thenoyltrifluoroacetone / trioctylphosphine oxide membrane extraction system can reach 54.25 and 50.60 (Chunqing Cai, Journal of Membrane Science, 2019). Although the permeability coefficient of this system to lithium is low (1.0056 μm·s -1 ) and the processing time is relatively long (120h), but the relatively environmentally friendly processing process still makes it a hot topic.

[0004] The external electric field coupled membrane extraction technology can significantly increase the extraction rate of ions by the system. However, in our previous studies, we found that the application of an external electric field can significantly increase the permeability coefficient of lithium (Meng Xiaorong, Hydrometallurgy, 2021). However, the external electric field will accelerate the leakage of the membrane-based material, which is also one of the main reasons for the reduction in the stability and selectivity of the external electric field coupled extraction membrane technology. Therefore, how to maintain the stability of the membrane while increasing the membrane permeability coefficient is still one of the important issues to be solved in membrane extraction technology. Summary of the invention

[0005] In order to solve the problems of slow lithium mass transfer rate in traditional lithium membrane extraction systems and leakage of membrane-based materials in external electric field coupled membrane extraction technology, the present invention provides a method for preparing a lithium-selective membrane extraction material with high efficiency and good circulation stability under an external electric field and its membrane lithium extraction technology, which provides a reference method for the efficient and stable extraction of lithium from liquid lithium resources under the background of lithium / sodium / potassium.

[0006] The present invention is achieved through the following technical solutions.

[0007] In one aspect of the present invention, a method for separating lithium, sodium and potassium using a lithium selective membrane extraction material is provided, comprising the following steps:

[0008] Step 1, preparation of lithium selective membrane extraction material:

[0009] Adding 40%-50% polyvinyl chloride, 30%-40% 2-thenoyltrifluoroacetone and 10%-30% co-extractant in a solvent in a mass ratio, stirring until homogeneous, transferring the obtained homogeneous solution to a flat-bottomed container, and preparing a lithium selective extraction membrane by a solvent volatilization method;

[0010] Step 2, electromembrane extraction application:

[0011] The prepared lithium selective extraction membrane lithium is loaded in the middle of two liquid pools, and platinum electrodes connected to an external DC regulated power supply are installed in the two liquid pools respectively. A lithium / sodium / potassium mixed solution is injected into the liquid pool on the anode side of the power supply, and an analytical solution for lithium recovery is injected into the liquid pool on the cathode side of the power supply. Under the set voltage, the extraction is completed when the lithium concentration in the solutions on both sides no longer changes.

[0012] Another aspect of the present invention provides a method for separating lithium, sodium and potassium using a lithium selective membrane extraction material, comprising the following steps:

[0013] Step 1, preparing modified lithium selective membrane extraction material:

[0014] Adding 30%-50% polyvinyl chloride, 20%-40% 2-thenoyltrifluoroacetone, 5%-23% co-extractant, and 5%-30% modifier in a solvent in a mass ratio, stirring until homogeneous, transferring the obtained homogeneous solution to a flat-bottomed container, and preparing a modified lithium selective extraction membrane by a solvent volatilization method;

[0015] Step 2, electromembrane extraction application:

[0016] The prepared modified lithium selective extraction membrane is loaded in the middle of a two-liquid pool device, and platinum electrodes connected to an external DC regulated power supply are installed in the two liquid pools respectively. A lithium / sodium / potassium mixed solution is injected into the liquid pool on the anode side of the power supply, and an analytical solution for lithium recovery is injected into the liquid pool on the cathode side of the power supply. Under the set voltage, the extraction is completed when the lithium concentration in the solutions on both sides no longer changes.

[0017] Preferably, the modifier is kerosene or dioctyl phthalate.

[0018] Preferably, the solvent is one or a mixture of two or more of dichloromethane, chloroform, tetrahydrofuran or cyclohexanone; the solvent accounts for 80%-90% of the total mixed liquid mass.

[0019] Preferably, the polyvinyl chloride is SG-8 type polyvinyl chloride.

[0020] Preferably, the synergist is trialkylphosphine oxide, tributyl phosphate or 1,10-phenanthroline.

[0021] Preferably, the lithium / sodium / potassium mixed solution contains NH3·H2O and Li + 、Na + , K + The mixed solution is a chloride or nitrate salt of Li, Na, and K; Na + , K + The concentration is Li + 1-5 times of.

[0022] Preferably, the analytical solution is one of HCl, H2SO4 or HNO3 solution; the concentration of the analytical solution is 0.1 mol / L.

[0023] Preferably, the pH of the lithium / sodium / potassium mixed solution is maintained at 11.13 and the pH of the analytical solution is maintained at 1.

[0024] Preferably, the applied DC voltage is 10-40 V and the separation time is 12-18 h.

[0025] The present invention adopts the above technical solution, which has the following beneficial effects:

[0026] One aspect of the present invention provides a method for preparing a lithium extraction membrane and an electric membrane lithium extraction technology thereof, wherein the lithium extraction rate of the prepared membrane is improved through the synergistic effect of a co-extractant on the lithium extraction of 2-thenoyltrifluoroacetone, thereby improving the stability of the prepared membrane under an external electric field and the lithium transfer rate. Compared with traditional lithium membrane extraction technology, this method can extract lithium from an aqueous solution more efficiently and quickly, and has a certain cyclic stability.

[0027] Another aspect of the present invention provides a method for preparing a modified lithium selective extraction membrane and a process for extracting lithium and separating lithium / sodium / potassium under an external electric field. The lithium selective extraction membrane is prepared by adding different hydrophobic modifiers to the lithium extraction membrane, so that the membrane has the hydrophobic characteristics of the modifier, thereby reducing the contact between the carrier in the membrane and water, and further improving the stability of the membrane under an external electric field. At the same time, the selected modifier does not affect the specific binding process between the carrier and lithium in the membrane, so that the modified lithium selective extraction membrane still has a certain lithium / sodium, lithium / potassium selectivity and a higher lithium extraction rate.

[0028] The method and technology provided by the present invention can achieve efficient extraction of lithium and have strong cyclic stability, and is a high-stability lithium selective extraction membrane that can be used in a lithium / sodium / potassium background. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] The drawings described herein are used to provide a further understanding of the present invention, constitute a part of the present application, and do not constitute an improper limitation of the present invention. In the drawings:

[0030] Figure 1 This is the infrared spectrum of the lithium selective membrane extraction material prepared in Examples 1-3 of the present invention. DETAILED DESCRIPTION

[0031] The present invention will be described in detail below in conjunction with the accompanying drawings and specific embodiments. The exemplary embodiments and descriptions of the present invention are used to explain the present invention but are not intended to limit the present invention.

[0032] The embodiment of the present invention provides a method for preparing a lithium selective extraction membrane without adding a modifier, and a method for separating lithium, sodium and potassium using the lithium selective extraction membrane, comprising the following steps:

[0033] Step 1, preparation of lithium selective extraction membrane:

[0034] 40%-50% polyvinyl chloride, 30%-40% 2-thenoyltrifluoroacetone and 10%-30% synergist are added to the solvent in a mass ratio, and stirred for 8-14 hours until the mixed solution is clear and transparent and is homogeneous. The obtained homogeneous solution is transferred to a flat-bottomed container, and a lithium selective extraction membrane is prepared by a solvent volatilization method.

[0035] The solvent is one or a mixture of two or more of dichloromethane, chloroform, tetrahydrofuran or cyclohexanone; the solvent accounts for 80%-90% of the total mixed liquid mass.

[0036] The polyvinyl chloride is SG-8 type polyvinyl chloride.

[0037] The synergistic extractant is trialkylphosphine oxide, tributyl phosphate or 1,10-phenanthroline.

[0038] Step 2, electromembrane extraction application:

[0039] The prepared lithium selective extraction membrane is loaded in the middle of two liquid pools, and platinum electrodes connected to an external DC voltage-stabilized power supply are installed in the two liquid pools respectively. A lithium / sodium / potassium mixed solution is injected into the liquid pool on the anode side of the power supply. The lithium / sodium / potassium mixed solution contains NH3·H2O and Li + 、Na + , K + The mixed solution is Li, Na, K chloride or nitrate, Na + , K + The concentration is Li + 1-5 times of. Inject the analytical solution for lithium recovery into the liquid pool on the cathode side of the power supply, the analytical solution concentration is 0.1mol / L, the analytical solution is one of HCl, H2SO4 or HNO3 solution, and the pH of the analytical solution is 1; apply a voltage of 10-40V at both ends of the electrode, separate for 12-18h, and complete the extraction when the lithium concentration in the solutions on both sides no longer changes.

[0040] The embodiment of the present invention further provides a method for preparing a lithium selective extraction membrane with a modifier, and a method for separating lithium, sodium and potassium using the modified lithium selective extraction membrane, comprising the following steps:

[0041] Step 1, preparation of modified lithium selective extraction membrane:

[0042] 30%-50% of polyvinyl chloride, 20%-40% of 2-thenoyltrifluoroacetone, 5%-23% of a co-extractant and 5%-30% of a modifier are added to a solvent in a mass ratio, and the mixture is stirred until a homogeneous phase is obtained. The obtained homogeneous phase solution is transferred to a flat-bottomed container, and a modified lithium selective extraction membrane is prepared by a solvent volatilization method.

[0043] The modifier is kerosene or dioctyl phthalate.

[0044] Step 2, electromembrane extraction application:

[0045] The prepared modified lithium selective extraction membrane is loaded in the middle of two liquid pools. Platinum electrodes connected to an external DC voltage regulator are installed in the two liquid pools respectively. A lithium / sodium / potassium mixed solution is injected into the liquid pool on the anode side of the power supply. The lithium / sodium / potassium mixed solution contains NH3·H2O and Li + 、Na + , K + The mixed solution is Li, Na, K chloride or nitrate, Na + , K + The concentration is Li + 1-5 times of. Inject the analytical solution for lithium recovery into the liquid pool on the cathode side of the power supply, the analytical solution concentration is 0.1mol / L, the analytical solution is one of HCl, H2SO4 or HNO3 solution, and the pH of the analytical solution is 1; apply a voltage of 10-40V at both ends of the electrode, separate for 12-18h, and complete the extraction when the lithium concentration in the solutions on both sides no longer changes.

[0046] The specific implementation modes of the present invention are further described in detail below through examples.

[0047] Embodiment 1:

[0048] Lithium extraction based on 2-thenoyltrifluoroacetone / trialkylphosphine oxide lithium selective extraction membrane:

[0049] Step 1, add 41.7% polyvinyl chloride, 33.3% 2-thenoyltrifluoroacetone, and 25% trialkylphosphine oxide in a mass ratio to dichloromethane solvent, the solvent accounting for 80% of the total mixed solution mass, stir the mixed solution for 8 hours and then transfer it to a flat-bottomed container, let it stand to evaporate the solvent, and obtain 2-thenoyltrifluoroacetone / trialkylphosphine oxide membrane extraction material.

[0050] Step 2, loading the prepared 2-thenoyltrifluoroacetone / trialkylphosphine oxide lithium membrane extraction material into a self-made two-chamber mass transfer device, after leak detection, inserting a platinum electrode connected to the anode of the power supply into the lithium-containing liquid side, inserting a platinum electrode connected to the cathode of the power supply into the lithium recovery analysis liquid side, applying a voltage of 40V to both ends of the electrodes, and separating for 12 hours; when the concentrations of the solutions on both sides no longer change, replacing the two-phase solutions and repeating the lithium extraction process at the same voltage.

[0051] The lithium-containing solution is 0.1 mol / L NH3·H2O, 20 mg / L Li + Mixed solution, lithium recovery solution is 0.1mol / LHCl, effective membrane area is 3.14cm 2The membrane thickness was 200 μm. During the total 12 h of mass transfer, samples were taken every 3-4 h, and 0.1 mol / L NH3·H2O and 0.1 mol / L HCl were used to adjust the pH of the two phases to maintain the pH of the feed phase and the analysis phase at about 11 and 1, respectively.

[0052] When the applied voltage is 40 V, the lithium extraction rate of 2-thenoyltrifluoroacetone / trialkylphosphine oxide lithium selective extraction membrane is 98.7% and the lithium recovery rate is 91.1% after 12 hours. The permeability coefficient can reach 33.20 μm·s -1 At a voltage of 40 V, only the two-phase solution was replaced and lithium extraction was performed with a cycle of 12 h. After four cycles, the membrane loss rate was 39.3%.

[0053] Embodiment 2:

[0054] Lithium extraction based on 2-thenoyltrifluoroacetone / tributyl phosphate lithium membrane extraction material:

[0055] Step 1: Add 50% polyvinyl chloride, 40% 2-thenoyl trifluoroacetone, and 10% tributyl phosphate in a mass ratio to chloroform solvent, with the solvent accounting for 85% of the total mixed solution. Stir the mixed solution for 10 hours and then transfer it to a flat-bottomed container. Let it stand to evaporate the solvent to obtain 2-thenoyl trifluoroacetone / tributyl phosphate lithium membrane extraction material. + The mixed solution is the feed liquid phase, 0.1 mol / L HCl is the analytical solution, and the effective membrane area is 3.14 cm 2 , the film thickness is 200μm.

[0056] Step 2, loading the prepared 2-thenoyltrifluoroacetone / tributyl phosphate lithium membrane extraction material into a self-made two-chamber mass transfer device, after leak detection, inserting a platinum electrode connected to the anode of the power supply into the lithium-containing liquid side, inserting a platinum electrode connected to the cathode of the power supply into the lithium recovery analysis liquid side, applying a voltage of 10V to both ends of the electrodes, and separating for 14 hours; when the concentrations of the solutions on both sides no longer change, replacing the two-phase solutions and repeating the lithium extraction process at the same voltage.

[0057] The lithium-containing solution is 0.1 mol / L NH3·H2O, 20 mg / L Li + Mixed solution, lithium recovery solution is 0.1mol / LHCl, effective membrane area is 3.14cm 2 The membrane thickness was 200 μm. During the total 14 h of mass transfer, samples were taken every 3-4 h, and 0.1 mol / L NH3·H2O and 0.1 mol / L H2SO4 were used to adjust the pH of the two phases, so that the pH of the feed phase and the analytical phase were maintained at about 11 and 1, respectively.

[0058] When the applied voltage was 10 V, the lithium extraction rate of the 2-thenoyltrifluoroacetone / tributyl phosphate lithium membrane extraction material after 14 h was 7.39 μm·s -1 When the applied voltage was 10 V, the lithium extraction rate was 93.6% after 14 h, the recovery rate was 92.1%, and the lithium permeability coefficient was 20.88 μm·s -1 At a voltage of 10 V, only the two-phase solution was replaced and lithium extraction was performed with a cycle of 14 h. After four cycles, the membrane loss rate was 27.4%.

[0059] Embodiment 3:

[0060] Lithium extraction based on 2-thenoyltrifluoroacetone / o-phenanthroline lithium membrane extraction material:

[0061] Step 1: Add 40% polyvinyl chloride, 30% 2-thenoyl trifluoroacetone, and 30% 1,10-phenanthroline in a mass ratio to tetrahydrofuran solvent, with the solvent accounting for 90% of the total mixed solution. Stir the mixed solution for 14 hours and then transfer it to a flat-bottomed container. Let it stand to evaporate the solvent to obtain 2-thenoyl trifluoroacetone / phenanthroline lithium membrane extraction material. + The mixed solution is the feed liquid phase, 0.1 mol / L HCl is the analytical solution, and the effective membrane area is 3.14 cm 2 , the film thickness is 200μm.

[0062] Step 2, loading the prepared 2-thenoyltrifluoroacetone / o-phenanthroline lithium membrane extraction material into a self-made two-chamber mass transfer device, after leak detection, inserting a platinum electrode connected to the anode of the power supply into the lithium-containing liquid side, inserting a platinum electrode connected to the cathode of the power supply into the lithium recovery analysis liquid side, applying a voltage of 20V to both ends of the electrodes, and separating for 18 hours; when the concentrations of the solutions on both sides no longer change, replacing the two-phase solutions and repeating the lithium extraction process at the same voltage.

[0063] The lithium-containing solution is 0.1 mol / L NH3·H2O, 20 mg / L Li + Mixed solution, lithium recovery solution is 0.1mol / LHCl, effective membrane area is 3.14cm 2 The membrane thickness was 200 μm. During the total 18-hour mass transfer process, samples were taken every 3-4 hours, and 0.1 mol / L NH3·H2O and 0.1 mol / L HNO3 were used to adjust the pH of the two phases, so that the pH of the feed phase and the analytical phase were maintained at about 11 and 1, respectively.

[0064] When the applied voltage was 10 V, the lithium extraction rate of the 2-thenoyltrifluoroacetone / o-phenanthroline lithium membrane extraction material after 18 h was 6.55 μm·s -1When the applied voltage was 40 V, the lithium extraction rate was 88.9% after 18 h, the recovery rate was 77.0%, and the lithium permeability coefficient was 16.86 μm·s -1 At a voltage of 20 V, only the two-phase solution was replaced and lithium extraction was performed with a cycle of 18 h. After four cycles, the membrane loss rate was 33.9%.

[0065] The infrared spectra of the lithium selective membrane extraction materials prepared in Examples 1-3 are shown in Figure 1 shown.

[0066] Embodiment 4:

[0067] Preparation and stability test of lithium selective extraction membrane using dioctyl phthalate as modifier and trialkylphosphine oxide as synergist:

[0068] Step 1, add 38.46% polyvinyl chloride, 30.77% 2-thenoyltrifluoroacetone, 23.08% trialkylphosphine oxide, and 7.69% dioctyl phthalate in tetrahydrofuran in a mass ratio in dichloromethane solvent, wherein the solvent accounts for 80% of the total mixed solution mass, stir the mixed solution for 14 hours and then transfer it to a flat-bottomed container, and let it stand to evaporate the solvent to obtain dioctyl phthalate modified 2-thenoyltrifluoroacetone / trialkylphosphine oxide lithium selective extraction membrane.

[0069] Step 2, loading the prepared modified lithium membrane extraction material into a self-made two-chamber mass transfer device, after leak detection, inserting a platinum electrode connected to the anode of the power supply into the lithium-containing liquid side, inserting a platinum electrode connected to the cathode of the power supply into the lithium recovery analysis liquid side, applying a voltage of 40V to both ends of the electrodes, and separating for 16 hours; when the concentrations of the solutions on both sides no longer change, replacing the two-phase solutions and repeating the lithium extraction process at the same voltage.

[0070] 0.1mol / L NH3·H2O, 20mg / L Li + The mixed solution is the feed liquid phase, 0.1 mol / L HCl is the analytical solution, and the effective membrane area is 3.14 cm 2 , the membrane thickness was controlled to be about 200μm. Under a voltage of 40V, only the two-phase solution was replaced and the lithium extraction application was carried out in a cycle of 16h. After four cycles, the loss rate of the dioctyl phthalate modified 2-thenoyltrifluoroacetone / trialkylphosphine oxide lithium selective extraction membrane was 31.9%.

[0071] Embodiment 5:

[0072] Preparation and stability test of lithium selective extraction membrane using dioctyl phthalate as modifier and tributyl phosphate as co-extractant:

[0073] 45.45% polyvinyl chloride, 36.36% 2-thenoyltrifluoroacetone, 9.10% tributyl phosphate and 9.09% dioctyl phthalate were added to the solvent dichloromethane in a mass ratio of 80% of the total mixed solution. The mixed solution was stirred for 16 hours and then transferred to a flat-bottomed container. The solvent was allowed to stand and evaporate to obtain a dioctyl phthalate modified 2-thenoyltrifluoroacetone / tributyl phosphate lithium selective extraction membrane.

[0074] Step 2, loading the prepared modified lithium membrane extraction material into a self-made two-chamber mass transfer device, after leak detection, inserting a platinum electrode connected to the anode of the power supply into the lithium-containing liquid side, inserting a platinum electrode connected to the cathode of the power supply into the lithium recovery analysis liquid side, applying a voltage of 40V to both ends of the electrodes, and separating for 16 hours; when the concentrations of the solutions on both sides no longer change, replacing the two-phase solutions and repeating the lithium extraction process at the same voltage.

[0075] 0.1mol / L NH3·H2O, 20mg / L Li + The mixed solution is the feed liquid phase, 0.1 mol / L HCl is the analytical solution, and the effective membrane area is 3.14 cm 2 , the membrane thickness was controlled to be about 200μm. Under a voltage of 40V, only the two-phase solution was replaced and the lithium extraction application was carried out with a cycle of 16h. After four cycles, the loss rate of the dioctyl phthalate modified 2-thenoyltrifluoroacetone / tributyl phosphate lithium selective extraction membrane was 20.5%.

[0076] Embodiment 6:

[0077] Preparation and stability test of lithium selective extraction membrane using dioctyl phthalate as modifier and o-phenanthroline as co-extractant:

[0078] 30.76% polyvinyl chloride, 40.47% 2-thenoyltrifluoroacetone, 23.48% phenanthroline and 5.29% dioctyl phthalate were added to the solvent dichloromethane in a mass ratio of 80% of the total mixed solution. The mixed solution was stirred for 14 hours and then transferred to a flat-bottomed container. The solvent was allowed to stand and evaporate to obtain a dioctyl phthalate-modified 2-thenoyltrifluoroacetone / phenanthroline lithium selective extraction membrane.

[0079] Step 2, loading the prepared modified lithium membrane extraction material into a self-made two-chamber mass transfer device, after leak detection, inserting a platinum electrode connected to the anode of the power supply into the lithium-containing liquid side, inserting a platinum electrode connected to the cathode of the power supply into the lithium recovery analysis liquid side, applying a voltage of 40V to both ends of the electrodes, and separating for 16 hours; when the concentrations of the solutions on both sides no longer change, replacing the two-phase solutions and repeating the lithium extraction process at the same voltage.

[0080] 0.1mol / L NH3·H2O, 20mg / L Li +The mixed solution is the feed liquid phase, 0.1 mol / L HCl is the analytical solution, and the effective membrane area is 3.14 cm 2 , the membrane thickness was controlled to be about 200μm. Under a voltage of 40V, only the two-phase solution was replaced and the lithium extraction application was carried out with a cycle of 16h. After four cycles, the loss rate of the dioctyl phthalate modified 2-thenoyltrifluoroacetone / o-phenanthroline lithium selective extraction membrane was 29.0%.

[0081] Compared with the lithium selective extraction membrane without adding modifier, the loss rate has been improved, indicating that dioctyl phthalate modification can enhance the stability of the mass transfer system.

[0082] Embodiment 7:

[0083] Preparation of 2-thenoyltrifluoroacetone / trialkylphosphine oxide lithium selective extraction membrane using kerosene as modifier and its application in lithium / sodium / potassium separation:

[0084] Step 1, add 31.25% polyvinyl chloride, 25% 2-thenoyltrifluoroacetone, 18.75% trialkylphosphine oxide, and 25% kerosene in a mass ratio to tetrahydrofuran solvent, wherein the solvent accounts for 85% of the total mixed solution mass, stir the mixed solution for 10 hours, transfer it to a flat-bottom container, and let it stand to volatilize the solvent to obtain a kerosene-modified 2-thenoyltrifluoroacetone / trialkylphosphine oxide lithium selective extraction membrane, and control the membrane thickness to be about 200 μm.

[0085] Step 2, loading the prepared kerosene-modified 2-thenoyltrifluoroacetone / trialkylphosphine oxide lithium selective extraction membrane into a self-made two-chamber mass transfer device, after leak detection, inserting a platinum electrode connected to the anode of the power supply into the lithium-containing liquid side, inserting a platinum electrode connected to the cathode of the power supply into the lithium recovery analysis liquid side, applying a voltage of 30V to both ends of the electrodes, and separating for 12 hours; when the concentration of the solutions on both sides no longer changes, the lithium extraction process is completed.

[0086] 0.1mol / L NH3·H2O, 20mg / L Li + The mixed solution is the feed liquid phase, 0.1 mol / L HCl is the analytical solution, and the effective membrane area is 3.14 cm 2 When the applied voltage was 30 V, the lithium extraction rate of the kerosene-modified 2-thenoyltrifluoroacetone / trialkylphosphine oxide lithium selective extraction membrane was 95.3% and the lithium recovery rate was 90.6% after 12 h. The permeability coefficient could reach 26.54 μm·s -1 At a voltage of 30 V, only the two-phase solution was replaced and lithium extraction was performed with a cycle of 12 h. After four cycles, the membrane loss rate was 18.2%.

[0087] The effective membrane area is 3.14 cm 2 When 0.1 mol / L HCl is used as the analytical solution, the feed liquid phase is Li+ 、Na + , K + The mixed solution with a concentration of 20 mg / L was subjected to lithium extraction at 30 V for 12 h. Li 25.4 μm·s -1 , P Na 3.02 μm·s -1 , P K 3.18 μm·s -1 , S Li(I) / Na(I) is 8.41, S Li(I) / K(I) 7.99. 0.1mol / L HCl was used as the analytical solution, and the feed liquid phase was 20mg / L Li + 、100mg / L Na + , K + Mixed solution, lithium extraction application at 30V for 12h, P Li 24.9 μm·s -1 , P Na 3.25 μm·s -1 , P K 3.36 μm·s -1 , S Li(I) / Na(I) is 7.66, S Li(I) / K(I) It is 7.41.

[0088] Embodiment 8:

[0089] Preparation of 2-thenoyltrifluoroacetone / lithium tributyl phosphate selective extraction membrane using kerosene as modifier and its application in lithium / sodium / potassium separation:

[0090] Step 1, adding 35.71% polyvinyl chloride, 28.57% 2-thenoyltrifluoroacetone, 5.15% tributyl phosphate, and 30.57% kerosene in a mass ratio to cyclohexanone solvent, wherein the solvent accounts for 90% of the total mixed solution mass, stirring the mixed solution for 10 hours and then transferring it to a flat-bottomed container, and standing the mixture to volatilize the solvent to obtain a kerosene-modified 2-thenoyltrifluoroacetone / tributyl phosphate lithium selective extraction membrane, wherein the membrane thickness is controlled to be about 200 μm.

[0091] Step 2, loading the prepared kerosene-modified 2-thenoyltrifluoroacetone / tributyl phosphate lithium selective extraction membrane into a self-made two-chamber mass transfer device, after leak detection, inserting a platinum electrode connected to the anode of the power supply into the lithium-containing liquid side, inserting a platinum electrode connected to the cathode of the power supply into the lithium recovery analysis liquid side, applying a voltage of 40V to both ends of the electrodes, and separating for 15 hours; when the concentration of the solutions on both sides no longer changes, the lithium extraction process is completed.

[0092] 0.1mol / L NH3·H2O, 20mg / L Li +The mixed solution is the feed liquid phase, 0.1 mol / L HCl is the analytical solution, and the effective membrane area is 3.14 cm 2 When the applied voltage was 40 V, the lithium extraction rate of the kerosene-modified 2-thenoyltrifluoroacetone / lithium tributyl phosphate selective extraction membrane was 91.8% after 15 h, the lithium recovery rate was 88.3%, and the permeability coefficient was 19.02 μm·s -1 At a voltage of 40 V, only the two-phase solution was replaced and lithium extraction was performed with a cycle of 15 h. After four cycles, the membrane loss rate was 16.0%.

[0093] The effective membrane area is 3.14 cm 2 When 0.1 mol / L HCl is used as the analytical solution, the feed liquid phase is Li + 、Na + , K + The mixed solution with a concentration of 20 mg / L was subjected to lithium extraction at 40 V for 15 h. Li 18.48 μm·s -1 , P Na 3.79 μm·s -1 , P K 3.98 μm·s -1 , S Li(I) / Na(I) is 4.88, S Li(I) / K(I) The analytical solution is 0.1 mol / L HCl and the feed liquid is 20 mg / L Li + 、100mg / L Na + , K + Mixed solution, lithium extraction application at 40V for 15h, P Li 17.96 μm·s -1 , P Na 3.93 μm·s -1 , P K 4.21 μm·s -1 , S Li(I) / Na(I) is 4.57, S Li(I) / K(I) is 4.26.

[0094] Embodiment 9:

[0095] Preparation of 2-thenoyltrifluoroacetone / o-phenanthroline lithium selective extraction membrane using kerosene as modifier and its application in lithium / sodium / potassium separation:

[0096] Step 1, adding 50.25% polyvinyl chloride, 20.25% 2-thenoyltrifluoroacetone, 14.5% phenanthroline and 15% kerosene in a mass ratio to dichloromethane solvent, wherein the solvent accounts for 80% of the total mixed solution mass, stirring the mixed solution for 10 hours and then transferring it to a flat-bottomed container, and standing the mixture to volatilize the solvent to obtain a kerosene-modified 2-thenoyltrifluoroacetone / phenanthroline lithium selective extraction membrane, wherein the membrane thickness is controlled to be about 200 μm.

[0097] Step 2, loading the prepared kerosene-modified 2-thenoyltrifluoroacetone / o-phenanthroline lithium selective extraction membrane into a self-made two-chamber mass transfer device, after leak detection, inserting a platinum electrode connected to the anode of the power supply into the lithium-containing liquid side, inserting a platinum electrode connected to the cathode of the power supply into the lithium recovery analysis liquid side, applying a voltage of 20V to both ends of the electrodes, and separating for 18 hours; when the concentration of the solutions on both sides no longer changes, the lithium extraction process is completed.

[0098] 0.1mol / L NH3·H2O, 20mg / L Li + The mixed solution is the feed liquid phase, 0.1 mol / L HCl is the analytical solution, and the effective membrane area is 3.14 cm 2 When the applied voltage was 20 V, the lithium extraction rate of the kerosene-modified 2-thenoyltrifluoroacetone / o-phenanthroline lithium selective extraction membrane was 88.1% after 18 h, the lithium recovery rate was 76.9%, and the permeability coefficient was 16.16 μm·s -1 At a voltage of 20 V, only the two-phase solution was replaced and lithium extraction was performed with a cycle of 18 h. After four cycles, the membrane loss rate was 20.2%.

[0099] The effective membrane area is 3.14 cm 2 When 0.1 mol / L HCl is used as the analytical solution, the feed liquid phase is Li + 、Na + , K + The concentration of the mixed solution was 20 mg / L, and the lithium extraction application was carried out at 20 V for 18 h. Li 15.37 μm·s -1 , P Na 3.95 μm·s -1 , P K 4.03 μm·s -1 , S Li(I) / Na(I) is 3.88, S Li(I) / K(I) The analytical solution is 0.1 mol / L HCl and the feed liquid is 20 mg / L Li + 、100mg / L Na + , K + Mixed solution, lithium extraction application at 20V for 18h, P Li 14.83 μm·s-1 , P Na 4.12 μm·s -1 , P K 4.39 μm·s -1 , S Li(I) / Na(I) is 3.60, S Li(I) / K(I) It is 3.38.

[0100] The lithium selective extraction membrane provided by the present invention not only solves the problem of slow rate of traditional lithium extraction membrane, but also improves the membrane loss problem in the electromembrane extraction system, so that the prepared membrane has a higher lithium extraction rate and cycle stability, and maintains a certain Li / Na, Li, K separation ability, which provides a reference method for the selective extraction of lithium from lithium / sodium / potassium solution.

[0101] The present invention is not limited to the above-mentioned embodiments. On the basis of the technical solution disclosed in the present invention, technicians in this field can make some substitutions and deformations to some technical features therein according to the disclosed technical content without creative labor, and these substitutions and deformations are all within the protection scope of the present invention.

Claims

1. A method for separating lithium, sodium and potassium using a lithium selective membrane extraction material, characterized in that: The following steps are involved: Step 1, preparation of lithium selective membrane extraction material: Adding 40%-50% polyvinyl chloride, 30%-40% 2-thenoyltrifluoroacetone and 10%-30% co-extractant in a solvent in a mass ratio, stirring until homogeneous, transferring the obtained homogeneous solution to a flat-bottomed container, and preparing a lithium selective extraction membrane by a solvent volatilization method; Step 2, electromembrane extraction application: The prepared lithium selective extraction membrane lithium is loaded in the middle of two liquid pools, and platinum electrodes connected to an external DC regulated power supply are installed in the two liquid pools respectively. A lithium / sodium / potassium mixed solution is injected into the liquid pool on the anode side of the power supply, and an analytical solution for lithium recovery is injected into the liquid pool on the cathode side of the power supply. Under the set voltage, the extraction is completed when the lithium concentration in the solutions on both sides no longer changes.

2. A method for separating lithium, sodium and potassium using a lithium selective membrane extraction material, characterized in that: The following steps are involved: Step 1, preparing modified lithium selective membrane extraction material: Adding 30%-50% polyvinyl chloride, 20%-40% 2-thenoyltrifluoroacetone, 5%-23% co-extractant, and 5%-30% modifier in a solvent in a mass ratio, stirring until homogeneous, transferring the obtained homogeneous solution to a flat-bottomed container, and preparing a modified lithium selective extraction membrane by a solvent volatilization method; Step 2, electromembrane extraction application: The prepared modified lithium selective extraction membrane is loaded in the middle of a two-liquid pool device, and platinum electrodes connected to an external DC regulated power supply are installed in the two liquid pools respectively. A lithium / sodium / potassium mixed solution is injected into the liquid pool on the anode side of the power supply, and an analytical solution for lithium recovery is injected into the liquid pool on the cathode side of the power supply. Under the set voltage, the extraction is completed when the lithium concentration in the solutions on both sides no longer changes.

3. The method for separating lithium, sodium and potassium using a lithium selective membrane extraction material according to claim 2, characterized in that: The modifier is kerosene or dioctyl phthalate.

4. The method for separating lithium, sodium and potassium using a lithium selective membrane extraction material according to claim 1 or 2, characterized in that: The solvent is one or a mixture of two or more of dichloromethane, chloroform, tetrahydrofuran or cyclohexanone; the solvent accounts for 80%-90% of the total mixed liquid mass.

5. The method for separating lithium, sodium and potassium using a lithium selective membrane extraction material according to claim 1 or 2, characterized in that: The polyvinyl chloride is SG-8 type polyvinyl chloride.

6. The method for separating lithium, sodium and potassium using a lithium selective membrane extraction material according to claim 1 or 2, characterized in that: The co-extractant is trialkylphosphine oxide, tributyl phosphate or 1,10-phenanthroline.

7. The method for separating lithium, sodium and potassium using a lithium selective membrane extraction material according to claim 1 or 2, characterized in that: The lithium / sodium / potassium mixed solution contains NH3·H2O and Li + 、Na + , K + The mixed solution is a chloride or nitrate salt of Li, Na, and K; Na + , K + The concentration is Li + 1-5 times of.

8. The method for separating lithium, sodium and potassium using a lithium selective membrane extraction material according to claim 1 or 2, characterized in that: The analytical solution is one of HCl, H2SO4 or HNO3 solution; the concentration of the analytical solution is 0.1 mol / L.

9. The method for separating lithium, sodium and potassium using a lithium selective membrane extraction material according to claim 1 or 2, characterized in that: The pH of the lithium / sodium / potassium mixed solution was maintained at 11.13 and the pH of the analytical solution was maintained at 1.

10. The method for separating lithium, sodium and potassium using a lithium selective membrane extraction material according to claim 1 or 2, characterized in that: The applied DC voltage is 10-40V and the separation time is 12-18h.

Citation Information

Patent Citations

  • Composite extractant for separating lithium in solution with high magnesium-lithium ratio and extraction method

    CN110669930A

  • Deep purification method for low-concentration heavy metal chromium (VI)

    CN110745901A

  • Plasticized polymer ionic liquid film and method for selective separation of chromium (VI) through same

    CN110759430A

  • Semi-interpenetrating network polymer support membrane, preparation thereof and application of semi-interpenetrating network polymer support membrane in electric membrane extraction

    CN112138547A

  • Gel liquid film with gelation structure as well as preparation method and application of gel liquid film

    CN114939352A