Preparation method of Fe monatomic catalyst for regulating and controlling different coordination environments
By using the combination method of ferric acetylacetonate, zinc nitrate hexahydrate and 2-methylimidazole in the preparation of Fe single atom catalyst, combined with high pressure reaction and annealing treatment, the local coordination environment of Fe single atom catalyst was successfully regulated, and the solution was solved. The problem of metal cluster generation in the prior art is achieved, the preparation of different coordination environments is achieved, and the smooth progress of the catalytic reaction is promoted.
Patent Information
- Application Number
- CN202410979457.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-22
- Publication Date
- 2024-11-12
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The prior art has difficulties in regulating the local coordination environment of Fe single-atom catalysts, which leads to the formation of metal clusters and hinders its practical application in the fields of water cracking and hydrogen production and carbon dioxide reduction.
By stirring iron acetylacetonate and zinc nitrate hexahydrate in methanol, adding 2-methylimidazole and reacting in an autoclave, followed by circulating centrifugation and annealing, a single-atom Fe catalyst with different coordination environments was prepared. FeNX(X=4, 5, 6).
This method is simple and universal, and successfully regulates single-atom Fe catalysts in different local coordination environments, avoids the formation of metal clusters, significantly reduces the reaction energy barrier, and promotes the smooth progress of the catalytic reaction.
Smart Images

Figure CN118925772A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of catalyst technology, and more particularly to a method for preparing a Fe single-atom catalyst by regulating different coordination environments. Background Art
[0002] Single-atom catalysts have been widely used in recent years in the fields of water splitting to produce hydrogen, carbon dioxide reduction, nitrate generation of ammonia, and advanced oxidation due to their minimal size effect, which enables them to achieve maximum atomic utilization, fully exposed catalytic active centers, and unique coordination structures. The local coordination environment of single-atom catalysts is the key to regulating their activity. A suitable local coordination environment can significantly regulate the electron density of the Fe active site and shift the d-band center downward, thereby reducing the reaction energy barrier of the activated intermediate product and promoting the smooth progress of the reaction. Currently, most studies focus on doping B, P, and S to tune the electron density of the Fe active center. The complex synthesis and the easy occurrence of metal clusters have seriously hindered its development and practical application. Summary of the invention
[0003] In view of this, the present invention provides a method for preparing a Fe single atom catalyst by regulating different coordination environments, comprising the following steps:
[0004] (1) adding ferric acetylacetonate and zinc nitrate hexahydrate into methanol and stirring thoroughly to obtain solution A;
[0005] (2) adding 2-methylimidazole to methanol and stirring thoroughly to obtain solution B;
[0006] (3) adding solution A dropwise into solution B and stirring thoroughly to obtain a mixed solution;
[0007] (4) putting the mixed solution into a high-pressure reactor for reaction, and cooling naturally after the reaction is completed to obtain a mixed material after the reaction;
[0008] (5) adding a cleaning agent to the mixed material, and subjecting the mixed material to a circulating centrifugal cleaning treatment to obtain a precipitate;
[0009] (6) drying the precipitate, and grinding the dried precipitate into powder;
[0010] (7) The ground precipitate is annealed at different temperatures to obtain single-atom Fe catalysts FeN with different coordination environments. X , X=4,5,6.
[0011] Preferably, the ratio of ferric acetylacetonate, zinc nitrate hexahydrate and methanol in step (1) is: 0.176 g ferric acetylacetonate and 1.19 g zinc nitrate hexahydrate are added to every 30 mL methanol.
[0012] Preferably, the stirring time in step (1) is 15 min.
[0013] Preferably, the ratio of 2-methylimidazole to methanol in step (2) is: 1.314 g of 2-methylimidazole is added to every 15 mL of methanol.
[0014] Preferably, the stirring time in step (2) is 15 min.
[0015] Preferably, in step (3), the volume ratio of solution A to solution B is 2:1, and the stirring time is 1 hour.
[0016] Preferably, in step (4), the reaction temperature is 120° C. and the reaction time is 4 h.
[0017] Preferably, the cleaning agent in step (5) is one or more of DMF and methanol.
[0018] Preferably, the drying temperature in step (6) is 60°C.
[0019] Preferably, the annealing treatment in step (7) is: heating to 80-1000°C at a heating rate of 5°C / min, maintaining for 2 hours, and then naturally cooling to room temperature.
[0020] It can be seen from the above technical solution that, compared with the prior art, the present invention discloses a method for preparing a Fe single-atom catalyst by regulating different coordination environments, which has the following beneficial effects:
[0021] The technical solution of the present invention simply regulates the material synthesis temperature to prepare single-atom Fe catalysts with different local coordination environments, and the preparation method is simple and universal. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on the provided drawings without paying creative work.
[0023] Figure 1 This is the XRD pattern of the single-atom Fe catalyst prepared in Example 1 of the present invention;
[0024] Figure 2 This is a spherical aberration correction-scanning electron microscope image of the single-atom Fe catalyst prepared in Example 1 of the present invention;
[0025] Figure 3 The Fe K edge expansion absorption spectrum fitting curve corresponding to the single-atom Fe catalyst prepared in Example 1 of the present invention;
[0026] Figure 4 Fourier transform spectra of the extended X-ray absorption fine structure spectra of Fe K edge of Fe-N4@NC, Fe-N5@NC and Fe-N6@NC catalysts prepared in Example 1 of the present invention;
[0027] Figure 5 Wavelet transform XAFS three-dimensional spectra of Fe-N4@NC, Fe-N5@NC and Fe-N6@NC catalysts prepared in Example 1 of the present invention. DETAILED DESCRIPTION
[0028] The technical solution of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0029] Example 1
[0030] (1) Add 0.176 g of ferric acetylacetonate and 1.19 g of zinc nitrate hexahydrate to 30 mL of methanol and stir for 15 min to obtain solution A;
[0031] (2) Add 1.314 g of 2-methylimidazole to 15 mL of methanol and stir for 15 min to obtain solution B;
[0032] (3) adding solution A dropwise into solution B, with the volume ratio of solution A to solution B being 2:1, and stirring for 1 h to obtain a mixed solution;
[0033] (4) placing the mixed solution into a high-pressure reactor at 120° C. for 4 hours, and cooling naturally after the reaction is completed to obtain a mixed material after the reaction;
[0034] (5) adding a cleaning agent, methanol, to the mixed material, and performing a cyclic centrifugal cleaning treatment on the mixed material for no less than 3 times to obtain a precipitate;
[0035] (6) drying the precipitate at 60° C. and grinding the dried precipitate into powder for 10 min or longer to ensure sufficient grinding;
[0036] (7) The ground precipitate is annealed at different temperatures to obtain single-atom Fe catalysts FeN with different coordination environments. X, X=4, 5, 6; specifically: annealing is carried out in a tubular annealing furnace, the annealing treatment is: the temperature in the furnace is increased to 800, 900, and 1000°C at a heating rate of 5°C / min, and maintained for 2h, and then naturally cooled to room temperature, and FeN6, FeN5, and FeN4 single-atom catalysts with different coordination environments are prepared accordingly, which are named Fe-N6@NC, Fe-N5@NC, and Fe-N4@NC, respectively.
[0037] The characterization diagram of the prepared product is shown in Figure 1-5 As shown, where:
[0038] The crystal phase structure of the single-atom Fe catalyst prepared in the example was tested by XRD to determine whether there was a cluster crystal phase in its crystal phase structure. Figure 1 The XRD patterns shown show that the XRD patterns of the single-atom Fe catalysts prepared at different temperatures are in an amorphous state, indicating that no clusters are generated, and it can be preliminarily determined that they are in a single-atom form;
[0039] Figure 2 a, b, and c correspond to single-atom Fe catalysts synthesized at annealing temperatures of 800, 900, and 1000 degrees, respectively. Spherical aberration-corrected scanning electron microscopy images further show that the synthesized catalyst exists in atomic form;
[0040] Figure 3 is the Fe K edge expansion absorption spectrum fitting curve corresponding to the single-atom Fe catalyst prepared in the embodiment of the present invention; the Fe-N bond on the spectrum reflects the Fe-N coordination in the catalyst, and the greater the Fe-N bond strength, the greater the number of N coordination;
[0041] Figure 4 It is the Fourier transform spectrum of the extended X-ray absorption fine structure spectrum of Fe K edge of Fe-N4@NC, Fe-N5@NC and Fe-N6@NC catalysts prepared in the embodiment of the present invention. The fitting range of this figure is The fitting results show that the fitting results are basically consistent with the actual measurement results;
[0042] Figure 5 It is a wavelet transform XAFS three-dimensional spectrum of Fe-N4@NC, Fe-N5@NC and Fe-N6@NC catalysts prepared in the embodiment of the present invention; Figure 5 It shows that Fe2O3 has and The bond lengths of are , corresponding to the Fe-O bond and the Fe-Fe bond, respectively; the bond length of Fe foil is only 2.5, indicating that there are only Fe-Fe bonds in Fe foil; Fe-N4@NC, Fe-N5@NC, and Fe-N6@NC catalysts only have Fe-N bonds, indicating that no metal clusters are generated and the synthesized catalysts are composed in atomic form.
[0043] In this specification, each embodiment is described in a progressive manner, and each embodiment focuses on the differences from other embodiments, and the same and similar parts between the embodiments can be referred to each other. The above description of the disclosed embodiments enables professionals and technicians in this field to implement or use the present invention. Various modifications to these embodiments will be obvious to professionals and technicians in this field, and the general principles defined herein can be implemented in other embodiments without departing from the spirit or scope of the present invention. Therefore, the present invention will not be limited to these embodiments shown in this article, but will comply with the widest range consistent with the principles and novel features disclosed herein.
Claims
1. A method for preparing a Fe single-atom catalyst by regulating different coordination environments, characterized in that: The following steps are involved: (1) adding ferric acetylacetonate and zinc nitrate hexahydrate into methanol and stirring thoroughly to obtain solution A; (2) adding 2-methylimidazole to methanol and stirring thoroughly to obtain solution B; (3) adding solution A dropwise into solution B and stirring thoroughly to obtain a mixed solution; (4) putting the mixed solution into a high-pressure reactor for reaction, and cooling naturally after the reaction is completed to obtain a mixed material after the reaction; (5) adding a cleaning agent to the mixed material, and subjecting the mixed material to a circulating centrifugal cleaning treatment to obtain a precipitate; (6) drying the precipitate, and grinding the dried precipitate into powder; (7) The ground precipitate is annealed at different temperatures to obtain single-atom Fe catalysts FeN with different coordination environments. X , X=4,5,6.
2. The method for preparing a Fe single-atom catalyst for regulating different coordination environments according to claim 1, characterized in that: The ratio of ferric acetylacetonate, zinc nitrate hexahydrate and methanol in step (1) is: 0.176 g ferric acetylacetonate and 1.19 g zinc nitrate hexahydrate are added to every 30 mL of methanol.
3. The method for preparing a Fe single-atom catalyst for regulating different coordination environments according to claim 1, characterized in that: The stirring time in step (1) is 15 min.
4. The method for preparing a Fe single-atom catalyst with different coordination environments according to claim 1, characterized in that: The ratio of 2-methylimidazole and methanol in step (2) is: 1.314 g of 2-methylimidazole is added to every 15 mL of methanol.
5. The method for preparing a Fe single atom catalyst with different coordination environments according to claim 1, characterized in that: The stirring time in step (2) is 15 min.
6. The method for preparing a Fe single-atom catalyst with different coordination environments according to claim 1, characterized in that: In step (3), the volume ratio of solution A to solution B is 2:1, and the stirring time is 1 h.
7. The method for preparing a Fe single atom catalyst with different coordination environments according to claim 1, characterized in that: In step (4), the reaction temperature is 120° C. and the reaction time is 4 h.
8. The method for preparing a Fe single atom catalyst with different coordination environments according to claim 1, characterized in that: The cleaning agent in step (5) is one or more of DMF and methanol.
9. The method for preparing a Fe single-atom catalyst with different coordination environments according to claim 1, characterized in that: The drying temperature in step (6) is 60°C.
10. The method for preparing a Fe single-atom catalyst with different coordination environments according to claim 1, characterized in that: The annealing treatment in step (7) is as follows: heating to 80-1000°C at a heating rate of 5°C / min, maintaining for 2 hours, and then naturally cooling to room temperature.
Citation Information
Patent Citations
Preparation method of metal monatomic site catalyst
CN107626294A
Dodecahedral monatomic iron Fenton catalyst, and preparation and application thereof
CN113070090A
Fe monatomic loaded electrochemical catalyst as well as preparation method and application thereof
CN113694948A