Preparation method of aluminum-magnesium explosive composite board

Through the grinding of aluminum alloy and magnesium alloy sheets and the explosive composite technology of powder emulsified explosives, combined with heat treatment and mechanical processing, the problems of bending deformation and low bonding rate of aluminum-magnesium composite sheets during the explosive composite process are solved, and high patching is achieved Aluminum-magnesium composite board with composite rate and high shear strength meets the needs of the new energy industry.

CN118926838AInactive Publication Date: 2024-11-12ANHUI PROVINCE BAOTAI SPECIAL MATERIAL CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411065097.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-05
Publication Date
2024-11-12
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing aluminum-magnesium composite panels often experience large bending deformation and low bonding rate during explosive composite, which is difficult to meet the new energy industry's demand for high strength and high bonding rate.

Method used

The aluminum alloy plate and magnesium alloy plate are polished and used for explosive composite, and the residual stress is eliminated through heat treatment, combined with mechanical processing to improve shear strength and bonding rate.

Benefits of technology

The high fit rate (up to 99.9%) and high shear strength (≥80Mpa) of aluminum-magnesium composite boards have been achieved, meeting the size and performance requirements of the new energy industry for chip research and development.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118926838A_ABST
    Figure CN118926838A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of an aluminum-magnesium explosive composite board. The preparation method comprises the following steps: S1, preparing raw materials; s2, assembling the substrate; s3, selecting explosives; s3, selecting explosives; s4, assembling a compound plate; s5, assembling detonators; s6, explosive cladding; s7, performing subsequent treatment; and S8, detecting the composite board. The method has the advantages that a large amount of explosive needs to be laid on the magnesium alloy plate, continuous welding is finally achieved through installation and arrangement in an angle mode on an explosion site, ultrasonic flaw detection is conducted on the magnesium alloy plate, the fitting rate can reach 99% or above, and the minimum shearing strength tau b is larger than or equal to 80 Mpa.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of composite plate manufacturing, and in particular to a method for preparing an aluminum-magnesium explosion composite plate. Background Art

[0002] The characteristics of magnesium materials mainly include low density, high strength, large elastic modulus, good heat dissipation, good shock absorption, strong ability to withstand impact loads, and good resistance to corrosion from organic matter and alkali.

[0003] Magnesium material is an alloy composed of magnesium and other elements. Its density is about 1.8g / cm3. It has the advantages of high specific strength and specific stiffness, good thermal and electrical conductivity, etc. In addition, magnesium alloy also has good electromagnetic shielding, damping, vibration reduction, cutting processability, low processing cost, processing energy is only 70% of aluminum alloy, and easy recycling. The specific strength of magnesium alloy is higher than that of aluminum alloy and steel, and slightly lower than the fiber reinforced plastic with the highest specific strength; the specific stiffness is equivalent to that of aluminum alloy and steel, and much higher than that of fiber reinforced plastic; the wear resistance is much better than that of low-carbon steel, and has exceeded that of die-cast aluminum alloy A380; the vibration reduction performance and magnetic shielding performance are much better than aluminum alloy. These characteristics of magnesium material make it more valuable than aluminum and plastic in the application of automotive structural materials.

[0004] With the rapid development of the domestic new energy industry in recent years, many companies have begun to look for the use of aluminum-magnesium composite materials to achieve resource integration, reduce costs and maximize resource utilization. Therefore, research on aluminum-magnesium composite plates has been carried out. The mechanism of explosive composite is to use the energy generated by the explosion of explosives to drive the composite plate to collide with the substrate at high speed to produce a high-speed jet, thereby obtaining metallurgical bonding between atoms. The explosion process will produce a jet, thereby self-cleaning the surface of the base composite plate and allowing fresh metal to bond. However, in conventional explosive welding, the composite plate produced has a large bending deformation and a low bonding rate.

[0005] To this end, we proposed a method for preparing aluminum-magnesium explosion composite plates to solve the above problems. Summary of the invention

[0006] The purpose of the present invention is to solve the problems in the prior art and to propose a method for preparing an aluminum-magnesium explosion composite plate.

[0007] In order to achieve the above object, the present invention adopts the following technical solutions:

[0008] A method for preparing an aluminum-magnesium explosion composite plate comprises the following steps:

[0009] S1. Raw material preparation: Select aluminum alloy plate as substrate and magnesium alloy plate as composite plate, grind the surface of substrate and composite plate to remove oxide layer and impurities, and make the explosion bonding surface flat, clean and smooth;

[0010] S2, assembling the substrate; adding a layer of cardboard between the substrate and the foundation, scrubbing the upper surface of the substrate with acetone, and evenly arranging a number of support blocks on the upper surface of the substrate, adding rubber pads on the side walls of the substrate, and the thickness of the rubber is equal to the thickness of the substrate;

[0011] S3, select explosives; the main explosive selected is powdered emulsion explosive, the parameters of the powdered emulsion explosive are: detonation velocity ≥ 2500m / s, explosion heat 3698KJ / Kg, explosion temperature 2234℃, explosion pressure 452Mpa, density (0.85~1.15)g / ㎝3, and force (lead column compression value) ≥ 13mm;

[0012] S4, assembling the composite plate; scrubbing the lower surface of the composite plate with acetone solution, and placing the composite plate on the upper surface of multiple support blocks, evenly brushing butter on the upper surface of the composite plate to form a butter protective layer with a buffer layer effect, the protective layer thickness is 1mm, and placing a medicine frame around the composite plate to prevent the powdered emulsion explosive from scattering, and spreading the powdered emulsion explosive with a thickness of 30 to 40mm on the butter layer;

[0013] S5. Assemble detonators; place and fix detonators on the long side of the double plate, and connect the leads of the detonators to 50m away from the explosion site to leave a safe distance for the explosion;

[0014] S6, explosive composite: using the fuse of the detonator to detonate the explosive to cause an explosion. After the explosion, conduct a preliminary inspection of the composite plate to check whether there are defects such as delamination and cracks;

[0015] S7, subsequent processing: heat treatment is performed on the plate after explosive compounding to eliminate residual stress, and then mechanical processing is performed, such as leveling, cutting, etc. The detonation point is located at the edge position and can be cut off during cutting;

[0016] S8. Composite board testing: Test the bonding rate and shear strength of the composite board. If the bonding rate is above 99.9% and the shear strength τb ≥ 80Mpa, the requirements are met.

[0017] In the above-mentioned method for preparing the copper-titanium explosion composite plate, in step S1, the substrate is made of 6013 aluminum alloy plate, and the substrate thickness is 10 mm, and the plate size is 350 mm×250 mm.

[0018] In the above-mentioned method for preparing the copper-titanium explosion composite plate, in step S1, the composite plate is made of AZ73 magnesium alloy plate, and the composite plate has a thickness of 3 mm and a plate width of 400 mm×300 mm.

[0019] In the above-mentioned method for preparing the copper-titanium explosion composite plate, in step S2, before installing the support block, the composite plate is preheated to a temperature of 350°C.

[0020] In the above-mentioned copper-titanium explosion composite plate preparation method, in step S2, the support block is divided into a conventional support frame and an auxiliary support frame. A number of equally spaced conventional support frames of the same shape as the substrate are distributed according to the shape of the substrate, and a number of auxiliary support frames are distributed within the edges of the several conventional support frames and the steel plates, and it is ensured that the several auxiliary support frames are equally spaced.

[0021] In the above-mentioned method for preparing the copper-titanium explosion composite plate, in step S7, the specific steps are:

[0022] Step 1, heating: heating the composite board in a heating furnace, the heating temperature is 800℃-900℃, and the heating time is 1h-2h;

[0023] Step 2: Heat preservation: After reaching the predetermined heat treatment temperature, keep it for a certain period of time to allow the internal structure of the plate to fully transform and homogenize;

[0024] Step 3: Cooling: Cool the composite board to room temperature.

[0025] Compared with the prior art, the present invention has the following beneficial effects:

[0026] A larger amount of explosives should be laid on the composite AZ73 plate, and the installation arrangement should be in the form of an angle method at the explosion site to achieve continuous welding. There is no corresponding standard specification for the aluminum-magnesium composite plate. Through ultrasonic testing, the bonding rate can reach more than 99%, and the minimum shear strength τb ≥ 80Mpa; the one-time molding of the unrepairable AZ73-6013 explosive composite is achieved, and its bonding rate can reach 99.9% and the shear strength can reach τb ≥ 80Mpa. The size of the produced AZ73-6013 composite plate can meet the needs of the development of new energy and other industries for chip research and development. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Figure 1 Schematic diagram of the explosion installation proposed by the present invention.

[0028] In the figure: 1 detonator, 2 explosive, 3 protective layer, 4 composite plate, 5 support block, 6 base plate, 7 foundation. DETAILED DESCRIPTION

[0029] The following examples are for illustrative purposes only and are not intended to limit the scope of the present invention.

[0030] Embodiment 1

[0031] Reference Figure 1 , a method for preparing an aluminum-magnesium explosion composite plate, comprising the following steps:

[0032] S1. Raw material preparation: an aluminum alloy plate is selected as the substrate 6, the substrate 6 adopts a 6013 aluminum alloy plate, and the substrate 6 has a thickness of 10 mm and a plate width of 350 mm×250 mm; a magnesium alloy plate is selected as the composite plate 4, the composite plate 4 adopts an AZ73 magnesium alloy plate, and the composite plate 4 has a thickness of 3 mm and a plate width of 400 mm×300 mm; the surfaces of the substrate 6 and the composite plate 4 are polished to remove the oxide layer and impurities, so that the explosion bonding surface is flat, clean and smooth;

[0033] S2, assembling the substrate 6; preheating the composite plate 4 to 350°C, adding a layer of cardboard between the substrate 6 and the foundation 7, scrubbing the upper surface of the substrate 6 with acetone solution, and evenly arranging a number of support blocks 5 on the upper surface of the substrate 6. The support blocks 5 are divided into conventional support frames and auxiliary support frames. A number of conventional support frames with the same shape as the substrate 6 and distributed at equal intervals are distributed according to the shape of the substrate 6. A number of auxiliary support frames are distributed within the edges of the conventional support frames and the steel plate, and the number of auxiliary support frames are ensured to be evenly spaced. Rubber is padded on the side wall of the substrate 6, and the thickness of the rubber is equal to the thickness of the substrate 6.

[0034] S3, select explosive 2; the main explosive selected is powdered emulsion explosive, the parameters of the powdered emulsion explosive are: detonation velocity ≥ 2500m / s, explosion heat 3698KJ / Kg, explosion temperature 2234℃, explosion pressure 452Mpa, density (0.85~1.15)g / ㎝3, and fierceness (lead column compression value) ≥ 13mm;

[0035] S4, assembling the double plate 4; scrubbing the lower surface of the double plate 4 with acetone solution, and placing the double plate 4 on the upper surface of the plurality of support blocks 5, evenly brushing butter on the upper surface of the double plate 4 to form a butter protective layer 3 having a buffer layer effect, the protective layer 3 having a thickness of 1 mm, and placing a medicine frame around the double plate 4 to prevent the powdered emulsion explosive from scattering, and spreading the powdered emulsion explosive 2 with a thickness of 30 mm on the butter layer;

[0036] S5, assemble detonator 1; place detonator 1 on the long side of the double plate 4 and fix detonator 1, connect the lead of detonator 1 to 50m away from the explosion site to leave a safe distance for the explosion;

[0037] S6, explosive composite: using the fuse of detonator 1 to detonate explosive 2, causing an explosion. After the explosion, a preliminary inspection is performed on the composite plate to check whether there are defects such as delamination and cracks;

[0038] S7, subsequent treatment; heat treatment is performed on the explosive composite plate to eliminate residual stress, the composite plate is heated in a heating furnace, the heating temperature is 800 ° C, the heating time is 2 hours, after reaching the predetermined heat treatment temperature, the temperature is kept for 1 hour to fully transform and homogenize the internal structure of the plate, the furnace cooling method is selected to cool the composite plate to room temperature, and then mechanical processing such as leveling, cutting, etc. is performed. The detonation point is located at the edge position and can be cut off when cutting;

[0039] S8. Composite board testing: Test the bonding rate and shear strength of the composite board. If the bonding rate is above 99.9% and the shear strength τb ≥ 80Mpa, the requirements are met.

[0040] Embodiment 2

[0041] Reference Figure 1 , a method for preparing an aluminum-magnesium explosion composite plate, comprising the following steps:

[0042] S1. Raw material preparation: an aluminum alloy plate is selected as the substrate 6, the substrate 6 adopts a 6013 aluminum alloy plate, and the substrate 6 has a thickness of 10 mm and a plate width of 350 mm×250 mm; a magnesium alloy plate is selected as the composite plate 4, the composite plate 4 adopts an AZ73 magnesium alloy plate, and the composite plate 4 has a thickness of 3 mm and a plate width of 400 mm×300 mm; the surfaces of the substrate 6 and the composite plate 4 are polished to remove the oxide layer and impurities, so that the explosion bonding surface is flat, clean and smooth;

[0043] S2, assembling the substrate 6; preheating the composite plate 4 to 350°C, adding a layer of cardboard between the substrate 6 and the foundation 7, scrubbing the upper surface of the substrate 6 with acetone solution, and evenly arranging a number of support blocks 5 on the upper surface of the substrate 6. The support blocks 5 are divided into conventional support frames and auxiliary support frames. A number of conventional support frames with the same shape as the substrate 6 and distributed at equal intervals are distributed according to the shape of the substrate 6. A number of auxiliary support frames are distributed within the edges of the conventional support frames and the steel plate, and the number of auxiliary support frames are ensured to be evenly spaced. Rubber is padded on the side wall of the substrate 6, and the thickness of the rubber is equal to the thickness of the substrate 6.

[0044] S3, select explosive 2; the main explosive selected is powdered emulsion explosive, the parameters of the powdered emulsion explosive are: detonation velocity ≥ 2500m / s, explosion heat 3698KJ / Kg, explosion temperature 2234℃, explosion pressure 452Mpa, density (0.85~1.15)g / ㎝3, and fierceness (lead column compression value) ≥ 13mm;

[0045] S4, assembling the double plate 4; scrubbing the lower surface of the double plate 4 with acetone solution, and placing the double plate 4 on the upper surface of the plurality of support blocks 5, evenly brushing butter on the upper surface of the double plate 4 to form a butter protective layer 3 having a buffer layer effect, the protective layer 3 having a thickness of 1 mm, and placing a medicine frame around the double plate 4 to prevent the powdered emulsion explosive from scattering, and spreading the powdered emulsion explosive 2 with a thickness of 35 mm on the butter layer;

[0046] S5, assemble detonator 1; place detonator 1 on the long side of the double plate 4 and fix detonator 1, connect the lead of detonator 1 to 50m away from the explosion site to leave a safe distance for the explosion;

[0047] S6, explosive composite: using the fuse of detonator 1 to detonate explosive 2, causing an explosion. After the explosion, a preliminary inspection is performed on the composite plate to check whether there are defects such as delamination and cracks;

[0048] S7, subsequent treatment; heat treatment is performed on the plate after explosive compounding to eliminate residual stress, the composite plate is heated in a heating furnace, the heating temperature is 900°C, the heating time is 1h, after reaching the predetermined heat treatment temperature, the plate is kept warm for 2 hours to fully transform and homogenize the internal structure of the plate, the composite plate is cooled to room temperature by air cooling, and then mechanical processing is performed, such as leveling, cutting, etc. The detonation point is located at the edge position and can be cut off during cutting;

[0049] S8. Composite board testing: Test the bonding rate and shear strength of the composite board. If the bonding rate is above 99.9% and the shear strength τb ≥ 80Mpa, the requirements are met.

[0050] Embodiment 3

[0051] Reference Figure 1 , a method for preparing an aluminum-magnesium explosion composite plate, comprising the following steps:

[0052] S1. Raw material preparation: an aluminum alloy plate is selected as the substrate 6, the substrate 6 adopts a 6013 aluminum alloy plate, and the substrate 6 has a thickness of 10 mm and a plate width of 350 mm×250 mm; a magnesium alloy plate is selected as the composite plate 4, the composite plate 4 adopts an AZ73 magnesium alloy plate, and the composite plate 4 has a thickness of 3 mm and a plate width of 400 mm×300 mm; the surfaces of the substrate 6 and the composite plate 4 are polished to remove the oxide layer and impurities, so that the explosion bonding surface is flat, clean and smooth;

[0053] S2, assembling the substrate 6; preheating the composite plate 4 to 350°C, adding a layer of cardboard between the substrate 6 and the foundation 7, scrubbing the upper surface of the substrate 6 with acetone solution, and evenly arranging a number of support blocks 5 on the upper surface of the substrate 6. The support blocks 5 are divided into conventional support frames and auxiliary support frames. A number of conventional support frames with the same shape as the substrate 6 and distributed at equal intervals are distributed according to the shape of the substrate 6. A number of auxiliary support frames are distributed within the edges of the conventional support frames and the steel plate, and the number of auxiliary support frames are ensured to be evenly spaced. Rubber is padded on the side wall of the substrate 6, and the thickness of the rubber is equal to the thickness of the substrate 6.

[0054] S3, select explosive 2; the main explosive selected is powdered emulsion explosive, the parameters of the powdered emulsion explosive are: detonation velocity ≥ 2500m / s, explosion heat 3698KJ / Kg, explosion temperature 2234℃, explosion pressure 452Mpa, density (0.85~1.15)g / ㎝3, and fierceness (lead column compression value) ≥ 13mm;

[0055] S4, assembling the double plate 4; scrubbing the lower surface of the double plate 4 with acetone solution, and placing the double plate 4 on the upper surface of the plurality of support blocks 5, evenly brushing butter on the upper surface of the double plate 4 to form a butter protective layer 3 having a buffer layer effect, the protective layer 3 having a thickness of 1 mm, and placing a medicine frame around the double plate 4 to prevent the powdered emulsion explosive from scattering, and spreading the powdered emulsion explosive 2 with a thickness of 40 mm on the butter layer;

[0056] S5, assemble detonator 1; place detonator 1 on the long side of the double plate 4 and fix detonator 1, connect the lead of detonator 1 to 50m away from the explosion site to leave a safe distance for the explosion;

[0057] S6, explosive composite: using the fuse of detonator 1 to detonate explosive 2, causing an explosion. After the explosion, a preliminary inspection is performed on the composite plate to check whether there are defects such as delamination and cracks;

[0058] S7, subsequent treatment; heat treatment is performed on the explosive composite plate to eliminate residual stress, the composite plate is heated in a heating furnace, the heating temperature is 850 ° C, the heating time is 1.5 hours, after reaching the predetermined heat treatment temperature, the temperature is kept for 1.5 hours to fully transform and homogenize the internal structure of the plate, the furnace cooling method is selected to cool the composite plate to room temperature, and then mechanical processing such as leveling, cutting, etc. is performed. The detonation point is located at the edge position and can be cut off during cutting;

[0059] S8. Composite board testing: Test the bonding rate and shear strength of the composite board. If the bonding rate is above 99.9% and the shear strength τb ≥ 80Mpa, the requirements are met.

[0060] A larger amount of explosives should be laid on the composite AZ73 plate, and the installation arrangement should be in the form of an angle method at the explosion site to achieve continuous welding. There is no corresponding standard specification for the aluminum-magnesium composite plate. Through ultrasonic testing, the bonding rate can reach more than 99%, and the minimum shear strength τb ≥ 80Mpa; the one-time molding of the unrepairable AZ73-6013 explosive composite is achieved, and its bonding rate can reach 99.9% and the shear strength can reach τb ≥ 80Mpa. The size of the produced AZ73-6013 composite plate can meet the needs of the development of new energy and other industries for chip research and development.

[0061] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.

Claims

1. A method for preparing an aluminum-magnesium explosion composite plate, characterized in that: The following steps are involved: S1. Raw material preparation: an aluminum alloy plate is selected as a substrate (6) and a magnesium alloy plate is selected as a composite plate (4); the surfaces of the substrate (6) and the composite plate (4) are polished to remove oxide layers and impurities, so that the explosion bonding surface is flat, clean and smooth; S2, assembling the substrate (6); adding a layer of cardboard between the substrate (6) and the foundation (7), scrubbing the upper surface of the substrate (6) with acetone solution, and evenly arranging a number of support blocks (5) on the upper surface of the substrate (6), adding rubber pads on the side walls of the substrate (6), and the thickness of the rubber is equal to the thickness of the substrate (6); S3, selecting explosive (2); the main explosive selected is powdered emulsion explosive, and the parameters of the powdered emulsion explosive are: detonation velocity ≥ 2500m / s, explosion heat 3698KJ / Kg, explosion temperature 2234°C, explosion pressure 452Mpa, density (0.85-1.15)g / ㎝3, and fierceness (lead column compression value) ≥ 13mm; S4, assembling the composite plate (4); scrubbing the lower surface of the composite plate (4) with acetone solution, and placing the composite plate (4) on the upper surface of a plurality of support blocks (5), evenly brushing butter on the upper surface of the composite plate (4) to form a butter protective layer (3) having a buffer layer function, wherein the thickness of the protective layer (3) is (1) mm, and placing a powder frame around the composite plate (4) to prevent the powdered emulsion explosive from scattering, and spreading the powdered emulsion explosive (2) with a thickness of 30 to 40 mm on the butter layer; S5, assembling the detonator (1); placing the detonator (1) on the long side of the double plate (4) and fixing the detonator (1), and connecting the lead of the detonator (1) to 50m from the explosion site to leave a safe distance for the explosion; S6, explosive compound; The explosive (2) is detonated by the fuse of the detonator (1) to cause an explosion. After the explosion, a preliminary inspection is performed on the composite plate to check whether there are defects such as delamination and cracks; S7, subsequent processing: heat treatment is performed on the plate after explosive compounding to eliminate residual stress, and then mechanical processing is performed, such as leveling, cutting, etc. The detonation point is located at the edge position and can be cut off during cutting; S8. Composite board testing: Test the bonding rate and shear strength of the composite board. If the bonding rate is above 99.9% and the shear strength τb ≥ 80Mpa, the requirements are met.

2. The method for preparing an aluminum-magnesium explosion composite plate according to claim 1, characterized in that: In step S1, the substrate (6) is made of 6013 aluminum alloy plate, and the thickness of the substrate (6) is 10 mm, and the plate size is 350 mm×250 mm.

3. The method for preparing an aluminum-magnesium explosion composite plate according to claim 1, characterized in that: In step S1, the composite plate (4) is made of AZ73 magnesium alloy plate, and the composite plate (4) has a thickness of 3 mm and a plate width of 400 mm×300 mm.

4. The method for preparing an aluminum-magnesium explosion composite plate according to claim 1, characterized in that: In step S2, before installing the support block (5), the composite plate (4) is preheated to a temperature of 350°C.

5. The method for preparing an aluminum-magnesium explosion composite plate according to claim 1, characterized in that: In step S2, the support block (5) is divided into a conventional support frame and an auxiliary support frame. A plurality of equally spaced conventional support frames having the same shape as the substrate (6) are distributed in the shape of the substrate (6). A plurality of auxiliary support frames are distributed within the plurality of conventional support frames and the edges around the steel plate, and the plurality of auxiliary support frames are ensured to be equally spaced.

6. The method for preparing an aluminum-magnesium explosion composite plate according to claim 1, characterized in that: In step S7, the specific steps are: Step 1, heating: heating the composite board in a heating furnace, the heating temperature is 800℃-900℃, and the heating time is 1h-2h; Step 2: Heat preservation: After reaching the predetermined heat treatment temperature, keep it for a certain period of time to allow the internal structure of the plate to fully transform and homogenize; Step 3: Cooling: Cool the composite board to room temperature.

Citation Information

Cited By

  • Preparation method of aluminum-magnesium explosive composite board

    CN121551797A