Preparation method of high-simulation synchronous wood grain digital printing board

Through the multi-step processing of high-precision digital printing and positioning equipment combined with UV coating and PET film, the problem of insufficient imitation wood grain digital printing boards in the existing technology is solved, and high-simulation and realistic natural wood is realized Improved texture effect and physical and chemical performance.

CN118927846APending Publication Date: 2024-11-12SHANGHAI YOULUPIN NEW MATERIALS CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202411083114.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-08
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The imitation wood grain of existing high-simulation synchronous wood grain digital printing boards is not realistic enough and has large errors, so it cannot effectively present the natural beauty of natural wood grain.

Method used

Using high-precision digital printing technology and high-precision positioning equipment, combined with UV coating and PET film, through multi-step pre-coating, digital printing and texture reproduction processes, the required images and natural wood grain texture are perfectly presented, enhancing the physical and chemical aspects of the board. performance.

Benefits of technology

It realizes high simulation and realistic natural wood grain effect, and is suitable for a variety of flat panels, improving the aesthetics and physical and chemical performance of the panels, and meeting the needs of different scenarios.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118927846A_ABST
    Figure CN118927846A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of a high-simulation synchronous wood grain digital printing board, and belongs to the technical field of board preparation, and the preparation method comprises the following steps: S1, pre-coating the surface of a base material, sanding the surface of an artificial board by adopting abrasive paper, roll-coating the surface of the artificial board with a color primer, and curing to form a ground color for later use; s2, high-definition digital coating is conducted on the prepared ground color, and the adjusted needed image is printed to a board through a high-precision printer and then cured; and S3, the physical and chemical properties of the surface of the board are enhanced, wood texture recarving is completed, the surface of the board is subjected to roller coating through paint, then natural wood texture is completely recarved through a PET film, and then curing is conducted. According to the invention, the physical and chemical properties required by the board in different scenes can be achieved by selecting different types of UV coatings, the required image is perfectly presented by adopting a high-precision digital printing technology, and the natural wood grain texture is manufactured by matching high-precision positioning equipment with a high-simulation texture PET film.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of board preparation, and in particular relates to a method for preparing a high-simulation synchronous wood grain digital printing board. Background Art

[0002] Digital lamination technology is a modern technology that combines digital image processing technology with traditional lamination technology. It uses professional equipment and technology to transfer digital images to the product surface through special printing media, and fix and enhance the pattern through lamination.

[0003] High-simulation synchronous wood grain digital printing panels are processed using digital film pressing technology. Existing high-simulation synchronous wood grain digital printing panels have problems such as insufficient fidelity of imitated wood grain and large errors. Summary of the invention

[0004] The present invention overcomes the deficiencies of the prior art and provides a method for preparing a high-simulation synchronous wood grain digital printing plate to solve the problems existing in the prior art.

[0005] To achieve the above object, the technical solution adopted by the present invention is: a method for preparing a high-simulation synchronous wood grain digital printing board, comprising the following steps:

[0006] S1. Pre-coating the surface of the substrate, sanding the surface of the artificial board with sandpaper, rolling the surface with color primer, and curing to form a base color for use;

[0007] S2. Perform high-definition digital painting on the prepared base color, print the adjusted required image on the plate with a high-precision printer and then cure it;

[0008] S3. To enhance the physical and chemical properties of the board surface and complete the wood texture reproduction, use paint to roll on the board surface, and then use PET film to completely replicate the natural wood texture, and then cure it.

[0009] In a preferred embodiment of the present invention, step S1 includes the following steps:

[0010] S101: Sanding of artificial boards, using 300-400 mesh sandpaper for wooden substrates and 200-300 mesh sandpaper for inorganic materials, and then using UV adhesive putty and UV filling putty, and curing to 40-50% by UV light;

[0011] S102: Roll-coat UV transparent primer, use film pressing equipment to fill and level the substrate, cure to 70-80%, and then sand with 300-400 grit sandpaper;

[0012] S103: Roll on the required UV color correction primer and cure to 50-60%;

[0013] S104: repeat S103;

[0014] S105: Roll-coat the required UV color correction primer, cure it to 80-90% and store it for future use.

[0015] In a preferred embodiment of the present invention, the amount of UV adhesive putty is 5-15g / m 2 The amount of UV filling putty is 20-30g / m 2 The amount of UV transparent primer is 35-45g / m 2 The amount of UV color correction primer is 15-25g / m 2 .

[0016] In a preferred embodiment of the present invention, step S2 includes the following steps:

[0017] S201: First, the semi-finished substrate with the primer stored is sanded with a sandpaper mesh of 400-600 mesh, and then UV adhesion primer is rolled and cured to 30-50%;

[0018] S202: Print the adjusted required image onto the plate using a high-precision printer, with the image pixel being above 400 DPI, the instantaneous curing degree being 30-50%, and then using a UV curing lamp to cure to above 70%.

[0019] In a preferred embodiment of the present invention, the amount of the UV adhesion primer is 6-10g / m 2 The digital printing ink used by the printer is 14-18g / m 2 .

[0020] In a preferred embodiment of the present invention, step S3 includes the following steps:

[0021] S301: Roll on UV hard primer and cure to 70-80%;

[0022] S302: Roll on UV wear-resistant primer, cure to 80-90%, and sand with 600-800 grit sandpaper;

[0023] S303: Roll-coat UV film pressing topcoat, with the aid of high-precision positioning device, use PET film to completely replicate the natural wood texture, pre-curing to 40-60% during film pressing, and then complete 100% curing through UV curing lamp.

[0024] In a preferred embodiment of the present invention, the amount of the UV hard primer is 15-25g / m 2 The amount of UV wear-resistant primer is 15-25g / m 2The amount of UV film topcoat is 100-300g / m 2 .

[0025] In a preferred embodiment of the present invention, the coating line speed in step S1 is 12-18 m / min, the digital printing speed in step S2 is 18-30 m / min, and the texture production speed in step S3 is 5-15 m / min.

[0026] The present invention solves the defects existing in the background technology and has the following beneficial effects:

[0027] The present invention is suitable for various flat boards such as multilayer boards, density boards, particle boards, calcium silicate boards, etc. The physical and chemical properties required for the boards in different scenarios can be achieved by selecting different types of UV coatings, and high-precision digital printing technology is used to perfectly present the required images. High-precision positioning equipment is used in conjunction with high-simulation texture PET film to produce natural wood grain texture, perfectly presenting the natural beauty of natural wood grain. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] The present invention is further described below in conjunction with the accompanying drawings and embodiments;

[0029] Figure 1 is an overall flow chart of a preferred embodiment of the present invention;

[0030] Figure 2 A first partial flow chart of a preferred embodiment of the present invention;

[0031] Figure 3 A second partial flow chart of a preferred embodiment of the present invention;

[0032] Figure 4 A third partial flow chart of a preferred embodiment of the present invention; DETAILED DESCRIPTION

[0033] The present invention is further described below in conjunction with the accompanying drawings and specific embodiments so that those skilled in the art can better understand the present invention and implement it, but the embodiments are not intended to limit the present invention.

[0034] The present embodiment provides a method for preparing a highly simulated synchronous wood grain digitally printed board. The preparation method is applicable to various flat boards such as multilayer boards, density boards, particle boards, calcium silicate boards, etc. Different types of UV coatings can be selected to achieve the physical and chemical properties required by the boards in different scenarios. High-precision digital printing technology is used to perfectly present the required image. High-precision positioning equipment is used in conjunction with a high-simulation texture PET film to produce natural wood grain texture, perfectly presenting the natural beauty of natural wood grain.

[0035] like Figure 1As shown, the method for preparing the highly simulated synchronous wood grain digital printing board of this embodiment includes the following steps:

[0036] S1. Pre-coating the surface of the substrate, sanding the surface of the artificial board with sandpaper, rolling the surface with color primer, and curing to form a base color for use;

[0037] S2. Perform high-definition digital painting on the prepared base color, print the adjusted required image on the plate with a high-precision printer and then cure it;

[0038] S3. To enhance the physical and chemical properties of the board surface and complete the wood texture reproduction, use paint to roll on the board surface, and then use PET film to completely replicate the natural wood texture, and then cure it.

[0039] Combination Figure 1 and Figure 2 As shown, step S1 of this embodiment specifically includes the following steps:

[0040] S101: Sanding of artificial boards, using 300-400 mesh sandpaper for wooden substrates and 200-300 mesh sandpaper for inorganic materials, and then using UV adhesive putty and UV filling putty, and curing to 40-50% by UV light;

[0041] S102: Roll-coat UV transparent primer, use film pressing equipment to fill and level the substrate, cure to 70-80%, and then sand with 300-400 grit sandpaper;

[0042] S103: Roll on the required UV color correction primer and cure to 50-60%;

[0043] S104: repeat S103;

[0044] S105: Roll-coat the required UV color correction primer, cure it to 80-90% and store it for future use.

[0045] In this embodiment, the amount of UV adhesive putty is 5-15g / m 2 , the dosage of UV filling putty is 20-30g / m 2 , UV transparent primer dosage is 35-45g / m 2 , UV color correction primer dosage is 15-25g / m 2 .

[0046] Combination Figure 1 and Figure 3 As shown, step S2 of this embodiment specifically includes the following steps:

[0047] S201: First, the semi-finished substrate with the primer stored is sanded with a sandpaper mesh of 400-600 mesh, and then UV adhesion primer is rolled and cured to 30-50%;

[0048] S202: Print the adjusted required image onto the plate using a high-precision printer, with the image pixel being above 400 DPI, the instantaneous curing degree being 30-50%, and then using a UV curing lamp to cure to above 70%.

[0049] In this embodiment, the amount of UV adhesion primer used is 6-10g / m 2 The digital printing ink used by the printer is 14-18g / m 2 .

[0050] Combination Figure 1 and Figure 4 As shown, step S3 of this embodiment specifically includes the following steps:

[0051] S301: Roll on UV hard primer and cure to 70-80%;

[0052] S302: Roll on UV wear-resistant primer, cure to 80-90%, and sand with 600-800 grit sandpaper;

[0053] S303: Roll-coat UV film pressing topcoat, with the aid of high-precision positioning device, use PET film to completely replicate the natural wood texture, pre-curing to 40-60% during film pressing, and then complete 100% curing through UV curing lamp.

[0054] In this embodiment, the amount of UV hard primer is 15-25g / m 2 , UV wear-resistant primer dosage is 15-25g / m 2 , UV film pressing topcoat dosage is 100-300g / m 2 .

[0055] Furthermore, in this embodiment, the coating line speed in step S1 is 12-18 m / min, the digital printing speed in step S2 is 18-30 m / min, and the texture production speed in step S3 is 5-15 m / min.

[0056] In the actual operation of the preparation method of the highly simulated synchronous wood grain digital printing board of this embodiment, first select a standard natural master, process the master to achieve a perfect effect, including wood grain morphology, wood thorn effect, and texture depth, scan the master with high precision, and perform 4-color decomposition of the scanned image by computer to meet the requirements of digital printing. Then use a thermosetting resin to cover the master, heat the resin after it is completely filled into the wooden texture, separate the resin from the master after cooling, and obtain a raised perfect wooden texture. Apply UV glue evenly on the PET film and press it with the resin template, and use UV lamp curing to perfectly print the wooden texture on the PET film to complete the reproduction of the entire texture for standby use.

[0057] Obviously, the above embodiments are merely examples for clear explanation and are not intended to limit the implementation methods. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here. The obvious changes or modifications derived from these are still within the protection scope of the invention.

Claims

1. A method for preparing a high-simulation synchronous wood grain digital printing board, It is characterized in that The following steps are involved: S1. Pre-coating the surface of the substrate, sanding the surface of the artificial board with sandpaper, rolling the surface with color primer, and curing to form a base color for use; S2. Perform high-definition digital painting on the prepared base color, print the adjusted required image on the plate with a high-precision printer and then cure it; S3. To enhance the physical and chemical properties of the board surface and complete the wood texture reproduction, use paint to roll on the board surface, and then use PET film to completely replicate the natural wood texture, and then cure it.

2. A method for preparing a high-simulation synchronous wood grain digital printing board according to claim 1, It is characterized in that Step S1 includes the following steps: S101: Sanding of artificial boards, using 300-400 mesh sandpaper for wooden substrates and 200-300 mesh sandpaper for inorganic materials, and then using UV adhesive putty and UV filling putty, and curing to 40-50% by UV light; S102: Roll UV transparent primer, use film pressing equipment to fill and level the substrate, cure to 70-80%, and then sand with 300-400 grit sandpaper; S103: Roll on the required UV color correction primer and cure to 50-60%; S104: repeat S103; S105: Roll-coat the required UV color correction primer, cure it to 80-90% and store it for future use.

3. The method for preparing a highly simulated synchronous wood grain digital printing plate according to claim 2, It is characterized in that The dosage of UV adhesive putty is 5-15g / m 2 The amount of UV filling putty is 20-30g / m 2 The amount of UV transparent primer is 35-45g / m 2 The amount of UV color correction primer is 15-25g / m 2 .

4. The method for preparing a highly simulated synchronous wood grain digital printing board according to claim 1, It is characterized in that Step S2 includes the following steps: S201: First, the semi-finished substrate with the primer stored is sanded with a sandpaper mesh of 400-600 mesh, and then UV adhesion primer is rolled and cured to 30-50%; S202: Print the adjusted required image onto the plate using a high-precision printer, with the image pixel being above 400 DPI, the instantaneous curing degree being 30-50%, and then using a UV curing lamp to cure to above 70%.

5. The method for preparing a highly simulated synchronous wood grain digital printing board according to claim 4, It is characterized in that The amount of UV adhesion primer is 6-10g / m 2 The digital printing ink used by the printer is 14-18g / m 2 .

6. The method for preparing a highly simulated synchronous wood grain digital printing board according to claim 1, It is characterized in that Step S3 includes the following steps: S301: Roll on UV hard primer and cure to 70-80%; S302: Roll on UV wear-resistant primer, cure to 80-90%, and sand with 600-800 grit sandpaper; S303: Roll-coat UV film pressing topcoat, with the aid of high-precision positioning device, use PET film to completely replicate the natural wood texture, pre-curing to 40-60% during film pressing, and then complete 100% curing through UV curing lamp.

7. The method for preparing a highly simulated synchronous wood grain digital printing board according to claim 6, It is characterized in that The amount of UV hard primer is 15-25g / m 2 The amount of UV wear-resistant primer is 15-25g / m 2 The amount of UV film topcoat is 100-300g / m 2 .

8. The method for preparing a highly simulated synchronous wood grain digital printing board according to claim 1, It is characterized in that The coating line speed in step S1 is 12-18 m / min, the digital printing speed in step S2 is 18-30 m / min, and the texture production speed in step S3 is 5-15 m / min.

Citation Information

Patent Citations

  • Transfer paper / film of imitation wood furniture open paint wood grains, preparation method thereof, and wood grain printing object

    CN109367267A

  • Preparation method of simulation wood grain three-dimensional decorative household board

    CN114434998A

  • Finishing process for numerical control color matching decoration of 3D hole display wood grain paint surface on surface of artificial board

    CN116060276A

  • Manufacturing device of digital variable gold stamping film and using method of manufacturing device

    CN116968459A

  • Method of simultaneous transfer printing and embossing or surface texturing

    GB1598836A