Preparation method and application of photosensitive glass
By performing double-sided masking and radiation treatment on the rear case glass of the smart watch, combined with heat treatment, the problems of light-sensitive glass in the smart watch are solved, and efficient light control and detection data accuracy are achieved.
Patent Information
- Application Number
- CN202410975705.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-19
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2044-07-19
AI Technical Summary
Traditional glass does not have light shading performance in the back case of smart watches, which leads to light-shading interference between LED light, which affects the accuracy of detection data. In addition, photosensitive glass is difficult to illuminate vertically during ultraviolet treatment, resulting in dizziness at the edge of the exposed area. Edge phenomenon.
By performing double-sided masking of the substrate glass and radiation treatment and heat treatment on both main surfaces, the wavelength, intensity and time of ultraviolet irradiation are controlled, and photosensitive glass with good light-shading performance is prepared by combining nucleation and crystallization treatment. .
The edge halo phenomenon of the exposure area of the photosensitive glass is significantly improved, and good light shading performance is achieved in the exposure area, improving the accuracy of the detection data.
Smart Images

Figure CN118930045A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the field of glass technology, and in particular to a preparation method and use of photosensitive glass. Background Art
[0002] In recent years, smart watches have developed rapidly, and their functions have become more and more diverse. They can not only detect the number of steps, but also measure body fat, blood oxygen, body temperature, heart rate, etc. The realization of these functions all depends on the LED on the back of the smart watch to emit light of the corresponding wavelength to the skin, convert the reflected light into an electrical signal, and then convert it into a digital signal through the corresponding receiver. However, in pursuit of better texture, the back of smart watches is usually made of glass, but traditional glass does not have light-shielding properties, which will cause the light emitted by the LED to interfere with each other, forming a cross-light phenomenon, affecting the accuracy of the detection data.
[0003] Photosensitive glass is Li-Al-Si glass containing photosensitizer. Compared with ordinary glass materials, after UV treatment and heat treatment, photosensitive glass can form an opaque area in the exposed area. The light transmittance of the exposed area is greatly reduced compared to the non-exposed area, and it has the performance of shading. It is expected to replace ordinary glass and be used in the back cover of smart watches. However, although there are many reports on the preparation of photosensitive glass, it is still difficult for conventional photosensitive glass to achieve the shading performance required by the back cover of smart watches.
[0004] In addition, during the UV treatment process of photosensitive glass, since the UV light source is difficult to irradiate vertically, there will be a certain inclination angle, which causes uncontrollable light to irradiate into other areas except the exposure area, expanding the range of the glass exposure area and causing haloing at the edge of the exposure area.
[0005] It should be noted that this part of the present invention only provides background technology related to the present invention and does not necessarily constitute prior art or known technology. Summary of the invention
[0006] The purpose of the present application is to provide a method for preparing photosensitive glass, which can improve the phenomenon of haloing at the edge of the exposure area of the photosensitive glass and at the same time ensure that the exposure area has good light-shielding performance.
[0007] In order to achieve the above objectives, this application provides the following technical solutions:
[0008] In a first aspect, a method for preparing a photosensitive glass is provided, comprising:
[0009] obtaining substrate glass;
[0010] The substrate glass comprises a first region and a second region, two main surfaces opposite to each other in the first region are masked, and the second region is not masked, so as to obtain a substrate glass having the same structure after double-sided masking;
[0011] The two main surfaces of the double-sided masked substrate glass with the same structure are irradiated and then heat-treated to obtain a photosensitive glass with a non-exposed area and an exposed area; wherein the non-exposed area corresponds to the first area, and the exposed area corresponds to the second area.
[0012] As an optional embodiment, the radiation treatment comprises ultraviolet irradiation treatment.
[0013] As an optional embodiment, the wavelength of the ultraviolet irradiation treatment is 300nm-320nm, and the intensity of the ultraviolet irradiation treatment is 20mw / cm 2 -360mw / cm 2 The UV irradiation treatment time is 5min-60min.
[0014] As an optional embodiment, the conditions for the double-sided radiation treatment are the same.
[0015] As an optional embodiment, the conditions for the double-sided UV irradiation treatment are the same.
[0016] As an optional embodiment, the masking process includes masking using a masking ink and / or a mask plate.
[0017] As an optional embodiment, masking ink is used to perform masking treatment on two main surfaces opposite to the first area.
[0018] As an optional embodiment, the heat treatment includes a nucleation treatment and a crystallization treatment.
[0019] As an optional embodiment, the heating rate of the nucleation treatment is 1°C / min-10°C / min; and / or,
[0020] The temperature of the nucleation treatment is 450°C-590°C; and / or,
[0021] The time of the nucleation treatment is 30min-240min; and / or,
[0022] The heating rate of the crystallization treatment is 1°C / min-10°C / min; and / or,
[0023] The temperature of the crystallization treatment is higher than the temperature of the nucleation treatment, and the temperature of the crystallization treatment is 590° C.-800° C.; and / or,
[0024] The crystallization treatment time is 30min-360min.
[0025] As an optional embodiment, the composition of the substrate glass, in terms of the mass percentage of oxides, comprises: SiO2: 65.00%-75.00%, Al2O3: 5.00%-10.00%, Li2O: 7.00%-13.00%, Na2O: 2.00%-4.00%, K2O: 2.00%-4.00%, ZrO2: 5.00%-7.00%, X: 0.05%-0.80%, CeO2: 0.05%-0.18% and Sb2O3: 0.05%-0.51%;
[0026] wherein X is Ag (silver), Cu (copper), Au (gold), Bi (bismuth) and / or their respective oxides.
[0027] As an optional embodiment, the composition of the photosensitive glass, in terms of the mass percentage of oxides, comprises: SiO2: 65.00%-75.00%, Al2O3: 5.00%-10.00%, Li2O: 7.00%-13.00%, Na2O: 2.00%-4.00%, K2O: 2.00%-4.00%, ZrO2: 5.00%-7.00%, X: 0.05%-0.80%, CeO2: 0.05%-0.18% and Sb2O3: 0.05%-0.51%;
[0028] wherein X is Ag (silver), Cu (copper), Au (gold), Bi (bismuth) and / or their respective oxides.
[0029] As an optional embodiment, the composition of the photosensitive glass, measured by mass percentage of oxides, comprises:
[0030] The content of SiO2 is 73.02%, 69.80% or 72.40%; and / or,
[0031] The content of Al2O3 is 7.35%, 8.06% or 5.87%; and / or,
[0032] The content of Li2O is 7.33%, 9.77% or 9.80%; and / or,
[0033] The content of Na2O is 2.41%, 2.32% or 2.84%; and / or,
[0034] The K2O content is 2.15%, 3.34% or 2.34%; and / or,
[0035] The content of ZrO2 is 6.71%, 5.54% or 5.77%; and / or,
[0036] The content of Ag2O is 0.43%, 0.48% or 0.43%; and / or,
[0037] The content of CeO2 is 0.13%, 0.18% or 0.12%; and / or,
[0038] The content of Sb2O3 is 0.47%, 0.50% or 0.43%.
[0039] In a second aspect, a photosensitive glass is provided, which is prepared by the preparation method according to any embodiment of the first aspect.
[0040] As an optional embodiment, when the thickness of the photosensitive glass is 0.40-1.00 mm, the transmittance T1 of the exposure area of the photosensitive glass at a wavelength of 850 nm is 0.00%-5.00%, preferably 0.00%-3%; and / or,
[0041] When the thickness of the photosensitive glass is 0.40-1.00 mm, the transmittance T2 of the exposure area of the photosensitive glass at a wavelength of 550 nm is 0.00%-5.00%, preferably 0.00%-2%; and / or,
[0042] When the thickness of the photosensitive glass is 0.40-1.00 mm, the transmittance T3 of the non-exposed area of the photosensitive glass at a wavelength of 850 nm is above 90%, and / or,
[0043] When the thickness of the photosensitive glass is 0.40-1.00 mm, the transmittance T4 of the non-exposed area of the photosensitive glass at a wavelength of 550 nm is above 90%.
[0044] In a third aspect, a cover glass is provided, wherein the cover glass is made of the photosensitive glass according to any embodiment of the second aspect.
[0045] In a fourth aspect, an electronic device is provided, wherein the electronic device comprises the photosensitive glass according to any embodiment of the second aspect.
[0046] As an optional embodiment, the electronic device includes a housing assembled on the outside of the electronic device, and the housing includes the photosensitive glass as in any embodiment of the second aspect.
[0047] As an optional embodiment, the electronic device also includes a camera assembly located inside the housing, the housing includes a camera protection cover, the camera protection cover is covered on the camera assembly, and the camera protection cover includes a photosensitive glass as in any embodiment of the second aspect.
[0048] In a fifth aspect, there is provided a use of a photosensitive glass according to any embodiment of the second aspect for use as a component in a mobile phone, a smart watch, a wearable device, a camera module or a vehicle.
[0049] One or more of the above technical solutions provided by the present application have the following advantages compared with the prior art:
[0050] The present application improves the preparation process of photosensitive glass by controlling the double-sided masking treatment of the first area of the substrate glass and the non-masking treatment of the second area, and then irradiating the two main surfaces, thereby significantly improving the halo phenomenon of the photosensitive glass; in addition, by controlling the time and intensity of the radiation treatment, the appearance of hollow transparent areas in the exposure area of the photosensitive glass can be suppressed; thereby, photosensitive glass with good light-shielding performance in the exposure area can be prepared. BRIEF DESCRIPTION OF THE DRAWINGS
[0051] In order to more clearly illustrate the technical solutions of the embodiments of the present application, the drawings required for use in the embodiments will be briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present application and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without paying creative work.
[0052] Figure 1 A schematic diagram of the structure of a substrate glass after being masked with masking ink provided in an embodiment of the present application.
[0053] Figure 2 A schematic diagram of the structure of the photosensitive glass provided in an embodiment of the present application.
[0054] Figure 3 This is a schematic diagram of the rear structure of the electronic device mentioned in the implementation mode of this application.
[0055] Figure 4 This is a schematic diagram of the structure of a smart watch in which the electronic device mentioned in the implementation manner of the present application is a smart watch.
[0056] Figure 5 Part (b) is a schematic diagram of the production process provided in the embodiment of the present application, and part (a) is a schematic diagram of the production process provided in Comparative Example 1.
[0057] Figure 6 A schematic diagram of the production process provided for Comparative Example 2 of the present application.
[0058] Figure 7 This is a schematic cross-sectional view of the photosensitive glass after cutting provided in Example 3 of the present application.
[0059] Figure 8 This is a schematic cross-sectional view of the photosensitive glass after cutting provided in Comparative Example 1 of the present application.
[0060] Fig. 9 This is a schematic cross-sectional view of the photosensitive glass after cutting provided in Comparative Example 3 of the present application.
[0061] Fig.10 This is a halo image of the main surface observed using a polarizing microscope for Comparative Example 1 of the present application.
[0062] Figure markings: 11-light-transmitting area; 12-light-shielding area; 21-exposure area; 22-non-exposure area; 31-camera protection cover; 32-camera assembly; 33-back cover; 41-back cover of smart watch; 51-mask plate; 51-upper main surface mask; 61-upper main surface shielding ink; 62-lower main surface shielding ink; 71 / 81 / 91-exposure area cross section. DETAILED DESCRIPTION
[0063] The embodiments of the present application will be described in detail below in conjunction with the examples, but it will be appreciated by those skilled in the art that the following examples are only used to illustrate the present application and should not be considered as limiting the scope of the present application. In the examples, if specific conditions are not specified, they are carried out according to normal conditions or the conditions recommended by the manufacturer. If the manufacturer is not specified for the reagents or instruments used, they are all conventional products that can be purchased commercially.
[0064] The endpoints and any values of the range disclosed in this article are not limited to the precise range or value, and these ranges or values should be understood to include values close to these ranges or values. For numerical ranges, the endpoint values of each range, the endpoint values of each range and the individual point values, and the individual point values can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article. Among them, the terms "optional" and "optional" all refer to including or not including (or may have or may not have). "And / or" as referred to herein is inclusive, for example, "A and / or B" means only A, or only B, or both A and B.
[0065] Explanation of terms and test methods:
[0066] In the present application, the main surface refers to the surface with the largest surface area, such as the upper surface or the lower surface of a horizontally placed substrate glass.
[0067] In this application, the thickness of the glass is measured by a micrometer.
[0068] In this application, the size specifications of the glass sheets are tested using a two-dimensional measuring machine (instrument model: MiyuMY-YXCL-4030).
[0069] In the present application, an ultraviolet-visible spectrophotometer is used to test the transmittance of the exposure area and the non-exposure area of the photosensitive glass. The ultraviolet-visible spectrophotometer used in the test of the present application is Shimadzu UV-2000 ultraviolet-visible spectrophotometer.
[0070] The specific method for testing the exposure area of the photosensitive glass is: first use a fixture that is consistent with the shape and size of the photosensitive glass, and the same area corresponding to the exposure area of the photosensitive glass is a hollow area and the non-exposure area corresponding to the photosensitive glass is an opaque area, and the connection position between the hollow area and the opaque area is an opaque fixture as a blank sample for test calibration, and then cut the exposure area of the photosensitive glass into samples that coincide with the shape of the hollow area of the fixture and put them into the hollow area of the aforementioned fixture for testing to obtain the transmittance. Use an ultraviolet-visible spectrophotometer to test the transmittance of the exposure area of 5 pieces of photosensitive glass in the same batch to light of different wavelengths, and then take the average value, which is recorded as the transmittance result of the exposure area of the photosensitive glass under the wavelength of light.
[0071] In addition, the transmittance of the non-exposed area of 5 pieces of photosensitive glass in the same batch to light of different wavelengths was tested using an ultraviolet-visible spectrophotometer. The average value of the transmittance of the non-exposed area of the 5 pieces of photosensitive glass under light of different wavelengths was taken as the transmittance result of the non-exposed area of the photosensitive glass under the light of the wavelength.
[0072] In this application, the obvious halo phenomenon at the edge of the exposure area of the photosensitive glass is called halo edge, see Fig.10 .
[0073] In some embodiments of the present application, a method for preparing a photosensitive glass is provided, comprising:
[0074] obtaining substrate glass;
[0075] The substrate glass comprises a first region and a second region, two main surfaces opposite to each other in the first region are masked, and the second region is not masked, so as to obtain a substrate glass having the same structure after double-sided masking;
[0076] The two main surfaces of the substrate glass with the same structure after double-sided masking are subjected to radiation treatment and then heat treatment to obtain a photosensitive glass with a non-exposed area and an exposed area; wherein the non-exposed area corresponds to the first area, and the exposed area corresponds to the second area. In the present application, the substrate glass with the same structure after double-sided masking means that the structure of the substrate glass after double-sided masking is the same.
[0077] In the present application, the substrate glass can be prepared by a molding method in the prior art, and the present application has no limitation on this. For example, the molding method of the substrate glass can include but is not limited to float, overflow, rolling or casting processes. For example, the substrate glass can be obtained by uniformly mixing the components according to the formula, melting and molding, cooling and annealing.
[0078] Exemplarily, each raw material (conventional industrial raw material) is configured according to the formula ratio, a clarifier is added, and then mixed for a period of time to obtain a uniform raw material mixture. The raw material mixture is placed in a platinum crucible, heated to 1250°C to 1680°C, preferably the melting temperature is 1480°C to 1680°C, and preferably kept warm for 3 to 12 hours under this temperature condition, and then poured into a molding mold for cooling and molding, preferably cooled to 750°C to 1000°C, and then placed in an annealing furnace for annealing treatment, preferably the annealing temperature is 400°C to 650°C, and the annealing time is preferably 10 to 48 hours; then cooled to room temperature with the furnace, the substrate glass can be obtained. Those skilled in the art can select the type and amount of clarifier according to needs, and they do not need to pay creative labor. Further, the clarifier may include but is not limited to one or more of sodium chloride, tin oxide, antimony oxide or arsenic oxide, and the amount of clarifier added may be 0wt%-1wt% of the total amount of each raw material.
[0079] In some embodiments of the present application, the radiation treatment comprises ultraviolet irradiation treatment.
[0080] In the present application, the intensity and duration of the ultraviolet irradiation treatment are not particularly limited, and depend on the composition of the photosensitive glass and the opacity of the exposure area, as long as the photosensitive glass meets the requirements of the present application. In some embodiments of the present application, the wavelength of the ultraviolet irradiation treatment is 300nm-320nm, and the intensity of the ultraviolet irradiation treatment is 20mw / cm 2 -360mw / cm 2 The UV irradiation treatment time is 5min-60min.
[0081] In some embodiments of the present application, the conditions of the double-sided radiation treatment are the same.
[0082] In some embodiments of the present application, the conditions for double-sided UV irradiation treatment are the same.
[0083] In some embodiments of the present application, the wavelength of the ultraviolet irradiation treatment is 300nm, 302nm, 305nm, 308nm, 310nm, 312nm, 315nm, 317nm or 320nm, or a value within a numerical range consisting of any two of the above specific values as endpoints. In some embodiments of the present application, the intensity of the ultraviolet irradiation treatment is 20mw / cm 2 、40mw / cm 2 、60mw / cm 2 、80mw / cm 2 、100mw / cm 2 、120mw / cm 2 、150mw / cm 2 、180mw / cm2 、200mw / cm 2 、210mw / cm 2 、220mw / cm 2 、230mw / cm 2 、240mw / cm 2 、250mw / cm 2 、260mw / cm 2 、270mw / cm 2 、280mw / cm 2 、290mw / cm 2 、300mw / cm 2 、310mw / cm 2 、320mw / cm 2 、330mw / cm 2 、340mw / cm 2 、350mw / cm 2 or 360mw / cm 2 , or a value within a numerical range consisting of any two of the above specific values as endpoints. In some embodiments of the present application, the time of ultraviolet irradiation treatment is 5min, 10min, 15min, 20min, 25min, 30min, 35min, 40min, 45min, 50min, 55min or 60min, or a value within a numerical range consisting of any two of the above specific values as endpoints. It should be understood that in a specific embodiment, any of the above ranges can be combined with any other ranges, as long as the photosensitive glass with the desired performance of the present application can be obtained.
[0084] In some embodiments of the present application, the masking process includes masking using masking ink and / or a mask plate.
[0085] For example, the schematic diagram of the structure of the substrate glass after masking with masking ink is as follows: Figure 1 The composite circular hole has a light-transmitting area 11 of the inner diameter and a light-shielding area 12 outside the inner diameter; the structural schematic diagram of the corresponding photosensitive glass is as shown in Figure 2 The position corresponding to the light-transmitting region 11 forms an exposure region 21, and the position corresponding to the light-shielding region 12 forms a non-exposure region 22. In some embodiments of the present application, the heat treatment includes a nucleation treatment and a crystallization treatment.
[0086] In some embodiments of the present application, the temperature of the nucleation treatment may be 450°C-590°C. In some embodiments of the present application, the temperature of the nucleation treatment may be 450°C, 480°C, 500°C, 520°C, 540°C, 550°C, 560°C, 570°C, 580°C or 590°C, or a value within the numerical range consisting of any two of the above specific values as endpoints. In some embodiments of the present application, the time of the nucleation treatment is 30min-240min. In some embodiments of the present application, the time of the nucleation treatment may be 30min, 45min, 50min, 55min, 60min, 90min, 100min, 120min, 140min, 150min, 160min, 170min, 180min, 190min, 200min, 220min or 240min, or a value within the numerical range consisting of any two of the above specific values as endpoints. In some embodiments of the present application, the heating rate of the nucleation treatment is 1°C / min-10°C / min. In some embodiments of the present application, the time of the nucleation treatment can be 1°C / min, 2°C / min, 3°C / min, 4°C / min, 5°C / min, 6°C / min, 7°C / min, 8°C / min, 9°C / min or 10°C / min, or a value within a numerical range consisting of any two of the above specific values as endpoints. It should be understood that in a specific embodiment, any of the above ranges can be combined with any other ranges, as long as the photosensitive glass with the performance required by the present application can be obtained.
[0087] In some embodiments of the present application, the temperature of the crystallization treatment is 590-800°C and / or the time of the crystallization treatment is 30-360min. In some embodiments of the present application, the temperature of the crystallization treatment can be 590°C, 600°C, 620°C, 640°C, 650°C, 660°C, 670°C, 680°C, 700°C, 720°C, 740°C, 760°C, 780°C or 800°C, or a value within the numerical range consisting of any two of the above specific values as endpoints. In some embodiments of the present application, the time of the crystallization treatment can be 30min, 50min, 60min, 80min, 90min, 100min, 120min, 140min, 160min, 180min, 200min, 240min, 260min, 280min, 300min, 320min or 360min, or a value within the numerical range consisting of any two of the above specific values as endpoints. It should be understood that in embodiments, any of the above ranges may be combined with any other ranges.
[0088] Before and / or after the heat treatment, those skilled in the art may also perform other conventional steps to obtain a photosensitive glass sample that meets the required specifications or requirements, such as shaping, cutting (such as cutting with a multi-wire cutting machine), CNC machining (computer numerical control, i.e., CNC machine tools), thinning, or polishing. In the present application, there is no limitation on the size of the substrate glass or photosensitive glass, such as 50 mm×50 mm×1.0 mm, 300 mm×120 mm×0.7 mm, etc.
[0089] In some embodiments of the present application, a photosensitive glass is provided, which is prepared by the above preparation method.
[0090] In some embodiments of the present application, the composition of the substrate glass is the same or substantially the same as the composition of the photosensitive glass in terms of mass percentage of oxides.
[0091] In some embodiments of the present application, the substrate glass or the photosensitive glass comprises the following components, in terms of the mass percentage of oxides: SiO2: 65.00%-75.00%; Al2O3: 5.00%-10.00%; Li2O: 7.00%-13.00%; Na2O: 2.00%-4.00%; K2O: 2.00%-4.00%; ZrO2: 5.00%-7.00%; CeO2: 0.05%-0.18%; Sb2O3: 0.05%-0.51%; and X: 0.05%-0.80%;
[0092] Wherein X is Ag (silver), Cu (copper), Au (gold), Bi (bismuth) and / or their respective oxides. It should be noted that X is Ag, Cu, Au, Bi and / or their respective oxides means that X is at least one of Ag, Cu, Au, Bi, Ag2O, CuO, Au2O3, and Bi2O3.
[0093] In the present application, SiO2 is a glass-forming oxide, which forms an irregular continuous network with the structural unit of silicon-oxygen tetrahedron, and is the skeleton of the glass. In some embodiments of the present application, the content of SiO2 in the substrate glass or photosensitive glass is 65.00%-75.00% by mass percentage of the oxide; preferably 65.00% to 73.00%. In some embodiments of the present application, the content of SiO2 in the substrate glass or photosensitive glass can be 65.00%, 66.00%, 67.00%, 68.00%, 69.00%, 70.00%, 71.00%, 72.00%, 73.00%, 74.00% or 75.00% by mass percentage of the oxide, or a value within the numerical range formed by any two of the above specific values as endpoints. It should be understood that in the embodiment, any of the above ranges can be combined with any other ranges.
[0094] In some embodiments of the present application, the Al2O3 content of the substrate glass or photosensitive glass is in the range of 5.00%-10.00% by mass percentage of oxide. In some embodiments of the present application, the Al2O3 content of the substrate glass or photosensitive glass can be 5.00%, 6.00%, 7.00%, 8.00%, 9.00% or 10.00% by mass percentage of oxide, or a value within the numerical range formed by any two of the above specific values as endpoints. It should be understood that in the embodiments, any of the above ranges can be combined with any other ranges.
[0095] In some embodiments of the present application, the content of Li2O in the substrate glass or photosensitive glass is 7.00%-13.00% by mass percentage of oxide. In some embodiments of the present application, the content of Li2O in the substrate glass or photosensitive glass can be 7.00%, 7.50%, 8.00%, 8.50%, 9.00%, 10.00%, 10.50%, 11.00%, 11.50%, 12.00%, 12.50% or 13.00% by mass percentage of oxide, or a value within the numerical range consisting of any two of the above specific values as endpoints. It should be understood that in the embodiment, any of the above ranges can be combined with any other ranges.
[0096] In some embodiments of the present application, the Na2O content of the substrate glass or photosensitive glass is 2.00%-4.00% by mass percentage of oxide. In some embodiments of the present application, the Na2O content of the substrate glass or photosensitive glass can be 2.00%, 2.50%, 3.00%, 3.50% or 4.00% by mass percentage of oxide, or a value within a numerical range consisting of any two of the above specific values as endpoints. It should be understood that in the embodiments, any of the above ranges can be combined with any other ranges.
[0097] In some embodiments of the present application, the K2O content of the substrate glass or photosensitive glass is 2.00%-4.00% by mass percentage of oxide. In some embodiments of the present application, the K2O content of the substrate glass or photosensitive glass can be 2.00%, 2.50%, 3.00%, 3.50% or 4.00% by mass percentage of oxide, or a value within a numerical range consisting of any two of the above specific values as endpoints. It should be understood that in the embodiments, any of the above ranges can be combined with any other ranges.
[0098] In some embodiments of the present application, the content of ZrO2 in the substrate glass or photosensitive glass is 5.00%-7.00% by mass percentage of oxide. In some embodiments of the present application, the content of ZrO2 in the substrate glass or photosensitive glass can be 5.00%, 5.50%, 6.00%, 6.50% or 7.00% by mass percentage of oxide, or a value within a numerical range consisting of any two of the above specific values as endpoints. It should be understood that in the embodiments, any of the above ranges can be combined with any other ranges.
[0099] In some embodiments of the present application, the content of X in the substrate glass or photosensitive glass is 0.05%-0.80% by mass percentage of oxide; X is Ag, Cu, Au, Bi and / or their respective oxides. In some embodiments of the present application, the content of X in the substrate glass or photosensitive glass can be 0.05%, 0.10%, 0.15%, 0.20%, 0.25%, 0.30%, 0.40%, 0.50%, 0.60%, 0.70% or 0.80% by mass percentage of oxide; or a value within the numerical range formed by any two of the above specific values as endpoints. It should be understood that in the embodiments, any of the above ranges can be combined with any other ranges.
[0100] In some embodiments of the present application, the CeO2 content of the substrate glass or photosensitive glass is 0.05%-0.18% by mass percentage of the oxide. In some embodiments of the present application, the X content of the substrate glass or photosensitive glass can be 0.05%, 0.10%, 0.15% or 0.18% by mass percentage of the oxide; or a value within a numerical range consisting of any two of the above specific values as endpoints. It should be understood that in the embodiments, any of the above ranges can be combined with any other ranges.
[0101] In some embodiments of the present application, the Sb2O3 content of the substrate glass or photosensitive glass is 0.05%-0.51% by mass percentage of the oxide. In some embodiments of the present application, the Sb2O3 content of the substrate glass or photosensitive glass can be 0.05%, 0.10%, 0.15%, 0.20%, 0.25%, 0.30%, 0.35%, 0.40%, 0.45%, 0.50% or 0.51% by mass percentage of the oxide; or a value within the numerical range formed by any two of the above specific values as endpoints. It should be understood that in the embodiments, any of the above ranges can be combined with any other ranges.
[0102] In some embodiments of the present application, when the thickness of the photosensitive glass is 0.40-1.00 mm, the transmittance T1 of the exposure area of the photosensitive glass at a wavelength of 850 nm is 0.00%-5.00%, and the transmittance T1 is preferably 0.00%-3.00%. In some embodiments of the present application, when the thickness of the photosensitive glass is 0.40-1.00 mm, the transmittance T1 of the exposure area of the photosensitive glass at a wavelength of 850 nm can be 0.00%, 0.21%, 0.50%, 0.70%, 0.90%, 1.00%, 1.25%, 1.35%, 1.50%, 1.70%, 2.00%, 2.51%, 3.00%, 3.50%, 4.00%, 4.50%, 4.80% or 5.00%; or a value within a numerical range consisting of any two of the above specific values as endpoints. It should be understood that in embodiments, any of the above ranges may be combined with any other ranges.
[0103] In some embodiments of the present application, when the thickness of the photosensitive glass is 0.40-1.00 mm, the transmittance T2 of the exposure area of the photosensitive glass at a wavelength of 550 nm is 0.00%-5.00%, and the transmittance T2 is preferably 0.00%-2.00%. In some embodiments of the present application, when the thickness of the photosensitive glass is 0.40-1.00 mm, the transmittance T2 of the exposure area of the photosensitive glass at a wavelength of 550 nm can be 0.00%, 0.20%, 0.50%, 0.70%, 0.90%, 1.00%, 1.35%, 1.50%, 1.70%, 2.00%, 2.50%, 3.00%, 3.50%, 4.00%, 4.20%, 4.50%, 4.90% or 5.00; or a value within a numerical range consisting of any two of the above specific values as endpoints. It should be understood that in embodiments, any of the above ranges may be combined with any other ranges.
[0104] In some embodiments of the present application, when the thickness of the photosensitive glass is 0.40-1.00 mm, the transmittance T3 of the non-exposed area of the photosensitive glass at a wavelength of 850 nm is above 90%. In some embodiments of the present application, when the thickness of the photosensitive glass is 0.40-1.00 mm, the transmittance T3 of the non-exposed area of the photosensitive glass at a wavelength of 550 nm can be 90.00%, 90.50%, 91.00%, 91.47%, 91.49%, 91.66%, 92.00%, 91.75%, 91.39%, 92.08% or 95.00%; or a value within the numerical range formed by any two of the above specific values as endpoints. It should be understood that in the embodiments, any of the above ranges can be combined with any other ranges.
[0105] In some embodiments of the present application, when the thickness of the photosensitive glass is 0.40-1.00 mm, the transmittance T4 of the non-exposed area of the photosensitive glass at a wavelength of 550 nm is above 90%. In some embodiments of the present application, when the thickness of the photosensitive glass is 0.40-1.00 mm, the transmittance T4 of the non-exposed area of the photosensitive glass at a wavelength of 550 nm can be 90.00%, 90.50%, 91.00%, 91.47%, 91.49%, 91.66%, 92.00%, 91.75%, 91.39%, 92.08%, 93.00% or 95.00%, or a value within the numerical range formed by any two of the above specific values as endpoints. It should be understood that in the embodiments, any of the above ranges can be combined with any other ranges.
[0106] In some embodiments of the present application, the thickness of the photosensitive glass of the present application is not particularly limited, for example, it can be 0.4-2.0 mm; preferably 0.4-1.0 mm. In some embodiments of the present invention, the thickness of the photosensitive glass of the present application can be 0.4 mm, 0.5 mm, 0.6 mm, 0.7 mm, 0.8 mm, 0.9 mm, 1.0 mm, 1.1 mm, 1.2 mm, 1.3 mm, 1.4 mm, 1.5 mm or 2.0 mm, or a value within a numerical range consisting of any two of the above specific values as endpoints. It should be understood that in the embodiments, any of the above ranges can be combined with any other ranges.
[0107] In a second aspect, a tempered glass is provided. The tempered glass is obtained by chemically tempering the photosensitive glass prepared by the above preparation method.
[0108] In the present application, chemical strengthening can be performed by a conventionally known method; for example, chemical strengthening includes single-step chemical strengthening or multi-step chemical strengthening.
[0109] In some embodiments of the present application, single-step chemical strengthening uses a salt bath containing NaNO3; preferably, the content of NaNO3 in the salt bath is 30wt%-100wt%; preferably, single-step chemical strengthening uses a mixed salt bath containing NaNO3 and KNO3, preferably, the content of KNO3 in the mixed salt bath is 80-100wt%, and the content of NaNO3 is 0-20wt%.
[0110] In some embodiments of the present application, the temperature of the single-step chemical strengthening is 380° C.-480° C.; preferably, the ion exchange time of the single-step chemical strengthening is 5 h-10 h.
[0111] In some embodiments of the present application, multi-step chemical strengthening includes two-step chemical strengthening, wherein the first step of chemical strengthening uses a salt bath containing NaNO3, preferably with a NaNO3 content of 30wt%-100wt%; the second step of chemical strengthening uses a salt bath containing KNO3, preferably with a KNO3 content of 60wt%-100wt%.
[0112] In some embodiments of the present application, the temperature of the first step chemical strengthening is 380°C-480°C, and the time of the first step chemical strengthening is preferably 3h-10h; and / or, the temperature of the second step chemical strengthening is 380°C-480°C, and the time of the second step chemical strengthening is preferably 1h-5h.
[0113] The photosensitive glass and tempered glass provided in the present application can be used in electronic devices, including but not limited to mobile phones, tablet computers, handheld game consoles, portable digital devices (such as digital cameras), smart homes, smart wearables (such as smart bracelets, smart watches, smart glasses), and can also be used in vehicles, aircraft or aircraft, and can also be used in any glass devices of required photosensitive glass. For example, it can be used for the back cover glass of mobile phones, the back cover glass of smart watches, etc.; for example, it can be used for the windshield of vehicles, aircraft or aircraft, such as the front windshield or the side windshield. Exemplarily, the photosensitive glass provided in the present application can be used to manufacture glass devices. The glass devices referred to here can be regular or irregular, and those skilled in the art can manufacture them according to needs.
[0114] For example, the photosensitive glass provided in the present application can be used to manufacture cover glass, and the cover glass can be a back cover or camera protection cover of an electronic device such as a mobile phone. For example, the photosensitive glass with excellent performance provided in the present application can be used in electronic devices. Figure 3 and Figure 4 In some embodiments of the present application, an electronic device is provided, which may be a mobile phone (such as Figure 3 As shown, the photosensitive glass can be used as the back cover of a mobile phone), a tablet computer, a smart wearable device (such as Figure 4 As shown, the photosensitive glass can be used as the back cover 41 of a smart watch and other electronic products, and the electronic device includes the photosensitive glass. In some embodiments of the present application, such as Figure 3 As shown, the electronic device also includes a camera assembly 32 located inside the housing, and the housing may include a camera protection cover 31, the camera protection cover 31 is covered on the camera assembly 32 to protect the camera assembly 32, and the camera protection cover 31 adopts the aforementioned photosensitive glass. In some embodiments of the present application, the camera protection cover 31 may be partially made of the aforementioned photosensitive glass, or may be made of the aforementioned photosensitive glass in its entirety. In some embodiments of the present application, the setting position of the camera protection cover 31 is determined according to the setting position of the camera assembly 32, and may be located on the front side of the electronic device, or may be located on the rear side of the electronic device. In some embodiments of the present application, the camera protection cover 31 may be a separate structure from the back cover 33. In other embodiments of the present application, the camera protection cover 31 may also be an integrated structure with the back cover 33.
[0115] The technical solution of the present application is further described in detail below in conjunction with the embodiments. The embodiments of the present application described in detail below are exemplary and are only used to explain the present application, and cannot be understood as limiting the present application.
[0116] Example 1
[0117] A method for preparing photosensitive glass comprises the following steps:
[0118] Step 1: Prepare the raw materials (conventional industrial raw materials) according to the proportions of the components in Table 1, the total mass of the prepared raw materials is 2000 g, and add 10 g of clarifier sodium chloride to the prepared raw materials, and then mix them in a V-type mixer for 30 minutes to obtain a uniform raw material mixture;
[0119] The raw material mixture is transferred to a melting furnace and then melted at 1450°C. The melt is stirred with a platinum stirring rod for 10 hours, and then pulled into shape and continuously drawn into glass bricks of the required specifications. The glass bricks are quickly placed in an annealing furnace at 500°C for 6 hours, and then naturally cooled to room temperature to obtain the base glass bricks;
[0120] The obtained substrate glass bricks are cut, CNC processed (the CNC equipment model used in this application is: RCG500S), and polished in turn for cold processing, and substrate glass with a size of 50mm×50mm×1.0mm can be obtained;
[0121] Step 2: ultrasonically clean the substrate glass obtained above in deionized water, anhydrous ethanol, propanol and deionized water for 10 minutes, and then dry it in a drying oven;
[0122] After cleaning, the substrate glass is coated with masking ink on the same local area of the upper and lower main surfaces. Figure 1 As shown, the black area is the masked area; then the double-sided irradiation treatment was carried out under parallel ultraviolet light with a wavelength of 310nm (UVHX800*850 drawer type) for a total of 25min, and the intensity of the irradiation treatment was 120mw / cm 2 ;
[0123] The UV-irradiated glass was heat-treated according to the heat treatment process in Table 1 to obtain photosensitive glass; the heat treatment included nucleation treatment and crystallization treatment; the heating rates of nucleation treatment and crystallization treatment were both 10°C / min; the photosensitive glass was subjected to cold processing such as laser cutting, splitting, polishing, chamfering, etc., to obtain photosensitive glass with a size of φ30*1.0mm, such as Figure 2 As shown in the actual picture.
[0124] Example 2
[0125] The process was carried out with reference to Example 1, except that the raw material composition, masking treatment method and UV irradiation treatment time of Example 2 were different as shown in Table 1.
[0126] Example 3
[0127] The process was carried out with reference to Example 1, except that the raw material composition and the time of ultraviolet irradiation treatment in Example 3 were different as shown in Table 1.
[0128] Example 4
[0129] The process is carried out with reference to Example 1, except that the raw material composition and the process parameters of ultraviolet irradiation of Example 4 are different as shown in Table 1.
[0130] Comparative Example 1-2
[0131] The process is carried out with reference to Example 3, except that the masking treatment method and the UV irradiation treatment area of Comparative Examples 1-2 are different as shown in Table 1-2.
[0132] Comparative Examples 3-4
[0133] The process is carried out with reference to Example 3, except that the process parameters of ultraviolet irradiation of Comparative Examples 3-4 are different as shown in Table 1-2.
[0134] Among them, the process flow charts of Examples 1-4 and Comparative Examples 3-4 are as follows Figure 5 As shown in part (b), the process flow chart of Comparative Example 1 is as follows Figure 5 As shown in part (a), the process flow chart of Comparative Example 2 is as follows Figure 6 As shown, 61 represents the upper main surface shielding ink; 62 represents the lower main surface shielding ink, and 51 represents the upper main surface mask.
[0135] Relevant performance tests were performed on Examples 1-4 and Comparative Examples 1-4, and the results are shown in Table 1-2.
[0136] Example 3, Comparative Example 1, and Comparative Example 3 were cut into cross sections using a laser cutting machine, wherein the cross-sectional schematic diagram of Example 3 is as shown in FIG. Figure 7 As shown, the cross section 71 of the exposure area of Example 3 is solid and the outline is a micro-arc; the cross-sectional schematic diagram of Comparative Example 1 is as shown Figure 8 As shown; the exposure area cross section 81 of comparative example 1 is solid but its outline is trapezoidal; the cross-sectional schematic diagram of comparative example 3 is as shown Fig. 9 As shown, the cross section 91 of the exposure area of Comparative Example 3 is partially hollow but the outline of its solid part is a slight arc.
[0137] Fig.10 The halo image of the main surface of Comparative Example 1 of the present application observed using a polarizing microscope shows that haloing occurs in Comparative Example 1.
[0138] Table 1
[0139]
[0140]
[0141] Table 2
[0142]
[0143]
[0144] According to the comparison between Example 3 and Comparative Examples 1-4, it can be seen that the present application performs ultraviolet irradiation treatment on the two main surfaces to solve the problem of haloing at the edges of the exposure area of the photosensitive glass; in addition, the present application can adjust the shading performance of the exposure area of the photosensitive glass by controlling the conditions of the ultraviolet irradiation treatment.
[0145] The above are only specific embodiments of the present application and are not intended to limit the present application. For those skilled in the art, the present application may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present application shall be included in the protection scope of the present application.
Claims
1. A method for preparing photosensitive glass, characterized in that: include: obtaining substrate glass; The substrate glass comprises a first region and a second region, two main surfaces opposite to each other in the first region are masked, and the second region is not masked, so as to obtain a substrate glass having the same structure after double-sided masking; The two main surfaces of the double-sided masked substrate glass with the same structure are subjected to radiation treatment and then heat treatment to obtain a photosensitive glass with a non-exposed area and an exposed area; wherein the non-exposed area corresponds to the first area, and the exposed area corresponds to the second area.
2. The preparation method according to claim 1, characterized in that: The radiation treatment method includes ultraviolet irradiation treatment.
3. The preparation method according to claim 2, characterized in that: The wavelength of the ultraviolet irradiation treatment is 300nm-320nm, and the intensity of the ultraviolet irradiation treatment is 20mw / cm 2 -360mw / cm 2 The ultraviolet irradiation treatment time is 5min-60min.
4. The preparation method according to any one of claims 1 to 3, characterized in that The masking process includes masking using masking ink and / or a mask plate.
5. The preparation method according to any one of claims 1 to 4, characterized in that: The heat treatment includes a nucleation treatment and a crystallization treatment.
6. The preparation method according to claim 5, characterized in that: The heating rate of the nucleation treatment is 1°C / min-10°C / min; and / or, The temperature of the nucleation treatment is 450°C-590°C; and / or, The time of the nucleation treatment is 30 min-240 min; and / or, The heating rate of the crystallization treatment is 1°C / min-10°C / min; and / or, The temperature of the crystallization treatment is higher than the temperature of the nucleation treatment, and the temperature of the crystallization treatment is 590° C.-800° C.; and / or, The crystallization treatment time is 30 min-360 min.
7. The preparation method according to any one of claims 1 to 6, characterized in that The composition of the substrate glass, in terms of percentage by mass of oxides, comprises: SiO2: 65.00%-75.00%, Al2O3: 5.00%-10.00%, Li2O: 7.00%-13.00%, Na2O: 2.00%-4.00%, K2O: 2.00%-4.00%, ZrO2: 5.00%-7.00%, X: 0.05%-0.80%, CeO2: 0.05%-0.18% and Sb2O3: 0.05%-0.51%; wherein X is Ag, Cu, Au, Bi and / or their respective oxides.
8. The preparation method according to any one of claims 1 to 7, characterized in that: The composition of the photosensitive glass, in terms of percentage by mass of oxides, comprises: SiO2: 65.00%-75.00%, Al2O3: 5.00%-10.00%, Li2O: 7.00%-13.00%, Na2O: 2.00%-4.00%, K2O: 2.00%-4.00%, ZrO2: 5.00%-7.00%, X: 0.05%-0.80%, CeO2: 0.05%-0.18% and Sb2O3: 0.05%-0.51%; wherein X is Ag, Cu, Au, Bi and / or their respective oxides.
9. A photosensitive glass, characterized in that: Prepared by the preparation method described in any one of claims 1 to 8.
10. The photosensitive glass according to claim 9, characterized in that: When the thickness of the photosensitive glass is 0.40-1.00 mm, the transmittance T1 of the exposure area of the photosensitive glass at a wavelength of 850 nm is 0.00%-5.00%, preferably 0.00%-3.00%; and / or, When the thickness of the photosensitive glass is 0.40-1.00 mm, the transmittance T2 of the exposure area of the photosensitive glass at a wavelength of 550 nm is 0.00%-5.00%, preferably the transmittance T2 is 0.00%-2.00%; and / or, When the thickness of the photosensitive glass is 0.40-1.00 mm, the transmittance T3 of the non-exposed area of the photosensitive glass at a wavelength of 850 nm is above 90%; and / or, When the thickness of the photosensitive glass is 0.40-1.00 mm, the transmittance T4 of the non-exposed area of the photosensitive glass at a wavelength of 550 nm is above 90%.
11. A cover glass, characterized in that: The cover glass comprises the photosensitive glass according to any one of claims 9 to 10.
12. An electronic device, characterized in that: The electronic device comprises the photosensitive glass according to any one of claims 9 to 10.
13. The electronic device according to claim 12, characterized in that: The electronic device comprises a housing, and the housing comprises the photosensitive glass according to any one of claims 9-10.
14. The electronic device according to claim 13, characterized in that: The electronic device further comprises a camera assembly, the housing comprises a camera protection cover, the camera protection cover is disposed on the camera assembly, and the camera protection cover comprises the photosensitive glass described in any one of claims 9-10.
15. Use of the photosensitive glass according to any one of claims 9 to 10 in components of mobile phones, smart watches, wearable devices, camera modules or vehicles.
Citation Information
Patent Citations
Sensitized photo-sensitive glass and manufacture method therefor
CN106167355A
Machining of fusion-drawn glass laminate structures containing a photomachinable layer
CN108046614A
Glass ceramics, glass ceramic product and manufacturing method thereof
CN113754290A
Cited By
Method for preparing photosensitive glass and use of photosensitive glass
WO2026017048A1