Single crystal glass ceramic and preparation method thereof, and glass powder and preparation method thereof
By using CaO-B2O3-SiO2 microcrystalline glass system and modifier ions in LTCC substrates, the crystallization kinetics of β-CaSiO3 are regulated and single crystal glass ceramics are prepared, which solves the problem of high dielectric constant and low bending strength in the existing technology. The problem of the reduction of dielectric constant and mechanical strength is achieved, and it is suitable for high-frequency communication technology.
Patent Information
- Application Number
- CN202411133831.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-16
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2044-08-16
AI Technical Summary
In high-frequency communication technology, existing LTCC substrate materials are difficult to meet the requirements of low dielectric constant, low dielectric loss and high flexural strength at the same time, especially in terms of sintering temperature and mechanical properties.
Using CaO-B2O3-SiO2 microcrystalline glass system, single crystal glass ceramics with highly ordered layered structures are prepared by regulating the crystallization kinetics of β-CaSiO3 and doping modifier ions, so as to achieve reduced dielectric constant and mechanical Increased intensity. The specific steps include mixing the glass powder with an organic solvent, casting and sintering, controlling the sintering temperature and rate to obtain a single crystal glass ceramic.
It realizes that the dielectric constant and dielectric loss of single crystal glass ceramics are reduced at lower sintering temperatures, while improving the bending strength, meeting the performance requirements of LTCC substrates in high-frequency communication.
Smart Images

Figure CN118930056A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of low-temperature co-fired ceramics, and in particular relates to a method for preparing single-crystal glass ceramics, a method for preparing glass powder, a glass powder, and a single-crystal glass ceramic. Background Art
[0002] Low Temperature Co-fired Ceramic (LTCC) technology is widely used in various electronic components due to its advantages of miniaturization, integration, and low cost. With the rapid development of high-frequency communication technology, the requirements for the comprehensive performance of LTCC materials are constantly increasing, and the contradictory relationship between the various properties of LTCC has become increasingly prominent.
[0003] The dielectric constant (K value) of existing low-dielectric-constant LTCC substrates is usually in the range of 5 to 8, and correspondingly, its bending strength is generally around 170 MPa. However, in the context of miniaturization and integration of high-frequency communication technology, LTCC substrates need to have certain bending and compression resistance to face high-load packaging environments. In addition, since the melting point of silver (Ag) is 961°C, the densification temperature of LTCC substrates is usually less than 900°C.
[0004] At present, the existing LTCC substrate materials are mainly microcrystalline glass systems and glass / ceramic composite systems. Among them, due to the advantages of low cost and high strength of Al2O3, the most commonly used glass / Al2O3 composite material in the glass / ceramic composite system. The prior art (for example, Chinese invention patent CN113372005A) uses lead borosilicate glass to pre-treat the surface of α-alumina to improve the interface contact strength between glass and alumina. Specifically, the mechanical properties of lead borosilicate glass are improved by doping α-alumina with high mechanical strength (300MPa) into lead borosilicate low-melting point glass (sintering aid). However, the high dielectric constant of alumina (9.8@10MHz) will cause the dielectric constant of the material to be too high. Moreover, lead glass is not in line with environmentally friendly development. In addition, in the microcrystalline glass system, a combination of multiple glasses is usually used to coordinate the comprehensive performance of LTCC materials. However, how to use traditional formulas and simple processes to meet the appropriate sintering temperature, low dielectric constant, low dielectric loss and high bending strength required for LTCC substrates is still a problem that needs to be solved urgently in this field.
[0005] In order to overcome the above-mentioned defects of the prior art, the art is in urgent need of a single crystal glass ceramic and a preparation method thereof, which can balance and improve the sintering temperature, dielectric constant, dielectric loss and bending strength of the LTCC substrate material. Summary of the invention
[0006] A brief summary of one or more aspects is given below to provide a basic understanding of these aspects. This summary is not an exhaustive overview of all conceived aspects, and is neither intended to identify the key or critical elements of all aspects nor to define the scope of any or all aspects. Its only purpose is to give some concepts of one or more aspects in a simplified form as a prelude to a more detailed description that will be given later.
[0007] In order to overcome the above-mentioned defects of the prior art, the present invention provides a method for preparing a single crystal glass ceramic, a method for preparing a glass powder, a glass powder, and a single crystal glass ceramic, which can balance and improve the sintering temperature, dielectric constant, dielectric loss, and flexural strength of LTCC substrate materials.
[0008] Specifically, the preparation method of the above-mentioned single crystal glass ceramic provided in the first aspect of the present invention comprises the steps of: mixing glass powder with an organic solvent, obtaining a green ceramic tape by tape casting, laminating and pressing the green ceramic tape, and then sintering it in a sintering furnace, wherein the glass powder comprises 41.68-47.2 mol% of CaO, 12.7-15.01 mol% of B2O3, 37.77-40.97 mol% of SiO2 and doped modifier ions in molar percentage. The modifier ions include one or more of Al2O3, Ta2O5, Nb2O5, La2O3, CeO2, CuO, and BaO, and the silicon-calcium ratio of the glass powder is 0.9-1; the sintering process includes: heating to 500-550°C at a rate of 1-2°C / min, keeping warm for 4-5 hours, and then debinding; heating to 860-880°C at a rate of 3-5°C / min, keeping warm for 10-30 minutes; and cooling to obtain single crystal glass ceramics.
[0009] Preferably, in an embodiment of the present invention, the sintering shrinkage of the glass powder is 15% to 18%.
[0010] Preferably, in one embodiment of the present invention, the doped modifier ion is Al2O3, and the glass powder comprises 0.34-3 mol% of the Al2O3 in terms of molar percentage.
[0011] Preferably, in one embodiment of the present invention, the preparation of the glass powder includes the steps of: preparing raw materials and fully mixing them, the raw materials including SiO2, H3BO3, CaCO3, and Al(OH)3 weighed in a stoichiometric ratio; melting the mixed raw materials, and pouring the molten glass into a cooling mill for rapid cooling to obtain glass sheets; placing the glass sheets into a grinder for preliminary crushing to obtain glass particles; and passing the glass particles through an air flow mill in combination with an air flow classifier to obtain glass powder within a preset particle size distribution range.
[0012] Preferably, in an embodiment of the present invention, the step of melting the mixed raw materials comprises: melting the prepared raw materials at 1350-1450° C. for 1-3 hours.
[0013] Preferably, in an embodiment of the present invention, the glass particles have a particle size ranging from 0.5 to 2.0 mm.
[0014] Preferably, in an embodiment of the present invention, the preset particle size distribution range of the glass powder is 3.0-4.0 μm.
[0015] According to the second aspect of the present invention, the single crystal glass ceramics are provided, and the single crystal glass ceramics are prepared by the preparation method of the single crystal glass ceramics provided by the first aspect of the present invention. BRIEF DESCRIPTION OF THE DRAWINGS
[0016] The above features and advantages of the present invention can be better understood after reading the detailed description of the embodiments of the present disclosure in conjunction with the following drawings. In the drawings, the components are not necessarily drawn to scale, and components with similar related properties or features may have the same or similar reference numerals.
[0017] Figure 1 A flow chart showing a method for preparing glass powder according to some embodiments of the present invention is shown;
[0018] Figure 2 A flow chart showing a method for preparing single crystal glass ceramics according to some embodiments of the present invention is shown;
[0019] Figure 3 The formula of the glass powder provided according to multiple embodiments and multiple comparative examples of the present invention is shown;
[0020] Figure 4 The performance test results of glass ceramics provided according to multiple embodiments and multiple comparative examples of the present invention are shown;
[0021] Figure 5 The bending strength of glass ceramics provided according to multiple embodiments of the present invention and multiple comparative examples is shown;
[0022] Figure 6 The ex-situ selected area electron diffraction pattern of the glass powder provided in Example 2 according to the present invention after sintering at 880° C. and keeping the temperature for 30 minutes is shown;
[0023] Figure 7 A microscopic morphology picture of the glass powder provided in Example 2 according to the present invention after sintering at 880° C. and keeping the temperature for 30 minutes is shown; and
[0024] Figure 8A comparison chart of the XRD spectra of the single crystal glass ceramics provided in Example 1 and Comparative Example 2 of the present invention is shown.
[0025] Reference numerals:
[0026] 100: Method for preparing glass powder;
[0027] S110~S140: steps;
[0028] 200: Preparation method of single crystal glass ceramics;
[0029] S210-S240: steps; and
[0030] 801, 802: lines. DETAILED DESCRIPTION
[0031] The present invention is described in detail below in conjunction with the accompanying drawings and specific embodiments. Note that the aspects described below in conjunction with the accompanying drawings and specific embodiments are only exemplary and should not be construed as limiting the scope of protection of the present invention in any way.
[0032] In the description of the present invention, it should be noted that, unless otherwise clearly specified and limited, the terms "installed", "connected", and "connected" should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection, or it can be indirectly connected through an intermediate medium, or it can be the internal communication of two components. For ordinary technicians in this field, the specific meanings of the above terms in the present invention can be understood according to specific circumstances.
[0033] In addition, the terms "upper", "lower", "left", "right", "top", "bottom", "horizontal" and "vertical" used in the following description should be understood as the directions shown in the paragraph and the related drawings. Such relative terms are only used for the convenience of description and do not mean that the device described therein must be manufactured or operated in a specific direction, and therefore should not be understood as limiting the present invention.
[0034] It is understood that although the terms "first", "second", "third", etc. may be used herein to describe various components, regions, layers and / or parts, these components, regions, layers and / or parts should not be limited by these terms, and these terms are only used to distinguish different components, regions, layers and / or parts. Therefore, the first component, region, layer and / or part discussed below may be referred to as a second component, region, layer and / or part without departing from some embodiments of the present invention.
[0035] As mentioned above, in the context of miniaturization and integration of high-frequency communication technology, LTCC substrates need to have certain bending and compression resistance to face high-load packaging environments. In addition, since the melting point of silver (Ag) is 961°C, the densification temperature of LTCC substrates is usually less than 900°C.
[0036] At present, the existing LTCC substrate materials are mainly microcrystalline glass systems and glass / ceramic composite systems. Among them, due to the advantages of low cost and high strength of Al2O3, the most commonly used glass / Al2O3 composite material in the glass / ceramic composite system. The prior art (for example, Chinese invention patent CN113372005A) uses lead borosilicate glass to pre-treat the surface of α-alumina to improve the interface contact strength between glass and alumina. Specifically, the mechanical properties of lead borosilicate glass are improved by doping α-alumina with high mechanical strength (300MPa) into lead borosilicate low-melting point glass (sintering aid). However, the high dielectric constant of alumina (9.8@10MHz) will cause the dielectric constant of the material to be too high. Moreover, lead glass is not in line with environmentally friendly development. In addition, in the microcrystalline glass system, a combination of multiple glasses is usually used to coordinate the comprehensive performance of LTCC materials. However, how to use traditional formulas and simple processes to meet the appropriate sintering temperature, low dielectric constant, low dielectric loss and high bending strength required for LTCC substrates is still a problem that needs to be solved urgently in this field.
[0037] In order to overcome the above-mentioned defects of the prior art, the present invention provides a method for preparing a single crystal glass ceramic, a method for preparing a glass powder, a glass powder, and a single crystal glass ceramic, which can balance and improve the sintering temperature, dielectric constant, dielectric loss, and flexural strength of LTCC substrate materials.
[0038] The above-mentioned glass powder will be described below in conjunction with some examples of the preparation method of the glass powder. Those skilled in the art will understand that these examples of the preparation method of the glass powder are only some non-limiting implementation methods provided by the present invention, which are intended to clearly demonstrate the main concept of the present invention and provide some specific solutions that are convenient for the public to implement. Similarly, the glass powder does not limit the execution subject and execution order of each step in the preparation method of the glass powder.
[0039] The glass powder for LTCC provided by the present invention is based on a CaO-B2O3-SiO2 (CBS, calcium borosilicate) glass-ceramic system, takes the Ostwald step rule and the nanometer-scale non-uniform structure as a guide for single crystallization, and promotes single crystallization by regulating the crystallization kinetics of β-CaSiO3. The single crystal β-CaSiO3 with a highly ordered layered structure accelerates the diffusion kinetics of ions and electrons, thereby reducing the dielectric constant of the substrate and improving the mechanical strength, solving the problem of low load of the existing LTCC material under the conditions of low dielectric constant and low dielectric loss.
[0040] In terms of molar percentage, the glass powder provided by the present invention may include 41.68-47.2 mol% of CaO (calcium oxide), 12.7-15.01 mol% of B2O3 (boron oxide), 37.77-40.97 mol% of SiO2 (silicon oxide) and doped modifier ions, and the silicon-calcium ratio of the glass powder may be 0.9-1. The doped modifier ions may include one or more of Al2O3 (aluminum oxide), Ta2O5 (tantalum oxide), Nb2O5 (niobium oxide), La2O3 (lanthanum oxide), CeO2 (cerium oxide), CuO (copper oxide), and BaO (barium oxide). The doped modifier ions may be used for the regulation of β-CaSiO3 single crystal materials. Preferably, the doped modifier ions are Al2O3, and in terms of molar percentage, the glass powder may include 0.34-3 mol% of Al2O3.
[0041] Please refer to Figure 1 , Figure 1 A flow chart of a method for preparing glass powder according to some embodiments of the present invention is shown.
[0042] like Figure 1 As shown, the method 100 for preparing glass powder may include step S110: preparing raw materials and fully mixing them, the raw materials including SiO2, H3BO3, CaCO3, and Al(OH)3 weighed in a stoichiometric ratio.
[0043] In a preferred embodiment, SiO2 included in the glass powder can use AR (Analytical Reagent) grade silicon oxide as a raw material, B2O3 can use electronic grade boric acid as a raw material, CaO can use calcium carbonate as a raw material, and Al2O3 can use aluminum hydroxide as a raw material.
[0044] After weighing the raw materials according to the stoichiometric ratio, the raw materials can be fully mixed using a mixer. In order to make the raw materials mixed more evenly, zirconium beads (i.e., grinding bodies) can be loaded into the mixing tank at a 1:1 ball-to-material ratio (ratio of material to grinding body mass) for mixing, and the mixing time is 2 to 3 hours.
[0045] Afterwards, if Figure 1 As shown, the method 100 for preparing glass powder may include step S120: melting the mixed raw materials, and pouring the melted glass liquid into a cooling rolling mill for rapid cooling to obtain a glass sheet.
[0046] In a preferred embodiment, after Al(OH)3 included in the raw material is introduced into the melted glass, Al(aluminum) ions participate in the glass network and replace part of the Si(silicon) sites, providing a very favorable environment for the subsequent heat treatment of β-CaSiO3 and its nucleation and growth, where the glass melt can form a β-CaSiO3 crystal phase with 95% and a residual glass phase with 5%. The generated ordered layered structure of β-CaSiO3 can provide good dynamics for ion and electron polarization, thereby providing a favorable environment for the formation of a low dielectric constant. At the same time, β-CaSiO3 is transformed into a single crystal structure, so the mechanical properties are also greatly improved.
[0047] In a preferred embodiment, the mixed raw materials can be melted at 1350-1450° C. for 1-3 hours. Specifically, to prevent contamination by other elements, a platinum crucible can be used during the melting process. In addition, to prevent excessive volatilization of the boron element, a cake-pressed batch feeding process can also be used for melting. The melted glass liquid is poured into a cooling mill for rapid cooling, thereby rapidly cooling the glass liquid into a glass sheet. Here, the cooling mill can be a double-roll cooling mill.
[0048] Please continue to refer to Figure 1 The method 100 for preparing glass powder may include step S130: placing a glass sheet into a grinder for preliminary crushing to obtain glass particles. In one embodiment, the glass sheet may be initially crushed into glass particles with a particle size range of about 0.5 to 2.0 mm by a three-cylinder grinder. Here, the glass particles are calcium borosilicate (CBS) glass particles.
[0049] The preparation method 100 of the glass powder may further include step S140: the glass particles are subjected to a jet mill in combination with an airflow classifier to obtain a glass powder within a preset particle size distribution range. Here, the preset particle size distribution range of the glass powder may be 3.0 to 4.0 μm, and in terms of molar percentage, the glass powder may include 41.68 to 47.2 mol% of CaO, 12.7 to 15.01 mol% of B2O3, 37.77 to 40.97 mol% of SiO2 and doped modifier ions, and the silicon-calcium ratio of the glass powder may be 0.9 to 1.
[0050] When the raw materials are SiO2, H3BO3, CaCO3, and Al(OH)3, the glass powder may include 41.68 to 47.2 mol% of CaO, 12.7 to 15.01 mol% of B2O3, 37.77 to 40.97 mol% of SiO2, and 0.34 to 3 mol% of Al2O3.
[0051] Those skilled in the art will appreciate that the above-mentioned steps for preparing the glass powder are only a non-limiting implementation method provided by the present invention, which is intended to clearly demonstrate the main concept of the present invention and to provide a specific scheme that is convenient for the public to implement, rather than to limit the scope of protection of the present invention. In other embodiments, those skilled in the art may also adopt other equivalent methods based on the concept of the present invention to obtain a glass powder having a formula of 41.68-47.2 mol% CaO, 12.7-15.01 mol% B2O3, 37.77-40.97 mol% SiO2 and 0.34-3 mol% Al2O3.
[0052] After obtaining the glass powder, single crystal glass ceramics can be prepared. Please refer to Figure 2 , Figure 2 A flow chart of a method for preparing single crystal glass ceramics provided according to some embodiments of the present invention is shown.
[0053] like Figure 2 As shown, the preparation method 200 of single crystal glass ceramics may include step S210: mixing glass powder with an organic solvent, obtaining a green ceramic tape by tape casting, laminating and pressing the green ceramic tape, and then placing the green ceramic tape in a sintering furnace for sintering.
[0054] Specifically, first mix the glass powder with an organic solvent. Put the glass powder into a zirconium can, use PVB resin as a binder, use one or more of butanone, butyl acetate, cyclohexane, cyclohexanone, pinene alcohol, methyl ethyl ketone, toluene, and xylene as an organic solvent, and add a certain amount of dispersant and mix for 4 to 6 hours to prepare the casting slurry. Here, the organic solvent can be used in combination according to the volatilization temperature. After that, a uniform and smooth raw porcelain tape can be prepared by casting. The configured casting slurry is heated to a certain viscosity, and a raw porcelain tape of a certain thickness is obtained by casting through a casting machine. After the raw porcelain tape has been processed by lamination, pressing, etc., it can be placed in a sintering furnace for sintering.
[0055] like Figure 2As shown, the preparation method 200 of single crystal glass ceramics may include a sintering process, which may include steps S220, S230 and S240: heating to 500-550°C at a rate of 1-2°C / min, keeping warm for 4-5 hours, and then debinding; then heating to 860-880°C at a rate of 3-5°C / min, keeping warm for 10-30 minutes; after cooling, single crystal glass ceramics can be obtained. The obtained single crystal glass ceramics can be co-fired with silver paste without silver diffusion. Preferably, the sintering shrinkage of the single crystal glass ceramics is 15-18% to ensure shrinkage matching, stress matching and co-firing matching at the interface between silver and LTCC substrate.
[0056] The following are multiple preferred embodiments, based on which the glass powder and the preparation method thereof proposed in the present invention and the single crystal glass ceramics obtained based on the glass powder and the preparation method thereof are described in detail.
[0057] Please refer to Figure 3 , Figure 3 The formulas of glass powders provided according to multiple embodiments of the present invention and multiple comparative examples are shown.
[0058] In the preparation process of the glass powder provided in Example 1, the raw materials can be prepared according to the stoichiometric ratio requirements. The SiO2 included in the glass powder can use AR-grade silicon oxide as a raw material, the raw material of B2O3 can be electronic-grade boric acid, the raw material of CaO can use calcium carbonate as a raw material, and the raw material of Al2O3 can use aluminum hydroxide as a raw material. Afterwards, a mixer is used to fully mix the raw materials, and zirconium beads can be loaded into the mixing tank at a ball-to-material ratio of 1:1, and the mixing time is 2 to 3 hours.
[0059] A platinum crucible is used to melt the raw materials, and a pressed cake batch feeding process is adopted to prevent excessive volatilization of the boron element. The melting temperature is 1450°C, and the melting time is 1 to 3 hours. Afterwards, the molten glass liquid is poured into a double-roll cooling mill for rapid cooling, thereby rapidly cooling the glass liquid into glass sheets. The glass sheets are then initially crushed into glass particles of about 0.5 to 2.0 mm by a three-drum grinder, and the glass particles are then passed through an air flow mill in combination with an air flow classifier to obtain a glass powder of 3 to 4 μm. Figure 3 As shown, the glass powder A1 provided in Example 1 may include 41.68 mol% CaO, 15.01 mol% B2O3, 40.97 mol% SiO2 and 2.34 mol% Al2O3, and the silicon-calcium ratio is 0.98.
[0060] Afterwards, the glass powder provided in Example 1 is mixed with an organic solvent, and a green porcelain tape is obtained by tape casting. The green porcelain tape is then stacked and pressed, and then placed in a sintering furnace for sintering.
[0061] Specifically, the glass powder is loaded into a zirconium can, PVB resin is used as a binder, one or more of butanone, butyl acetate, cyclohexane, cyclohexanone, pinene alcohol, methyl ethyl ketone, toluene, and xylene are used as organic solvents, and a certain amount of dispersant is added and mixed for 4 to 6 hours to prepare the casting slurry. Here, the organic solvent can be used in combination according to the volatilization temperature. After that, the configured casting slurry is heated to a certain viscosity and cast by a casting machine to obtain a raw porcelain tape of a certain thickness. After the raw porcelain tape is processed by lamination, pressing, etc., it can be placed in a sintering furnace for sintering to obtain single crystal glass ceramics. In Example 1, the sintering process can be heated to 500°C at a rate of 2°C / min, and the binder can be removed after keeping warm for 4 hours, and then heated to 880°C at a rate of 5°C / min, kept warm for 30 minutes, and cooled to obtain single crystal glass ceramics.
[0062] Please refer to Figure 4 and Figure 5 , Figure 4 The performance test results of glass ceramics provided by multiple embodiments and multiple comparative examples according to the present invention are shown. Figure 5 The flexural strength of glass ceramics provided according to various embodiments of the present invention and various comparative examples is shown.
[0063] like Figure 4 , Figure 5 As shown, the single crystal glass ceramics prepared based on the glass powder provided in Example 1 have a dielectric constant k of 4.01 and a dielectric loss of 0.00317 at 10 MHz; a dielectric constant k of 4.04 and a dielectric loss of 0.00315 at 15 GHz; and a bending strength of 256 MPa. It can be seen that the single crystal glass ceramics provided by the present invention have a lower sintering temperature (880°C), a smaller dielectric constant (4.04@15GHz) and dielectric loss (0.00315@15GHz) and a high mechanical strength (256 MPa).
[0064] In the preparation process of the glass powder provided in Example 2, the raw materials can be prepared according to the stoichiometric ratio requirements. The SiO2 included in the glass powder can use AR-grade silicon oxide as a raw material, the raw material of B2O3 can be electronic-grade boric acid, the raw material of CaO can use calcium carbonate as a raw material, and the raw material of Al2O3 can use aluminum hydroxide as a raw material. Afterwards, a mixer is used to fully mix the raw materials, and zirconium beads can be loaded into the mixing tank at a ball-to-material ratio of 1:1, and the mixing time is 2 to 3 hours.
[0065] A platinum crucible is used to melt the raw materials, and a pressed cake batch feeding process is adopted to prevent excessive volatilization of the boron element. The melting temperature is 1450°C, and the melting time is 1 to 3 hours. Afterwards, the molten glass liquid is poured into a double-roll cooling mill for rapid cooling, thereby rapidly cooling the glass liquid into glass sheets. The glass sheets are then initially crushed into glass particles of about 0.5 to 2.0 mm by a three-drum grinder, and the glass particles are then passed through an air flow mill in combination with an air flow classifier to obtain a glass powder of 3 to 4 μm. Figure 3 As shown, the glass powder A2 provided in Example 2 may include 42.04 mol% CaO, 15.14 mol% B2O3, 41.32 mol% SiO2 and 1.5 mol% Al2O3, and the silicon-calcium ratio is 0.98.
[0066] Afterwards, the glass powder provided in Example 2 is loaded into a zirconium can, PVB resin is used as a binder, one or more of butanone, butyl acetate, cyclohexane, cyclohexanone, pinene alcohol, methyl ethyl ketone, toluene, and xylene are used as organic solvents, and a certain amount of dispersant is added and mixed for 4 to 6 hours to prepare the casting slurry. Here, the organic solvent can be used in combination according to the volatilization temperature. Afterwards, the prepared casting slurry is heated to a certain viscosity and cast by a casting machine to obtain a raw porcelain tape of a certain thickness. After the raw porcelain tape is processed by lamination, pressing, etc., it can be placed in a sintering furnace for sintering to obtain single crystal glass ceramics. In Example 2, the sintering process can be heated to 500°C at a rate of 2°C / min, and the binder can be removed after keeping warm for 4 hours, and then heated to 880°C at a rate of 5°C / min, kept warm for 30 minutes, and cooled to obtain single crystal glass ceramics.
[0067] like Figure 4 , Figure 5 As shown, the single crystal glass ceramic provided in Example 2 has a dielectric constant k of 4.10 and a dielectric loss of 0.00386 at 10 MHz; a dielectric constant k of 4.12 and a dielectric loss of 0.00386 at 15 GHz; and a flexural strength of 237 MPa.
[0068] In addition, please refer to Figure 6 and Figure 7 , Figure 6 The figure shows the non-in-situ selected area electron diffraction pattern of the glass powder provided in Example 2 according to the present invention after sintering at 880° C. and keeping the temperature for 30 minutes. Figure 7 The microscopic morphology of the glass powder provided in Example 2 according to the present invention after sintering at 880° C. and keeping warm for 30 minutes is shown.
[0069] like Figure 6As shown, the glass powder provided in Example 2 is sintered at 880°C and kept warm for 30 minutes to form a regular diffraction spot sample, which exhibits the properties of a single crystal, consistent with the crystal system of β-CaSiO3, and the sample can be judged to be a monoclinic system by the arrangement mode. Therefore, it can be judged that the β-CaSiO3 in the sample forms a single crystal during the sintering process.
[0070] like Figure 7 As shown, the sample formed after the glass powder provided in Example 2 was sintered at 880°C and kept warm for 30 minutes showed dense and non-porous characteristics, the bright field area (lighter color area) was a single crystal β-CaSiO3 crystal phase, and the dark field area (darker color area) was a residual glass phase. The single crystal β-CaSiO3 crystal phase content is high, and the residual glass phase content is very low. Dense single crystal glass ceramics can greatly reduce the dielectric loss of LTCC materials.
[0071] pass Figure 6 and Figure 7 It can be explained that when the glass powder provided in Example 2 is used to prepare single-crystal glass ceramics, its crystal phase only precipitates β-CaSiO3 phase, and the precipitated crystal phase can be converted into single-crystal β-CaSiO3 at a lower sintering temperature, thereby improving the mechanical strength of the LTCC material and achieving a low dielectric constant.
[0072] The following are a number of comparative examples compared with the above-mentioned embodiments, based on which the performance effects of the glass powder proposed in the present invention and the single crystal glass ceramics obtained based on the glass powder are further explained.
[0073] In the preparation process of the glass powder provided in Comparative Example 1, the raw materials can be prepared according to the stoichiometric ratio requirements. The SiO2 included in the glass powder can use AR-grade silicon oxide as a raw material, the raw material of B2O3 can be electronic-grade boric acid, the raw material of CaO can use calcium carbonate as a raw material, and the raw material of Al2O3 can use aluminum hydroxide as a raw material. Afterwards, a mixer is used to fully mix the raw materials, and zirconium beads can be loaded into the mixing tank at a ball-to-material ratio of 1:1, and the mixing time is 2 to 3 hours.
[0074] A platinum crucible is used to melt the raw materials, and a pressed cake batch feeding process is adopted to prevent excessive volatilization of the boron element. The melting temperature is 1450°C, and the melting time is 1 to 3 hours. Afterwards, the molten glass liquid is poured into a double-roll cooling mill for rapid cooling, thereby rapidly cooling the glass liquid into glass sheets. The glass sheets are then initially crushed into glass particles of about 0.5 to 2.0 mm by a three-drum grinder, and the glass particles are then passed through an air flow mill in combination with an air flow classifier to obtain a glass powder of 3 to 4 μm. Figure 3As shown, the glass powder A3 provided in Comparative Example 1 may include 42.53 mol% of CaO, 15.32 mol% of B2O3, 41.81 mol% of SiO2 and 0.34 mol% of Al2O3, and the silicon-calcium ratio is 0.98.
[0075] Afterwards, the glass powder provided in Comparative Example 1 is loaded into a zirconium can, PVB resin is used as a binder, one or more of butanone, butyl acetate, cyclohexane, cyclohexanone, pinene alcohol, methyl ethyl ketone, toluene, and xylene are used as organic solvents, and a certain amount of dispersant is added and mixed for 4 to 6 hours to prepare the casting slurry. Here, the organic solvent can be used in combination according to the volatilization temperature. Afterwards, the prepared casting slurry is heated to a certain viscosity, and cast by a casting machine to obtain a raw porcelain tape of a certain thickness. After the raw porcelain tape is processed by lamination, pressing, etc., it can be placed in a sintering furnace for sintering to obtain glass ceramics. In Comparative Example 1, the sintering process can be heated to 500°C at a rate of 2°C / min, and the binder can be removed after keeping warm for 4 hours, and then heated to 850°C at a rate of 5°C / min, kept warm for 30 minutes, and cooled to obtain glass ceramics.
[0076] like Figure 4 , Figure 5 As shown, the single crystal glass ceramic provided in Comparative Example 1 has a dielectric constant k of 4.23 and a dielectric loss of 0.00379 at 10 MHz; a dielectric constant k of 4.30 and a dielectric loss of 0.00391 at 15 GHz; and a flexural strength of 181 MPa. Compared with a sintering temperature of 880°C, a sintering temperature of 850°C cannot promote the transformation of single crystal β-CaSiO3 well, so the flexural strength of the glass ceramic provided in Comparative Example 1 is significantly lower than that of Examples 1 and 2, but is improved compared to the flexural strength of other existing LTCC materials.
[0077] In the preparation process of the glass powder provided in Comparative Example 2, the raw materials can be prepared according to the stoichiometric ratio requirements. The SiO2 included in the glass powder can use AR-grade silicon oxide as a raw material, the raw material of B2O3 can be electronic-grade boric acid, the raw material of CaO can use calcium carbonate as a raw material, and the raw material of Al2O3 can use aluminum hydroxide as a raw material. Afterwards, a mixer is used to fully mix the raw materials, and zirconium beads can be loaded into the mixing tank at a ball-to-material ratio of 1:1, and the mixing time is 2 to 3 hours.
[0078] A platinum crucible is used to melt the raw materials, and a pressed cake batch feeding process is adopted to prevent excessive volatilization of the boron element. The melting temperature is 1450°C, and the melting time is 1 to 3 hours. Afterwards, the molten glass liquid is poured into a double-roll cooling mill for rapid cooling, thereby rapidly cooling the glass liquid into glass sheets. The glass sheets are then initially crushed into glass particles of about 0.5 to 2.0 mm by a three-drum grinder, and the glass particles are then passed through an air flow mill in combination with an air flow classifier to obtain a glass powder of 3 to 4 μm. Figure 3 As shown, the glass powder A4 provided in Comparative Example 2 may include 47.2 mol% of CaO, 12.7 mol% of B2O3, 37.76 mol% of SiO2 and 2.34 mol% of Al2O3, and the silicon-calcium ratio is 0.80.
[0079] Afterwards, the glass powder provided in Comparative Example 2 is loaded into a zirconium can, PVB resin is used as a binder, one or more of butanone, butyl acetate, cyclohexane, cyclohexanone, pinene alcohol, methyl ethyl ketone, toluene, and xylene are used as organic solvents, and a certain amount of dispersant is added and mixed for 4 to 6 hours to prepare the casting slurry. Here, the organic solvent can be used in combination according to the volatilization temperature. Afterwards, the prepared casting slurry is heated to a certain viscosity and cast by a casting machine to obtain a raw porcelain tape of a certain thickness. After the raw porcelain tape is processed by lamination, pressing, etc., it can be placed in a sintering furnace for sintering to obtain glass ceramics. In Comparative Example 2, the sintering process can be heated to 500°C at a rate of 2°C / min, and the binder can be removed after keeping warm for 4 hours, and then heated to 850°C at a rate of 5°C / min, kept warm for 30 minutes, and cooled to obtain glass ceramics.
[0080] like Figure 4 , Figure 5 As shown, the glass ceramic provided in Comparative Example 2 has a dielectric constant k of 4.31 and a dielectric loss of 0.00257 at 10 MHz; a dielectric constant k of 4.36 and a dielectric loss of 0.00234 at 15 GHz; and a flexural strength of 160 MPa.
[0081] Please refer to Figure 8 , Figure 8 A comparison chart of the XRD spectra of the single crystal glass ceramics provided in Example 1 and Comparative Example 2 of the present invention is shown.
[0082] like Figure 8As shown, the crystal type of the single crystal glass ceramics provided in Example 1 and Comparative Example 2 can be determined by the XRD (X-Ray Diffraction) spectrum according to the intensity of the diffraction peak. Line 801 is the result of the XRD spectrum of the single crystal glass ceramics provided in Example 1, and line 802 is the result of the XRD spectrum of the single crystal glass ceramics provided in Comparative Example 2. The difference between the glass powder formulas of Example 1 and Comparative Example 2 is the silicon-calcium ratio (Si / Ca). The silicon-calcium ratio of Example 1 is 0.98, and the silicon-calcium ratio of Comparative Example 2 is 0.80. From Figure 8 It can be seen that the diffraction peak intensity of line 801 is greater than that of line 802, indicating that a high silicon-calcium ratio (ie, Example 1) is more conducive to the precipitation of high-strength β-CaSiO3. Therefore, the flexural strength of Example 1 is better than that of Comparative Example 2.
[0083] The preparation method of the glass powder and glass ceramic provided in Comparative Example 3 is the same as that in Example 1. Figure 3 As shown, the difference between Comparative Example 3 and Example 1 is that in the formula of the glass powder provided in Comparative Example 3, the content of Al2O3 is 0 mol%. Therefore, in the preparation process of the glass powder provided in Comparative Example 3, the prepared raw materials do not include aluminum hydroxide. Specifically, the glass powder A5 provided in Comparative Example 3 includes 42.68 mol% of CaO, 15.37 mol% of B2O3, and 41.95 mol% of SiO2, and the silicon-calcium ratio is 0.98.
[0084] like Figure 4 , Figure 5 As shown, the glass ceramic provided in Comparative Example 3 has a dielectric constant k of 5.54 and a dielectric loss of 0.002 at 10 MHz; a dielectric constant k of 5.61 and a dielectric loss of 0.0018 at 15 GHz; and a bending strength of 156 MPa. This shows that without the introduction of modifier ions (such as Al2O3), it is impossible to promote the single crystallization of β-CaSiO3, and therefore it is impossible to improve the mechanical strength and dielectric properties of LTCC materials.
[0085] The preparation method of the glass powder and glass ceramic provided in Comparative Example 4 is the same as that in Example 1. Figure 3 As shown, the difference between Comparative Example 4 and Example 1 is that the content of Al2O3 in the formula of the glass powder provided in Comparative Example 4 is higher than that in Example 1, and the content of Al2O3 in Comparative Example 4 is 5.34 mol%. Specifically, the glass powder A6 provided in Comparative Example 4 includes 40.4 mol% of CaO, 14.55 mol% of B2O3, 39.71 mol% of SiO2 and 5.34 mol% of Al2O3, and the silicon-calcium ratio is 0.98.
[0086] like Figure 4 , Figure 5 As shown, the glass ceramic provided in Comparative Example 4 has a dielectric constant k of 4.87 and a dielectric loss of 0.00321 at 10 MHz; a dielectric constant k of 4.93 and a dielectric loss of 0.00473 at 15 GHz; and a flexural strength of 81 MPa. This indicates that when the content of the introduced modifier ions (such as Al2O3) is too high, the glass liquid phase will be excessive and the crystal phase content will be reduced, so the flexural strength of the glass ceramic will drop sharply.
[0087] Furthermore, the preparation method of the glass powder and glass ceramic provided in Comparative Example 5 is the same as that in Example 1, such as Figure 3 As shown, the difference between Comparative Example 5 and Example 1 is that the content of Al2O3 in Comparative Example 5 is higher than that in Example 1, and the silicon-calcium ratio is lower than that in Example 1. Specifically, the glass powder A7 provided in Comparative Example 5 includes 46.8 mol% of CaO, 10.41 mol% of B2O3, 37.45 mol% of SiO2 and 5.34 mol% of Al2O3, and the silicon-calcium ratio is 0.80.
[0088] like Figure 4 , Figure 5 As shown, the glass ceramic provided in Comparative Example 5 has a dielectric constant k of 5.24 and a dielectric loss of 0.00322 at 10 MHz; a dielectric constant k of 5.29 and a dielectric loss of 0.00312 at 15 GHz; and a flexural strength of 75 MPa. This shows that when the content of the introduced modifier ions (such as Al2O3) is too high and the silicon-calcium ratio is reduced, the flexural strength of the glass ceramic will drop sharply, and the dielectric constant of the LTCC material will increase, which cannot meet the requirements of low dielectric constant.
[0089] The preparation method of the glass powder and glass ceramic provided in Comparative Example 6 is the same as that in Example 2. Figure 3 As shown, the difference between Comparative Example 6 and Example 2 is that the silicon-calcium ratio of the glass powder provided in Comparative Example 6 is lower than that in Example 2. The silicon-calcium ratio in Example 2 is 0.98, and the silicon-calcium ratio in Comparative Example 6 is 0.80. Specifically, the glass powder A8 provided in Comparative Example 6 includes 46.51 mol% of CaO, 14.78 mol% of B2O3, 37.21 mol% of SiO2, and 1.5 mol% of Al2O3.
[0090] like Figure 4 , Figure 5As shown, the glass ceramic provided in Comparative Example 6 has a dielectric constant k of 5.46 and a dielectric loss of 0.00248 at 10 MHz; a dielectric constant k of 5.47 and a dielectric loss of 0.00217 at 15 GHz; and a bending strength of 176 MPa. This indicates that the reduction of the silicon-calcium ratio, that is, when the silicon content is too low, will cause the content of precipitated calcium silicate to decrease, and due to the presence of a small amount of impurity phases with high dielectric constant and high sintering temperature (such as α-CaSiO3 and Ca2O4), the dielectric constant of the LTCC material will be too high, the dielectric properties of the LTCC substrate will decrease, and the mechanical strength of the LTCC material will decrease.
[0091] In addition, the preparation method of the glass powder and glass ceramic provided in Comparative Example 7 is the same as that in Comparative Example 1. Figure 3 As shown, the difference between Comparative Example 7 and Comparative Example 1 is that in the formula of the glass powder provided in Comparative Example 7, the content of B2O3 is increased and the content of silicon is reduced, that is, the silicon-calcium ratio of Comparative Example 7 is reduced compared with Comparative Example 1. The silicon-calcium ratio in Comparative Example 1 is 0.98, and the silicon-calcium ratio in Comparative Example 7 is 0.80. Specifically, the glass powder A9 provided in Comparative Example 7 includes 45.95 mol% of CaO, 16.94 mol% of B2O3, 36.77 mol% of SiO2, and 0.34 mol% of Al2O3.
[0092] like Figure 4 , Figure 5 As shown, the glass ceramic provided in Comparative Example 7 has a dielectric constant k of 5.32 and a dielectric loss of 0.00364 at 10 MHz; a dielectric constant k of 5.38 and a dielectric loss of 0.00425 at 15 GHz; and a bending strength of 164 MPa. This indicates that the reduction of the silicon-calcium ratio, that is, when the silicon content is too low, will lead to an excessively high dielectric constant of the LTCC material, a decrease in the dielectric properties of the LTCC substrate, and a decrease in the mechanical strength of the LTCC material.
[0093] In summary, the single crystal glass ceramic provided by the present invention does not contain any externally doped ceramic powder, has a lower sintering temperature, a smaller dielectric constant and dielectric loss, and a high mechanical strength, and can balance and improve the sintering temperature, dielectric constant, dielectric loss, and bending strength of the LTCC substrate, thereby being widely used in modern 5G / 6G electronic communications fields such as mobile communications, high-frequency electronics, wireless local area networks, satellite communications, and aerospace electronics.
[0094] Although the above methods are illustrated and described as a series of actions for simplicity of explanation, it should be understood and appreciated that these methods are not limited by the order of the actions, because according to one or more embodiments, some actions may occur in a different order and / or concurrently with other actions from those illustrated and described herein or not illustrated and described herein but understandable to those skilled in the art.
[0095] The previous description of the disclosure is provided to enable any person skilled in the art to make or use the disclosure. Various modifications to the disclosure will be apparent to those skilled in the art, and the general principles defined herein may be applied to other variations without departing from the spirit or scope of the disclosure. Thus, the disclosure is not intended to be limited to the examples and designs described herein, but should be granted the widest scope consistent with the principles and novel features disclosed herein.
Claims
1. A method for preparing single crystal glass ceramics, characterized in that: Includes steps: Mixing glass powder with an organic solvent, casting to obtain a green porcelain tape, laminating and pressing the green porcelain tape, and then sintering it in a sintering furnace, wherein the glass powder comprises 41.68-47.2 mol% of CaO, 12.7-15.01 mol% of B2O3, 37.77-40.97 mol% of SiO2 and doped modifier ions, wherein the modifier ions comprise one or more of Al2O3, Ta2O5, Nb2O5, La2O3, CeO2, CuO, and BaO, and the silicon-calcium ratio of the glass powder is 0.9-1; The sintering process comprises: Raise the temperature to 500-550°C at a rate of 1-2°C / min, keep warm for 4-5 hours, and then perform binder removal; Raising the temperature to 860-880°C at a rate of 3-5°C / min and keeping the temperature for 10-30 minutes; and After cooling, single crystal glass ceramics are obtained.
2. The method for preparing a single crystal glass ceramic according to claim 1, wherein: The sintering shrinkage of the glass powder is 15% to 18%.
3. The method for preparing a single crystal glass ceramic according to claim 1, wherein: The doped modifier ion is Al2O3, and the glass powder includes 0.34-3 mol% of the Al2O3 in terms of molar percentage.
4. The method for preparing a single crystal glass ceramic according to claim 1, wherein: The preparation of the glass powder comprises the following steps: Prepare raw materials and mix them thoroughly, wherein the raw materials include SiO2, H3BO3, CaCO3, and Al(OH)3 weighed in a stoichiometric ratio; Melting the mixed raw materials, and pouring the melted glass into a cooling rolling mill for rapid cooling to obtain a glass sheet; placing the glass flakes into a grinder for preliminary crushing to obtain glass particles; and The glass particles are passed through an air flow mill in combination with an air flow classifier to obtain glass powder within a preset particle size distribution range.
5. The method for preparing a single crystal glass ceramic according to claim 4, characterized in that: The step of melting the mixed raw materials comprises: The prepared raw materials are melted at 1350-1450° C. for 1-3 hours.
6. The method for preparing a single crystal glass ceramic according to claim 4, characterized in that: The particle size of the glass particles ranges from 0.5 to 2.0 mm.
7. The method for preparing a single crystal glass ceramic according to claim 4, characterized in that: The preset particle size distribution range of the glass powder is 3.0-4.0 μm.
8. A single crystal glass ceramic, characterized in that: The single crystal glass ceramics are made by the preparation method of single crystal glass ceramics as described in claims 1-7.
Citation Information
Patent Citations
Reinforced calcium borosilicate microcrystalline glass composite material and preparation method thereof
CN110683769A
Calcium borosilicate glass powder-based composite ceramic powder and preparation process thereof
CN112321164A
Composition for ceramic substrates and ceramic circuit component
US20160086732A1
Low-temperature co-fired ceramic material and preparation method thereof
US20180057395A1