Preparation method of ceramic-based composite material blade provided with tiny turbulent flow columns

Through chemical vapor phase impregnation technology and mold processing technology, the problem of long preparation period and cumbersome process of microspoiler column blades under online riveting welding is solved, and the efficient preparation of ceramic matrix composite blades and stable heat dissipation performance under high temperature environments are achieved. .

CN118930298AActive Publication Date: 2024-11-12XIAN XINGUI CERAMIC COMPOSITE MATERIAL CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202411033581.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-30
Publication Date
2024-11-12
Estimated Expiration
2044-07-30

AI Technical Summary

Technical Problem

The existing online riveting welding method to prepare microspoiler column blades has long cycles and cumbersome processes, which is difficult to meet the efficient heat dissipation needs of the new generation of aero engine blades in high temperature and high pressure environments.

Method used

The fiber cloth is prepared by using chemical vapor phase impregnation technology to prepare boron nitride interface and silicon carbide matrix. Combined with mold processing and fiber cloth wrapping technology, the ceramic matrix composite blades are gradually formed and fixed to ensure the precise installation of spoiler columns and the height of the blades. Density seal.

Benefits of technology

The blade preparation process is simplified, the cost and time are reduced, the process accuracy and efficiency are improved, and the structural stability and heat dissipation performance of the blade in high temperature environments are ensured.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118930298A_ABST
    Figure CN118930298A_ABST
Patent Text Reader

Abstract

The invention relates to a preparation method of a ceramic matrix composite blade provided with a tiny turbulent flow column, belongs to the technical field of preparation of aero-engine parts, and solves the technical problems of long period and tedious process in the process of preparing the blade provided with the turbulent flow column in an online rivet welding manner. Comprising the steps of spoiler column machining, mold spoiler hole machining, blade fiber cloth wrapping, mold closing and shaping, blade chemical vapor infiltration and blade secondary chemical vapor infiltration. The preparation method is used for preparing the ceramic-based composite material blade provided with the tiny turbulent flow column.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of aero-engine component preparation, and in particular relates to a method for preparing a ceramic-based composite material blade equipped with micro-spoiler columns. Background Art

[0002] Blades are an important part of aircraft engines. They have high strength, stiffness and structural stability under high temperature and dynamic and static load environments of aircraft engines. The new generation of aircraft engine blades need to withstand increasingly harsh working stresses and environmental loads such as high temperature and high pressure. Their research and development technology and manufacturing level have an important impact on engine performance. Rapid ventilation and heat dissipation of aircraft engine blades is an important means to ensure that their structure is more stable in harsh environments such as high temperature. Due to the small size of the blades, the number of tiny heat dissipation vents distributed on their surface is limited and the processing is difficult. Therefore, reserving a heat dissipation slit gap at the tail of the blade has become a research trend for new blades. In order to avoid overheating of the heat dissipation slit gap at the tail of the blade, a tiny spoiler column needs to be designed at the slit gap to disperse the heat, thereby increasing its service life.

[0003] The blade spoiler column structure is generally prepared by online riveting and welding. The blade and the carbon-ceramic composite pin are riveted online and welded by chemical vapor infiltration. The blade spoiler column structure needs to use special riveting tools for precision control during the preparation process, and its preparation is relatively cumbersome. Summary of the invention

[0004] In order to overcome the shortcomings of long cycle and complicated process in preparing blades equipped with tiny spoiler columns by online riveting and welding, the present invention proposes a method for preparing ceramic-based composite blades equipped with tiny spoiler columns.

[0005] The technical solution adopted by the present invention to solve the technical problem is:

[0006] A method for preparing a ceramic-based composite blade equipped with a micro-turbulent column comprises the following steps:

[0007] Step S1, spoiler column processing: according to the design structure size of the spoiler column, the fiber cloth is formed into a flat plate of required thickness; the boron nitride interface and silicon carbide matrix are prepared on the flat plate by chemical vapor infiltration process, and when the density of the flat plate matrix reaches the required density, the flat plate is processed into a spoiler column of required size;

[0008] Step S2, processing of spoiler holes in the mold: designing the mold according to the reserved machining allowance of the blade, and processing spoiler holes on the outer mold surface of the mold;

[0009] Step S3, wrapping the blade with fiber cloth: wrapping the fiber cloth on the surface of the inner mold according to the designed thickness of the blade, and filling the heat dissipation gap at the tail of the blade with hard paper;

[0010] Step S4, mold closing and shaping: the inner mold and the outer mold of the blade are molded and shaped, and the spoiler column is inserted into the spoiler hole reserved in the outer mold so that both ends of the spoiler column extend out of the outer mold surface;

[0011] Step S5, chemical vapor infiltration of blades: using chemical vapor infiltration process, prepare boron nitride interface and silicon carbide matrix of the blade; after the boron nitride interface is prepared, remove the hard paper padded by the heat dissipation slit at the tail of the blade, and pad the local area of ​​the slit with high-density C / SiC composite strips of the same height as the slit as support, and remove the inner mold and outer mold when the density of the blade matrix reaches the required density;

[0012] Step S6, chemical vapor infiltration of the blade again: the silicon carbide matrix is ​​further prepared for the blade, and when the density of the blade matrix reaches the final required density; mechanical processing is performed according to the actual size requirements of the blade to obtain a blade equipped with a spoiler column.

[0013] In the above-mentioned preparation method, in step S1, the process of shaping the fiber cloth into a flat plate of a desired thickness is: the fiber cloth is laid flat and fixed tightly with a flat plate mold of a corresponding size.

[0014] In the above-mentioned preparation method, in step S1, the boron nitride interface and silicon carbide substrate are prepared on the flat plate, and the density of the flat plate substrate is required to be greater than 1.4g / cm 3 ; Process the flat plate into a spoiler column of the required size, leaving a 15mm to 20mm margin on one side in the length direction.

[0015] The column preparation method described above, step S2, further comprises:

[0016] According to the size and position of the blade spoiler column, the corresponding spoiler holes are processed.

[0017] In the above-mentioned preparation method, in step S5, the blade substrate requires a density greater than 1.4 g / cm 3 .

[0018] In the above-mentioned preparation method, in step S6, the final required density of the blade substrate is greater than 2.0 g / cm 3 .

[0019] The beneficial effects of the present invention are:

[0020] A method for preparing a ceramic-based composite blade equipped with tiny spoiler columns. The processing process requires the use of special riveting tooling for precision control, which overcomes the shortcomings of long cycle, high cost and complicated process in preparing blades equipped with tiny spoiler columns by online riveting and welding. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] Figure 1 2 is a schematic diagram of the structure of the spoiler column discharge plate according to an embodiment of the present invention;

[0022] Figure 2 is a schematic diagram of a fiber cloth wrapping structure according to an embodiment of the present invention;

[0023] Figure 3 Schematic diagram of blade mold closing in an embodiment of the present invention;

[0024] Figure 4 Schematic diagram of the installation of the spoiler column after mold closing according to the embodiment of the present invention;

[0025] Figure 5 Schematic diagram of the blade spoiler column after demoulding according to an embodiment of the present invention;

[0026] Figure 6 is a schematic diagram of a blade spoiler column after processing according to an embodiment of the present invention;

[0027] Figure 7 It is a front view of the blade spoiler column after processing according to an embodiment of the present invention. DETAILED DESCRIPTION

[0028] The present invention is further described in detail below with reference to the accompanying drawings and specific embodiments.

[0029] Embodiment 1

[0030] A method for preparing a ceramic-based composite blade equipped with a micro-spoiler column comprises the following steps:

[0031] Step S1: According to the design size of the spoiler column, a fiber cloth is used to shape a flat plate of the required thickness (the fiber cloth is laid flat and a flat plate mold of the corresponding size is used to tightly mold and fix it). The boron nitride interface and silicon carbide matrix are prepared on the flat plate by chemical vapor infiltration. When the density of the flat plate matrix is ​​greater than 1.4g / cm 3 When processing the flat plate into a spoiler column of the required size (with a 15-20mm margin on one side in the length direction);

[0032] Step S2, designing a mold according to the reserved machining allowance size of the blade, and machining spoiler holes of corresponding size and quantity on the outer mold surface according to the size and position of the spoiler columns of the blade;

[0033] Step S3, wrap the fiber cloth on the inner mold surface according to the designed thickness of the blade. Fill the heat dissipation gap at the tail of the blade with hard paper;

[0034] Step S4, after the inner and outer molds of the blade are molded and finalized, the spoiler column processed in advance is inserted into the spoiler hole reserved in the outer mold, ensuring that both ends of the spoiler column extend out of the outer mold surface;

[0035] Step S5, using the same process as the spoiler column, prepare the boron nitride interface and silicon carbide matrix of the blade. After the boron nitride interface is prepared, remove the hard paper padding of the heat dissipation slit at the tail of the blade, and pad the local area of ​​the slit with a high-density C / SiC composite strip of the same height as the support. When the blade matrix density is greater than 1.4g / cm 3 When removing the inner and outer molds;

[0036] Step S6, continue to prepare the silicon carbide matrix of the blade until the matrix density is greater than 2.0g / cm 3 When manufacturing the blade, the blade is processed according to its actual size to obtain a blade equipped with a spoiler column.

Claims

1. A method for preparing a ceramic-based composite blade equipped with a micro-turbulent column, characterized in that: The following steps are involved: Step S1, shaping the fiber cloth into a flat plate of required thickness according to the design structure size of the spoiler column; using chemical vapor infiltration process to prepare boron nitride interface and silicon carbide matrix on the flat plate, and when the density of the flat plate matrix reaches the required density, processing the flat plate into a spoiler column of required size; Step S2, designing a mold according to the reserved machining allowance of the blade, and machining spoiler holes on the outer mold surface of the mold; Step S3, wrapping the fiber cloth on the surface of the inner mold according to the designed thickness of the blade, and filling the heat dissipation gap at the tail of the blade with hard paper; Step S4, the inner and outer molds of the blade are molded together and shaped, and the spoiler column is inserted into the spoiler hole reserved in the outer mold so that both ends of the spoiler column extend out of the outer mold surface; Step S5, using chemical vapor infiltration process to prepare boron nitride interface and silicon carbide matrix of the blade; after the boron nitride interface is prepared, the hard paper padded by the heat dissipation slit at the tail of the blade is removed, and a high-density C / SiC composite strip of the same height is padded in the local area of ​​the slit as support, and when the density of the blade matrix reaches the required density, the inner mold and the outer mold are removed; Step S6, continue to prepare the silicon carbide matrix for the blade, and when the density of the blade matrix reaches the final required density, perform mechanical processing according to the actual size requirements of the blade to obtain a blade equipped with a spoiler column.

2. The preparation method according to claim 1, characterized in that: In step S1, the process of shaping the fiber cloth into a flat plate of required thickness is as follows: the fiber cloth is laid flat and fixed tightly with a flat plate mold of corresponding size.

3. The preparation method according to claim 1, characterized in that: In step S1, the boron nitride interface and silicon carbide substrate are prepared on the flat plate, and the density of the flat plate substrate is required to be greater than 1.4 g / cm 3 ; Process the flat plate into a spoiler column of the required size, leaving a 15mm to 20mm margin on one side in the length direction.

4. The preparation method according to claim 1, characterized in that: The step S2 further comprises: According to the size and position of the blade spoiler column, the corresponding spoiler holes are processed.

5. The preparation method according to claim 1, characterized in that: In step S5, the blade substrate requires a density greater than 1.4 g / cm 3 .

6. The preparation method according to claim 1, characterized in that: In step S6, the final required density of the blade substrate is greater than 2.0 g / cm 3 .

Citation Information

Patent Citations

  • 2D carbon / silicon-silicon carbide composite material pin preparation method and preparation method and structure of 2D carbon / silicon-silicon carbide composite material pin preform

    CN105835455A

  • Ceramic matrix composite turbine guide blade with turbulent flow structures and preparation method thereof

    CN113898417A

  • Preparation method of SiC / SiC ceramic composite blade body component with tiny turbulent flow column cooling gaps

    CN113929467A

  • Ceramic matrix composite turbine rotor blade with internal cooling channels, mold and preparation method

    CN114427481A

  • Preparation method of ceramic matrix composite multi-cavity structure high-pressure turbine guide blade

    CN117774081A