Method for pressing grain containing aluminum powder

By preheating and talc powder for NTO-based aluminum-containing powder and mold, combined with precise control of environment and pressing parameters, the problem of cracks and density unstable in the pressing process of large-sized medicine columns is solved, and stability and appearance are obtained Upgrade.

CN118930387APending Publication Date: 2024-11-12GUOYING CHANGHONG MASCH FACTORY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411067787.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-06
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

When pressing large-size columns of NTO-based aluminum-containing powder, cracks, density and size unstable occur, and there is a lack of effective processing technology.

Method used

By preheating the powder and mold, applying talc powder into the mold, adjusting the mold taper and calculating the pressing force, setting appropriate pressing parameters, including ambient temperature and pressure control, ensuring the stability of the pressing process.

Benefits of technology

It achieves density and size stability, has a smooth and tidy appearance, and is not prone to cracks when removed from the mold, reducing the scrap rate.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004979854170000021
    Figure BDA0004979854170000021
  • Figure BDA0004979854170000031
    Figure BDA0004979854170000031
  • Figure FDA0004979854160000011
    Figure FDA0004979854160000011
Patent Text Reader

Abstract

The invention relates to a method for pressing a grain containing aluminum powder, and provides a pressing method aiming at the problems that when NTO-based aluminum-containing powder is used for pressing a large-size grain with the diameter of 210-230 mm, cracks are prone to occurring, the density and the size are unstable, and the rejection rate is high, namely, firstly, the powder and a mold are preheated, meanwhile, it is checked that the taper of the mold meets 1 / 200-1 / 250, talcum powder is smeared in the mold to assist in demolding, and then the powder is pressed; calculating pressing force according to the diameter of the grain, and finally setting pressing parameters and finishing pressing. When the method is used for pressing the NTO-based aluminum-containing powder grain with the diameter of 210 mm-230 mm, a product which is stable in density and size, smooth and neat in appearance and not prone to cracking after demolding can be obtained, and the method can be popularized and applied to pressing production of NTO-based aluminum-containing powder of more sizes.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of powder charging technology, and relates to an invention of a processing method for a large-size NTO-based aluminum-containing powder column. Background Art

[0002] NTO-based aluminum-containing powder is a new type of insensitive powder. It has been widely used abroad. Its application in China is still in its initial stage. There is a lack of experience, data and methods for the processing of large-sized NTO-based aluminum-containing powder columns. Currently, no literature or patents on the processing technology applicable to large-sized NTO-based aluminum-containing powder columns have been found. Summary of the invention

[0003] In view of the problems of cracks, unstable density and size, and high scrap rate when NTO-based aluminum-containing powder is pressed into large-sized drug columns with a diameter of 210mm to 230mm, the present invention proposes a pressing method, that is, preheating the powder and the mold, checking that the mold taper meets 1 / 200 to 1 / 250, applying talcum powder in the mold to assist demolding, and then calculating the pressing force according to the size of the drug column, and finally setting the pressing parameters and completing the pressing. The product with stable density and size, smooth and neat appearance, and not easy to crack when demolding can be obtained, which can be promoted and applied to the pressing production of NTO-based aluminum-containing powder of more sizes.

[0004] A method for processing a powder-containing aluminum column is suitable for pressing a column with a diameter of 210 mm to 230 mm. The pressing steps are as follows:

[0005] Step 1. The ambient temperature of the pressing site should be 25°C and the relative humidity should be 45%;

[0006] Step 2. Take out the powder and weigh it. The weighing accuracy should reach 0.1g.

[0007] Step 3. Put the powder into a non-ferrous metal tray and spread it flat with a thickness of no more than 25 mm; preheat it in an explosion-proof oven at 60°C to 65°C for 1h to 1.5h;

[0008] Step 4. Check that the taper of the pill pressing mold sleeve is 1 / 200 to 1 / 250. Place the pill pressing mold in an oven and preheat at 65°C to 70°C for 1h to 1.5h;

[0009] Step 5. Apply a layer of 3000 mesh talcum powder evenly on the mold base, the inner wall of the mold sleeve, and the upper punch;

[0010] Step 6. Evenly and naturally load the powder into the medicine pressing mold, and use a wooden tool to flatten the surface of the powder;

[0011] Step 7. Calculate the compression pressure F according to the radius r of the medicine column. The specific pressure P is 1500. The calculation formula is:

[0012]

[0013] Where F is the pressure of medicine, N;

[0014] P—compression ratio, kg / cm2;

[0015] r—grain column radius, mm;

[0016] Step 8. According to the calculated pressure, set the medicine pressing parameters, where the pressing speed is not more than 0.3 mm / s, the demolding speed is not more than 0.5 mm / s, and the holding time is 20 min to 30 min;

[0017] Step 9. Start the medicine pressing equipment, complete the medicine column pressing and demolding. DETAILED DESCRIPTION

[0018] The specific implementation of the present invention is described below by taking the compression of a drug column with a drug column diameter of 220 mm, a height of 100 mm, and a density of 1.84 g / cm3 as an example.

[0019] Step 1. Use air conditioning and dehumidifier to adjust the ambient temperature of the medicine pressing site to 25°C and the relative humidity to 45%; Step 2. Calculate the volume of the medicine column based on its diameter of 220mm and height of 100mm; then calculate the theoretical dosage of medicine based on its density of 1.84g / cm3 to be 6994.4g, and consider the loss of medicine pressing, so the dosage is set to 6995g; take out the medicine powder and weigh it using an explosion-proof balance, with a weighing accuracy of 0.1g.

[0020] Step 3. Spread the weighed powder evenly on an aluminum tray with a thickness of about 20 mm. Open the explosion-proof oven, set the oven temperature to 62.5°C, and after the temperature stabilizes, preheat the powder for 1.2 hours.

[0021] Step 4. Use an internal micrometer to check that the taper of the mold sleeve is 1 / 200. Place the mold in an oven and set the temperature to 67.5°C. After the temperature stabilizes, preheat the mold for 1.2 hours.

[0022] Step 5. Take out the preheated mold and wrap a layer of heat-insulating cotton on the outer surface of the mold; quickly assemble the medicine pressing mold and clean it, and evenly apply a layer of 3000 mesh talcum powder on the mold base, the inner wall of the mold sleeve, and the upper punch. Step 6. Evenly and naturally load the preheated powder into the medicine pressing mold, and use a wooden tool to flatten the surface of the powder. Step 7. According to the diameter of the medicine column of 220mm (radius r110mm), calculate the pressing pressure F. When calculating, the specific pressure P is taken as 1500, and the calculated pressure is 5699100N.

[0023]

[0024] Where F is the pressure of medicine, N;

[0025] P—compression ratio, kg / cm2;

[0026] r—grain column radius, mm;

[0027] Step 8. Start the medicine pressing equipment, input and set the pressing parameters to 5699100N, the pressing speed to 0.3mm / s, the demolding speed to 0.5mm / s, and the holding time to 25min.

[0028] Step 9. The operation process of pressing the medicine equipment completes the pressing and demolding of the medicine column.

[0029] The method provided in the present invention can effectively solve the problems of cracks, density and unstable external dimensions in large-sized NTO-based aluminum-containing powder columns, and can effectively solve the problem of pressing large-sized NTO-based aluminum-containing powders.

Claims

1. A method for pressing a powder-containing aluminum column, characterized in that: Step 1. The processing environment temperature should be between 15℃ and 35℃, and the relative humidity should be between 30% and 50%; Step 2. Take out the powder and weigh it. The weighing accuracy should reach 0.1g. Step 3. Put the powder into a non-ferrous metal tray and spread it flat with a thickness of no more than 25 mm; preheat it in an explosion-proof oven at 60°C to 65°C for 1h to 1.5h; Step 4. Check that the taper of the pill pressing mold sleeve is 1 / 200 to 1 / 250; put the pill pressing mold and mold sleeve into an oven and preheat at 65°C to 70°C for 1h to 1.5h; Step 5. Take out the preheated mold and wrap a layer of insulation cotton on the outer surface of the mold; quickly assemble the medicine pressing mold and clean it, and evenly apply a layer of talcum powder on the mold base, the inner wall of the mold sleeve, and the upper punch. The talcum powder is 3000 mesh; Step 6. Evenly and naturally load the powder into the medicine pressing mold, and use a wooden tool to flatten the surface of the powder; Step 7. Calculate the compression pressure F according to the radius r of the medicine column. The specific pressure P is 1500. The calculation formula is: Where F is the pressure of medicine, N; P—compression ratio, kg / cm2; r—grain column radius, mm; Step 8. According to the calculated pressure, set the pressing parameters, where the pressing speed is not more than 0.3 mm / s, the demolding speed is not more than 0.5 mm / s, and the holding time is 20 min to 30 min.