Waterborne polyurethane dispersion, preparation method thereof and polyurethane adhesive
By using a mixing reaction of specific components in aqueous polyurethane adhesives, the problem of insufficient tensile strength and elongation at break is solved, and the improvement of high tensile strength and elongation at break is achieved, which is suitable for high temperature and high humidity environments.
Patent Information
- Application Number
- CN202410984676.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-22
- Publication Date
- 2024-11-12
AI Technical Summary
The tensile strength and elongation of breaking existing water-based polyurethane adhesives are poor, making it difficult to meet certain application needs.
Crosslinking agents, radical initiators, hydrophilic chain extenders, amine chain extenders, ocyanates, polyethylene glycol chain extenders and carbon-carbon double bonds using polyester polyols, amine chain extenders, and capping agents. The mixture is carried out with components such as organic solvents to form an aqueous polyurethane dispersion with high tensile strength and elongation of break.
It significantly improves the tensile strength and elongation of breaking water-based polyurethane, enhances its stability and adhesion in aqueous media, and is suitable for high temperature and high humidity environments.
Smart Images

Figure CN118930751A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of adhesives, and in particular relates to an aqueous polyurethane dispersion and a preparation method thereof, and a polyurethane adhesive. Background Art
[0002] Polyurethane water dispersion adhesives have the advantages of excellent wear resistance, chemical corrosion resistance, good flexibility, good adhesion, high gloss, low volatile organic solvent content, non-toxic, non-flammable, no odor, no pollution to the environment, no health hazards to operators, etc., which is the key development direction of polyurethane adhesives. Water-based polyurethane adhesives are synthetic water-based adhesive products that are focused on development in my country. Because polyurethane adhesives have good bonding properties, they have been widely used in industries such as footwear, clothing, construction, automobiles, food packaging, kitchen supplies, and composite films. Its characteristics are that the dispersion contains no or only a very small amount of organic solvents, and at the same time has the inherent advantages of wear resistance and high strength of general polyurethanes. However, the current water-based polyurethanes have poor tensile strength and poor elongation at break.
[0003] Therefore, the research on waterborne polyurethane adhesives needs to be further deepened. Summary of the invention
[0004] The present invention aims to solve one of the technical problems in the related art at least to a certain extent. To this end, one object of the present invention is to provide an aqueous polyurethane dispersion and a preparation method thereof, and an adhesive, wherein the aqueous polyurethane obtained by the method provided by the present application has high tensile strength and elongation at break.
[0005] In the first aspect of the present invention, the present invention provides a method for preparing an aqueous polyurethane dispersion. According to an embodiment of the present invention, the method comprises: mixing polyester polyol, hydroxyl-containing acrylate, isocyanate, a crosslinking agent containing a polyethylene glycol segment and a carbon-carbon double bond, a free radical initiator, a hydrophilic chain extender, an amine chain extender, a capping agent, an organic solvent and water to obtain an aqueous polyurethane dispersion; the structural formula of the hydroxyl-containing acrylate is:
[0006]
[0007] Wherein, R is any one of a C1-C9 alkane, a benzene ring or a saturated aliphatic ring;
[0008] X represents any one of hydroxyl group and hydrogen;
[0009] Y represents any one of hydrogen and methyl.
[0010] According to the preparation method of the above embodiment of the present invention, the hydroxyl groups in the hydroxyl-containing acrylate and the polyester polyol can react with the isocyanate groups in the isocyanate to form a carbamate bond (-NHCOO-), so that the carbon-carbon double bond groups in the hydroxyl-containing acrylate can be introduced into the side chains of the polymer molecules, providing active sites for subsequent polymerization reactions. Under the action of a free radical initiator, the carbon-carbon double bonds in the hydroxyl-containing acrylate can be polymerized with the carbon-carbon double bonds in the cross-linking agent containing a polyethylene glycol segment and a carbon-carbon double bond, increasing the cross-linking points between molecules, forming a denser three-dimensional network structure, providing better support, increasing the ability to resist external forces, and thus improving the tensile strength of the waterborne polyurethane dispersion. In addition, the polyethylene glycol segment can also be introduced into the side chains of the waterborne polyurethane molecules. The presence of the ether chain in the polyethylene glycol segment increases the hydrophilicity of the waterborne polyurethane, helps to form a stable dispersion in the aqueous system, and improves its stability in the aqueous medium. Furthermore, the addition of a hydrophilic chain extender can introduce a hydrophilic group (such as a carboxylate or sulfonate) into the waterborne polyurethane molecule, thereby improving the compatibility of the polyurethane with water and enabling the polyurethane to self-emulsify in water. The addition of an amine chain extender can provide additional amino groups, which react with the isocyanate groups in the isocyanate to form urea groups, thereby increasing the crosslinking density between the polyurethane molecular chains and thus improving the tensile strength of the waterborne polyurethane. The addition of a capping agent can react with the active groups (such as -NCO) in the polymer to terminate the chain growth, thereby controlling the molecular weight of the waterborne polyurethane. The addition of an organic solvent is used to adjust the viscosity of the waterborne polyurethane, facilitating subsequent processing and mixing. Water, as a dispersion medium, reacts with the hydrophilic component to form a stable waterborne polyurethane dispersion.
[0011] Furthermore, in the waterborne polyurethane structure, the polyester polyol contains a relatively long carbon chain, which is soft at room temperature and can constitute a soft segment in the polyurethane structure, providing good flexibility and elasticity. The saturated long carbon chain in the hydrophilic chain extender increases the length and flexibility of the polyurethane molecular chain, which helps to improve the sliding ability between the molecular chains. Therefore, the flexibility of the soft segment and the sliding ability of the long carbon chain work together to improve the elongation at break of the waterborne polyurethane. Thus, the waterborne polyurethane obtained by the method provided by the present application has high tensile strength and elongation at break.
[0012] In addition, the preparation method according to the above embodiment of the present invention may also have the following additional technical features:
[0013] In some embodiments of the present invention, the hydroxyl-containing acrylate comprises at least one of the chemical formulas (1) to (3):
[0014]
[0015]
[0016] In some embodiments of the present invention, the method comprises: S1, mixing polyester polyol and hydroxyl-containing acrylate for the first time, and performing a first reduced pressure distillation to obtain a mixture A; S2, mixing the mixture A and isocyanate for the second time to obtain a mixture B; S3, mixing the mixture B, a crosslinker containing a polyethylene glycol segment and a carbon-carbon double bond, and a free radical initiator for the third time to obtain a mixture C; S4, mixing the mixture C and an organic solvent for the fourth time to obtain a polyurethane prepolymer; S5, mixing the polyurethane prepolymer and a hydrophilic chain extender for the fifth time to obtain a mixture D; S6, mixing the mixture D, an amine chain extender, a capping agent, and water for the sixth time, and performing a second reduced pressure distillation to obtain an aqueous polyurethane dispersion. Thus, the obtained aqueous polyurethane has high tensile strength and elongation at break.
[0017] In some embodiments of the present invention, the mass ratio of the polyester polyol to the hydroxyl-containing acrylate is 1:(0.01-0.05). This is conducive to obtaining a waterborne polyurethane with a higher elongation at break.
[0018] In some embodiments of the present invention, the number average molecular weight of the polyester polyol is 1000-4000. Thus, the emulsification effect of the polyurethane can be improved.
[0019] In some embodiments of the present invention, the polyester polyol includes at least one of polybutylene adipate diol, polyhexane adipate diol, polycaprolactone diol, and polycarbonate diol, thereby improving the emulsification effect of polyurethane.
[0020] In some embodiments of the present invention, the temperature of the first reduced pressure distillation is 100° C.-130° C. Thus, small molecules such as water that may exist therein are removed to prevent the curing reaction between water and the polyurethane raw material and affect the stability of the emulsion.
[0021] In some embodiments of the present invention, the pressure of the first reduced pressure distillation is less than -0.08 MPa, so as to remove small molecules such as water that may exist therein, and avoid curing reaction between water and polyurethane raw materials, which affects the stability of the emulsion.
[0022] In some embodiments of the present invention, the first reduced pressure distillation lasts for 1 hour to 3 hours, thereby removing small molecules such as water that may exist therein, and preventing water from reacting with the polyurethane raw material to cure and affect the stability of the emulsion.
[0023] In some embodiments of the present invention, the mass of water in the mixture A is 0.05%-0.1% based on the total mass of the mixture A. Thus, it is possible to avoid the occurrence of a situation where water reacts with isocyanate groups to form ammonium carbamate salts.
[0024] In some embodiments of the present invention, the temperature of the second mixing is 40° C. to 80° C. This is conducive to obtaining a waterborne polyurethane with higher tensile strength and elongation at break.
[0025] In some embodiments of the present invention, the isocyanate includes at least one of hexamethylene diisocyanate, isophorone diisocyanate, toluene diisocyanate, dicyclohexylmethane diisocyanate, tetramethylxylylene diisocyanate, dicyclohexylmethane diisocyanate, polymethylene polyphenyl polyisocyanate, and xylylene diisocyanate. Thus, it is beneficial to obtain a waterborne polyurethane with higher tensile strength and elongation at break.
[0026] In some embodiments of the present invention, the isocyanate includes hexamethylene diisocyanate and isophorone diisocyanate, thereby facilitating the acquisition of a polyurethane prepolymer with a higher molecular weight.
[0027] In some embodiments of the present invention, the mass ratio of the hexamethylene diisocyanate to the isophorone diisocyanate is (90-70):(10-30). Thus, a polyurethane prepolymer with a higher molecular weight can be obtained.
[0028] In some embodiments of the present invention, the molar ratio of the isocyanate group in the isocyanate to the hydroxyl group in the mixture A is (1.01-2.5): 1. This is beneficial to improve the tensile strength and elongation at break of the waterborne polyurethane.
[0029] In some embodiments of the present invention, the third mixing time is 1 to 2 hours, thereby providing sufficient time for various reactions to proceed, ensuring that the polymerization reaction between the carbon-carbon double bonds in the mixture B and the carbon-carbon double bonds in the cross-linking agent containing polyethylene glycol segments and carbon-carbon double bonds can proceed more fully.
[0030] In some embodiments of the present invention, the cross-linking agent containing polyethylene glycol segments and carbon-carbon double bonds includes at least one of polyethylene glycol monoacrylate and polyethylene glycol diacrylate. Thus, under the action of a free radical initiator, a polymerization reaction can occur with other molecules containing carbon-carbon double bonds to form a three-dimensional cross-linked network, thereby improving the cohesion and strength of the waterborne polyurethane.
[0031] In some embodiments of the present invention, the free radical initiator includes at least one of azobisisobutyronitrile and dibenzoyl peroxide. Thus, the free radical initiator can rapidly decompose to generate free radicals during the polymerization process, react with the cross-linking agent containing carbon-carbon double bonds, and start the growth of the polymer chain.
[0032] In some embodiments of the present invention, the temperature of the fourth mixing is 20° C. to 60° C. Thus, the organic solvent is more easily mixed with the polyurethane prepolymer, and the problem of excessively high or low local concentration is reduced.
[0033] In some embodiments of the present invention, the organic solvent includes acetone. Thus, the viscosity of the polyurethane prepolymer can be significantly reduced, making it easier to stir and mix.
[0034] In some embodiments of the present invention, the mass ratio of the polyurethane prepolymer to the hydrophilic chain extender is (70-99):(0.8-20). This helps to form a smaller emulsion particle size, thereby improving the stability of the polyurethane emulsion.
[0035] In some embodiments of the present invention, the hydrophilic chain extender includes at least one of a carboxylate and a sulfonate, thereby being able to introduce a hydrophilic group (such as a carboxylate or a sulfonate) into the waterborne polyurethane molecule, forming hydrogen bonds with water molecules, and improving the solubility and stability of the polyurethane prepolymer in water.
[0036] In some embodiments of the present invention, the amine chain extender includes ethylenediamine, which can react with the isocyanate groups in the prepolymer to form urethane bonds, thereby increasing the length and complexity of the polyurethane chain.
[0037] In some embodiments of the present invention, the end-capping agent includes at least one of succinimidyl alcohol and ethanolamine, thereby being able to react with active groups (such as unreacted isocyanate groups) in the prepolymer to terminate chain growth and control molecular weight and molecular weight distribution.
[0038] In the second aspect of the present invention, the present application provides an aqueous polyurethane dispersion, which is prepared by the above method. The aqueous polyurethane dispersion has high stability and adhesion.
[0039] In some embodiments of the present invention, the mass proportion of the aqueous polyurethane in the aqueous polyurethane dispersion is 40% to 75%.
[0040] In the third aspect of the present invention, the present application provides a polyurethane adhesive, comprising the above-mentioned aqueous polyurethane dispersion. Thus, the obtained polyurethane adhesive has strong bonding force, good high temperature and humidity resistance, strong mechanical properties and excellent hydrophilicity, and the two-component polyurethane adhesive has a large molecular weight, high solid content and high crosslinking degree.
[0041] Additional aspects and advantages of the present invention will be given in part in the following description and in part will be obvious from the following description, or will be learned through practice of the present invention. BRIEF DESCRIPTION OF THE DRAWINGS
[0042] The above and / or additional aspects and advantages of the present invention will become apparent and easily understood from the description of the embodiments in conjunction with the following drawings, in which:
[0043] Figure 1 The flowchart of the preparation method of the aqueous polyurethane dispersion of the embodiment of the present application is shown. DETAILED DESCRIPTION
[0044] Embodiments of the present invention are described in detail below, examples of which are shown in the accompanying drawings, wherein the same or similar reference numerals throughout represent the same or similar elements or elements having the same or similar functions. The embodiments described below are exemplary and are intended to be used to explain the present invention, and should not be construed as limiting the present invention.
[0045] In the first aspect of the present invention, the present invention provides a method for preparing an aqueous polyurethane dispersion. According to an embodiment of the present invention, the method comprises: mixing polyester diol, hydroxyl-containing acrylate, isocyanate, a crosslinking agent containing a polyethylene glycol segment and a carbon-carbon double bond, a free radical initiator, a hydrophilic chain extender, an amine chain extender, a capping agent, an organic solvent and water to obtain an aqueous polyurethane dispersion; wherein the structural formula of the hydroxyl-containing acrylate is:
[0046]
[0047] Wherein, R is any one of a C1-C9 alkane, a benzene ring or a saturated aliphatic ring;
[0048] X represents any one of hydroxyl group or hydrogen;
[0049] Y represents either hydrogen or methyl.
[0050] According to the preparation method of the above embodiment of the present invention, the hydroxyl groups in the hydroxyl-containing acrylate and the polyester polyol can react with the isocyanate group in the isocyanate to form a carbamate bond (-NHCOO-), so that the carbon-carbon double bond group in the hydroxyl-containing acrylate can be introduced into the side chain of the polymer molecule, which can provide an active site for the subsequent polymerization reaction. Under the action of a free radical initiator, the carbon-carbon double bond in the hydroxyl-containing acrylate can be polymerized with the carbon-carbon double bond in the cross-linking agent containing a polyethylene glycol segment and a carbon-carbon double bond, increasing the cross-linking points between molecules, forming a denser three-dimensional network structure, providing better support, and increasing the ability to resist external forces, thereby improving the tensile strength of the waterborne polyurethane dispersion. In addition, the polyethylene glycol segment can also be introduced into the side chain of the waterborne polyurethane molecule. The presence of the ether chain in the polyethylene glycol segment increases the hydrophilicity of the waterborne polyurethane, helps to form a stable dispersion in the aqueous system, and improves its stability in the aqueous medium. Furthermore, the addition of a hydrophilic chain extender can introduce a hydrophilic group (such as a carboxylate or sulfonate) into the waterborne polyurethane molecule, thereby improving the compatibility of the polyurethane with water and enabling the polyurethane to self-emulsify in water. The addition of an amine chain extender can provide additional amino groups, which react with the isocyanate groups in the isocyanate to form urea groups, thereby increasing the crosslinking density between the polyurethane molecular chains and thus improving the tensile strength of the waterborne polyurethane. The addition of a capping agent can react with the active groups in the polymer (such as the isocyanate group -NCO) to terminate the chain growth, thereby controlling the molecular weight of the waterborne polyurethane. The addition of an organic solvent is used to adjust the viscosity of the waterborne polyurethane, which is convenient for subsequent processing and mixing. Water, as a dispersion medium, reacts with the hydrophilic component to form a stable waterborne polyurethane dispersion.
[0051] Furthermore, in the waterborne polyurethane structure, the polyester polyol contains a relatively long carbon chain, which is soft at room temperature and can constitute a soft segment in the polyurethane structure, providing good flexibility and elasticity. The saturated long carbon chain in the hydrophilic chain extender increases the length and flexibility of the polyurethane molecular chain, which helps to improve the sliding ability between the molecular chains. Therefore, the flexibility of the soft segment and the sliding ability of the long carbon chain work together to improve the elongation at break of the waterborne polyurethane. Thus, the waterborne polyurethane obtained by the method provided by the present application has high tensile strength and elongation at break.
[0052] According to some specific embodiments of the present invention, the hydroxyl-containing acrylate comprises at least one of chemical formula (1) to chemical formula (3):
[0053]
[0054] By selecting the above-mentioned hydroxyl-containing acrylate, the hydroxyl-containing acrylate contains multiple hydroxyl groups, and the hydroxyl group can react with the isocyanate group in the isocyanate to form a carbamate bond (-NHCOO-), so that the carbon-carbon double bond group in the hydroxyl-containing acrylate can be introduced into the side chain of the polymer molecule, which can provide an active site for the subsequent polymerization reaction. Further, under the action of a free radical initiator, the carbon-carbon double bond in the hydroxyl-containing acrylate can be polymerized with the carbon-carbon double bond in the cross-linking agent containing a polyethylene glycol segment and a carbon-carbon double bond, increasing the crosslinking points between molecules, forming a denser three-dimensional network structure, providing better support, and increasing the ability to resist external forces, thereby improving the tensile strength of the waterborne polyurethane dispersion. In addition, the polyethylene glycol segment can also be introduced into the side chain of the waterborne polyurethane molecule. The presence of the ether chain in the polyethylene glycol segment increases the hydrophilicity of the waterborne polyurethane, helps to form a stable dispersion in the aqueous system, and improves its stability in the aqueous medium. Thus, the tensile strength of the waterborne polyurethane dispersion can be improved.
[0055] It should be noted that chemical formula (2) and chemical formula (3) are self-made, wherein chemical formula (2) is prepared by esterification reaction of methacrylic acid with 1,2,4-butanetriol (CAS: 44603-18-1), and chemical formula (3) is prepared by esterification reaction of methacrylic acid with 1,2,8-octantriol (CAS: 382631-43-8).
[0056] According to some specific embodiments of the present invention, Figure 1 , the preparation method comprises the following steps:
[0057] S1. Mixing polyester diol and hydroxyl-containing acrylate for the first time, and performing reduced pressure distillation for the first time to obtain a mixture A.
[0058] In this step, the polyester polyol and the hydroxyl-containing acrylate are mixed for the first time to form a prepolymer, and then the small molecular substances and water in the polyester polyol are removed by the first reduced pressure distillation to obtain a mixture A.
[0059] According to some specific embodiments of the present invention, the mass ratio of the polyester polyol and the hydroxyl-containing acrylate is 1:(0.01-0.05). For example, it can be 1:0.01, 1:0.02, 1:0.03, 1:0.05, etc. Polyester polyol is the main raw material for forming the soft segment of polyurethane. The hydroxyl group in the polyester polyol can react with the isocyanate group of isocyanate to form a carbamate bond (-NHCOO-). The carbamate bond can be used as a linking point to connect the soft segment (such as polyester polyol) in polyurethane with the hard segment (such as isocyanate and chain extension monomer) to form a soft and hard segmented waterborne polyurethane structure, so that the waterborne polyurethane has flexibility and elasticity, etc., which is conducive to improving the elongation at break and tensile strength of the waterborne polyurethane. If the content of hydroxyl-containing acrylate is high, it will cause the reaction degree to be difficult to control, easy to gel, and the elongation at break of the formed polyurethane will be reduced. If the content of hydroxyl-containing acrylate is low, the proportion of the introduced polyethylene glycol segment is small, which will cause the hydrophilicity of the polyurethane to be poor, the emulsion particle size to be large, and the storage stability to be poor. Therefore, by limiting the ratio of the polyester polyol to the hydroxyl-containing acrylate within the above range, it is advantageous to obtain an aqueous polyurethane having a higher elongation at break.
[0060] According to some specific embodiments of the present invention, the number average molecular weight of the polyester polyol is 1000-4000. For example, it can be 1000, 2000, 3000, 4000, etc. By limiting the number average molecular weight of the polyester polyol to the above range, the emulsification effect of polyurethane can be improved. The polyester polyol can be obtained by methods well known in the art, or can be obtained commercially, such as various polyester polyols purchased from Huide Technology Company.
[0061] As an example, the polyester polyol includes, but is not limited to, at least one of polybutylene adipate diol, polyhexamethylene adipate diol, polycaprolactone diol, polycarbonate diol, and the like.
[0062] According to some specific embodiments of the present invention, the temperature of the first vacuum distillation is 100° C.-130° C. For example, it can be 100° C., 110° C., 120° C., 130° C., etc. By limiting the temperature of the first vacuum distillation to the above range, small molecules such as water that may exist therein can be removed, and curing reaction between water and polyurethane raw materials can be avoided to affect the stability of the emulsion, which is conducive to obtaining a water-based polyurethane with higher tensile strength and elongation at break.
[0063] According to some specific embodiments of the present invention, the pressure of the first vacuum distillation is less than -0.08 MPa. For example, it can be -0.08 MPa, -0.1 MPa, -0.2 MPa, etc. By limiting the pressure of the first vacuum distillation to the above range, small molecules such as water that may exist therein can be removed, and curing reaction between water and polyurethane raw materials can be avoided to affect the stability of the emulsion, which is conducive to obtaining a water-based polyurethane with higher tensile strength and elongation at break.
[0064] According to some specific embodiments of the present invention, the time of the first vacuum distillation is 1h-3h. For example, it can be 1h, 2h, 3h, etc. By limiting the time of the first vacuum distillation to the above range, small molecules such as water that may exist therein can be removed, and curing reaction between water and polyurethane raw materials can be avoided to affect the stability of the emulsion, which is conducive to obtaining a water-based polyurethane with higher tensile strength and elongation at break.
[0065] According to some specific embodiments of the present invention, based on the total mass of the mixture A, the mass proportion of water in the mixture A is 0.05%-0.1%. For example, it can be 0.05%, 0.07%, 0.09%, 0.1%, etc. The water in the mixture A will consume the isocyanate groups, resulting in insufficient isocyanate groups required for subsequent reactions, and the chain extender in the subsequent chain extension cannot be completely bonded to the polyurethane molecules, thereby affecting the final product structure and performance. Therefore, by limiting the mass proportion of water in the mixture A to the above range, the consumption of isocyanate groups by water in the mixture A can be effectively reduced.
[0066] S2, mixing the mixture A and isocyanate for a second time to obtain a mixture B.
[0067] In this step, a mixture B is obtained by mixing and stirring a mixture A containing a hydroxyl group and an isocyanate.
[0068] According to some specific embodiments of the present invention, the temperature of the second mixing is 40° C. to 80° C. For example, it can be 40° C., 50° C., 60° C., 70° C., 80° C., etc. By limiting the temperature of the second mixing to the above range, side reactions or polymer degradation caused by excessively high temperature can be avoided, while ensuring that the reaction is carried out under controllable conditions, which is conducive to obtaining a waterborne polyurethane with higher tensile strength and elongation at break.
[0069] As an example, the isocyanate includes but is not limited to at least one of hexamethylene diisocyanate, isophorone diisocyanate, toluene diisocyanate, dicyclohexylmethane diisocyanate, tetramethylxylylene diisocyanate, di-cyclohexylmethane diisocyanate, polymethylene polyphenyl polyisocyanate, and xylylene diisocyanate.
[0070] According to some specific embodiments of the present invention, the isocyanate includes hexamethylene diisocyanate and isophorone diisocyanate. In a mixed system, hexamethylene diisocyanate and isophorone diisocyanate can react with compounds containing active hydrogen (such as polyols, water or amines) to form carbamate or urea bonds, which can constitute the hard segment of polyurethane, improve the Young's modulus (i.e., stiffness) of polyurethane, make the waterborne polyurethane less deformed when subjected to force, and help improve the tensile strength of waterborne polyurethane.
[0071] According to some specific embodiments of the present invention, the mass ratio of the hexamethylene diisocyanate and the isophorone diisocyanate is (90-70): (10-30). For example, it can be 90:10, 80:20, 70:30, etc. Since the structure of hexamethylene diisocyanate is symmetrical and regular, if it accounts for a large proportion, it is conducive to the rapid crystallization of waterborne polyurethane, so that the obtained glue layer has a large strength; isophorone diisocyanate has a small contribution to the crystallization of waterborne polyurethane, but because the activity difference of its two isocyanate groups is large, usually only one participates in the reaction, and it can be used as a capping agent. The retained isocyanate group reacts with the highly active amino group in the post-emulsification stage, further extending the chain, and further increasing the molecular weight of the waterborne polyurethane. Thus, a polyurethane prepolymer with a higher molecular weight can be obtained.
[0072] According to some specific embodiments of the present invention, the molar ratio of the isocyanate groups in the isocyanate to the hydroxyl groups in the mixture A is (1.01-2.5): 1. For example, it can be 1.01: 1, 2: 1, 2.5: 1, etc. By limiting the molar ratio of the isocyanate groups in the isocyanate to the hydroxyl groups in the mixture A within the above range, the polyurethane can take into account the mechanical characteristics of the polyester polyol, high tensile strength and elongation at break. At the same time, hydrophilic modification can be achieved, and reactive crosslinking points can be introduced later. When the molar ratio of the isocyanate groups in the isocyanate to the hydroxyl groups in the mixture A is too low, it is difficult for the polyurethane to introduce enough hydrophilic groups to achieve chain extension and cannot achieve water dispersion. When the molar ratio of the isocyanate groups in the isocyanate to the hydroxyl groups in the mixture A is too high, the proportion of the introduced chain extender increases, the rigid segment is enhanced, and the hardness of the polyurethane is too high and the molecular weight is too small, which ultimately leads to a small elongation at break and low tensile strength. Thus, by limiting the molar ratio of the isocyanate group in the isocyanate to the hydroxyl group in the mixture A within the above range, the tensile strength and the elongation at break of the waterborne polyurethane can be improved.
[0073] S3, mixing the mixture B, the cross-linking agent containing polyethylene glycol segments and carbon-carbon double bonds, and the free radical initiator for a third time to obtain a mixture C.
[0074] In this step, the mixture B, the cross-linking agent containing polyethylene glycol segments and carbon-carbon double bonds, and the free radical initiator are mixed for the third time. Specifically, in the mixing process of step 2, isocyanate is added to the mixture A, and after the isocyanate content in the reaction system is tracked and determined by chemical titration to reach a theoretical value, the cross-linking agent containing polyethylene glycol segments and carbon-carbon double bonds and the free radical initiator are added. Under the action of the free radical initiator, the carbon-carbon double bonds in the mixture B can undergo polymerization reaction with the carbon-carbon double bonds in the cross-linking agent containing polyethylene glycol segments and carbon-carbon double bonds, increasing the cross-linking points between molecules and forming a denser three-dimensional network structure, which can provide better support and increase the ability to resist external forces, thereby improving the tensile strength of the waterborne polyurethane dispersion. The three-dimensional network structure can also provide better energy absorption capacity, can withstand greater deformation without breaking during the stretching process, and is conducive to improving the elongation at break of the waterborne polyurethane dispersion. In addition, polyethylene glycol segments can be introduced into the side chains of waterborne polyurethane molecules. The ether chains in the polyethylene glycol segments increase the hydrophilicity of the waterborne polyurethane, help form a stable dispersion in the aqueous system, and improve its stability in the aqueous medium, thereby obtaining mixture C.
[0075] According to some specific embodiments of the present invention, the third mixing time is 1 hour to 2 hours. For example, it can be 1 hour, 1.5 hours, 2 hours, etc. By limiting the third mixing time to the above range, sufficient time can be provided for various reactions to proceed, ensuring that the polymerization reaction of the carbon-carbon double bonds in the mixture B and the carbon-carbon double bonds in the cross-linking agent containing polyethylene glycol segments and carbon-carbon double bonds can proceed more fully.
[0076] According to some specific embodiments of the present invention, the cross-linking agent containing polyethylene glycol segments and carbon-carbon double bonds includes at least one of polyethylene glycol methacrylate and polyethylene glycol diacrylate. The carbon-carbon double bonds in polyethylene glycol monoacrylate or polyethylene glycol diacrylate can undergo polymerization reaction with other molecules containing carbon-carbon double bonds under the action of a free radical initiator, increase the cross-linking points between molecules, form a denser three-dimensional network structure, provide better support, increase the ability to resist external forces, thereby improving the tensile strength of the aqueous polyurethane dispersion, and the three-dimensional network structure can also provide better energy absorption capacity, can withstand greater deformation without breaking during the stretching process, and is conducive to improving the elongation at break of the aqueous polyurethane dispersion. In addition, the polyethylene glycol segment can also be introduced into the side chain of the aqueous polyurethane molecule, and the ether chain in the polyethylene glycol segment has a higher hydrophilicity, can form hydrogen bonds with water molecules, increase the hydrophilicity of the aqueous polyurethane, help to form a stable dispersion in the aqueous system, and improve its stability in the aqueous medium.
[0077] As an example, the cross-linking agent containing polyethylene glycol segments and carbon-carbon double bonds includes but is not limited to at least one of polyethylene glycol 300 methacrylate, polyethylene glycol 400 dimethacrylate, polyethylene glycol 600 methacrylate and polyethylene glycol 1000 methacrylate.
[0078] It should be noted that polyethylene glycol 300 methacrylate, polyethylene glycol 400 dimethacrylate, polyethylene glycol 600 methacrylate and polyethylene glycol 1000 methacrylate can all be purchased from Aladdin Chemical Reagent, Yongzheng Chemical, McLean Reagent and other companies.
[0079] According to some specific embodiments of the present invention, the free radical initiator includes at least one of azobisisobutyronitrile and dibenzoyl peroxide. The free radical initiator can rapidly decompose and generate free radicals during the polymerization process, react with a cross-linking agent containing a carbon-carbon double bond, start the growth of the polymer chain, form cross-links between polyurethane molecular chains, construct a three-dimensional network structure, provide better support, and increase the ability to resist external forces, thereby improving the tensile strength of the waterborne polyurethane dispersion.
[0080] S4, mixing the mixture C and the organic solvent for the fourth time to obtain a polyurethane prepolymer.
[0081] In this step, by mixing the mixture C and the organic solvent for the fourth time, the viscosity of the mixed system can be adjusted to make it easier to handle and process, so as to obtain a polyurethane prepolymer.
[0082] According to some specific embodiments of the present invention, the temperature of the fourth mixing is 20° C. to 60° C. For example, it can be 20° C., 30° C., 50° C., 60° C., etc. By limiting the temperature of the fourth mixing to the above range, the organic solvent is more easily mixed with the polyurethane prepolymer, reducing the problem of excessively high or low local concentration.
[0083] According to some specific embodiments of the present invention, the organic solvent includes acetone. The addition of acetone can significantly reduce the viscosity of the polyurethane prepolymer, making it easier to stir and mix, and can also serve as a dispersion medium to help the polyurethane prepolymer mix better with other additives or pigments.
[0084] S5. Mixing the polyurethane prepolymer and the hydrophilic chain extender for a fifth time to obtain a mixture D.
[0085] In this step, the polyurethane prepolymer and the hydrophilic chain extender are mixed for the fifth time, specifically, the dripping rate is controlled to be completed within 10 minutes to 30 minutes under high-speed stirring, and the hydrophilic chain extender is added to the polyurethane prepolymer obtained in step S4. After the dripping is completed, the reaction is continued for 20 minutes to 60 minutes under high-speed stirring to obtain a mixture D. The addition of the hydrophilic chain extender can introduce hydrophilic groups (such as carboxylate or sulfonate) into the waterborne polyurethane molecules, can form hydrogen bonds with water molecules, improve the solubility and stability of the polyurethane prepolymer in water, and can also make the polyurethane prepolymer form a stable emulsion or dispersion when mixed with water.
[0086] According to some specific embodiments of the present invention, the mass ratio of the polyurethane prepolymer to the hydrophilic chain extender is (70-99):(0.8-20). For example, it can be 70:0.8, 80:10, 99:20, etc. By limiting the mass ratio of the polyurethane prepolymer to the hydrophilic chain extender to the above range, on the one hand, it is helpful to prepare a high solid content emulsion and can reduce the use of organic solvents. On the other hand, it can make the particle size of the aqueous polyurethane emulsion smaller and the emulsion storage stability better.
[0087] As an example, the hydrophilic chain extender includes, but is not limited to, at least one of carboxylate and sulfonate.
[0088] As an example, the hydrophilic chain extender includes, but is not limited to, at least one of dimethylbutyric acid and sodium 2-(2-aminoethyl)aminoethanesulfonate.
[0089] S6, mixing the mixture D, the amine chain extender, the end-capping agent and water for the sixth time, and performing reduced pressure distillation for the second time to obtain an aqueous polyurethane dispersion.
[0090] In this step, the mixture D, the amine chain extender, the end capping agent and water are mixed for the sixth time, and the amine chain extender reacts with the isocyanate group in the prepolymer to form a carbamate bond, thereby increasing the length and complexity of the polyurethane chain. The end capping agent reacts with the active group (such as unreacted isocyanate group) in the prepolymer to terminate the chain growth and control the molecular weight and molecular weight distribution. Finally, after mixing with water, an aqueous polyurethane dispersion is formed by emulsification, and the hydrophilic chain extender helps to improve the stability of the dispersion. A second vacuum distillation is performed to remove the organic solvent in the reaction system by vacuum distillation, which helps to improve the purity and stability of the final product, so as to obtain an aqueous polyurethane dispersion, and the structure of the aqueous polyurethane contains polyether acrylate groups.
[0091] Further, the chemical structure of polyether acrylate is:
[0092]
[0093] Wherein, Y represents any one of hydrogen and methyl; R represents any one of hydrogen and C1-C6 alkane; X represents hydrogen, methacrylate group and acrylate groups Any one of; n is a positive integer from 1 to 20.
[0094] According to some specific embodiments of the present invention, the amine chain extender includes ethylenediamine. The amine chain extender reacts with the isocyanate group in the prepolymer to form a urethane bond, thereby increasing the length and complexity of the polyurethane chain.
[0095] According to some specific embodiments of the present invention, the end-capping agent includes at least one of succinol and ethanolamine. The end-capping agent reacts with active groups (such as unreacted isocyanate groups) in the prepolymer to terminate chain growth and control molecular weight and molecular weight distribution.
[0096] According to the preparation method of the embodiment of the present application, the hydroxyl groups in the hydroxyl-containing acrylate and the polyester polyol can react with the isocyanate group in the isocyanate to form a carbamate bond (-NHCOO-), so that the carbon-carbon double bond group in the hydroxyl-containing acrylate can be introduced into the side chain of the polymer molecule. Under the action of the free radical initiator, the carbon-carbon double bond in the hydroxyl-containing acrylate can undergo polymerization reaction with the carbon-carbon double bond in the cross-linking agent containing the polyethylene glycol segment and the carbon-carbon double bond, and the polyethylene glycol segment containing the ether chain can be introduced into the side chain of the waterborne polyurethane molecule, thereby enhancing the hydrophilicity of the waterborne polyurethane and realizing polyacrylate modification at the same time, thereby improving the wetting, adhesion and hydrolysis resistance of the waterborne polyurethane dispersion to the low surface tension substrate; further, the addition of the hydrophilic chain extender can introduce the hydrophilic group (such as the carboxylate or sulfonate group) into the waterborne polyurethane molecule, realizing the modification of the hydrophilic group, so that the polyurethane molecule can achieve self-emulsification. The saturated carbon-carbon segments in polyacrylates have low polarity, which can improve the wettability of waterborne polyurethane dispersions on substrates with low surface tension. In addition, the polar ester groups on the acrylate side groups can form hydrogen bonds with the aminomethyl anion ester groups and urea groups in the polyurethane molecules, and the two effectively form an interconductive network. The adhesive prepared with waterborne polyurethane has uniform performance after film formation, excellent hydrolysis resistance, and enhanced adhesion.
[0097] Furthermore, the hydrophilic group acts synergistically with the ether chain in the hydrophilic polyethylene glycol segment, so that the particle size of the waterborne polyurethane is smaller, thereby improving the stability of the waterborne polyurethane.
[0098] Furthermore, the cross-linking agent containing polyethylene glycol segments and carbon-carbon double bonds is also the cross-linking point of the reaction system. The carbon-carbon double bonds in the cross-linking agent containing polyethylene glycol segments and carbon-carbon double bonds can undergo polymerization reaction with the carbon-carbon double bonds in the hydroxyl-containing acrylate to form a three-dimensional network structure, which is beneficial to improving the adhesion of the adhesive containing the water-based polyurethane dispersion, the strength of the adhesive layer, the elongation at break, and the ability to withstand high temperature and high humidity environments for a long time.
[0099] Furthermore, polyurethane itself is a block copolymer of soft segments and hard segments. After the introduction of acrylate segments, three block copolymers are formed, which are thermodynamically incompatible and produce microscopic phase separation. Inside the adhesive layer of the adhesive containing waterborne polyurethane dispersion, the hard segment phase plays a reinforcing role and provides multifunctional physical crosslinking. The soft segment matrix is used to provide flexibility. The more severe the phase separation, the stronger the crystallinity, and the higher its high temperature and humidity resistance, mechanical stretching, elongation at break, and modulus.
[0100] Furthermore, compared with small molecule hydrophilic monomers, hydrophilic groups (such as carboxylate or sulfonate) can be introduced into waterborne polyurethane molecules by adding hydrophilic chain extenders, and the hydrophilic groups enable the polyurethane molecules to self-emulsify while introducing more rigid groups such as urea groups and carbamate groups. The hydrophilic groups introduced into the waterborne polyurethane of the present invention do not increase the proportion of rigid groups (urea groups, carbamate groups, etc.), thereby ensuring the wettability of the adhesive containing waterborne polyurethane to the substrate. At the same time, the polar groups (ester groups, hydroxyl groups) on the polyurethane molecular chains and polyacrylate molecules enable the adhesive layer of the adhesive containing waterborne polyurethane to have a certain cohesive force, and the adhesive does not have residual glue and has high bonding strength.
[0101] Furthermore, under the combined action of the hydrophilic chain extender and the polyester polyol, the solid content of the prepared waterborne polyurethane dispersion can reach 75%, which greatly reduces the storage space and transportation costs. During the processing, the drying time is greatly shortened, and the production hours and production costs are reduced.
[0102] Furthermore, waterborne polyurethane containing polyether acrylate groups has two types of crosslinking points: ① Multiple hydroxyl groups in hydroxyl-containing acrylates in the prepolymerization stage can react with isocyanate groups in isocyanate to form crosslinking points; ② In crosslinking agents containing polyethylene glycol segments and carbon-carbon double bonds, the carbon-carbon double bonds in acrylates can react with the carbon-carbon double bonds in the crosslinking agent to form crosslinking points. At the same time, if it is a single acrylate polyethylene glycol, the hydroxyl group at one end can also react with the isocyanate group in isocyanate to form a crosslinking point. As a result, the adhesive layer of the adhesive containing waterborne polyurethane presents a three-dimensional network structure, with a large degree of crosslinking, and better heat resistance, hydrolysis resistance, weather resistance, and high and low temperature resistance.
[0103] Furthermore, in the process of preparing waterborne polyurethane, it is not necessary to introduce a large amount of low-boiling point solvents such as acetone and butanone to dilute the viscosity of the polyurethane prepolymer, thereby significantly reducing the use of organic solvents.
[0104] In the second aspect of the present invention, the present invention proposes an aqueous polyurethane dispersion. According to an embodiment of the present invention, the aqueous polyurethane dispersion is prepared by the above method. During the preparation process, the hydroxyl groups in the hydroxyl-containing acrylate and the polyester polyol can react with the isocyanate group in the isocyanate to form a carbamate bond (-NHCOO-), so that the carbon-carbon double bond group in the hydroxyl-containing acrylate can be introduced into the side chain of the polymer molecule, providing an active site for the subsequent polymerization reaction. Under the action of a free radical initiator, the carbon-carbon double bond in the hydroxyl-containing acrylate can be polymerized with the carbon-carbon double bond in the cross-linking agent containing a polyethylene glycol segment and a carbon-carbon double bond, increasing the cross-linking points between molecules, forming a denser three-dimensional network structure, providing better support, and increasing the ability to resist external forces, thereby improving the tensile strength of the aqueous polyurethane dispersion. In addition, the polyethylene glycol segment can also be introduced into the side chain of the aqueous polyurethane molecule. The presence of the ether chain in the polyethylene glycol segment increases the hydrophilicity of the aqueous polyurethane, helps to form a stable dispersion in the aqueous system, and improves its stability in the aqueous medium. Furthermore, the addition of a hydrophilic chain extender can introduce a hydrophilic group (such as a carboxylate or sulfonate) into the waterborne polyurethane molecule, thereby improving the compatibility of the polyurethane with water and enabling the polyurethane to self-emulsify in water. The addition of an amine chain extender can provide additional amino groups, which react with the isocyanate groups in the isocyanate to form urea groups, thereby increasing the crosslinking density between the polyurethane molecular chains and thus improving the tensile strength of the waterborne polyurethane. The addition of a capping agent can react with the active groups (such as -NCO) in the polymer to terminate the chain growth, thereby controlling the molecular weight of the waterborne polyurethane. The addition of an organic solvent is used to adjust the viscosity of the waterborne polyurethane, facilitating subsequent processing and mixing. Water, as a dispersion medium, reacts with the hydrophilic component to form a stable waterborne polyurethane dispersion.
[0105] Furthermore, in the waterborne polyurethane structure, the polyester polyol contains a relatively long carbon chain, which is soft at room temperature and can constitute a soft segment in the polyurethane structure, providing good flexibility and elasticity. The saturated long carbon chain in the hydrophilic chain extender increases the length and flexibility of the polyurethane molecular chain, which helps to improve the sliding ability between the molecular chains. Therefore, the flexibility of the soft segment and the sliding ability of the long carbon chain work together to improve the elongation at break of the waterborne polyurethane. Thus, the waterborne polyurethane obtained by the method provided by the present application has high tensile strength and elongation at break.
[0106] According to some specific embodiments of the present invention, the mass proportion of the aqueous polyurethane in the aqueous polyurethane dispersion is 40% to 75%. For example, it can be 40%, 50%, 60%, 75%, etc. Therefore, the solid content of the aqueous polyurethane dispersion is relatively high, indicating that the concentration of polyurethane in the dispersion is large, which can reduce the drying time and improve the use efficiency of the material. It can also reduce the dependence on organic solvents and better meet environmental protection requirements.
[0107] According to some specific embodiments of the present invention, the average particle size of the aqueous polyurethane dispersion is 125nm-164nm, for example, 125nm, 130nm, 150nm, 164nm, etc. As a result, the Brownian motion of the dispersion is more significant, which helps to prevent particle sedimentation and agglomeration, thereby improving the stability of the dispersion.
[0108] In the third aspect of the present invention, the present invention provides a polyurethane adhesive. According to an embodiment of the present invention, the polyurethane adhesive comprises component A and component B, wherein component A contains the aqueous polyurethane dispersion provided by the second aspect of the present invention, and component B contains a second isocyanate.
[0109] According to some specific embodiments of the present invention, the component A may further include an additive, which may be selected with reference to existing two-component polyurethane adhesives. In some embodiments, the additive includes at least one of a thickener, a defoamer, and a leveling agent. The additive is typically a water-based material.
[0110] Furthermore, in the component A, based on 100 parts by total weight of the component A, the mass content of the aqueous polyurethane dispersion is 70 parts to 90 parts.
[0111] According to some specific embodiments of the present invention, in the component A, the aqueous polyurethane dispersion is 70 parts to 90 parts, the aqueous thickener is 0 parts to 2.5 parts, the aqueous defoamer is 0.01 parts to 2 parts, the aqueous leveling agent is 0.01 parts to 2 parts, and the total amount of component A is 100 parts by mass.
[0112] According to some specific embodiments of the present invention, the B component may further include water-based color paste and water. The water-based color paste may be a window pigment, and in the mixing stage, it is convenient for operators to clearly determine whether the A and B components are mixed evenly.
[0113] According to some specific embodiments of the present invention, in the B component, by weight, isocyanate is 80-90 parts, water-based color paste is 0.001 parts-0.05 parts, water is 10 parts-20 parts, and the total amount of B component is 100 parts by weight.
[0114] According to some specific embodiments of the present invention, the polyurethane adhesive is prepared according to the following method: component A containing an aqueous polyurethane emulsion and component B containing an isocyanate are separately prepared to obtain the polyurethane adhesive.
[0115] According to some specific embodiments of the present invention, the polyurethane adhesive is prepared according to the following method: separately preparing component A containing an aqueous polyurethane emulsion and component B containing an isocyanate; then mixing component A containing an aqueous polyurethane emulsion and component B containing a second isocyanate to obtain a polyurethane adhesive. The mixing can be performed at room temperature.
[0116] Further, the isocyanate is an isocyanate curing agent, for example, an isocyanate polymer. The isocyanate curing material can be obtained commercially, for example, including at least one of BASF Desmodur DN, Desmodur N3600, Bayhydur 3100, Bayhydur XP 2547, Bayhydur XP 2451 and NPU AQ-140. In addition, the mass percentage content of isocyanate groups (NCO) in the isocyanate curing agent can be 13%-25%.
[0117] Those skilled in the art can understand that the polyurethane adhesive of the present invention is a two-component reaction curing adhesive, that is, when the adhesive is applied to the surface of the object to be bonded, the polyurethane in the A component and the isocyanate in the B component can undergo a curing reaction to form a cured film on the surface of the object to be bonded. The curing conditions may include: a temperature of 20°C-50°C and a time of 24h-168h.
[0118] The polyurethane adhesive of the invention has the advantages of strong bonding force, high temperature and high humidity resistance, strong mechanical properties, high hydrophilicity, large molecular weight, high solid content, high crosslinking degree and the like.
[0119] The scheme of the present disclosure will be explained below in conjunction with the examples. Those skilled in the art will appreciate that the following examples are only used to illustrate the present disclosure and should not be considered to limit the scope of the present disclosure. Where specific techniques or conditions are not indicated in the examples, the techniques or conditions described in the literature in this area or the product instructions are used. Where the manufacturers of reagents or instruments are not indicated, they are all conventional products that can be obtained commercially.
[0120] Example 1
[0121] 1) Preparation of waterborne polyurethane dispersion
[0122] (1) After mixing 80 g of polybutylene adipate diol (number average molecular weight of 2000) and 0.8 g of glycerol monoacrylate, water was removed under reduced pressure at 120° C. for 3 h, and the reduced pressure was controlled to be -0.06 MPa so that the water content in the system was controlled to be 0.07%, thereby obtaining a mixture A.
[0123] (2) After the water removal in step (1) is completed, the temperature is lowered to 50° C., 2.22 g of isophorone diisocyanate and 12.29 g of hexamethylene diisocyanate are added to the system and stirred, and the isocyanate content in the reaction system is tracked and determined by chemical titration method. After reaching the theoretical value (-NCO content is 2.9%), a mixture B is obtained.
[0124] (3) Add 3.69 g of polyethylene glycol 300 monoacrylate and azobisisobutyronitrile to the mixture B in step (2) and react for 2 h to obtain a mixture C.
[0125] (4) After the reaction in step (3) is completed, the temperature is lowered to 50° C., and 150 g of acetone is added to adjust the viscosity of the system to obtain a polyurethane prepolymer.
[0126] (5) Under high-speed stirring, the dropping rate was controlled so that the addition was completed within 30 minutes, and 3.80 g of sodium 2-(2-aminoethyl)aminoethanesulfonate was added dropwise to the polyurethane prepolymer in step (4). After the addition was completed, the stirring reaction was continued for 50 minutes to obtain a mixture D.
[0127] (6) Add 0.3 g of ethylenediamine and 1.64 g of succinimidyl alcohol to the mixture D obtained in step (5) for post-chain extension, stir and react at 30° C. for 25 min, add 100 g of deionized water dropwise for emulsification to form an emulsion, remove acetone under reduced pressure, and obtain an aqueous polyurethane dispersion with a solid content of 51%.
[0128] 2) Preparation of polyurethane adhesive
[0129] (1) Prepare component A: 90 parts by weight of aqueous polyurethane dispersion, 2.5 parts by weight of thickener, 1 part by weight of defoamer, and 2 parts by weight of leveling agent;
[0130] (2) Preparation of component B: by weight: 85 parts of BASF Desmodur DN, 0.02 parts of water-based color paste, and 14 parts of water.
[0131] (3) The above component A and component B are mixed uniformly at room temperature in a mass ratio of 20:1 to obtain a polyurethane adhesive.
[0132] The preparation processes of the aqueous polyurethane dispersions and polyurethane adhesives of Examples 2-6 and Comparative Examples 1-2 are the same as those of Example 1 except for some experimental parameters.
[0133] Some experimental parameters of the aqueous polyurethane dispersions of Examples 1-6 and Comparative Examples 1-2 are shown in Table 1.
[0134] Table 1
[0135]
[0136] “ / ” means no
[0137] Testing and analysis
[0138] Under the same conditions, the average particle size, tensile strength and elongation at break of the water polyurethane dispersions obtained in the above Examples 1-6 and Comparative Examples 1-2 were tested respectively. The specific test methods are as follows:
[0139] 1. Test method for average particle size of waterborne polyurethane dispersion: After diluting a small amount of waterborne polyurethane dispersion into deionized water, use a laser particle size analyzer to test the particle size of the emulsion. The test temperature is (23±2)°C and the relative humidity is (50±5)%.
[0140] 2. Tensile strength and elongation at break are tested according to GB / T 1040.3 2006:
[0141] Sample preparation: Pour component A into a polytetrahydrofuran mold on a horizontal platform, cast into a film, place at room temperature for 3 hours, and let it stand to remove bubbles. Then heat and dry in a 60±2℃ forced air drying oven for 6 hours, and then cool naturally at room temperature to prepare a film. According to GB / T1040.3, the prepared film is cut into strips with a width of 25±0.5mm, a thickness of 4±0.5mm, and a length of 200mm.
[0142] Test conditions: Place the sample under test in the standard environment specified in GB / T2918 at (23±2)°C and (50±5)% relative humidity for more than 24 hours, and test it in this environment, with a tensile speed of 100 mm / min.
[0143] The test results are shown in Table 2.
[0144] Table 2
[0145] Particle size / nm Tensile strength / MPa Elongation at break / % Example 1 125 26 1152 Example 2 143 24 1074 Example 3 158 23 1201 Example 4 147 23 1124 Example 5 164 25 1150 Example 6 173 24 1183 Comparative Example 1 180 10 531 Comparative Example 2 159 7 852
[0146] According to Table 1, compared with Comparative Examples 1-2, the aqueous polyurethane dispersions obtained in Examples 1-6 have a particle size of less than 200 nm, a tensile strength of more than 20 MPa, and an elongation at break of more than 1000%, while the products obtained in Comparative Examples 1-2 have a small particle size and can be stably stored, but have a small tensile strength of only 10 MPa at most, and an elongation at break of less than 1000%, and the overall mechanical properties are low. When used as an adhesive, the bonding performance is poor.
[0147] In the description of this specification, the description with reference to the terms "one embodiment", "some embodiments", "example", "specific example", "some implementation schemes" or "some examples" etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representations of the above terms do not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described may be combined in any one or more embodiments or examples in a suitable manner. In addition, those skilled in the art may combine and combine the different embodiments or examples described in this specification and the features of the different embodiments or examples, unless they are contradictory.
[0148] Although the embodiments of the present invention have been shown and described above, it is to be understood that the above embodiments are exemplary and are not to be construed as limitations of the present invention. A person skilled in the art may change, modify, replace and vary the above embodiments within the scope of the present invention.
Claims
1. A method for preparing an aqueous polyurethane dispersion, characterized in that: include: The polyester polyol, hydroxyl-containing acrylate, isocyanate, a cross-linking agent containing a polyethylene glycol segment and a carbon-carbon double bond, a free radical initiator, a hydrophilic chain extender, an amine chain extender, a capping agent, an organic solvent and water are mixed and reacted to obtain an aqueous polyurethane dispersion; Wherein, the structural formula of the hydroxyl-containing acrylate is: Wherein, R is any one of a C1-C9 alkane, a benzene ring, and a saturated aliphatic ring; X represents any one of hydroxyl group and hydrogen; Y represents any one of hydrogen and methyl.
2. The preparation method according to claim 1, characterized in that: The hydroxyl-containing acrylate comprises at least one of the chemical formulas (1) to (3):
3. The preparation method according to claim 1 or 2, characterized in that: The preparation method comprises: S1, mixing the polyester polyol and the hydroxyl-containing acrylate for the first time, and performing a first reduced pressure distillation to obtain a mixture A; S2, mixing the mixture A and isocyanate for a second time to obtain a mixture B; S3, mixing the mixture B, the cross-linking agent containing polyethylene glycol segments and carbon-carbon double bonds, and the free radical initiator for a third time to obtain a mixture C; S4, mixing the mixture C and the organic solvent for a fourth time to obtain a polyurethane prepolymer; S5, mixing the polyurethane prepolymer and the hydrophilic chain extender for a fifth time to obtain a mixture D; S6, mixing the mixture D, the amine chain extender, the end-capping agent and water for the sixth time, and performing reduced pressure distillation for the second time to obtain an aqueous polyurethane dispersion.
4. The preparation method according to claim 3, characterized in that: The mass ratio of the polyester polyol to the hydroxyl-containing acrylate is 1:(0.01-0.05); Optionally, the number average molecular weight of the polyester polyol is 1000-4000; Optionally, the polyester polyol includes at least one of polybutylene adipate diol, polyhexane adipate diol, polycaprolactone diol, and polycarbonate diol; Optionally, the temperature of the first reduced pressure distillation is 100°C-130°C; Optionally, the pressure of the first reduced pressure distillation is less than -0.08 MPa; Optionally, the time of the first reduced pressure distillation is 1h-3h; Optionally, based on the total mass of the mixture A, the mass proportion of water in the mixture A is 0.05%-0.1%.
5. The preparation method according to claim 3, characterized in that: The temperature of the second mixing is 40°C to 80°C; Optionally, the isocyanate includes at least one of hexamethylene diisocyanate, isophorone diisocyanate, toluene diisocyanate, dicyclohexylmethane diisocyanate, tetramethylxylylene diisocyanate, di-cyclohexylmethane diisocyanate, polymethylene polyphenyl polyisocyanate, and xylylene diisocyanate; Optionally, the isocyanate comprises hexamethylene diisocyanate and isophorone diisocyanate; Optionally, the mass ratio of the hexamethylene diisocyanate to the isophorone diisocyanate is (90-70):(10-30); Optionally, the molar ratio of the isocyanate groups in the isocyanate to the hydroxyl groups in the mixture A is (1.01-2.5):
1.
6. The preparation method according to claim 3, characterized in that: The third mixing time is 1h to 2h; Optionally, the cross-linking agent containing polyethylene glycol segments and carbon-carbon double bonds includes at least one of polyethylene glycol methacrylate and polyethylene glycol diacrylate; Optionally, the free radical initiator comprises at least one of azobisisobutyronitrile and dibenzoyl peroxide; Optionally, the temperature of the fourth mixing is 20°C to 60°C; Optionally, the organic solvent comprises acetone.
7. The preparation method according to claim 3, characterized in that: The mass ratio of the polyurethane prepolymer to the hydrophilic chain extender is (70-99):(0.8-20); Optionally, the hydrophilic chain extender comprises at least one of a carboxylate and a sulfonate; Optionally, the amine chain extender comprises ethylenediamine; Optionally, the capping agent comprises at least one of serine alcohol and ethanolamine.
8. An aqueous polyurethane dispersion, characterized in that The method is prepared by any one of claims 1 to 7.
9. The aqueous polyurethane dispersion according to claim 8, characterized in that The mass proportion of the aqueous polyurethane in the aqueous polyurethane dispersion is 40% to 75%.
10. A polyurethane adhesive, characterized in that: The invention comprises the aqueous polyurethane dispersion according to claim 8.
Citation Information
Cited By
UV light-cured shielding glue as well as preparation method and application thereof
CN121379486A
Polyurethane resin dispersion, adhesive composition, and adhesive
WO2026203905A1