Chiral MOFs material and preparation method thereof
Through a novel preparation method, the reaction of 1,2-cyclohexanediamine, triethylamine, oxalyl chloride monoethyl ester and organic solvents is combined with alkaline hydrolysis and acidification treatment, followed by 4,4'- The reaction between pyridine and transition metal salt solves the problems of poor structural controllability, high cost and poor durability of chiral MOFs materials, and prepares chiral MOFs materials with permanent pores and good stability.
Patent Information
- Application Number
- CN202411091352.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-09
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2044-08-09
AI Technical Summary
The existing preparation methods of chiral MOFs materials have problems such as poor structural controllability, difficulty in processing, high cost and poor durability, which limits the practical application of the materials.
The intermediate product was obtained by mixing 1,2-cyclohexanediamine, triethylamine, oxalyl chloride monoethyl ester with organic solvents, and hydrolyzing under alkaline conditions and acidifying to obtain chiral carboxylic acid The ligand was then mixed with 4,4'-bipyridine, N,N-dimethylformamide and transition metal salt to prepare chiral MOFs materials.
The prepared chiral MOFs material has permanent pores and uniform chiral space, and has good stability in acid phosphate buffered solutions, laying a solid foundation for its future applications.
Smart Images

Figure CN118930887A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of metal-organic framework materials, and in particular to a chiral MOFs material and a preparation method thereof. Background Art
[0002] Metal-organic framework (MOFs) materials are connected to metals or metal clusters through ligands to form a periodically arranged framework structure. By introducing asymmetric properties into the framework, chiral MOFs materials with chiral characteristics can be further obtained. In recent years, chiral MOFs materials have attracted great attention from researchers due to their inherent chirality, permanent pores, and unique physical properties. Due to their good stability and inherent chiral structure, chiral MOFs materials are very suitable for various applications that require asymmetric properties, such as asymmetric catalysis, enantiomeric separation, enantiomeric detection, and advanced optical devices.
[0003] At present, the methods for constructing chiral MOFs are mainly divided into two types: using chiral ligands and inducing framework chirality. The chiral ligand construction method is mainly limited by the availability and high cost of chiral sources, which leads to a lack of material diversity; while the inducing framework chirality method lacks structural controllability. In addition, shortcomings such as difficult processing, high cost, and poor durability further limit the practical application of chiral MOFs materials.
[0004] Therefore, it is of great significance to provide a new chiral MOFs material with simple preparation method, low cost and stable structure. Summary of the invention
[0005] The purpose of the present invention is to provide a chiral MOFs material and a preparation method thereof, so as to solve the problems of poor structural controllability, difficult processing, high cost and poor durability existing in the existing methods of inducing framework chirality.
[0006] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:
[0007] The present invention provides a method for preparing a chiral MOFs material, comprising the following steps:
[0008] 1) mixing 1,2-cyclohexanediamine, triethylamine, ethyl oxalyl chloride and an organic solvent, and reacting to obtain an intermediate product;
[0009] 2) subjecting the intermediate product prepared in step 1) to a hydrolysis reaction under alkaline conditions, and acidifying the intermediate product after the hydrolysis reaction to obtain a chiral carboxylic acid ligand;
[0010] 3) The chiral carboxylic acid ligand prepared in step 2), 4,4'-bipyridine, N,N-dimethylformamide, transition metal salt and water are mixed to react to obtain a chiral MOFs material.
[0011] Preferably, the mass ratio of 1,2-cyclohexanediamine, triethylamine, ethyl oxalyl chloride and the organic solvent in step 1) is 1:1-5:1-6:25-45.
[0012] Preferably, the 1,2-cyclohexanediamine in step 1) is (1R, 2R)-cyclohexane-1,2-diamine or (1S, 2S)-cyclohexane-1,2-diamine;
[0013] The organic solvent includes one or more of dichloromethane, acetonitrile and tetrahydrofuran.
[0014] Preferably, the reaction temperature in step 1) is -5 to 20°C, the reaction time is 6 to 12 hours, and the reaction atmosphere is an inert atmosphere.
[0015] Preferably, the hydrolysis reaction in step 2) is to mix the intermediate product obtained in step 1) with a base and a solvent to react;
[0016] The ratio of the intermediate product to the base and the solvent added is 1 mol: 1-5 mol: 2-7 L;
[0017] The alkali includes one or more of sodium hydroxide, potassium hydroxide and lithium hydroxide;
[0018] The solvent of the hydrolysis reaction is a mixture of alcohol and water.
[0019] Preferably, the temperature of the hydrolysis reaction in step 2) is 85-95° C., and the time of the hydrolysis reaction is 8-16 h;
[0020] The pH value of the system after acid addition is ≤1.
[0021] Preferably, in step 3), the molar ratio of the chiral carboxylic acid ligand, 4,4'-bipyridine and the transition metal salt is 1:0.5-2:0.5-4;
[0022] The addition ratio of the N,N-dimethylformamide, water and chiral carboxylic acid ligand is 7-13L:30-45L:1mol.
[0023] Preferably, the transition metal salt in step 3) is nickel sulfate or cupric chloride.
[0024] Preferably, the reaction temperature in step 3) is 80-120° C., and the reaction time is 1-5 days.
[0025] The present invention also provides a chiral MOFs material prepared by the above preparation method.
[0026] The present invention has at least the following beneficial effects:
[0027] The chiral MOFs material of the present invention has permanent pores and uniform chiral space, and has good stability in acidic phosphate buffer solution. Its aqueous phase stability lays a solid foundation for its future application research. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] Figure 1 The coordination mode diagram of 4,4'-bipyridine in the chiral S-Ni-MOFs material prepared in Example 1;
[0029] Figure 2 This is a coordination pattern diagram of the chiral carboxylic acid ligand in the chiral S-Ni-MOFs material prepared in Example 1;
[0030] Figure 3 The three-dimensional structure diagram of the chiral S-Ni-MOFs material prepared in Example 1;
[0031] Figure 4 This is the thermogravimetric analysis curve of the chiral S-Ni-MOFs material prepared in Example 1;
[0032] Figure 5 This is the thermogravimetric analysis curve of the chiral S-Cu-MOFs material prepared in Example 7;
[0033] Figure 6 XRD patterns of the chiral S-Ni-MOFs material prepared in Example 1 after being immersed in a phosphate buffer solution with a pH value of 3.5 for different lengths of time;
[0034] Figure 7 XRD patterns of the chiral S-Cu-MOFs material prepared in Example 7 after being immersed in a phosphate buffer solution with a pH value of 3.5 for different lengths of time;
[0035] Figure 8 This is the result of detecting L / D histidine enantiomers using the chiral S-Cu-MOFs material prepared in Example 7. DETAILED DESCRIPTION
[0036] The present invention provides a method for preparing a chiral MOFs material, comprising the following steps:
[0037] 1) mixing 1,2-cyclohexanediamine, triethylamine, ethyl oxalyl chloride and an organic solvent, and reacting to obtain an intermediate product;
[0038] 2) subjecting the intermediate product prepared in step 1) to a hydrolysis reaction under alkaline conditions, and acidifying the intermediate product after the hydrolysis reaction to obtain a chiral carboxylic acid ligand;
[0039] 3) The chiral carboxylic acid ligand prepared in step 2), 4,4'-bipyridine, N,N-dimethylformamide, transition metal salt and water are mixed to react to obtain a chiral MOFs material.
[0040] In the present invention, the method of mixing 1,2-cyclohexanediamine, triethylamine, ethyl oxalyl chloride and the organic solvent in step 1) is preferably to first dissolve 1,2-cyclohexanediamine and triethylamine in part of the organic solvent to form a mixed solution, and dissolve ethyl oxalyl chloride in the remaining organic solvent to form an ethyl oxalyl chloride solution, and then add the mixed solution dropwise into the ethyl oxalyl chloride solution.
[0041] In the present invention, step 1) also includes the step of separating and purifying the intermediate product, and the specific operation steps are as follows: after the reaction is completed, the reaction is quenched with a saturated NaHCO3 solution, the mixed system after the reaction is extracted and separated with dichloromethane, the organic phase is dried with anhydrous sodium sulfate, and then rotary evaporation and silica gel column purification are performed in sequence.
[0042] In the present invention, the eluent for the silica gel column purification is petroleum ether and ethyl acetate in a volume ratio of 1:1.
[0043] In the present invention, the mass ratio of 1,2-cyclohexanediamine, triethylamine, ethyl oxalyl chloride and the organic solvent in step 1) is 1:1-5:1-6:25-45, preferably 1:2-4:2-5:30-40, and more preferably 1:3-4:3-4:34-36.
[0044] In the present invention, the 1,2-cyclohexanediamine in step 1) is (1R, 2R)-cyclohexane-1,2-diamine or (1S, 2S)-cyclohexane-1,2-diamine.
[0045] In the present invention, the organic solvent includes one or more of dichloromethane, acetonitrile and tetrahydrofuran.
[0046] In the present invention, the reaction temperature in step 1) is -5 to 20°C, preferably -3 to 15°C, more preferably -1 to 10°C, and more preferably 0 to 5°C; the reaction time is 6 to 12h, preferably 7 to 10h, and more preferably 8 to 9h; the reaction atmosphere is an inert atmosphere, specifically one or more of a nitrogen atmosphere, a helium atmosphere, and an argon atmosphere.
[0047] In the present invention, after the acidification in step 2), the following steps are further included: filtering and washing with water for 2 to 4 times, and drying.
[0048] In the present invention, the hydrolysis reaction in step 2) is to mix the intermediate product obtained in step 1) with a base and a solvent to carry out a reaction.
[0049] In the present invention, the addition ratio of the intermediate product to the base and the solvent is 1 mol: 1-5 mol: 2-7 L, preferably 1 mol: 2-4 mol: 3-6 L, and more preferably 1 mol: 2-3 mol: 4-5 L.
[0050] In the present invention, the alkali includes one or more of sodium hydroxide, potassium hydroxide and lithium hydroxide.
[0051] In the present invention, the solvent of the hydrolysis reaction is a mixture of alcohol and water, wherein the alcohol includes one or more of methanol, ethanol and propanol, and the volume ratio of the alcohol to water is 1:1, wherein water as a solvent helps the hydrolysis reaction, and the addition of alcohol helps to improve the solubility of the reactants.
[0052] In the present invention, the temperature of the hydrolysis reaction in step 2) is 85-95°C, preferably 88-92°C, and more preferably 90°C; the time of the hydrolysis reaction is 8-16h, preferably 10-14h, and more preferably 12-13h.
[0053] In the present invention, the acidification is preferably carried out by adding acid solution to the system after the hydrolysis reaction is completed to adjust the pH value and complete the acidification treatment.
[0054] In the present invention, the pH value of the system after adding the acid solution is ≤1, preferably 0.1 to 1, and more preferably 0.3 to 0.5.
[0055] In the present invention, the structural formula of the chiral carboxylic acid ligand is
[0056] In the present invention, after the reaction in step 3) is completed, the steps of filtering, washing with alcohol for 4 to 6 times, and drying are also sequentially performed.
[0057] In the present invention, the molar ratio of the chiral carboxylic acid ligand, 4,4'-bipyridine and transition metal salt in step 3) is 1:0.5-2:0.5-4, preferably 1:0.8-1.8:1-3.5, more preferably 1:1-1.5:1.5-3.5, and more preferably 1:1.2:2-3.
[0058] In the present invention, the addition ratio of N,N-dimethylformamide, water and chiral carboxylic acid ligand is 7-13L:30-45L:1mol, preferably 9-11L:35-42L:1mol, and more preferably 10L:38-40L:1mol.
[0059] In the present invention, the transition metal salt in step 3) is nickel sulfate or copper chloride.
[0060] In the present invention, the reaction temperature in step 3) is 80-120°C, preferably 85-110°C, more preferably 90-105°C, and more preferably 95-100°C; the reaction time is 1-5 days, preferably 2-4 days, and more preferably 3 days.
[0061] The present invention also provides a chiral MOFs material prepared by the above preparation method.
[0062] The technical solutions provided by the present invention are described in detail below in conjunction with the embodiments, but they should not be construed as limiting the protection scope of the present invention.
[0063] Example 1
[0064] (1) Under argon protection, 4.57 g (1S, 2S)-cyclohexane-1,2-diamine and 18.0 mL triethylamine were dissolved in 100 mL anhydrous dichloromethane to obtain a colorless and transparent mixed solution; 20 mL anhydrous dichloromethane solution containing 11.3 g ethyl oxalyl chloride was then added dropwise thereto; after the addition was completed, the mixture was stirred at 0°C for 12 h to obtain a light yellow solid-liquid mixture; the reaction was quenched with a saturated NaHCO3 solution, and then extracted and separated with dichloromethane to obtain a yellow organic phase, which was dried with anhydrous Na2SO4, spin-dried and purified by a silica gel column (the eluent was petroleum ether and ethyl acetate in a volume ratio of 1:1) to obtain the intermediate product S-1 (11.6 g, yield 92.3%).
[0065] (2) 6.28 g of the intermediate product S-1 was dissolved in a mixed solvent of 50 mL of methanol and 50 mL of water, and 2 g of sodium hydroxide was added. The mixture was heated to 85°C for hydrolysis reaction. The reaction was completed after 12 h. The pH value of the system was adjusted to 1 using hydrochloric acid for acidification. After the treatment, the mixture was filtered and washed with water three times and dried (70°C, 12 h) to obtain a chiral carboxylic acid ligand S-H2L (4.23 g, yield 81.9%).
[0066] (3) 25.8 mg of chiral carboxylic acid ligand S-H2L and 15.6 mg of 4,4'-bipyridine were dissolved in 1 mL of N,N-dimethylformamide, and 26.3 mg of nickel sulfate hexahydrate and 4 mL of water were added. The mixture was heated to 90 °C and reacted for 72 h. After the reaction, the product was filtered, washed with methanol 5 times, and naturally air-dried to obtain chiral S-Ni-MOFs material (23.8 mg, yield 46%).
[0067] The reaction formula of the above reaction is as follows:
[0068]
[0069] The crystal structure data of the chiral S-Ni-MOFs material prepared in this example is shown in Table 1.
[0070] Table 1 Crystal structure data of chiral S-Ni-MOFs material prepared in Example 1
[0071]
[0072]
[0073]
[0074] The asymmetric unit diagram and three-dimensional structure diagram of the chiral S-Ni-MOFs material prepared in this example are shown in Figures 1 to 3 As shown. Figures 1 to 3 It can be seen that the nickel ions in the chiral S-Ni-MOFs material are hexacoordinated, including four oxygen atoms from chiral carboxylic acid ligands and two nitrogen atoms from 4,4'-bipyridine ligands. The material obtained by the present invention connects the transition metal ions into a one-dimensional chiral spiral chain through the chiral carboxylic acid ligand, and then connects the chiral spiral chain into a three-dimensional interpenetrating network metal-organic framework material through 4,4'-bipyridine.
[0075] Example 2
[0076] The only difference between this embodiment and embodiment 1 is that in step (3), the amount of chiral carboxylic acid ligand S-H2L is 0.05 mmol, the amount of 4,4'-bipyridine is 0.10 mmol, and the amount of nickel sulfate hexahydrate is 0.12 mmol.
[0077] Example 3
[0078] The only difference between this embodiment and embodiment 1 is that the heating reaction temperature in step (3) is 95° C. and the time is 3 days.
[0079] Example 4
[0080] (1) Under argon protection, 4.57 g (1R, 2R)-cyclohexane-1,2-diamine and 18.0 mL triethylamine were dissolved in 100 mL anhydrous dichloromethane to obtain a colorless and transparent mixed solution; 20 mL anhydrous dichloromethane solution containing 11.3 g ethyl oxalyl chloride was then added dropwise thereto; after the addition was completed, the mixture was stirred at 0°C for 12 h to obtain a light yellow solid-liquid mixture; the reaction was quenched with a saturated NaHCO3 solution, and then extracted and separated with dichloromethane to obtain a yellow organic phase, which was dried with anhydrous Na2SO4, spin-dried and purified by a silica gel column (the eluent was petroleum ether and ethyl acetate in a volume ratio of 1:1) to obtain the intermediate product R-1.
[0081] (2) 6.28 g of the intermediate product R-1 was dissolved in a mixed solvent of 50 mL of methanol and 50 mL of water, and 2 g of sodium hydroxide was added. The mixture was heated to 85 °C for hydrolysis. The reaction was completed after 12 h. The pH value of the system was adjusted to 1 with hydrochloric acid. The mixture was filtered and washed with water three times, and dried (70 °C, 12 h) to obtain the chiral carboxylic acid ligand R-H2L.
[0082] (3) 25.8 mg of chiral carboxylic acid ligand R-H2L and 15.6 mg of 4,4'-bipyridine were dissolved in 1 mL of N,N-dimethylformamide, and 26.3 mg of nickel sulfate hexahydrate and 4 mL of water were added. The mixture was heated to 90 °C and reacted for 72 h. After the reaction, the product was filtered, washed with methanol 5 times, and naturally air-dried to obtain chiral R-Ni-MOFs material.
[0083] The difference between this embodiment and embodiment 1 is that in step (1), (1S, 2S)-cyclohexane-1,2-diamine is replaced by (1R, 2R)-cyclohexane-1,2-diamine. The crystal structure data of the prepared chiral R-Ni-MOFs material are: tetragonal system, space group is P4122, unit cell parameters are
[0084] Example 5
[0085] The only difference between this embodiment and embodiment 4 is that in step (3), the amount of chiral carboxylic acid ligand R-H2L is 0.02 mmol, the amount of 4,4'-bipyridine is 0.05 mmol, and the amount of nickel sulfate hexahydrate is 0.05 mmol.
[0086] Example 6
[0087] The only difference between this embodiment and embodiment 4 is that the temperature of the heating reaction in step (3) is 85° C. and the time is 2.5 days.
[0088] Example 7
[0089] (1) Under argon protection, 4.57 g (1S, 2S)-cyclohexane-1,2-diamine and 18.0 mL triethylamine were dissolved in 100 mL anhydrous dichloromethane to obtain a colorless and transparent mixed solution; 20 mL anhydrous dichloromethane solution containing 11.3 g ethyl oxalyl chloride was then added dropwise thereto; after the addition was completed, the mixture was stirred at 0°C for 12 h to obtain a light yellow solid-liquid mixture; the reaction was quenched with a saturated NaHCO3 solution, and then extracted and separated with dichloromethane to obtain a yellow organic phase, which was dried with anhydrous Na2SO4, spin-dried and purified by a silica gel column (the eluent was petroleum ether and ethyl acetate in a volume ratio of 1:1) to obtain the intermediate product S-1.
[0090] (2) 6.28 g of the intermediate product S-1 was dissolved in a mixed solvent of 50 mL of methanol and 50 mL of water, and 2 g of sodium hydroxide was added. The mixture was heated to 85 °C for hydrolysis. The reaction was completed after 12 h. The pH value of the system was adjusted to 1 with hydrochloric acid. The mixture was filtered and washed with water three times, and dried (70 °C, 12 h) to obtain a chiral carboxylic acid ligand S-H2L.
[0091] (3) 25.8 mg of chiral carboxylic acid ligand S-H2L and 15.6 mg of 4,4'-bipyridine were dissolved in 1 mL of N,N-dimethylformamide, and 0.1 mmol of copper chloride dihydrate and 4 mL of water were added. The mixture was heated to 90 °C and reacted for 72 h. After the reaction, the product was filtered, washed with methanol 5 times, and naturally air-dried to obtain a chiral S-Cu-MOFs material.
[0092] The difference between this embodiment and embodiment 1 is that nickel sulfate hexahydrate is replaced by copper chloride dihydrate in step (3). The crystal structure data of the prepared chiral S-Cu-MOFs material is: tetragonal system, space group is P43, unit cell parameters are
[0093] Example 8
[0094] The only difference between this embodiment and embodiment 7 is that in step (3), the amount of chiral carboxylic acid ligand S-H2L used is 0.07 mmol, the amount of 4,4'-bipyridine used is 0.07 mmol, and the amount of cupric chloride dihydrate used is 0.07 mmol.
[0095] Example 9
[0096] The only difference between this embodiment and embodiment 7 is that the heating reaction time in step (3) is 2 days.
[0097] Example 10
[0098] (1) Under argon protection, 4.57 g (1R, 2R)-cyclohexane-1,2-diamine and 18.0 mL triethylamine were dissolved in 100 mL anhydrous dichloromethane to obtain a colorless and transparent mixed solution; 20 mL anhydrous dichloromethane solution containing 11.3 g ethyl oxalyl chloride was then added dropwise thereto; after the addition was completed, the mixture was stirred at 0°C for 12 h to obtain a light yellow solid-liquid mixture; the reaction was quenched with a saturated NaHCO3 solution, and then extracted and separated with dichloromethane to obtain a yellow organic phase, which was dried with anhydrous Na2SO4, spin-dried and purified by a silica gel column (the eluent was petroleum ether and ethyl acetate in a volume ratio of 1:1) to obtain the intermediate product R-1.
[0099] (2) 6.28 g of the intermediate product R-1 was dissolved in a mixed solvent of 50 mL of methanol and 50 mL of water, and 2 g of sodium hydroxide was added. The mixture was heated to 85 °C for hydrolysis. The reaction was completed after 12 h. The pH value of the system was adjusted to 1 with hydrochloric acid. The mixture was filtered and washed with water three times, and dried (70 °C, 12 h) to obtain the chiral carboxylic acid ligand R-H2L.
[0100] (3) 25.8 mg of chiral carboxylic acid ligand R-H2L and 15.6 mg of 4,4'-bipyridine were dissolved in 1 mL of N,N-dimethylformamide, and 26.3 mg of copper chloride dihydrate and 4 mL of water were added. The mixture was heated to 90 °C and reacted for 72 h. After the reaction, the product was filtered, washed with methanol 5 times, and air-dried to obtain chiral R-Cu-MOFs material.
[0101] The difference between this embodiment and embodiment 4 is that nickel sulfate hexahydrate is replaced by copper chloride dihydrate in step (3). The crystal structure data of the prepared chiral R-Cu-MOFs material is: tetragonal system, space group is P4122, unit cell parameters are Z=8.
[0102] Embodiment 11
[0103] The only difference between this embodiment and embodiment 10 is that in step (3), the amount of chiral carboxylic acid ligand R-H2L used is 0.015 mmol, the amount of 4,4'-bipyridine used is 0.015 mmol, and the amount of cupric chloride dihydrate used is 0.015 mmol.
[0104] Example 12
[0105] The only difference between this embodiment and embodiment 10 is that the heating reaction time in step (2) is 5 days.
[0106] The chiral S-Ni-MOFs material prepared in Example 1 and the chiral S-Cu-MOFs material prepared in Example 7 were subjected to thermogravimetric analysis and stability test (stability test method: XRD test after immersion in an acidic phosphate buffer solution with pH = 3.5 for 1 to 5 days). The results are as follows Figures 4 to 7 As shown, Figure 4 This is the thermogravimetric analysis curve of the chiral S-Ni-MOFs material prepared in Example 1. Figure 5 This is the thermogravimetric analysis curve of the chiral S-Cu-MOFs material prepared in Example 7. It can be seen from the figure that the chiral S-Ni-MOFs material has good stability below 300°C, and the chiral S-Ni-MOFs material has good stability below 240°C. Figure 6The XRD spectra of the chiral S-Ni-MOFs material prepared in Example 1 after being immersed in an acidic phosphate buffer solution with a pH of 3.5 for different time periods are shown in FIG. Figure 7 XRD spectra of the chiral S-Cu-MOFs material prepared in Example 7 after being immersed in an acidic phosphate buffer solution with pH = 3.5 for different time periods. It can be seen that both have good stability in the acidic PBS aqueous solution.
[0107] The chiral S-Cu-MOFs material prepared in Example 7 is used to identify histidine enantiomers, and the specific application method is as follows:
[0108] The chiral MOFs material, Nafion·D-520 dispersion (5% w / w in water / 1-propanol, ≥1meq / g, purchased from Alfa Aesar (China) Chemical Co., Ltd.) and N,N-dimethylformamide were mixed at a ratio of 3mg:20μL:280μL, ultrasonicated for 1h, and settled for 15min to obtain a stable suspension; the stable suspension was dripped onto the carbon paper material electrode and air-dried for 24h to obtain a loaded working electrode.
[0109] The D / L-histidine enantiomer to be tested was prepared into a 1 mmol / L solution using a 0.01 mol / L phosphate buffer solution with a pH of 3.5; a three-electrode system was formed using a loaded working electrode, an Ag / AgCl reference electrode and a graphite rod counter electrode; and the D-histidine solution and the L-histidine solution were electrochemically tested using linear sweep voltammetry, and the LSV conditions were: a potential range of -1.5 V to 1.5 V, a scan rate of 0.05 V / s, and a sensitivity of 1 mA.
[0110] The electrochemical recognition results are as follows Figure 8 As shown in the figure, it can be seen that the detection working electrode loaded with chiral S-Cu-MOFs material has a chiral recognition effect on L-histidine. When the potential is -1.5V, the L-histidine current decays by 32.5% compared with the background current, and the D-histidine current decays by 2.4% compared with the background current, indicating that the chiral MOFs material prepared by the present invention has an obvious chiral recognition effect on the histidine enantiomer.
[0111] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A method for preparing a chiral MOFs material, characterized in that: The following steps are involved: 1) mixing 1,2-cyclohexanediamine, triethylamine, ethyl oxalyl chloride and an organic solvent, and reacting to obtain an intermediate product; 2) subjecting the intermediate product prepared in step 1) to a hydrolysis reaction under alkaline conditions, and acidifying the intermediate product after the hydrolysis reaction to obtain a chiral carboxylic acid ligand; 3) The chiral carboxylic acid ligand prepared in step 2), 4,4'-bipyridine, N,N-dimethylformamide, transition metal salt and water are mixed to react to obtain a chiral MOFs material.
2. The method for preparing a chiral MOFs material according to claim 1, characterized in that: The mass ratio of 1,2-cyclohexanediamine, triethylamine, ethyl oxalyl chloride and organic solvent in step 1) is 1:1-5:1-6:25-45.
3. The method for preparing a chiral MOFs material according to claim 2, characterized in that: The 1,2-cyclohexanediamine in step 1) is (1R, 2R)-cyclohexane-1,2-diamine or (1S, 2S)-cyclohexane-1,2-diamine; The organic solvent includes one or more of dichloromethane, acetonitrile and tetrahydrofuran.
4. The method for preparing a chiral MOFs material according to claim 3, characterized in that: The reaction temperature in step 1) is -5 to 20°C, the reaction time is 6 to 12 hours, and the reaction atmosphere is an inert atmosphere.
5. The method for preparing a chiral MOFs material according to any one of claims 1 to 4, characterized in that: The hydrolysis reaction in step 2) is to mix the intermediate product obtained in step 1) with a base and a solvent to react; The ratio of the intermediate product to the base and the solvent added is 1 mol: 1-5 mol: 2-7 L; The alkali includes one or more of sodium hydroxide, potassium hydroxide and lithium hydroxide; The solvent of the hydrolysis reaction is a mixture of alcohol and water.
6. The method for preparing a chiral MOFs material according to claim 5, characterized in that: The temperature of the hydrolysis reaction in step 2) is 85-95° C., and the time of the hydrolysis reaction is 8-16 hours.
7. The method for preparing a chiral MOFs material according to claim 6, characterized in that: In step 3), the molar ratio of the chiral carboxylic acid ligand, 4,4'-bipyridine and transition metal salt is 1:0.5-2:0.5-4; The addition ratio of the N,N-dimethylformamide, water and chiral carboxylic acid ligand is 7-13L:30-45L:1mol.
8. The method for preparing a chiral MOFs material according to claim 7, characterized in that: In step 3), the transition metal salt is nickel sulfate or cupric chloride.
9. The method for preparing a chiral MOFs material according to claim 7 or 8, characterized in that: The reaction temperature in step 3) is 80-120° C., and the reaction time is 1-5 days.
10. A chiral MOFs material prepared by the method for preparing a chiral MOFs material according to any one of claims 1 to 9.
Citation Information
Patent Citations
Novel chiral MOF material as well as preparation method and application thereof
CN111378147A
Chiral Cd-MOFs material and preparation method thereof
CN114561022A
Recyclable chiral catalyst for asymmetric nitroaldol reaction and process for the preparation thereof
US20150368181A1