Steady-state small-particle-size natural latex and preparation method thereof
By using emulsified composite stabilizers and ultrasonic oscillation technology in natural latex, small-particle-sized latex and increasing negative charge on the surface of particles, the problems of ammonia irritability and environmental pollution are solved, and high stability and antibacterial effects are achieved. natural latex preparation.
Patent Information
- Application Number
- CN202411129268.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-16
- Publication Date
- 2024-11-12
AI Technical Summary
The stability of existing natural latex depends on ammonia, which has strong irritating odors, is harmful to the human body and the environment, and wastewater treatment causes damage to the environment, and ammonia has limited inhibitory effect on bacteria and mold.
The emulsified composite stabilizer is prepared by dissolving distilled rosin acid soap, sodium laurate, sodium orthophenylphenol and potassium hydroxide in distilled water. It is made into a small-particle-sized rubber latex by ultrasonic oscillation homogenization treatment and formed on the particle surface. The emulsified layer increases the negative charge on the surface of the particles and improves the stability of the latex.
The latex stability without ammonia or low ammonia is achieved, which improves the mechanical stability and antibacterial ability of the latex, and has no odor, reducing the risk of pollution to the environment.
Smart Images

Figure CN118930900A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of natural latex preparation, and in particular relates to a stable small-particle natural latex and a preparation method thereof. Background Art
[0002] Natural latex is an agricultural product, mainly from the Brazilian Hevea brasiliensis tree, which is naturally synthesized in the body. The latex is mainly composed of rubber particles and water. Rubber particles are a special organelle in the latex cells of the rubber tree, accounting for 25% to 45% of the latex cytoplasm. Its main biological function is to carry out the biosynthesis and storage of Hevea brasiliensis. Therefore, the formation mechanism, morphological size, and structural characteristics of rubber particles are closely related to the biosynthesis and accumulation of Hevea brasiliensis. With the development of science and technology, people have gradually discovered that rubber particles are a mixed system composed of lipids and proteins, and form a single-layer membrane core structure with the rubber hydrocarbon core, and the thickness of the outer membrane is about 10nm to 20nm; that is, the rubber particles are composed of hydrophobic rubber hydrocarbons as the core and are covered by a hydrophilic protein / phospholipid mixed outer layer. Among them, the protein part accounts for about 84% of the total surface, and the phospholipid accounts for about 16%; inside the particle, the ω-end group (initiating end group) is connected to the protein, and the α-end group (terminating end group) is connected to the phospholipid. The main components of the protein are water-insoluble α-globulin with a molecular weight of about 200 kDa and water-soluble protein with a molecular weight of 5 kDa; these proteins are composed of neutral, acidic, and basic oxygen acids, with an isoelectric point of pH 4 to 4.6, and can be separated and identified by electrophoretic mobility.
[0003] Removing the protein adsorbed on the particles will lead to the destruction of the stability of natural latex. The protein and phospholipid adsorbed on the surface of the stable latex particles are at the interface between the polymer particles and the aqueous medium. The lipophilic groups are attached to the particle surface inward, and the hydrophilic groups are in contact with the medium outward, forming an adsorption layer of a monomolecular film. Due to the relative motion of the particles to the liquid, the sliding surface is not on the solid surface, but on the surface of the adsorption layer in the liquid. At the same time, the hydrophilic particles form a diffusion layer in the process of outward diffusion, and its potential gradually decreases at an exponential rate. The potential at the sliding surface is called the diffusion potential or Zeta potential. The more charged the latex particles are, the higher the stability of the latex. On the other hand, the size of the latex particles also has a certain influence on the stability of the latex. The intermolecular forces between the latex particles will make them tend to aggregate and make the emulsion unstable. Therefore, within a certain range, the smaller the particle size, the higher the stability of the latex.
[0004] At present, the main method for stabilizing latex is to introduce a large amount of ammonia. Ammonia can adjust the pH value of the latex system, hydrolyze the phospholipids on the surface of the latex, and produce amino acids, linoleic acid, oleic acid, sodium laurate, etc. Further, it can react to generate fatty acid ammonium, which adheres to the surface of the latex particles, increases the absolute value of the Zeta potential, and improves the stability of the latex. Ammonia also has a certain inhibitory effect on bacteria and mold. However, ammonia has a strong irritating odor and is volatile. It is not only harmful to the human body in the production environment and affects the quality of downstream products, but also the treatment of wastewater will cause damage to the environment.
[0005] Therefore, the development of new ammonia-free and low-ammonia preservation systems and related processes is the development trend of green upgrading in the latex industry. Summary of the invention
[0006] In order to solve the deficiencies of the prior art, the present invention provides a stable small-particle natural latex, which is fully and evenly dispersed on the surface of latex particles by an emulsified composite stabilizer to form an emulsified layer on the surface of the particles, thereby increasing the negative charge on the surface of the particles and improving the stability of the latex; wherein the emulsified composite stabilizer is prepared by disproportionate rosin acid soap, sodium laurate, sodium o-phenylphenol, and potassium hydroxide dissolved in distilled water; the disproportionate rosin acid soap and sodium laurate can be hydrolyzed in the system and dispersed on the surface of the latex particles to form an emulsified layer; potassium hydroxide adjusts the pH of the system; sodium o-phenylphenol has a good inhibitory ability against fungi, bacteria, molds and enzyme bacteria, has a strong bactericidal effect, and is long-lasting and odor-free.
[0007] The present invention also provides a method for preparing a stable small-particle natural latex. By studying the surface components of latex particles and the mechanism of latex stability, and considering the latex particle size and surface Zeta potential value, the latex is first homogenized by ultrasonic oscillation to prepare a small-particle fine emulsion, and then an emulsified composite stabilizer is added, and the stabilizer is fully and evenly dispersed on the surface of the latex particles by emulsification by an emulsifier, an emulsified layer is formed on the particle surface, the negative charge on the particle surface is increased, and the stability of the latex is improved. Zeta potential is an important indicator for characterizing the stability of a dispersed system. The larger the absolute value of the Zeta potential, the more stable the dispersed system. When the absolute value of the Zeta potential is greater than 30mV, it can be considered that the dispersed system is relatively stable.
[0008] The technical effects to be achieved by the present invention are achieved through the following technical solutions:
[0009] The stable small-particle natural latex of the present invention is composed of natural fresh latex and an emulsified composite stabilizer accounting for 0.1%-0.5% of the mass of the natural fresh latex; wherein the emulsified composite stabilizer is prepared by disproportionated rosin acid soap, sodium laurate, sodium o-phenylphenol and potassium hydroxide dissolved in distilled water.
[0010] Furthermore, based on 100 parts of natural fresh latex, the emulsified composite stabilizer is composed of the following components and their mass fractions:
[0011] Disproportionated rosin acid soap 0.05-0.25 parts
[0012] Sodium laurate 0.02-0.1 parts
[0013] Sodium o-phenylphenol 0.01-0.05 parts
[0014] Potassium hydroxide 0.03-0.15 parts
[0015] 10 parts of distilled water.
[0016] Furthermore, the solid content of the natural fresh latex is 20%-40%.
[0017] The method for preparing the stable small-particle natural rubber latex of the present invention comprises the following steps:
[0018] S01, subjecting natural fresh latex to high-intensity ultrasonic oscillation homogenization treatment to obtain a small-particle latex emulsion;
[0019] S02, adding disproportionated rosin acid soap, sodium laurate and potassium hydroxide, stirring and dissolving in distilled water to obtain a uniformly dispersed emulsion, then adding sodium o-phenylphenol, continuing to stir and dissolve, to obtain an emulsified composite stabilizer;
[0020] S03, adding the emulsified composite stabilizer to the prepared fine latex emulsion, and after emulsification, obtaining a stable small-particle natural latex.
[0021] Furthermore, in the step S01, the ultrasonic frequency of the ultrasonic oscillation homogenization is 40 kHz, and the time is 10 min-30 min.
[0022] Furthermore, in the step S01, the average particle size of the small-particle latex emulsion obtained is ≤1000nm.
[0023] Furthermore, in the step S02, after adding sodium o-phenylphenolate, the stirring time is continued for 20 min-40 min.
[0024] Furthermore, in the step S03, the emulsification speed is 6000r / min-10000r / min, and the emulsification time is 5min-20min.
[0025] Furthermore, in the step S03, the absolute value of the Zeta potential of the obtained stable small-particle natural latex is greater than 30 mV; preferably, the absolute value of the Zeta potential of the stable small-particle natural latex is 55 mV-70 mV.
[0026] Furthermore, in the step S03, the mechanical stability of the obtained stable small-particle natural latex stored for more than 5 days is greater than 800s.
[0027] In summary, the present invention has at least the following benefits:
[0028] 1. The stable small-particle natural latex in the present invention is fully and evenly dispersed on the surface of latex particles by an emulsified composite stabilizer to form an emulsified layer on the surface of the particles, thereby increasing the negative charge on the surface of the particles and improving the stability of the latex; wherein the emulsified composite stabilizer is prepared by disproportionate rosin acid soap, sodium laurate, sodium o-phenylphenol and potassium hydroxide dissolved in distilled water; disproportionate rosin acid soap and sodium laurate can be hydrolyzed in the system and dispersed on the surface of latex particles to form an emulsified layer; potassium hydroxide adjusts the pH of the system; sodium o-phenylphenol has a good inhibitory ability against fungi, bacteria, molds and enzyme bacteria, has a strong bactericidal effect, and is long-lasting and odor-free.
[0029] 2. The method for preparing stable small-particle natural latex in the present invention studies the surface composition of latex particles and the mechanism of latex stability, and considers the size of latex particles and the surface Zeta potential value. The latex is first homogenized by ultrasonic oscillation to make a small-particle fine emulsion, and then an emulsified composite stabilizer is added. The stabilizer is fully and evenly dispersed on the surface of the latex particles through emulsification by an emulsifier, an emulsified layer is formed on the surface of the particles, the negative charge on the surface of the particles is increased, and the stability of the latex is improved. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] Figure 1 The present invention is a schematic diagram of a process for preparing a stable small-particle natural latex product according to an embodiment of the present invention. DETAILED DESCRIPTION
[0031] To better illustrate the purpose, technical solutions and advantages of the present invention, the present invention will be described more comprehensively below in conjunction with specific embodiments. The present invention provides preferred embodiments. However, the present invention can be implemented in many different forms and is not limited to the embodiments described herein. On the contrary, the purpose of providing these embodiments is to make the disclosure of the present invention more thoroughly and comprehensively understood.
[0032] In the examples, the experimental methods used are conventional methods unless otherwise specified, and the materials, reagents, etc. used are all commercially available unless otherwise specified.
[0033] As used herein, any reference to "one embodiment" or "an embodiment" means that a particular element, feature, structure, or characteristic described in conjunction with the implementation is included in at least one embodiment. The phrase "in one embodiment" appearing in multiple places in the specification does not necessarily refer to the same embodiment.
[0034] Unless otherwise defined herein, scientific and technical terms used in conjunction with the present disclosure shall have the meanings commonly understood by those of ordinary skill in the art. In addition, unless otherwise required by context, singular terms shall include pluralities and plural terms shall include the singular.
[0035] In the first aspect, the present invention provides a stable small-particle natural latex, which is composed of natural fresh latex and an emulsified composite stabilizer accounting for 0.1%-0.5% of the mass of the natural fresh latex; wherein the emulsified composite stabilizer is prepared by disproportionated rosin acid soap, sodium laurate, sodium o-phenylphenol, and potassium hydroxide dissolved in distilled water.
[0036] Furthermore, based on 100 parts of natural fresh latex, the emulsified composite stabilizer is composed of the following components and their mass fractions: 0.05-0.25 parts of disproportionate rosin acid soap, 0.02-0.1 parts of sodium laurate, 0.01-0.05 parts of sodium o-phenylphenol, 0.03-0.15 parts of potassium hydroxide, and 10 parts of distilled water. Preferably, the solid content of natural fresh latex is 20%-40%.
[0037] In a second aspect, the present invention also provides a method for preparing the above-mentioned stable small-particle natural latex, comprising the following steps:
[0038] S01, subjecting natural fresh latex to high-intensity ultrasonic oscillation homogenization treatment to obtain a small-particle latex emulsion;
[0039] S02, adding disproportionated rosin acid soap, sodium laurate and potassium hydroxide, stirring and dissolving in distilled water to obtain a uniformly dispersed emulsion, then adding sodium o-phenylphenol, continuing to stir and dissolve, to obtain an emulsified composite stabilizer;
[0040] S03, adding the emulsified composite stabilizer to the prepared fine latex emulsion, and after emulsification, obtaining a stable small-particle natural latex.
[0041] Further, in step S01, the ultrasonic frequency of ultrasonic oscillation homogenization is 40kHz, the time is 10min-30min, and the average particle size of the obtained small particle size latex emulsion is ≤1000nm. In step S02, after adding sodium o-phenylphenolate, the stirring time is continued for 20min-40min.
[0042] Furthermore, in step S03, the emulsification speed is 6000r / min-10000r / min, the emulsification time is 5min-20min, and the absolute value of the Zeta potential of the obtained stable small-particle natural latex is greater than 30mV; preferably, the absolute value of the Zeta potential of the stable small-particle natural latex is 55mV-70mV. And the mechanical stability of the obtained stable small-particle natural latex stored for more than 5 days is greater than 800s.
[0043] In the following specific embodiments, the sources of the main raw materials and main equipment used are as follows:
[0044] Natural fresh latex: Guangken Maoming Gaozhou latex factory
[0045] Disproportionated rosin acid soap: Lanabai Pharmaceutical Chemicals
[0046] Sodium laurate: Adamas
[0047] Sodium o-phenylphenol: Adamas
[0048] Potassium hydroxide: Adamas
[0049] Embodiment 1:
[0050] This embodiment provides a stable small-particle natural latex product 1, and the preparation method thereof comprises the following steps:
[0051] S01, weighing 1000 parts of natural fresh latex (solid content of 30%), and homogenizing it with high-intensity ultrasonic oscillation at an ultrasonic frequency of 40 kHz for 20 minutes to obtain a small-particle latex emulsion with an average particle size of ≤1000 nm;
[0052] S02, weigh 0.5 parts of disproportionated rosin acid soap, 1 part of sodium laurate and 1.5 parts of potassium hydroxide, stir and dissolve in 100 parts of distilled water to obtain a uniformly dispersed emulsion, then add 0.1 parts of sodium o-phenylphenol, continue stirring for 30 minutes, fully dissolve, and obtain an emulsified composite stabilizer;
[0053] S03, adding the emulsified composite stabilizer to the obtained fine latex emulsion, and emulsifying it for 10 minutes at a speed of 8000r / min by an emulsifier to obtain a stable small-particle natural latex product 1.
[0054] Embodiment 2:
[0055] This embodiment provides a stable small-particle natural latex product 2, and its preparation method comprises the following steps:
[0056] S01, weighing 1000 parts of natural fresh latex (solid content of 30%), and homogenizing it with high-intensity ultrasonic oscillation at an ultrasonic frequency of 40 kHz for 20 minutes to obtain a small-particle latex emulsion with an average particle size of ≤1000 nm;
[0057] S02, weigh 2.5 parts of disproportionate rosin acid soap, 0.2 parts of sodium laurate and 0.3 parts of potassium hydroxide, stir and dissolve in 100 parts of distilled water to obtain a uniformly dispersed emulsion, then add 0.3 parts of sodium o-phenylphenol, continue stirring for 30 minutes, fully dissolve, and obtain an emulsified composite stabilizer;
[0058] S03, adding the emulsified composite stabilizer to the obtained fine latex emulsion, and emulsifying it for 10 minutes at a speed of 8000r / min by an emulsifier to obtain a stable small-particle natural latex product 2.
[0059] Embodiment 3:
[0060] This embodiment provides a stable small-particle natural latex product 3, and its preparation method comprises the following steps:
[0061] S01, weighing 1000 parts of natural fresh latex (solid content of 30%), and homogenizing it with high-intensity ultrasonic oscillation at an ultrasonic frequency of 40 kHz for 20 minutes to obtain a small-particle latex emulsion with an average particle size of ≤1000 nm;
[0062] S02, weigh 2.5 parts of disproportionate rosin acid soap, 0.2 parts of sodium laurate and 0.3 parts of potassium hydroxide, stir and dissolve in 100 parts of distilled water to obtain a uniformly dispersed emulsion, then add 0.5 parts of sodium o-phenylphenol, continue stirring for 30 minutes, fully dissolve, and obtain an emulsified composite stabilizer;
[0063] S03, adding the emulsified composite stabilizer to the obtained fine latex emulsion, and emulsifying it for 10 minutes at a speed of 8000r / min by an emulsifier to obtain a stable small-particle natural latex product 3.
[0064] Embodiment 4:
[0065] This embodiment provides a stable small-particle natural latex product 4, and its preparation method comprises the following steps:
[0066] S01, weighing 1000 parts of natural fresh latex (solid content of 30%), and homogenizing it with high-intensity ultrasonic oscillation at an ultrasonic frequency of 40 kHz for 20 minutes to obtain a small-particle latex emulsion with an average particle size of ≤1000 nm;
[0067] S02, weigh 2 parts of disproportionate rosin acid soap, 0.2 parts of sodium laurate and 0.3 parts of potassium hydroxide, stir and dissolve in 100 parts of distilled water to obtain a uniformly dispersed emulsion, then add 0.5 parts of sodium o-phenylphenol, continue stirring for 30 minutes, fully dissolve, and obtain an emulsified composite stabilizer;
[0068] S03, adding the emulsified composite stabilizer to the obtained fine latex emulsion, and emulsifying it for 10 minutes at a speed of 8000r / min by an emulsifier to obtain a stable small-particle natural latex product 4.
[0069] Embodiment 5:
[0070] This embodiment provides a stable small-particle natural latex product 5, and its preparation method comprises the following steps:
[0071] S01, weighing 1000 parts of natural fresh latex (solid content of 30%), and homogenizing it with high-intensity ultrasonic oscillation at an ultrasonic frequency of 40 kHz for 20 minutes to obtain a small-particle latex emulsion with an average particle size of ≤1000 nm;
[0072] S02, weigh 1 part of disproportionate rosin acid soap, 0.8 parts of sodium laurate and 1.5 parts of potassium hydroxide, stir and dissolve in 100 parts of distilled water to obtain a uniformly dispersed emulsion, then add 0.3 parts of sodium o-phenylphenol, continue stirring for 30 minutes, fully dissolve, and obtain an emulsified composite stabilizer;
[0073] S03, adding the emulsified composite stabilizer to the obtained fine latex emulsion, and emulsifying it for 10 minutes at a speed of 8000r / min by an emulsifier to obtain a stable small-particle natural latex product 5.
[0074] Embodiment 6:
[0075] This embodiment provides a stable small-particle natural latex product 6, and the preparation method thereof comprises the following steps:
[0076] S01, weighing 1000 parts of natural fresh latex (solid content of 20%), and homogenizing it with high-intensity ultrasonic oscillation at an ultrasonic frequency of 40 kHz for 10 minutes to obtain a small-particle latex emulsion with an average particle size of ≤1000 nm;
[0077] S02, weigh 1.5 parts of disproportionate rosin acid soap, 0.8 parts of sodium laurate and 0.9 parts of potassium hydroxide, stir and dissolve in 100 parts of distilled water to obtain a uniformly dispersed emulsion, then add 0.3 parts of sodium o-phenylphenol, continue stirring for 20 minutes, fully dissolve, and obtain an emulsified composite stabilizer;
[0078] S03, adding the emulsified composite stabilizer to the obtained fine latex emulsion, and emulsifying it for 20 minutes at a speed of 6000r / min by an emulsifier to obtain a stable small-particle natural latex product 6.
[0079] Embodiment 7:
[0080] This embodiment provides a stable small-particle natural latex product 7, and its preparation method comprises the following steps:
[0081] S01, weighing 1000 parts of natural fresh latex (solid content of 40%), and homogenizing it with high-intensity ultrasonic oscillation at an ultrasonic frequency of 40 kHz for 30 minutes to obtain a small-particle latex emulsion with an average particle size of ≤1000 nm;
[0082] S02, weigh 2 parts of disproportionated rosin acid soap, 0.6 parts of sodium laurate and 1.5 parts of potassium hydroxide, stir and dissolve in 100 parts of distilled water to obtain a uniformly dispersed emulsion, then add 0.3 parts of sodium o-phenylphenol, continue stirring for 40 minutes, fully dissolve, and obtain an emulsified composite stabilizer;
[0083] S03, adding the emulsified composite stabilizer to the obtained fine latex emulsion, and emulsifying it for 10 minutes at a speed of 10000 r / min by an emulsifier to obtain a stable small-particle natural latex product 7.
[0084] Embodiment 8:
[0085] This embodiment provides a stable small-particle natural latex product 8, and the preparation method thereof comprises the following steps:
[0086] S01, weighing 1000 parts of natural fresh latex (solid content of 30%), and homogenizing it with high-intensity ultrasonic oscillation at an ultrasonic frequency of 40 kHz for 20 minutes to obtain a small-particle latex emulsion with an average particle size of ≤1000 nm;
[0087] S02, weigh 1 part of disproportionate rosin acid soap, 0.6 parts of sodium laurate and 1.2 parts of potassium hydroxide, stir and dissolve in 100 parts of distilled water to obtain a uniformly dispersed emulsion, then add 0.3 parts of sodium o-phenylphenol, continue stirring for 30 minutes, fully dissolve, and obtain an emulsified composite stabilizer;
[0088] S03, adding the emulsified composite stabilizer to the obtained fine latex emulsion, and emulsifying it for 5 minutes at a speed of 10000r / min by an emulsifier to obtain a stable small-particle natural latex product 8.
[0089] Comparative Example 1:
[0090] This comparative example provides a natural latex product, which is prepared by the following method:
[0091] Weigh 1000 parts of natural fresh latex (solid content 30%), and add 5 parts of 25% ammonia water under stirring.
[0092] (1) Latex particle size and Zeta potential test
[0093] After the latex prepared in Examples 1-8 and Comparative Example 1 was left to stand for more than 2 hours, 100 g of the latex prepared in Examples 1-8 and Comparative Example 1 was taken respectively, diluted with distilled water to 0.02% (mass fraction), and the Zetasizer Pro nanoparticle size analyzer of Malvern Company, UK, was used to perform particle size analysis on the diluted latex; Zeta potential analysis was performed using a zeta potential analyzer, and the remaining latex was sealed and stored. The test results are shown in Table 1.
[0094] Table 1 Average particle size and Zeta potential of latex in each test example
[0095]
[0096]
[0097] As can be seen from Table 1, the stable small-particle natural latex products prepared by using emulsified composite stabilizers in the embodiments of the present invention have an average particle size of less than 1000nm, the smallest of which can reach 772nm, and the absolute value of Zeta potential is between 59.4-67.2, which is consistent with the expected absolute value of Zeta potential (55mV-70mV) of stable small-particle natural latex; while the natural fresh latex prepared by ammonia water has an average particle size of 1053nm and an absolute value of Zeta potential of 51.2. Zeta potential is an important indicator for characterizing the stability of a dispersed system. The larger the absolute value of Zeta potential, the more stable the dispersed system. When the absolute value of Zeta potential is greater than 30mV, it can be considered that the dispersed system is relatively stable. It can be seen from this that the stable small-particle natural latex prepared by using emulsified composite stabilizers in the embodiments of the present invention has an absolute value of Zeta potential that is significantly higher than the natural latex prepared by using ammonia water in the comparative example, and the stability of the stable small-particle natural latex in the present invention has been significantly improved. Moreover, the use of emulsified composite stabilizers instead of ammonia water can not only reduce the harm of the production environment to the human body and reduce the impact on the quality of downstream products, but also make industrial wastewater less likely to cause damage to the environment.
[0098] (2) Mechanical stability value (MST)
[0099] The latex prepared in Examples 1-8 and Comparative Example 1 was dehydrated using a disc centrifuge. After dehydration, the solid content of the latex increased to 60%. The mechanical stability of the concentrated latex after 0 days, 5 days, 10 days, 30 days and 60 days of storage was measured according to the method specified in GB / T 8301-2008. The test results are shown in Table 2.
[0100] Table 1 Mechanical stability of latex in each test example
[0101]
[0102] As shown in Table 2, the mechanical stability of the stable small-particle natural latex products prepared by using the emulsified composite stabilizer in the embodiments of the present invention is all greater than 800s, while the mechanical stability of the natural latex prepared by using ammonia water in the comparative example drops to below 800s after 5 days, and the mechanical stability drops to 578s after 60 days. It can be seen that the stable small-particle natural latex prepared by using the emulsified composite stabilizer in the embodiments of the present invention can not only effectively improve the stability of the natural latex, but also the use of the emulsified composite stabilizer instead of ammonia water can reduce the harm of the production environment to the human body, reduce the impact on the quality of downstream products, and industrial wastewater is not easy to damage the environment.
[0103] It is obvious to those skilled in the art that the embodiments of the present disclosure can be practiced without these specific details. In other cases, features known to those skilled in the art are not described in detail to avoid unnecessary complex descriptions. It is intended that all substitutions, replacements, modifications and equivalents obvious to those skilled in the art are included within the scope of the present disclosure. Based on the present disclosure, all compounds / compositions disclosed herein and their preparation methods, applications and uses can be prepared and implemented without undue experimentation.
[0104] Although the compounds / compositions and methods of the present disclosure have been described according to specific embodiments, it will be apparent to those skilled in the art that changes may be made to the formulations, compounds or compositions and / or methods, as well as the steps or order of steps of the methods described herein, without departing from the spirit and scope of the inventive concepts of the present disclosure.
[0105] Although the present invention is described in conjunction with the above specific embodiments, it is obvious that those skilled in the art can make many substitutions, modifications and changes according to the above content. Therefore, all such substitutions, improvements and changes are included in the spirit and scope of the appended claims.
Claims
1. A stable small particle size natural rubber latex, characterized in that: The invention is composed of natural fresh latex and an emulsified composite stabilizer accounting for 0.1%-0.5% of the mass of the natural fresh latex; wherein the emulsified composite stabilizer is prepared by disproportionated rosin acid soap, sodium laurate, sodium o-phenylphenol and potassium hydroxide dissolved in distilled water.
2. The stable small particle size natural rubber latex according to claim 1, characterized in that: Based on 100 parts of natural fresh latex, the emulsified composite stabilizer is composed of the following components and their mass fractions: Disproportionated rosin acid soap 0.05-0.25 parts Sodium laurate 0.02-0.1 parts Sodium o-phenylphenol 0.01-0.05 parts Potassium hydroxide 0.03-0.15 parts 10 parts of distilled water.
3. The stable small particle size natural rubber latex according to claim 1, characterized in that: The solid content of the natural fresh latex is 20%-40%.
4. The method for preparing a stable small-particle natural rubber latex according to any one of claims 1 to 3, characterized in that: The following steps are involved: S01, subjecting natural fresh latex to high-intensity ultrasonic oscillation homogenization treatment to obtain a small-particle latex emulsion; S02, adding disproportionated rosin acid soap, sodium laurate and potassium hydroxide, stirring and dissolving in distilled water to obtain a uniformly dispersed emulsion, then adding sodium o-phenylphenol, continuing to stir and dissolve, to obtain an emulsified composite stabilizer; S03, adding the emulsified composite stabilizer to the prepared fine latex emulsion, and after emulsification, obtaining a stable small-particle natural latex.
5. The method for preparing a stable small-particle natural rubber latex according to claim 4, characterized in that: In the step S01, the ultrasonic frequency of the ultrasonic oscillation homogenization is 40 kHz, and the time is 10 min-30 min.
6. The method for preparing a stable small-particle natural rubber latex according to claim 4, characterized in that: In the step S01, the average particle size of the small-particle latex emulsion is ≤1000nm.
7. The method for preparing a stable small-particle natural rubber latex according to claim 4, characterized in that: In the step S02, after adding sodium o-phenylphenolate, the stirring time is continued for 20 min-40 min.
8. The method for preparing a stable small-particle natural rubber latex according to claim 4, characterized in that: In the step S03, the emulsification speed is 6000r / min-10000r / min, and the emulsification time is 5min-20min.
9. The method for preparing a stable small-particle natural rubber latex according to claim 4, characterized in that: In the step S03, the absolute value of the Zeta potential of the obtained stable small-particle natural rubber latex is greater than 30 mV.
10. The method for preparing a stable small-particle natural rubber latex according to claim 4, characterized in that: In the step S03, the mechanical stability of the obtained stable small-particle natural latex stored for more than 5 days is greater than 800s.