Lining layer material and application thereof
By adding modified nanofillers and hydrogen sulfide absorption fillers to the lining material of the oil and gas conveying pipeline, the problem of poor anti-seepage performance of existing materials on hydrogen sulfide is solved, and the high gas barrier properties and antibacterial properties are improved, avoiding the Hydrogen sulfide poisoning accident occurred.
Patent Information
- Application Number
- CN202310532867.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-11
- Publication Date
- 2024-11-12
AI Technical Summary
The lining material of the existing oil and gas conveying pipeline has poor anti-seepage performance for small-molecule gases such as oxygen, carbon dioxide, and hydrogen sulfide in oil and gas, resulting in easy permeability of hydrogen sulfide and may cause poisoning accidents.
The inner lining material containing high-density polyethylene, modified nanofillers and hydrogen sulfide absorption filler is used to improve gas barrier properties by adding modified nanofillers and additives, and the metal oxides in the filler are absorbed by hydrogen sulfide. Hydrogen sulfide undergoes chemical reactions to absorb and fix hydrogen sulfide gas.
It significantly improves the gas barrier properties of the inner lining material, prevents hydrogen sulfide from oozing out, avoids the occurrence of hydrogen sulfide poisoning accidents, and enhances the antibacterial properties of the material.
Smart Images

Figure CN118931004A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of oil and gas transmission pipelines, and in particular to an inner lining material and application thereof. Background Art
[0002] With the development of oil and gas resources, fiber reinforced composite pipe (RTP) is widely used in the field of oil and gas gathering and transportation due to its advantages such as light weight, flexible coiling and corrosion resistance. RTP pipe is usually composed of three layers: an inner lining layer made of polymer material, a reinforcement layer made of continuous fiber material, and an outer pipe made of anti-aging and impact thermoplastic plastic. The main function of the inner lining layer is to seal the conveying material and prevent leakage; the main function of the reinforcement layer is to provide the required pressure bearing capacity of the pipe body; the main function of the outer pipe is to protect the entire pipe body. The inner lining material plays a key role in the quality of the composite pipe.
[0003] The lining material of RTP pipe is generally made of high-density polyethylene (HDPE). HDPE has good anti-seepage performance against water vapor. However, oil and gas gathering and transportation are usually medium- and high-pressure oil and gas, which often contain small molecules such as oxygen, carbon dioxide, hydrogen sulfide, and methane, which are easily permeable media. In high-pressure oil and gas, HDPE has poor anti-seepage performance against oxygen, carbon dioxide, hydrogen sulfide, methane and other gases in oil and gas, which makes it easy for these small molecules to penetrate outside the composite pipe. If hydrogen sulfide penetrates from the composite pipe and gathers, it is easy to cause hydrogen sulfide poisoning accidents. Therefore, it is of great significance to develop an inner lining material with good gas barrier properties and the ability to prevent hydrogen sulfide gas leakage. Summary of the invention
[0004] The purpose of the present invention is to overcome the problem that the existing lining materials in the prior art have poor gas barrier properties and are prone to hydrogen sulfide poisoning accidents, and to provide an lining material and its application, wherein the lining material has high gas barrier properties and can prevent hydrogen sulfide gas leakage.
[0005] In order to achieve the above object, the present invention provides an inner lining material on one hand, wherein the inner lining material comprises high-density polyethylene a and a composite material.
[0006] The composite material contains high-density polyethylene b, modified nano filler, hydrogen sulfide absorbing filler and a first auxiliary agent.
[0007] The hydrogen sulfide absorbing filler contains a metal oxide modified by a silane coupling agent, and the metal oxide can chemically react with hydrogen sulfide;
[0008] The modified nanofiller is obtained by modifying a sheet-like nanofiller with a cationic surfactant, and the first auxiliary agent is a coupling agent and / or a compatibilizer.
[0009] Preferably, the metal oxide is nano zinc oxide and / or nano iron oxide.
[0010] Preferably, the hydrogen sulfide absorbing filler further contains an inorganic antibacterial agent modified by a silane coupling agent.
[0011] Preferably, the inorganic antibacterial agent is nano copper oxide and / or nano silver oxide.
[0012] Preferably, the hydrogen sulfide absorbing filler is prepared according to the following process:
[0013] Mixing a silane coupling agent with an ethanol aqueous solution, adjusting the pH of the obtained mixed solution to 3.5 to 5 and reacting to obtain a coupling agent solution;
[0014] The coupling agent solution is mixed with the metal oxide, and then ultrasonically dispersed and reacted, the obtained reaction solution is separated into solid and liquid, and the obtained solid phase is washed, dried, activated, ground and sieved.
[0015] Preferably, the volume ratio of the silane coupling agent to the ethanol aqueous solution is 1:15-25.
[0016] Preferably, in the ethanol aqueous solution, the volume ratio of ethanol to water is 2 to 4:1.
[0017] Preferably, the weight ratio of the silane coupling agent to the metal oxide is 1:15-25.
[0018] Preferably, based on the total weight of the composite material, the content of the high-density polyethylene b is 85-94wt%, the content of the modified nanofiller is 2-6wt%, the content of the hydrogen sulfide absorbing filler is 3-10wt%, and the content of the first auxiliary agent is 1-2wt%.
[0019] Preferably, the flaky nanofiller is selected from one or more of muscovite, biotite, phlogopite, kaolin and montmorillonite.
[0020] Preferably, the cationic surfactant is a long-chain alkyl quaternary ammonium salt, preferably one or more of dodecyltrimethylammonium chloride, hexadecyltrimethylammonium bromide, hexadecyltrimethylammonium chloride, octadecyltrimethylammonium chloride and octadecyldimethylbenzylammonium chloride.
[0021] Preferably, the modified nanofiller is prepared according to the following process:
[0022] S10, heating water to 70-90° C., and then mixing the water with the flaky nanofiller to obtain a mixture;
[0023] S20, adjusting the pH of the mixture to 6.8-7.5 and continuing heating for 30-50 minutes, then reacting with a cationic surfactant, separating the obtained reaction liquid into solid and liquid, and then washing, drying, grinding and sieving the obtained solid.
[0024] Preferably, in step S10, the weight ratio of the flaky nanofiller to water is 1:25-50.
[0025] Preferably, the weight ratio of the cationic surfactant to the flaky nanofiller is 1:10-20.
[0026] Preferably, the melt index of the high-density polyethylene b is 0.3-0.5 g / min.
[0027] Preferably, the compatibilizer is selected from one or more of maleic anhydride grafted high density ethylene, maleic anhydride grafted ethylene-1-octene block copolymer, acrylic acid grafted polyethylene and maleic anhydride grafted ethylene-vinyl acetate copolymer.
[0028] Preferably, the coupling agent is a silane coupling agent and / or a titanate coupling agent.
[0029] Preferably, the composite material is prepared according to the following process: high-density polyethylene, modified nano filler, hydrogen sulfide absorbing filler and the first auxiliary agent are co-blended and extruded.
[0030] Preferably, the blending extrusion is carried out in a twin-screw extruder.
[0031] Preferably, the working temperature of the twin-screw extruder is 160-200° C., the working speed is 300-350 r / min, and the working time is 3-6 min.
[0032] Preferably, based on the total weight of the inner lining material, the content of the high-density polyethylene a is 85-98wt%, and the content of the composite material is 2-15wt%.
[0033] Preferably, the high-density polyethylene a and the high-density polyethylene b are the same.
[0034] Preferably, the inner lining material further contains a second auxiliary agent, and the second auxiliary agent is selected from one or more of a plasticizer, a flame retardant and an antioxidant.
[0035] Preferably, in the inner lining material, the content of the second auxiliary agent is 1-2 wt %.
[0036] A second aspect of the present invention provides a method for preparing an inner lining layer, wherein the method uses the inner lining layer material as described above for preparation, and the method comprises the following steps:
[0037] A1, blending and extruding high-density polyethylene b, modified nano filler, hydrogen sulfide absorbing filler and the first auxiliary agent, cooling and granulating to obtain a composite material;
[0038] A2, blending and extruding the composite material and high-density polyethylene a, and cooling and shaping;
[0039] Among them, in step A1, the hydrogen sulfide absorbing filler contains a metal oxide modified by a silane coupling agent, the metal oxide can react chemically with hydrogen sulfide, the modified nanofiller is a sheet-like nanofiller modified by a cationic surfactant, and the first auxiliary agent is a coupling agent and / or a compatibilizer.
[0040] Preferably, in step A1, based on the total weight of the composite material, the content of the high-density polyethylene b is 85-94wt%, the content of the modified nanofiller is 2-6wt%, the content of the hydrogen sulfide absorbing filler is 3-10wt%, and the content of the first auxiliary agent is 1-2wt%.
[0041] Preferably, in step A1, the blending extrusion is carried out in a twin-screw extruder, wherein the working temperature of the twin-screw extruder is 160-200° C., the working speed is 300-350 r / min, and the working time is 3-6 min.
[0042] Preferably, in step A2, the blending extrusion is carried out in a twin-screw extruder.
[0043] Preferably, in step A2, the body temperature of the twin-screw extruder includes three temperature zones arranged in sequence along the material flow direction, the temperature of zone one is 110-130°C, the temperature of zone two is 140-160°C, and the temperature of zone three is 180-200°C.
[0044] Preferably, in step A2, the head temperature of the twin-screw extruder is 165-185°C.
[0045] A third aspect of the present invention provides a composite pipe, comprising an inner lining layer, a reinforcement layer and an outer pipe arranged in sequence from the inside to the outside, wherein the inner lining layer is made of the inner lining layer material as described above or is made by the method as described above.
[0046] In the present invention, by adding modified nano fillers and the first auxiliary agent, the inner lining material has high gas barrier properties; at the same time, by adding hydrogen sulfide absorbing fillers that can chemically react with hydrogen sulfide gas, the hydrogen sulfide gas that penetrates into the inner lining material is absorbed, thereby preventing hydrogen sulfide from leaking out of the composite pipe, thereby avoiding safety accidents such as hydrogen sulfide poisoning. BRIEF DESCRIPTION OF THE DRAWINGS
[0047] Figure 1This is a diagram showing the bacterial attachment results after the inner lining layer prepared in Example 1 of the present invention is immersed in a bacterial solution;
[0048] Figure 2 This is a diagram showing the bacterial attachment results after the inner lining layer prepared in comparative example 5 of the present invention is immersed in bacterial solution. DETAILED DESCRIPTION
[0049] The specific implementation of the present invention is described in detail below in conjunction with the accompanying drawings. It should be understood that the specific implementation described here is only used to illustrate and explain the present invention, and is not used to limit the present invention.
[0050] The endpoints and any values of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values should be understood to include values close to these ranges or values. For numerical ranges, the endpoint values of each range, the endpoint values of each range and the individual point values, and the individual point values can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.
[0051] The inner lining material of the present invention contains high-density polyethylene a and a composite material, wherein the composite material contains high-density polyethylene b, a modified nanofiller, a hydrogen sulfide absorbing filler and a first auxiliary agent, the hydrogen sulfide absorbing filler contains a metal oxide modified by a silane coupling agent, and the metal oxide can react chemically with hydrogen sulfide; the modified nanofiller is a sheet-like nanofiller modified by a cationic surfactant, and the first auxiliary agent is a coupling agent and / or a compatibilizer. Preferably, the first auxiliary agent is a coupling agent and a compatibilizer.
[0052] The present invention improves the compatibility of high-density polyethylene and fillers (including modified nano fillers and hydrogen sulfide absorbing fillers) by adding the first auxiliary agent, so that the high-density polyethylene can be better combined with the filler, thereby avoiding the "debonding" phenomenon of the filler; at the same time, the addition of the first auxiliary agent can also improve the bonding between the lining layer material and the reinforcement layer material, thereby improving its resistance to interlayer delamination.
[0053] In order to make the inner lining material have a better absorption effect on hydrogen sulfide gas, in the present invention, the metal oxide is nano zinc oxide and / or nano iron oxide. Among them, the nano zinc oxide is preferably a tetrapod-shaped zinc oxide whisker. The nano zinc oxide and nano iron oxide also have an antibacterial effect, so the inner lining material has antibacterial properties.
[0054] In order to make the antibacterial property of the lining material better and thus prevent bacteria in the oil and gas medium from adhering and growing on the surface of the lining, in the lining material described in the present invention, the hydrogen sulfide absorbing filler also contains an inorganic antibacterial agent modified by a silane coupling agent, wherein the inorganic antibacterial agent is nano copper oxide and / or nano silver oxide, and nano copper oxide and nano silver oxide have excellent antibacterial properties.
[0055] In the inner lining material of the present invention, based on the total weight of the inner lining material, the content of the high-density polyethylene a is 85-98wt%, and the content of the composite material is 2-15wt%. Within the above range, the performance of the obtained inner lining is better.
[0056] In the inner lining material of the present invention, the hydrogen sulfide absorbing filler is prepared according to the following process:
[0057] Mixing a silane coupling agent with an ethanol aqueous solution, adjusting the pH of the obtained mixed solution to 3.5 to 5 and reacting to obtain a coupling agent solution;
[0058] The coupling agent solution is mixed with the metal oxide, and then ultrasonically dispersed and reacted, the obtained reaction solution is separated into solid and liquid, and the obtained solid phase is washed, dried, activated, ground and sieved.
[0059] The hydrogen sulfide absorbing filler prepared by the above process has good dispersibility in high-density polyethylene, so it can better play its role, thereby making the inner lining material have a good effect of absorbing hydrogen sulfide gas.
[0060] Further preferably, the volume ratio of the silane coupling agent to the ethanol aqueous solution is 1:15-25, specifically, for example, 1:15, 1:17, 1:19, 1:20, 1:22, 1:23 or 1:25.
[0061] Further preferably, in the ethanol aqueous solution, the volume ratio of ethanol to water is 2 to 4:1, specifically, for example, 2:1, 2.2:1, 2.5:1, 2.7:1, 3:1, 3.5:1 or 4:1.
[0062] More preferably, the weight ratio of the silane coupling agent to the metal oxide is 1:15-25.
[0063] More preferably, the activation temperature is 140-160° C. and the activation time is 6-10 h.
[0064] It is understood that when the hydrogen sulfide absorbing filler also contains an inorganic antibacterial agent modified by a silane coupling agent, the step of mixing the coupling agent solution with the metal oxide includes: mixing the coupling agent solution, the inorganic antibacterial agent and the metal oxide. The weight ratio of the silane coupling agent to the inorganic antibacterial agent is 1:5-10.
[0065] In the lining material described in the present invention, in order to make the performance of the composite material better, in a preferred embodiment, based on the total weight of the composite material, the content of the high-density polyethylene b is 85-94wt%, the content of the modified nanofiller is 2-6wt%, the content of the hydrogen sulfide absorbing filler is 3-10wt%, and the content of the first auxiliary agent is 1-2wt%.
[0066] If the flaky nanofiller is added directly, it is easy to agglomerate, so that the flaky nanofiller cannot be distributed in the polyethylene in a flaky manner, thereby making the gas barrier property of the liner material poor. The present invention further improves its dispersibility in the resin matrix by modifying the flaky nanofiller. In a preferred embodiment, the cationic surfactant is a long-chain alkyl quaternary ammonium salt, more preferably one or more of dodecyltrimethylammonium chloride, hexadecyltrimethylammonium bromide, octadecyltrimethylammonium chloride and octadecyldimethylbenzylammonium chloride.
[0067] In order to make the modified nanofiller more dispersible in high-density polyethylene (i.e., resin matrix), in the lining layer material described in the present invention, the flaky nanofiller is a layered nanomaterial with a large aspect ratio, specifically one or more of muscovite, biotite, phlogopite, kaolin and montmorillonite.
[0068] In a preferred embodiment, the modified nanofiller is prepared according to the following process:
[0069] Step S10, heating water to 70-90° C., and then mixing the water with the flaky nanofiller to obtain a mixture;
[0070] Step S20, adjusting the pH of the mixture to 6.8-7.5 and continuing heating for 30-50 minutes, then reacting with a cationic surfactant, separating the obtained reaction liquid from the solid-liquid, and then washing, drying, grinding and sieving the obtained solid.
[0071] Wherein, in step S10, the weight ratio of the flaky nanofiller to water is 1:25-50, specifically, for example, 1:25, 1:30, 1:33, 1:35, 1:40, 1:45 or 1:50.
[0072] Preferably, the weight ratio of the cationic surfactant to the flaky nanofiller is 1:10-20, specifically, for example, 1:10, 1:12, 1:15, 1:17, 1:18 or 1:20.
[0073] In a specific embodiment, step S20 includes: adjusting the pH of the mixture to 6.8-7.5 and continuing heating for 30-50 minutes, then mixing with a cationic surfactant and adjusting the pH value to 6.8-7.5, reacting for 2-4 hours, filtering the obtained reaction solution, washing the filtered solid with deionized water for 3-5 times, then drying at 70-90° C. for 30-50 hours, and finally grinding and sieving.
[0074] In the inner lining material of the present invention, the melt index of the high-density polyethylene b is 0.3-0.5 g / min.
[0075] In the inner lining material of the present invention, the compatibilizer is selected from one or more of maleic anhydride grafted high-density ethylene, maleic anhydride grafted ethylene-1-octene block copolymer, acrylic acid grafted polyethylene and maleic anhydride grafted ethylene-vinyl acetate copolymer.
[0076] In the lining layer material described in the present invention, the coupling agent is a silane coupling agent and / or a titanate coupling agent.
[0077] In the inner liner material of the present invention, the composite material is prepared according to the following process: high-density polyethylene, modified nano filler, hydrogen sulfide absorbing filler and the first auxiliary agent are co-blended and extruded.
[0078] Further preferably, the co-extrusion is carried out in a twin-screw extruder, wherein the operating temperature of the twin-screw extruder is 160-200°C, the operating speed is 300-350r / min, and the working time is 3-6min. More preferably, the operating temperature of the twin-screw extruder is divided into three sections along the screw extrusion direction, the temperature of the first section is 160-170°C, the temperature of the second section is 175-185°C, and the temperature of the third section is 190-200°C.
[0079] In the inner lining material of the present invention, the high-density polyethylene a and the high-density polyethylene b may be the same or different. For better compatibility and ease of operation, they are preferably the same.
[0080] In order to improve the performance of the inner lining material such as processability, flame retardancy and service life, the inner lining material further contains a second auxiliary agent, which is selected from one or more of a plasticizer, a flame retardant and an antioxidant.
[0081] Furthermore, in the inner lining material, the content of the second auxiliary agent is 1-2 wt %.
[0082] The present invention also provides a method for preparing an inner lining layer, the method comprising the following steps:
[0083] Step A1, blending and extruding the high-density polyethylene b, the modified nano filler, the hydrogen sulfide absorbing filler and the first auxiliary agent, cooling and granulating to obtain a composite material;
[0084] Step A2, blending and extruding the composite material and high-density polyethylene a, and cooling and shaping;
[0085] Among them, in step A1, the hydrogen sulfide absorbing filler contains a metal oxide modified by a silane coupling agent, the metal oxide can react chemically with hydrogen sulfide, the modified nanofiller is a sheet-like nanofiller modified by a cationic surfactant, and the first auxiliary agent is a coupling agent and / or a compatibilizer.
[0086] In the method described in the present invention, the high-density polyethylene b, the modified nanofiller, the hydrogen sulfide absorbing filler and the first auxiliary agent are first blended and extruded to form a composite material, and then blended and extruded with the high-density polyethylene a (matrix) to prepare the inner liner. This can further improve the dispersibility of the nanofiller and the hydrogen sulfide absorbing filler in the high-density polyethylene, so that the modified nanofiller and the hydrogen sulfide absorbing filler are evenly dispersed in the high-density polyethylene, thereby making the gas barrier property of the inner liner excellent and the effect of absorbing hydrogen sulfide gas good.
[0087] In the method described in the present invention, in step A1, based on the total weight of the composite material, the content of the high-density polyethylene b is 85-94wt%, the content of the modified nanofiller is 2-6wt%, the content of the hydrogen sulfide absorbing filler is 3-10wt%, and the content of the first auxiliary agent is 1-2wt%.
[0088] In the method of the present invention, in step A1, the blending extrusion is carried out in a twin-screw extruder, wherein the working temperature of the twin-screw extruder is 160-200°C, the working speed is 300-350r / min, and the working time is 3-6min. Preferably, the working temperature of the twin-screw extruder is divided into three sections along the screw extrusion direction, the temperature of the first section is 160-170°C, the temperature of the second section is 175-185°C, and the temperature of the third section is 190-200°C.
[0089] In the method described in the present invention, in step A2, the blending extrusion is carried out in a twin-screw extruder, wherein the body temperature of the twin-screw extruder includes three temperature zones arranged in sequence along the material flow direction, the temperature of zone one (the temperature of the rear part of the body) is 110-130°C, the temperature of zone two (the temperature of the middle part of the body) is 140-160°C, and the temperature of zone three (the temperature of the front part of the body) is 180-200°C.
[0090] In the method of the present invention, in step A2, the head temperature of the twin-screw extruder is 165-185° C. Preferably, the head temperature includes the neck temperature and the die temperature, wherein the neck temperature is 175-185° C., and the die temperature is 165-175° C.
[0091] In the method of the present invention, in step A2, based on the total weight of the high-density polyethylene a and the composite material, the content of the high-density polyethylene a is 85-98wt%, and the content of the composite material is 2-15wt%.
[0092] In the method of the present invention, in step A2, the step of co-extruding the composite material and high-density polyethylene a comprises: co-extruding the composite material, high-density polyethylene a and a second auxiliary agent. Preferably, based on the total weight of the composite material, high-density polyethylene a and the second auxiliary agent, the content of the second auxiliary agent is 1-2wt%.
[0093] In the method described in the present invention, the high-density polyethylene a and the high-density polyethylene b may be the same or different, and are preferably the same for better compatibility and ease of operation.
[0094] In the method of the present invention, the metal oxide is nano zinc oxide and / or nano iron oxide. The nano zinc oxide is preferably a tetrapod-shaped zinc oxide whisker. The nano zinc oxide and nano iron oxide also have antibacterial effects, so the lining material has antibacterial properties.
[0095] The method of the present invention also includes preparing the hydrogen sulfide absorbing filler according to the following steps:
[0096] Mixing a silane coupling agent with an ethanol aqueous solution, adjusting the pH of the obtained mixed solution to 3.5 to 5 and reacting to obtain a coupling agent solution;
[0097] The coupling agent solution is mixed with the metal oxide, and then ultrasonically dispersed and reacted, the obtained reaction solution is separated into solid and liquid, and the obtained solid phase is washed, dried, activated, ground and sieved.
[0098] In the method described in the present invention, the volume ratio of the silane coupling agent to the ethanol aqueous solution is 1:15-25, specifically, for example, 1:15, 1:17, 1:19, 1:20, 1:22, 1:23 or 1:25.
[0099] Further preferably, in the ethanol aqueous solution, the volume ratio of ethanol to water is 2 to 4:1, specifically, for example, 2:1, 2.2:1, 2.5:1, 2.7:1, 3:1, 3.5:1 or 4:1.
[0100] More preferably, the weight ratio of the silane coupling agent to the metal oxide is 1:15-25.
[0101] More preferably, the activation temperature is 140-160° C. and the activation time is 6-10 h.
[0102] In order to improve the antibacterial performance of the prepared lining layer, in the method of the present invention, the step of mixing the coupling agent solution with the metal oxide includes: mixing the coupling agent solution, the inorganic antibacterial agent and the metal oxide. The weight ratio of the silane coupling agent to the inorganic antibacterial agent is 1:5-10.
[0103] In the method of the present invention, the cationic surfactant is a long-chain alkyl quaternary ammonium salt, more preferably one or more of dodecyltrimethylammonium chloride, hexadecyltrimethylammonium bromide, octadecyltrimethylammonium chloride and octadecyldimethylbenzylammonium chloride.
[0104] In order to make the modified nanofiller more dispersible in high-density polyethylene (i.e., resin matrix), in the method described in the present invention, the flaky nanofiller is a layered nanomaterial with a large aspect ratio, specifically one or more of muscovite, biotite, phlogopite, kaolin and montmorillonite.
[0105] The method of the present invention also includes preparing the modified nanofiller according to the following steps:
[0106] The water is heated to 70-90° C., and then mixed with the flaky nanofiller to obtain a mixture;
[0107] The pH of the mixture is adjusted to 6.8-7.5 and the mixture is heated for 30-50 minutes. The mixture is then reacted with a cationic surfactant, the obtained reaction liquid is separated into solid and liquid, and the obtained solid is then washed, dried, ground and sieved.
[0108] The present invention also provides a composite pipe, comprising an inner lining layer, a reinforcement layer and an outer pipe arranged in sequence from the inside to the outside; wherein the inner lining layer is made of the inner lining layer material as described above or is made by the method as described above.
[0109] The present invention will be described in detail below through examples, but the protection scope of the present invention is not limited thereto. In the following examples, high-density polyethylene a and high-density polyethylene b are the same, with a grade of YGH041 and a melt index of 0.4 g / 10 min.
[0110] Example 1
[0111] This embodiment is used to illustrate the inner lining material and its application (the preparation method of the inner lining) described in the present invention.
[0112] 1. Preparation of modified nanofillers:
[0113] S10, heating deionized water to 80° C., then adding nano-montmorillonite and stirring evenly to obtain a mixture, wherein the weight ratio of the nano-montmorillonite to water is 1:25;
[0114] S20, adjusting the pH of the mixture to 7.0-7.2 and continuing heating for 30 minutes, then adding octadecyltrimethylammonium chloride and stirring evenly (the weight ratio of the octadecyltrimethylammonium chloride to the nano-montmorillonite is 1:12), and adjusting the pH value to 7.0-7.2, reacting for 3 hours, filtering the obtained reaction solution, washing the filtered solid with deionized water for 3 times, and then drying at 80° C. for 48 hours, and finally grinding and sieving to obtain modified nano-montmorillonite, i.e., modified nano-filler.
[0115] 2. Preparation of hydrogen sulfide absorption filler:
[0116] Mixing a silane coupling agent (vinyl triethoxysilane) with an ethanol aqueous solution (in the ethanol aqueous solution, the volume ratio of ethanol to water is 3:1), adjusting the pH of the obtained mixed solution to 4-5.5, and hydrolyzing at room temperature for 1.5 hours to obtain a coupling agent solution, wherein the volume ratio of the silane coupling agent to the ethanol aqueous solution is 1:15;
[0117] Add metal oxide (the metal oxide includes four-needle zinc oxide whisker and nano iron oxide in a weight ratio of 1:1) and inorganic antibacterial agent (nano silver oxide) to the coupling agent solution, wherein the weight ratio of the silane coupling agent, the metal oxide and the inorganic antibacterial agent is 1:20:10, and then ultrasonically disperse at 50°C while mechanically stirring. After reacting for 3 hours, the obtained reaction solution is filtered, and then the obtained solid phase is washed with deionized water until there is no chloride ion, vacuum dried, and then activated at 150°C for 8 hours, ground and sieved to obtain a nano-scale hydrogen sulfide absorbing filler (containing an inorganic antibacterial agent).
[0118] 3. Preparation of lining layer
[0119] A11, weighing the raw material components according to the following weight percentages: 87wt% of high-density polyethylene b, 2wt% of modified nanofiller, 10wt% of hydrogen sulfide absorbing filler and 1wt% of a first auxiliary agent, wherein the first auxiliary agent comprises a silane coupling agent (vinyl triethoxysilane) and a compatibilizer (maleic anhydride grafted high-density ethylene) in a weight ratio of 1:1;
[0120] A12, adding the raw material components in step A11 into a twin-screw extruder and mixing them evenly, heating the screw extruder, and performing kneading in the twin-screw extruder, wherein the temperature of the twin-screw extruder is divided into a first section, a second section, and a third section along the extrusion direction of the screw, wherein the temperature of the first section is 160° C., the temperature of the second section is 180° C., and the temperature of the third section is 190° C., the extruder speed of the twin-screw extruder is 300 r / min, the total residence time of the lining material in the twin-screw extruder is 5 min, and the material is cooled and pelletized after being extruded from the twin-screw extruder to obtain a composite material;
[0121] A21. Weigh the raw material components according to the following weight percentages: 89 wt% of high-density polyethylene a, 10 wt% of the composite material and 1 wt% of the second auxiliary agent, wherein the second auxiliary agent is a plasticizer (polyolefin elastomer POE), an antioxidant (pentaerythritol tetrakis(3,5-di-tert-butyl-4-hydroxy)phenylpropionate) and an anti-ultraviolet agent (2-hydroxy-4-n-octyloxybenzophenone) mixed in a weight ratio of 1:1:1;
[0122] A22. Add the raw material components in step A21 into a twin-screw extruder and mix them evenly. In the twin-screw extruder, the body temperature includes three temperature zones arranged in sequence along the material flow direction, the temperature of zone one is 120°C, the temperature of zone two is 150°C, and the temperature of zone three is 190°C. The head temperature includes the neck temperature and the die temperature, wherein the neck temperature is 180°C, and the die temperature is 170°C. After the material is extruded from the twin-screw extruder, it is cooled and shaped to obtain an inner lining layer with a wall thickness of 5 mm and an inner diameter of 65 mm.
[0123] Example 2
[0124] This embodiment is used to illustrate the inner lining material and its application (the preparation method of the inner lining) described in the present invention.
[0125] 1. Preparation of modified nanofillers:
[0126] S10, heating deionized water to 80° C., then adding nano-montmorillonite and stirring evenly to obtain a mixture, wherein the weight ratio of the nano-montmorillonite to water is 1:25;
[0127] S20, adjusting the pH of the mixture to 7.0-7.2 and continuing heating for 30 minutes, then adding octadecyltrimethylammonium chloride and stirring evenly (the weight ratio of the octadecyltrimethylammonium chloride to the nano-montmorillonite is 1:12), and adjusting the pH value to 7.0-7.2, reacting for 3 hours, filtering the obtained reaction solution, washing the filtered solid with deionized water for 3 times, and then drying at 80° C. for 48 hours, and finally grinding and sieving to obtain modified nano-montmorillonite, i.e., modified nano-filler.
[0128] 2. Preparation of hydrogen sulfide absorption filler:
[0129] Mixing a silane coupling agent (vinyl triethoxysilane) with an ethanol aqueous solution (in the ethanol aqueous solution, the volume ratio of ethanol to water is 3:1), adjusting the pH of the obtained mixed solution to 4-5.5, and hydrolyzing at room temperature for 1.5 hours to obtain a coupling agent solution, wherein the volume ratio of the silane coupling agent to the ethanol aqueous solution is 1:15;
[0130] Add metal oxide (the metal oxide includes four-needle zinc oxide whiskers and nano iron oxide in a weight ratio of 1:1) and an inorganic antibacterial agent (nano copper oxide) to the coupling agent solution, wherein the weight ratio of the silane coupling agent, the metal oxide and the inorganic antibacterial agent is 1:20:10, and then ultrasonically disperse at 50°C while mechanically stirring. After reacting for 3 hours, the obtained reaction solution is filtered, and then the obtained solid phase is washed with deionized water until there is no chloride ion, vacuum dried, and then activated at 150°C for 8 hours, ground and sieved to obtain a nano-scale hydrogen sulfide absorbing filler (containing an inorganic antibacterial agent).
[0131] 3. Preparation of lining layer
[0132] A11, weighing the raw material components according to the following weight percentages: 88wt% of high-density polyethylene b, 2wt% of modified nanofiller, 9wt% of hydrogen sulfide absorbing filler and 1wt% of a first auxiliary agent, wherein the first auxiliary agent comprises a silane coupling agent (vinyl triethoxysilane) and a compatibilizer (maleic anhydride grafted high-density ethylene) in a weight ratio of 1:1;
[0133] A12, adding the raw material components in step A11 into a twin-screw extruder and mixing them evenly, heating the screw extruder, and performing kneading in the twin-screw extruder, wherein the temperature of the twin-screw extruder is divided into a first section, a second section, and a third section along the extrusion direction of the screw, wherein the temperature of the first section is 160° C., the temperature of the second section is 180° C., and the temperature of the third section is 190° C., the extruder speed of the twin-screw extruder is 300 r / min, the total residence time of the lining material in the twin-screw extruder is 5 min, and the material is cooled and pelletized after being extruded from the twin-screw extruder to obtain a composite material;
[0134] A21. Weigh the raw material components according to the following weight percentages: 89 wt% of high-density polyethylene a, 10 wt% of the composite material and 1 wt% of the second auxiliary agent, wherein the second auxiliary agent is a plasticizer (polyolefin elastomer POE), an antioxidant (pentaerythritol tetrakis(3,5-di-tert-butyl-4-hydroxy)phenylpropionate) and an anti-ultraviolet agent (2-hydroxy-4-n-octyloxybenzophenone) mixed in a weight ratio of 1:1:1;
[0135] A22. Add the raw material components in step A21 into a twin-screw extruder and mix them evenly. In the twin-screw extruder, the body temperature includes three temperature zones arranged in sequence along the material flow direction, the temperature of zone one is 120°C, the temperature of zone two is 150°C, and the temperature of zone three is 190°C. The head temperature includes the neck temperature and the die temperature, wherein the neck temperature is 180°C, and the die temperature is 170°C. After the material is extruded from the twin-screw extruder, it is cooled and shaped to obtain an inner lining layer with a wall thickness of 5 mm and an inner diameter of 65 mm.
[0136] Example 3
[0137] This embodiment is used to illustrate the inner lining material and its application (the preparation method of the inner lining) described in the present invention.
[0138] 1. Preparation of modified nanofillers:
[0139] S10, heating deionized water to 80° C., then adding nano-montmorillonite and stirring evenly to obtain a mixture, wherein the weight ratio of the nano-montmorillonite to water is 1:25;
[0140] S20, adjusting the pH of the mixture to 7.0-7.2 and continuing heating for 30 minutes, then adding octadecyltrimethylammonium chloride and stirring evenly (the weight ratio of the octadecyltrimethylammonium chloride to the nano-montmorillonite is 1:12), and adjusting the pH value to 7.0-7.2, reacting for 3 hours, filtering the obtained reaction solution, washing the filtered solid with deionized water for 3 times, and then drying at 80° C. for 48 hours, and finally grinding and sieving to obtain modified nano-montmorillonite, i.e., modified nano-filler.
[0141] 2. Preparation of hydrogen sulfide absorption filler:
[0142] Mixing a silane coupling agent (vinyl triethoxysilane) with an ethanol aqueous solution (in the ethanol aqueous solution, the volume ratio of ethanol to water is 3:1), adjusting the pH of the obtained mixed solution to 4-5.5, and hydrolyzing at room temperature for 1.5 hours to obtain a coupling agent solution, wherein the volume ratio of the silane coupling agent to the ethanol aqueous solution is 1:15;
[0143] Add metal oxide (the metal oxide includes four-needle zinc oxide whiskers and nano iron oxide in a weight ratio of 1:1) and an inorganic antibacterial agent (nano silver oxide) to the coupling agent solution, wherein the weight ratio of the silane coupling agent, the metal oxide and the inorganic antibacterial agent is 1:20:10, and then ultrasonically disperse at 50°C while mechanically stirring. After reacting for 3 hours, the obtained reaction solution is filtered, and then the obtained solid phase is washed with deionized water until there is no chloride ion, vacuum dried, and then activated at 150°C for 8 hours, ground and sieved to obtain a nano-scale hydrogen sulfide absorbing filler (containing an inorganic antibacterial agent).
[0144] 3. Preparation of lining layer
[0145] A11, weighing the raw material components according to the following weight percentages: 87wt% of high-density polyethylene b, 3wt% of modified nanofiller, 9wt% of hydrogen sulfide absorbing filler and 1wt% of a first auxiliary agent, wherein the first auxiliary agent comprises a silane coupling agent (vinyl triethoxysilane) and a compatibilizer (maleic anhydride grafted high-density ethylene) in a weight ratio of 1:1;
[0146] A12, adding the raw material components in step A11 into a twin-screw extruder and mixing them evenly, heating the screw extruder, and performing kneading in the twin-screw extruder, wherein the temperature of the twin-screw extruder is divided into a first section, a second section, and a third section along the extrusion direction of the screw, wherein the temperature of the first section is 160° C., the temperature of the second section is 180° C., and the temperature of the third section is 190° C., the extruder speed of the twin-screw extruder is 300 r / min, the total residence time of the lining material in the twin-screw extruder is 5 min, and the material is cooled and pelletized after being extruded from the twin-screw extruder to obtain a composite material;
[0147] A21. Weigh the raw material components according to the following weight percentages: 89 wt% of high-density polyethylene a, 10 wt% of the composite material and 1 wt% of the second auxiliary agent, wherein the second auxiliary agent is a plasticizer (polyolefin elastomer POE), an antioxidant (pentaerythritol tetrakis(3,5-di-tert-butyl-4-hydroxy)phenylpropionate) and an anti-ultraviolet agent (2-hydroxy-4-n-octyloxybenzophenone) mixed in a weight ratio of 1:1:1;
[0148] A22. Add the raw material components in step A21 into a twin-screw extruder and mix them evenly. In the twin-screw extruder, the body temperature includes three temperature zones arranged in sequence along the material flow direction, the temperature of zone one is 120°C, the temperature of zone two is 150°C, and the temperature of zone three is 190°C. The head temperature includes the neck temperature and the die temperature, wherein the neck temperature is 180°C, and the die temperature is 170°C. After the material is extruded from the twin-screw extruder, it is cooled and shaped to obtain an inner lining layer with a wall thickness of 5 mm and an inner diameter of 65 mm.
[0149] Example 4
[0150] The method described in Example 1 was used for implementation, except that the modified nanofiller and hydrogen sulfide absorbing filler were prepared according to the following process:
[0151] 1. Preparation of modified nanofillers:
[0152] S10, heating deionized water to 70° C., then adding kaolin and stirring evenly to obtain a mixture, wherein the weight ratio of kaolin to water is 1:25;
[0153] S20, adjusting the pH of the mixture to 7.0-7.2 and continuing heating for 40 minutes, then adding hexadecyltrimethylammonium chloride and stirring evenly (the weight ratio of the hexadecyltrimethylammonium chloride to kaolin is 1:15), and adjusting the pH value to 7.0-7.2, reacting for 3 hours, filtering the obtained reaction solution, washing the filtered solid with deionized water for 3 times, and then drying at 80°C for 48 hours, and finally grinding and sieving to obtain modified nano kaolin, i.e., modified nano filler.
[0154] 2. Preparation of hydrogen sulfide absorption filler:
[0155] Mixing a silane coupling agent (vinyl triethoxysilane) with an ethanol aqueous solution (in the ethanol aqueous solution, the volume ratio of ethanol to water is 3:1), adjusting the pH of the obtained mixed solution to 4-5.5, and hydrolyzing at room temperature for 1.5 hours to obtain a coupling agent solution, wherein the volume ratio of the silane coupling agent to the ethanol aqueous solution is 1:25;
[0156] Add metal oxide (the metal oxide includes four-needle zinc oxide whisker and nano iron oxide in a weight ratio of 1:1) and inorganic antibacterial agent (nano silver oxide) to the coupling agent solution, wherein the weight ratio of the silane coupling agent, the metal oxide and the inorganic antibacterial agent is 1:20:10, and then ultrasonically disperse at 50°C while mechanically stirring. After reacting for 3 hours, the obtained reaction solution is filtered, and then the obtained solid phase is washed with deionized water until there is no chloride ion, vacuum dried, and then activated at 150°C for 8 hours, ground and sieved to obtain a nano-scale hydrogen sulfide absorbing filler (containing an inorganic antibacterial agent).
[0157] Example 5
[0158] The method described in Example 1 is used for implementation, except that when preparing the hydrogen sulfide resistant absorption filler, the weight ratio of the silane coupling agent, the metal oxide and the inorganic antibacterial agent is 1:15:5.
[0159] Example 6
[0160] The method described in Example 1 is followed, except that step A11 comprises: weighing the raw material components according to the following weight percentages: 86 wt% of high-density polyethylene b, 6 wt% of modified nano filler, 5 wt% of hydrogen sulfide absorbing filler and 2 wt% of the first auxiliary agent.
[0161] Example 7
[0162] The method described in Example 1 is followed, except that step A11 comprises: weighing the raw material components according to the following weight percentages: 90 wt% of high-density polyethylene b, 4 wt% of modified nano filler, 5 wt% of hydrogen sulfide absorbing filler and 1 wt% of the first auxiliary agent.
[0163] Example 8
[0164] The method described in Example 1 is followed, except that step A21 includes: weighing the raw material components according to the following weight percentages: 86 wt% of high-density polyethylene a, 12 wt% of the composite material and 2 wt% of the second auxiliary agent.
[0165] Example 9
[0166] The method described in Example 1 is followed, except that step A21 includes: weighing the raw material components according to the following weight percentages: 93 wt% of high-density polyethylene a, 6 wt% of the composite material and 1 wt% of the second auxiliary agent.
[0167] Example 10
[0168] The method described in Example 1 was followed, except that no inorganic antibacterial agent was added when preparing the hydrogen sulfide absorbing filler.
[0169] Comparative Example 1
[0170] The method described in Example 1 was followed, except that the metal oxide and the inorganic antibacterial agent were not modified;
[0171] Specifically, the hydrogen sulfide absorbing filler is a mixture of metal oxide and inorganic antibacterial agent in a weight ratio of 2:1.
[0172] Comparative Example 2
[0173] The method described in Example 1 is used for implementation, except that no hydrogen sulfide absorbing filler is added. Specifically, step A11 comprises: weighing the raw material components according to the following weight percentages: 94wt% of high-density polyethylene b, 2wt% of modified nanofiller, 3% of modified antibacterial filler and 1wt% of the first auxiliary agent;
[0174] Wherein, the preparation method of modified antibacterial filler is:
[0175] Mixing a silane coupling agent (vinyl triethoxysilane) with an ethanol aqueous solution (in the ethanol aqueous solution, the volume ratio of ethanol to water is 3:1), adjusting the pH of the obtained mixed solution to 4-5.5, and hydrolyzing at room temperature for 1.5 hours to obtain a coupling agent solution, wherein the volume ratio of the silane coupling agent to the ethanol aqueous solution is 1:15;
[0176] An inorganic antibacterial agent (nano copper oxide) is added to the coupling agent solution, wherein the weight ratio of the silane coupling agent to the inorganic antibacterial agent is 1:10, and then ultrasonic dispersion is carried out at 50°C while mechanical stirring is performed. After reacting for 3 hours, the obtained reaction liquid is filtered, and then the obtained solid phase is washed with deionized water until there is no chloride ion, vacuum dried, and then activated at 150°C for 8 hours, ground and sieved to obtain a nano-scale modified antibacterial filler.
[0177] Comparative Example 3
[0178] The method described in Example 1 was followed, except that no modified nanofiller was added (the modified nanofiller was replaced with an equal amount of high-density polyethylene b);
[0179] Specifically, step A11 comprises: weighing the raw material components according to the following weight percentages: 89 wt % of high-density polyethylene b, 10 wt % of hydrogen sulfide absorbing filler and 1 wt % of the first auxiliary agent.
[0180] Comparative Example 4
[0181] The method described in Example 1 is used for implementation, except that the composite material is not prepared first. Specifically, the raw material components are directly mixed and co-extruded using the method of step A22.
[0182] Comparative Example 5
[0183] The method described in Example 1 was followed, except that no composite material was added (the composite material was replaced with an equal amount of high-density polyethylene a);
[0184] Specifically, step A21 includes: weighing the raw material components according to the following weight percentages: 99 wt % of high-density polyethylene a and 1 wt % of the second auxiliary agent.
[0185] Test Case
[0186] The inner lining layer sample prepared in Example 1 was cut into small pieces of about 5 g, put into a flat vulcanizer, and the tableting temperature was 150°C, the pressure was 10 MPa, the time was 3 min, and air-cooled. After cutting, a 50mm×50mm×0.2mm film sample was obtained; then the inner lining layers in Examples 2-10 and Comparative Examples 1-5 were also made into film samples according to the same method, and the following tests were performed respectively.
[0187] (1) The inner liner film samples prepared in Examples 1-10 and Comparative Examples 1-5 were subjected to hydrogen sulfide gas permeability tests. The results are shown in Table 1.
[0188] Table 1
[0189]
[0190]
[0191] It can be seen from Table 1 that the inner lining layers prepared in Examples 1-10 of the present invention have low permeability to H2S gas, which means that the inner lining layer prepared by the inner lining layer material provided by the present invention has high gas barrier properties and can effectively prevent the leakage of H2S.
[0192] It can be seen from Example 1 and Comparative Examples 1-2 that if the metal oxide is not modified, the gas barrier property of the inner lining layer obtained therefrom (i.e., Comparative Example 1) changes little compared with the inner lining layer obtained without adding hydrogen sulfide filler (Comparative Example 2). This may be due to the poor dispersibility of the metal oxide in high-density polyethylene and insufficient absorption of H2S; and the gas barrier property of Comparative Examples 1-2 is not as good as that of Example 1, indicating that the gas barrier property of the inner lining layer can be further improved by adding hydrogen sulfide filler.
[0193] By comparing Example 1 with Comparative Example 3, it can be seen that the gas barrier property of the liner layer can be greatly improved by adding the modified nanofiller.
[0194] By comparing Comparative Examples 4 and 5, it can be seen that if the composite material is not prepared first, the gas barrier property of the prepared lining layer (i.e., Comparative Example 4) is worse than that of the lining layer without adding the composite material (i.e., Comparative Example 5). This may be due to the uneven dispersion of the hydrogen sulfide absorbing filler and the modified nanofiller in the HDPE and the poor compatibility of the composite material with the HDPE. Compared with Example 1, the gas barrier property of Comparative Examples 4 and 5 is greatly reduced, indicating that the gas barrier property of the lining layer can be significantly improved by adding the composite material.
[0195] (2) The inner lining film samples prepared in Example 1, Example 10 and Comparative Examples 1-5 were subjected to antibacterial tests in accordance with the antibacterial test standard QB / T2591-2003A "Test methods and antibacterial effects of antibacterial plastics". Detection bacteria: sulfate-reducing bacteria. After the inner lining film samples were immersed in sulfate-reducing bacteria solution for 7 days, the bacterial adhesion on the sample surface was observed under a fluorescence microscope. The Imagine pro 6.0 software was used to calculate the coverage area ratio of live / dead bacteria on the material surface, and the average value was taken. The test results of the bacterial adhesion rate of the materials are shown in Table 2. Among them, the bacterial adhesion results of Example 1 and Comparative Example 5 are shown in Table 2. Figure 1 and Figure 2 shown.
[0196] Table 2
[0197] project Bacterial attachment rate / % Example 1 0.1 Example 10 79 Comparative Example 1 7.8 Comparative Example 2 28 Comparative Example 3 0.73 Comparative Example 4 71.79 Comparative Example 5 91.03
[0198] It can be seen from Table 2 that the inner lining layer prepared by the inner lining layer material of the present invention has good antibacterial properties. By comparing Example 1 with Example 10, it can be seen that by adding an inorganic antibacterial agent when preparing the hydrogen sulfide absorbing filler, the antibacterial properties of the inner lining layer material can be further improved.
[0199] It should be noted that the preparation principles of Examples 2 to 9 are similar to those of Example 1, and therefore, the antibacterial properties of Examples 2 to 9 are also good.
[0200] The preferred embodiments of the present invention are described in detail above, but the present invention is not limited thereto. Within the technical concept of the present invention, the technical solution of the present invention can be subjected to a variety of simple modifications, including the combination of various technical features in any other suitable manner, and these simple modifications and combinations should also be regarded as the contents disclosed by the present invention and belong to the protection scope of the present invention.
Claims
1. A lining material, characterized in that: The inner lining material contains high-density polyethylene a and a composite material. The composite material contains high-density polyethylene b, modified nano filler, hydrogen sulfide absorbing filler and a first auxiliary agent. The hydrogen sulfide absorbing filler contains a metal oxide modified by a silane coupling agent, and the metal oxide can chemically react with hydrogen sulfide; The modified nanofiller is obtained by modifying a sheet-like nanofiller with a cationic surfactant, and the first auxiliary agent is a coupling agent and / or a compatibilizer.
2. The lining material according to claim 1, characterized in that: The metal oxide is nano zinc oxide and / or nano iron oxide; Preferably, the hydrogen sulfide absorbing filler further contains an inorganic antibacterial agent modified by a silane coupling agent, wherein the inorganic antibacterial agent is nano copper oxide and / or nano silver oxide.
3. The lining material according to claim 1 or 2, characterized in that: The hydrogen sulfide absorbing filler is prepared according to the following process: Mixing a silane coupling agent with an ethanol aqueous solution, adjusting the pH of the obtained mixed solution to 3.5 to 5 and reacting to obtain a coupling agent solution; The coupling agent solution is mixed with the metal oxide, and then ultrasonically dispersed and reacted, the obtained reaction solution is separated into solid and liquid, and the obtained solid phase is washed, dried, activated, ground and sieved.
4. The lining material according to claim 3, characterized in that: The volume ratio of the silane coupling agent to the ethanol aqueous solution is 1:15-25; Preferably, in the ethanol aqueous solution, the volume ratio of ethanol to water is 2 to 4:1; Preferably, the weight ratio of the silane coupling agent to the metal oxide is 1:15-25.
5. The lining material according to claim 1, characterized in that: Based on the total weight of the composite material, the content of the high-density polyethylene b is 85-94wt%, the content of the modified nanofiller is 2-6wt%, the content of the hydrogen sulfide absorbing filler is 3-10wt%, and the content of the first auxiliary agent is 1-2wt%; Preferably, the flaky nanofiller is selected from one or more of muscovite, biotite, phlogopite, kaolin and montmorillonite; Preferably, the cationic surfactant is a long-chain alkyl quaternary ammonium salt, preferably one or more of dodecyltrimethylammonium chloride, hexadecyltrimethylammonium bromide, hexadecyltrimethylammonium chloride, octadecyltrimethylammonium chloride and octadecyldimethylbenzylammonium chloride.
6. The lining material according to claim 1 or 2, characterized in that: The modified nanofiller is prepared according to the following process: S10, heating water to 70-90° C., and then mixing the water with the flaky nanofiller to obtain a mixture; S20, adjusting the pH of the mixture to 6.8-7.5 and continuing heating for 30-50 minutes, then reacting with a cationic surfactant, separating the obtained reaction liquid into solid and liquid, and then washing, drying, grinding and sieving the obtained solid.
7. The lining material according to claim 6, characterized in that: In step S10, the weight ratio of the flaky nanofiller to water is 1:25-50; Preferably, the weight ratio of the cationic surfactant to the flaky nanofiller is 1:10-20.
8. The lining material according to claim 1, characterized in that: The melt index of the high-density polyethylene b is 0.3 to 0.5 g / min; Preferably, the compatibilizer is selected from one or more of maleic anhydride grafted high-density ethylene, maleic anhydride grafted ethylene-1-octene block copolymer, acrylic acid grafted polyethylene and maleic anhydride grafted ethylene-vinyl acetate copolymer; Preferably, the coupling agent is a silane coupling agent and / or a titanate coupling agent.
9. The lining material according to claim 1, characterized in that: The composite material is prepared according to the following process: high-density polyethylene, modified nano filler, hydrogen sulfide absorbing filler and a first auxiliary agent are blended and extruded; Preferably, the blending extrusion is carried out in a twin-screw extruder; Preferably, the working temperature of the twin-screw extruder is 160-200° C., the working speed is 300-350 r / min, and the working time is 3-6 min.
10. The lining material according to claim 1, characterized in that: Based on the total weight of the inner lining material, the content of the high-density polyethylene a is 85-98wt%, and the content of the composite material is 2-15wt%; Preferably, the high-density polyethylene a and the high-density polyethylene b are the same; Preferably, the inner lining material further contains a second auxiliary agent, and the second auxiliary agent is selected from one or more of a plasticizer, a flame retardant and an antioxidant; Preferably, in the inner lining material, the content of the second auxiliary agent is 1-2 wt %.
11. A method for preparing an inner lining layer, characterized in that: The method comprises the following steps: A1, blending and extruding high-density polyethylene b, modified nano filler, hydrogen sulfide absorbing filler and the first auxiliary agent, cooling and granulating to obtain a composite material; A2, blending and extruding the composite material and high-density polyethylene a, and cooling and shaping; Among them, in step A1, the hydrogen sulfide absorbing filler contains a metal oxide modified by a silane coupling agent, the metal oxide can react chemically with hydrogen sulfide, the modified nanofiller is a sheet-like nanofiller modified by a cationic surfactant, and the first auxiliary agent is a coupling agent and / or a compatibilizer.
12. The method according to claim 11, characterized in that In step A1, based on the total weight of the composite material, the content of the high-density polyethylene b is 85-94wt%, the content of the modified nanofiller is 2-6wt%, the content of the hydrogen sulfide absorbing filler is 3-10wt%, and the content of the first auxiliary agent is 1-2wt%; Preferably, in step A1, the blending extrusion is carried out in a twin-screw extruder, wherein the working temperature of the twin-screw extruder is 160-200° C., the working speed is 300-350 r / min, and the working time is 3-6 min.
13. The method according to claim 11, characterized in that In step A2, the blending extrusion is carried out in a twin-screw extruder; Preferably, in step A2, the body temperature of the twin-screw extruder includes three temperature zones arranged in sequence along the material flow direction, the temperature of zone 1 is 110-130° C., the temperature of zone 2 is 140-160° C., and the temperature of zone 3 is 180-200° C.; Preferably, in step A2, the head temperature of the twin-screw extruder is 165-185°C.
14. A composite pipe, characterized in that: The composite pipe comprises an inner lining layer, a reinforcement layer and an outer pipe arranged in sequence from the inside to the outside; Wherein, the lining layer is made of the lining layer material described in any one of claims 1-10 or is made of the method described in any one of claims 11-13.
Citation Information
Patent Citations
Pipe having barrier property
CN101072822A
Antibacterial polypropylene composite material and preparation method thereof
CN112920509A
Limited permeability sheath and application to pressure pipes
US6110550A