Mildew-proof and salt-fog-resistant sheath as well as preparation method and application thereof
By adding anti-mold and anti-bacterial masterbatches to the cable sheath material and using extrusion granulation and extrusion processing, we prepare mold, acid, alkali and salt spray-resistant sheath, which solves the problem of the cable in humid and heat and saline-alkali environments. The problem of mesogenic mold corrosion extends the service life of the cable and improves its reliability in complex environments.
Patent Information
- Application Number
- CN202411074240.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-07
- Publication Date
- 2024-11-12
AI Technical Summary
Existing cable sheaths are prone to mold and rot in humid and heat and salt-alkali corrosion environments, resulting in a shortened service life of the cable and is not resistant to acid and alkali corrosion, and cannot effectively prevent the erosion of mold and salt spray.
Add anti-mold and anti-bacterial masterbatches to the cable sheath, including polyethylene resin, anti-mold agent, anti-bacterial agent, compatibilizer and coupling agent, and prepare anti-mold salt spray sheath through extrusion granulation and extrusion processing. , improve its mildew, acid, alkali and salt spray resistance.
It realizes the long-term and stable operation of cable sheath in high temperature and high humidity environments, extends service life, effectively inhibits mold growth, meets the performance requirements of GB/T12706.1 and GJB150.10A standards, and ensures the reliability of cables in complex environments. .
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_3
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of marine cable transmission, relates to a cable sheath, and in particular to a mildew-proof and salt-spray-resistant sheath and a preparation method and application thereof. Background Art
[0002] At present, the structural design of power transmission line cables used in power engineering projects such as power transmission in rainy season, plum rain season, islands with hot and humid climate, between islands and between islands and coastlines, offshore wind power projects and wind power projects in saline-alkali areas, etc. is not much different from that of ordinary power cables. When the cable sheath is laid and operated in an environment with water or seawater penetration, seawater or acid-base corrosion, the wood, metal brackets and other materials in the surrounding environment will first grow mold, and then the cable surface in contact with them may be corroded by mold. The cable sheath is directly exposed to the mold environment, and this type of material is easy to be used as a nutrient for mold and is easily directly corroded by mold, resulting in large-scale mold growth, which seriously affects the service life of the cable.
[0003] In the rainy season, plum rain season and areas with hot and humid climate, the environment is extremely harsh and complex. The ordinary cables or some special cables used, the cable sheath will be bred by various molds such as Aspergillus niger, Paecilomyces variotii, Penicillium funiculosum, Penicillium ochregreenii, Trichoderma viride, etc. in a humid environment, which will cause serious cable corrosion, short circuit, leakage, and breakage of the cable, making it unable to work normally.
[0004] For example, the Chinese patent, publication number CN104292673A, publication date 2015-01-21, is entitled "Anti-mildew rubber sheath material for cable", and the raw materials are composed of 100 parts of chlorinated polyethylene, 10-30 parts of anti-mildew filler, 25-45 parts of plasticizer, 2.5-4 parts of vulcanizer, 3-6 parts of co-vulcanizer, 9-11.5 parts of activator, 1-6 parts of antioxidant, and 0.5-2 parts of coupling agent.
[0005] Although this patent adds anti-mildew filler, which plays a certain anti-mildew role, this type of material is still not resistant to acid and alkali corrosion and salt spray in coastal areas or environments with certain acid and alkali corrosion. Summary of the invention
[0006] In order to solve the above problems, the present invention provides a mildew-proof and salt-spray-resistant sheath and a preparation method and application thereof. The sheath material of the present invention can achieve properties such as mildew resistance, acid and alkali corrosion resistance, and salt spray resistance, thereby more effectively protecting various cable products laid in marine engineering, photovoltaic wind power, saline-alkali desert areas, and the like. The long-term operating temperature of the material of the present invention is 90°C, the maximum temperature is 250°C, and the service life is not less than 32 years.
[0007] In order to achieve the above object, the present invention adopts the following technical solutions:
[0008] The invention provides a mildew-proof and salt-spray-resistant sheath. The mildew-proof and salt-spray-resistant sheath is prepared by adding 1-5 parts by weight of mildew-proof and antibacterial masterbatch to every 100 parts by weight of sheath material raw materials; the raw materials of the mildew-proof and antibacterial masterbatch include, by weight, 100 parts of polyethylene resin, 25-35 parts of mildewcide, 10-17 parts of antibacterial agent, 2.2-3.4 parts of compatibilizer, 1.1-3.34 parts of coupling agent and 3.03-4.36 parts of black masterbatch.
[0009] As a preferred solution of the present invention, the mildew inhibitor is a lamellar nano silver powder with a diameter of ≤2 μm.
[0010] As a preferred embodiment of the present invention, the antibacterial agent is ultrafine zinc oxide with a particle size of 20-40 μm, a purity of ≥99.9%, a drying loss of ≤0.5%, and a burning loss of ≤1.0%.
[0011] As a preferred solution of the present invention, the compatibilizer is a copolymer of acrylonitrile, styrene, acrylate and olefin, with a butadiene content of ≥25%, an acrylate content of ≥45%, and a tensile elongation at break of >500%; and a melting starting temperature of 165-190°C.
[0012] As a preferred embodiment of the present invention, the coupling agent is a silane coupling agent.
[0013] As a preferred solution of the present invention, the raw material of the sheath material is linear low-density polyethylene or high-density polyethylene sheath material particles.
[0014] As a preferred embodiment of the present invention, when the mildew and antibacterial grade is 0, 3.41-4.06 parts by weight of mildew and antibacterial masterbatch is added to every 100 parts by weight of the sheath material raw material;
[0015] When the mildew and antibacterial grade is 1, 2.88-3.40 parts by weight of mildew and antibacterial masterbatch is added to every 100 parts by weight of the sheath material raw material;
[0016] When the mildew and antibacterial grade is 2, 2.35-2.87 parts by weight of mildew and antibacterial masterbatch is added to every 100 parts by weight of the sheath material raw material;
[0017] When the mildew and antibacterial grade is 3, 1.83-2.34 parts by weight of mildew and antibacterial masterbatch is added to every 100 parts by weight of the sheath material raw material;
[0018] When the mildew and antibacterial grade is 4, 1.32-1.82 parts by weight of mildew and antibacterial masterbatch is added to every 100 parts by weight of the sheath material raw material.
[0019] The present invention also provides a method for preparing the above-mentioned mildew-proof and salt-spray-resistant sheath, the preparation method comprising the following steps:
[0020] 1) Preparation of anti-mildew and antibacterial masterbatch:
[0021] 1) Weigh polyethylene resin, mildew inhibitor, antibacterial agent, compatibilizer, coupling agent and black masterbatch according to the formula, mix and stir evenly, and continue mixing at elevated temperature to obtain mixed material A;
[0022] 2) The mixed material A obtained in step 1) is granulated by twin-screw extrusion to obtain black mildew-proof and antibacterial masterbatch B in the form of 3 mm×3 mm×3 mm square granules or cylindrical granules of comparable size;
[0023] 2) Weigh the mildew-proof and antibacterial masterbatch B and the raw material of the sheath material obtained in step 1), mix and stir for 11 minutes to 17 minutes, stir at 360 degrees for 25 to 30 circles per minute, and stir at a temperature of 30°C to 45°C. After fully mixing, flow to the hopper of the extruder and the barrel of the extruder through the hopper of the self-priming system, and obtain the mildew-proof and salt-spray-resistant sheath through plasticization, homogenization, molding and shaping at 120°C to 155°C.
[0024] As a preferred embodiment of the present invention, in step 1), the mixing and stirring is as follows: the stirring frequency is 3000 rpm-5800 rpm, after stirring for 17 minutes-21 minutes, the temperature is raised to 110°C-145°C, and the mixing and stirring is continued for 25 minutes-35 minutes.
[0025] Finally, the present invention provides the use of the mildew-proof and salt-spray-resistant sheath in the preparation of control cables, power cables or cables for marine engineering.
[0026] Compared with the prior art, the present invention has the following beneficial effects:
[0027] 1) The present invention adds mildew-proof and antibacterial masterbatch to the sheath material, thereby improving various properties such as mildew resistance, acid and alkali corrosion resistance, and salt spray resistance; the performance of the sheath material meets the ST7 requirements of GB / T12706.1, and the extrusion processing performance is excellent.
[0028] 2) The preparation method of the present invention is simple and easy to operate.
[0029] 3) The sheath material of the present invention has a wide range of applications, and can be widely used in cable sheaths laid in high temperature and high humidity environments such as marine engineering, photovoltaic wind power, saline-alkali desert areas, etc. The cable can effectively inhibit various molds such as Aspergillus niger, Penicillium variotii, Penicillium funiculum, Penicillium ochregreenii, Trichoderma viride, etc., avoiding the growth of microorganisms and molds.
[0030] 4) The sheath material of the present invention has passed the mold test specified in GJB150.10A, simulating the mold environment that the cable may encounter in actual use, and detecting the performance changes and reliability performance of the cable under the action of mold; effectively evaluating the performance and reliability of the cable and its sheath material in a mold growth environment, ensuring the stable operation of the cable in a complex environment. DETAILED DESCRIPTION
[0031] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.
[0032] The invention first provides a mildew-proof and salt-spray-resistant sheath. The mildew-proof and salt-spray-resistant sheath is prepared by adding 1-5 parts by weight of mildew-proof and antibacterial masterbatch to every 100 parts by weight of sheath material raw materials. The raw materials of the mildew-proof and antibacterial masterbatch include, by weight, 100 parts of polyethylene resin, 25-35 parts of mildewcide, 10-17 parts of antibacterial agent, 2.2-3.4 parts of compatibilizer, 1.1-3.34 parts of coupling agent and 3.03-4.36 parts of black masterbatch.
[0033] In the present invention, polyethylene resin is purchased from Ningbo Tianyuan SP-0510 or Shanghai Yexin 0510 and used as a carrier of the masterbatch.
[0034] The mildew inhibitor was purchased from Anhui Zhenghe Yaju New Materials KF30 or Fujian Ruisen, high-quality lamellar high-purity nano silver powder antibacterial silver ion, with a diameter of no more than 2μm, and white powder.
[0035] The antibacterial agent was purchased from Shanghai Yingcheng New Materials YC-Zn30, ZnO high-purity ultrafine zinc oxide, particle size 30±10μm, light yellow powder, purity not less than 99.9%, drying loss not more than 0.5%; ignition loss not more than 1.0%.
[0036] The compatibilizer was purchased from Dongguan Chuangzhiyuan New Materials EP308. The toughening compatibilizer EP308 is a multi-polymer of acrylonitrile, styrene, acrylate, and olefin. It has a light yellow elastic particle appearance. This product is a widely used engineering plastic toughening compatibilizer. Rubber (butadiene) content ≥ 25%, acrylate content ≥ 45%, tensile elongation at break > 500%; melting start temperature: 165-190℃; MI (g / 10min) 9.5.
[0037] The coupling agent was purchased from Nanjing Changhu Chemical A171, which is a silane coupling agent.
[0038] The black masterbatch was purchased from Maokang Materials BB571L, Kasong Chemical KS2000 or Zhongbei Fine Chemical ZB808.
[0039] The mildew-proof and antibacterial masterbatch of the present invention is prepared by the following method:
[0040] 1) According to the formula, polyethylene resin, mildewproof agent, antibacterial agent, compatibilizer, silane coupling agent and black masterbatch are weighed and mixed evenly (mixing and stirring parameters are: stirring frequency is 3000 rpm-5800 rpm, stirring for 17 minutes-21 minutes, heating to 110°C-145°C, mixing for 25 minutes-35 minutes), stirring for a period of time, heating and continuing to mix to obtain mixed material A.
[0041] 2) The mixed material A is extruded and granulated by a twin-screw extruder to obtain black mildew-proof and antibacterial masterbatch B in the form of 3mm×3mm×3mm square granules or cylindrical granules of comparable size.
[0042] The test was carried out according to the test method specified in the GJB 150.10A-2009 "Military Equipment Laboratory Environmental Test Methods Part 10: Mold Test" standard. At the same time, the direct contact method was used in the alternating mold test box JMS-225. There were 5 groups of samples, 0.7 meters, and the test duration was 28 days. After 672 hours, the growth of mold on the surface of the cable sheath was observed.
[0043] Appearance, density of bacterial growth, check whether the anti-mildew and anti-bacterial effect of the sheath sample complies with the requirements of Table 1.
[0044] Table 1. Addition amount of cable sheath anti-mildew and anti-bacterial masterbatch and anti-mildew and anti-bacterial effect
[0045]
[0046]
[0047] Example 1
[0048] This embodiment provides a method for processing and preparing a mildew-proof and antibacterial grade 0 sheath, comprising:
[0049] Referring to Table 1, 3.41-4.06 parts of the above-mentioned black mildew-proof and antibacterial masterbatch B and 100 parts of high-density polyethylene sheath material particles are weighed according to the formula, mixed and stirred for 11 minutes to 17 minutes, stirred 25 to 30 times at 360° per minute, and the stirring temperature is 30°C to 45°C to fully mix them, and then flow to the hopper of the SJ-120 or SJ-150 extruder and the barrel of the extruder through the self-priming system hopper. At 120°C to 155°C for extrusion, the material is plasticized, homogenized, formed, and shaped in the barrel, so that the plastic is uniformly plasticized (i.e., melted) and passed through the right-angle head and the semi-extrusion tooling die to extrude into an integral mildew-proof sheath; the physical and mechanical, mildew-resistant, acid and alkali-resistant, salt spray-resistant and other properties of the finished sheath are tested, as shown in Table 2.
[0050] Example 2
[0051] This embodiment provides a method for processing and preparing a mildew-proof and antibacterial grade 1 sheath, comprising:
[0052] Referring to Table 1, 2.88-3.40 parts of black mildew and antibacterial masterbatch B are taken by weight, and the remaining raw materials and processes are the same as those in Example 1; the physical and mechanical, mildew resistance, acid and alkali resistance, salt spray resistance and other properties of the processed finished sheath are tested, see Table 2.
[0053] Example 3
[0054] This embodiment provides a method for processing and preparing a mildew-proof and antibacterial second-level sheath, comprising:
[0055] Referring to Table 1, 2.35-2.87 parts of black mildew and antibacterial masterbatch B are taken by weight, and the remaining raw materials and processes are the same as those in Example 1; the physical and mechanical, mildew resistance, acid and alkali resistance, salt spray resistance and other properties of the processed finished sheath are tested, see Table 2.
[0056] Example 4
[0057] This embodiment provides a method for processing and preparing a mildew-proof and antibacterial level 3 sheath, comprising:
[0058] Referring to Table 1, 1.83-2.34 parts of black mildew and antibacterial masterbatch B are taken by weight, and the remaining raw materials and processes are the same as those in Example 1; the physical and mechanical, mildew resistance, acid and alkali resistance, salt spray resistance and other properties of the processed finished sheath are tested, see Table 2.
[0059] Example 5
[0060] This embodiment provides a method for processing and preparing a mildew-proof and antibacterial 4-level sheath, comprising:
[0061] Referring to Table 1, 1.32-1.82 parts of black mildew-proof and antibacterial masterbatch B are taken by weight, and the remaining raw materials and processes are the same as those in Example 1; the physical and mechanical, mildew-resistant, acid and alkali-resistant, salt spray-resistant and other properties of the processed finished sheath are tested, see Table 2.
[0062] Table 2. Test data of Examples 1-5
[0063]
[0064]
[0065]
[0066]
[0067] The main technical parameters of mildew-proof and salt-spray-resistant sheath are as follows:
[0068] 1) Raw material properties: in accordance with GB / T 15065 "Black polyethylene plastic for wires and cables" standard.
[0069] 2) Excellent anti-mildew and antibacterial properties: The anti-mildew test can reach level 0, and there is no mold growth on the material (the growth area is 0%). Other levels can reach the levels specified in Table 1 according to the requirements of the installation and operation environment.
[0070] 3) Excellent corrosion resistance: The sample is in oxalic acid (1mol / L), sodium hydroxide (1mol / L), test temperature 23±2℃, duration 168h, tensile strength change rate ≤±30%, elongation at break change rate: minimum 100%.
[0071] 4) Water-blocking performance: After the sheath is immersed in 85°C water for 336 hours, the weight increase is no more than 1mg / cm 2 .
[0072] 5) Cable UV protection performance: Meets 1008 hours of UV protection: After 0h-1008h aging, the change rate of tensile strength is ≤±30%, and the change rate of elongation at break is ≤±30%; after 504h-1008h aging, the change rate of tensile strength is ≤±15%, and the change rate of elongation at break is ≤±15%.
[0073] 6) Salt spray resistance: It can meet the salt spray test for 336 hours, 5% NaCL solution, pH 7.0, 35°C, the change rate of tensile strength is ≤±30%, and the change rate of elongation at break is ≤±30%.
[0074] The mildew-proof and salt-spray-resistant sheath prepared by the present invention can be used as a cable sheath laid in high-temperature and high-humidity environments such as marine engineering, photovoltaic wind power, and saline-alkali desert areas for a long time. The cable can effectively inhibit various molds such as Aspergillus niger, Penicillium variotii, Penicillium funiculum, Penicillium ochregreenii, and Trichoderma viride, thereby avoiding the growth of microorganisms and molds.
[0075] The mildew-proof and salt-spray-resistant sheath of the present invention has been put into mass production in the application of cables. The product has passed the mold test specified in GJB150.10A, simulated the mold environment that the cable may encounter in actual use, and detected the performance changes and reliability performance of the cable under the action of mold; effectively evaluated the performance and reliability of the cable and its sheath material in a mold growth environment, ensuring the stable operation of the cable in a complex environment.
[0076] The above is only a preferred embodiment of the present invention, and is not any formal or substantial limitation of the present invention. It should be pointed out that ordinary technicians in this technical field can make several improvements and supplements without departing from the method of the present invention, and these improvements and supplements should also be regarded as the protection scope of the present invention. Any technician familiar with this profession, without departing from the spirit and scope of the present invention, can make some changes, modifications and evolutions of the technical content disclosed above, which are equivalent embodiments of the present invention; at the same time, any changes, modifications and evolutions of any equivalent changes made to the above embodiments based on the essential technology of the present invention are still within the scope of the technical solution of the present invention.
Claims
1. A mildew-proof and salt-spray-resistant sheath, characterized in that: The mildew-proof and salt-spray-resistant sheath is prepared by adding 1-5 parts by weight of mildew-proof and antibacterial masterbatch to every 100 parts by weight of the sheath material raw material; the raw materials of the mildew-proof and antibacterial masterbatch include, by weight, 100 parts of polyethylene resin, 25-35 parts of mildewcide, 10-17 parts of antibacterial agent, 2.2-3.4 parts of compatibilizer, 1.1-3.34 parts of coupling agent and 3.03-4.36 parts of black masterbatch.
2. The mildew-proof and salt-spray-resistant sheath according to claim 1, characterized in that: The mildew inhibitor is a lamellar nano silver powder with a diameter of ≤2 μm.
3. The mildew-proof and salt-spray-resistant sheath according to claim 1, characterized in that: The antibacterial agent is ultrafine zinc oxide with a particle size of 20-40 μm, a purity of ≥99.9%, a drying loss of ≤0.5%, and a burning loss of ≤1.0%.
4. The mildew-proof and salt-spray-resistant sheath according to claim 1, characterized in that: The compatibilizer is a copolymer of acrylonitrile, styrene, acrylate and olefin, with a butadiene content of ≥25%, an acrylate content of ≥45%, a tensile elongation at break of >500%, and a melting starting temperature of 165-190°C.
5. The mildew-proof and salt-spray-resistant sheath according to claim 1, characterized in that: The coupling agent is a silane coupling agent.
6. A mildew-proof and salt-spray-resistant sheath according to any one of claims 1 to 5, characterized in that: The raw material of the sheath material is linear low-density polyethylene or high-density polyethylene sheath material particles.
7. The mildew-proof and salt-spray-resistant sheath according to claim 6, characterized in that: When the mildew and antibacterial grade is 0, 3.41-4.06 parts by weight of mildew and antibacterial masterbatch is added to every 100 parts by weight of the sheath material raw material; When the mildew and antibacterial grade is 1, 2.88-3.40 parts by weight of mildew and antibacterial masterbatch is added to every 100 parts by weight of the sheath material raw material; When the mildew and antibacterial grade is 2, 2.35-2.87 parts by weight of mildew and antibacterial masterbatch is added to every 100 parts by weight of the sheath material raw material; When the mildew and antibacterial grade is 3, 1.83-2.34 parts by weight of mildew and antibacterial masterbatch is added to every 100 parts by weight of the sheath material raw material; When the mildew and antibacterial grade is 4, 1.32-1.82 parts by weight of mildew and antibacterial masterbatch is added to every 100 parts by weight of the sheath material raw material.
8. A method for preparing the mildew-proof and salt-spray-resistant sheath according to any one of claims 1 to 7, characterized in that: The preparation method comprises the following steps: 1) Preparation of anti-mildew and antibacterial masterbatch: 1) Weigh polyethylene resin, mildew inhibitor, antibacterial agent, compatibilizer, coupling agent and black masterbatch according to the formula, mix and stir evenly, and continue mixing at elevated temperature to obtain mixed material A; 2) The mixed material A obtained in step 1) is granulated by twin-screw extrusion to obtain black mildew-proof and antibacterial masterbatch B in the form of 3 mm×3 mm×3 mm square granules or cylindrical granules of comparable size; 2) Weigh the mildew-proof and antibacterial masterbatch B and the raw material of the sheath material obtained in step 1), mix and stir for 11 minutes to 17 minutes, stir at 360 degrees for 25 to 30 circles per minute, and stir at a temperature of 30°C to 45°C. After fully mixing, flow to the hopper of the extruder and the barrel of the extruder through the hopper of the self-priming system, and obtain the mildew-proof and salt-spray-resistant sheath through plasticization, homogenization, molding and shaping at 120°C to 155°C.
9. The method for preparing the mildew-proof and salt-spray-resistant sheath according to claim 8, characterized in that: In the step 1), the mixing and stirring is as follows: the stirring frequency is 3000 rpm-5800 rpm, after stirring for 17 minutes-21 minutes, the temperature is raised to 110° C.-145° C., and the mixing and stirring is continued for 25 minutes-35 minutes.
10. Use of the mildew-proof and salt-spray-resistant sheath according to any one of claims 1 to 7 in the preparation of control cables, power cables or cables for marine engineering.
Citation Information
Patent Citations
Special computer and instrument cable for efficient photovoltaic system
CN105374423A
Polypropylene random (PPR) tube antibacterial coloring master batch and preparation method thereof
CN108948503A
Preparation method of air-conditioning duct with antibacterial and anti-mildew properties
CN111645348A
Anti-algae and antibacterial sheath, online mixing extrusion molding production process method and application
CN113427735A
Flame-retardant sheath rubber material for salt-fog-resistant offshore wind power cable and preparation method of flame-retardant sheath rubber material
CN114854115A