Magnetic interference shielding film and preparation method thereof

By using a magnetic interference shielding film combined with FeNi, FeCr and FeSiCr, the problem of electromagnetic wave interference in the 13.56MHz band is solved, effective noise suppression and stability of the electronic control unit are achieved, and the magnetic permeability is between 120 and 180.

CN118931122APending Publication Date: 2024-11-12NANJING BOPING ELECTRONICS TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411021330.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-29
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The electromagnetic wave interference source in the 13.56MHz frequency band is prone to affect the operation of other chips, especially in cars, which causes the click converter to generate noise and affect the radio reception status and cause the electronic control unit to act incorrectly.

Method used

Magnetic interference shielding film made of a combination of FeNi, FeCr and FeSiCr, polyester of PA12 powder, hindered phenol 1010 and phosphite auxiliary antioxidant, calcium stearate processing lubricant, through high-speed mixing and extrusion Preparation of casting process, the thickness is controlled between 0.5 and 1.5 mm, effectively suppressing the noise radiation of the radio frequency chip.

Benefits of technology

It effectively solves the problem of noise radiation exceeding the standard in the 13.56MHz band of radio frequency chips, suppresses noise, and has a magnetic permeability of 120 to 180, avoiding erroneous actions of the electronic control unit.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118931122A_ABST
    Figure CN118931122A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of wireless communication, and particularly discloses a magnetic interference shielding film and a preparation method thereof, and the magnetic interference shielding film comprises the following components in percentage by mass: 70-85 wt% of an absorbent, 10-15 wt% of polyester, 1-3 wt% of an antioxidant, 1-2 wt% of a dispersant and 1-2 wt% of a processing lubricant. By adopting the extrusion casting process, the problems that the noise radiation of the radio frequency chip exceeds the standard at the frequency band of 13.56 MHz and the equipment has radiation interference can be effectively solved, meanwhile, the error action of the electronic control unit is not influenced, and the magnetic conductivity of the noise suppression sheet at the frequency band of 13.56 MHz is 120-180.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of wireless communication technology, and in particular to a magnetic interference shielding film and a preparation method thereof. Background Art

[0002] At present, with the development of wireless communication systems and the popularization of Internet of Things devices, digital devices are used in large quantities. During operation, the devices will generate various electromagnetic radiations including magnetic field interference.

[0003] In the existing technology, 13.56MHz is the most likely source of electromagnetic interference. It has a low operating voltage and is easy to interfere with the operation of other chips. In automobiles, the noise generated by the click converter will affect the reception status of the radio and cause malfunctions of the electronic control unit. Summary of the invention

[0004] The purpose of the present invention is to provide a magnetic interference shielding film, aiming to solve the technical problem in the prior art that 13.56MHz is the most likely source of electromagnetic interference, has a low operating voltage, and is likely to interfere with the operation of other chips. In the automotive field, the noise generated by the click converter will affect the reception status of the radio and cause the electronic control unit to malfunction.

[0005] To achieve the above object, the present invention adopts a magnetic interference shielding film, including the following mass fractions:

[0006] 70 wt% to 85 wt% of absorbent, 10 wt% to 15 wt% of polyester, 1 wt% to 3 wt% of antioxidant, 1 wt% to 2 wt% of dispersant and 1 wt% to 2 wt% of processing lubricant.

[0007] Wherein, the absorbent is any one or more combinations of FeNi, FeCr and FeSiCr.

[0008] Wherein, the polyester is PA12 powder.

[0009] The antioxidant is prepared by mixing high molecular hindered phenol 1010 and phosphite auxiliary antioxidant 168.

[0010] Wherein, the processing lubricant is calcium stearate.

[0011] Wherein, the thickness of the magnetic interference shielding film is 0.5-1.5 mm.

[0012] The present invention also provides a method for preparing a magnetic interference shielding film, and the method for preparing the magnetic interference shielding film as described above comprises the following steps:

[0013] Add the raw materials of each component into the high-speed mixer according to the proportion;

[0014] The high-speed mixer was stirred at a speed of 1000 RPM and a temperature of 80°C for 30 min;

[0015] Pour the evenly mixed powder into the extrusion casting machine;

[0016] The thickness of the cast film is controlled to be between 0.7 and 1.0 mm, and the preparation of the magnetic interference shielding film is now completed.

[0017] The beneficial effects of the magnetic interference shielding film and the preparation method thereof of the present invention are as follows: the extrusion casting process can effectively solve the problem of excessive noise radiation of the RF chip in the 13.56MHz frequency band and radiation interference of the equipment, and at the same time will not affect the erroneous operation of the electronic control unit. The magnetic permeability of the noise suppression sheet at 13.56MHz is 120-180. BRIEF DESCRIPTION OF THE DRAWINGS

[0018] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0019] Figure 1 This is a flow chart of the method steps of Example 1 of a method for preparing a magnetic interference shielding film of the present invention.

[0020] Figure 2 It is a flow chart of the method steps of Example 2 of a method for preparing a magnetic interference shielding film of the present invention.

[0021] Figure 3 This is a flow chart of the method steps of Example 3 of a method for preparing a magnetic interference shielding film of the present invention.

[0022] Figure 4 It is a flow chart of the method steps of Example 4 of a method for preparing a magnetic interference shielding film of the present invention.

[0023] Figure 5 It is a flow chart of the method steps of Example 5 of the method for preparing a magnetic interference shielding film of the present invention. DETAILED DESCRIPTION

[0024] The present invention provides a magnetic interference shielding film, comprising the following mass fractions:

[0025] 70 wt% to 85 wt% of absorbent, 10 wt% to 15 wt% of polyester, 1 wt% to 3 wt% of antioxidant, 1 wt% to 2 wt% of dispersant and 1 wt% to 2 wt% of processing lubricant.

[0026] Furthermore, the absorbent is any one or more combinations of FeNi, FeCr and FeSiCr.

[0027] Furthermore, the polyester is PA12 powder.

[0028] Furthermore, the antioxidant is prepared by mixing a high molecular weight hindered phenol 1010 and a phosphite auxiliary antioxidant 168.

[0029] Furthermore, the processing lubricant is calcium stearate.

[0030] Furthermore, the thickness of the magnetic interference shielding film is 0.5 to 1.5 mm.

[0031] The present invention also provides a method for preparing a magnetic interference shielding film, and the method for preparing the magnetic interference shielding film as described above comprises the following steps:

[0032] S1: Add the raw materials of each component into the high-speed mixer according to the proportion;

[0033] S2: high-speed mixer at 1000 RPM and 80°C for 30 min;

[0034] S3: pouring the evenly mixed powder into an extrusion casting machine;

[0035] S4: Controlling the thickness of the cast film to be between 0.7 and 1.0 mm. At this point, the magnetic interference shielding film is completed.

[0036] See also Figure 1 , Embodiment 1, the present invention also provides a method for preparing a magnetic interference shielding film, comprising the following steps:

[0037] S1: 15wt% PA12 powder, 1wt% dispersant, 70wt% FeNi, 10wt% FeSiCr, 2wt% high molecular hindered phenol 1010, 1wt% phosphite auxiliary antioxidant 168 and 1wt% calcium stearate were weighed and added into a high-speed mixer;

[0038] S2: high-speed mixer at 500 RPM and 80 °C for 30 min;

[0039] S3: pouring the evenly mixed powder into an extrusion casting machine;

[0040] S4: Extrusion to obtain a magnetic interference shielding film with a thickness of 0.7 mm.

[0041] In this embodiment, the prepared magnetic interference shielding film is cut into annular sheets with an outer diameter of 7 mm and an inner diameter of 3 mm. The magnetic permeability is 123 at 13.56 MHz tested using an EA4991 impedance meter.

[0042] See also Figure 2 , Embodiment 2, the present invention also provides a method for preparing a magnetic interference shielding film, comprising the following steps:

[0043] S1: 15wt% PA12 powder, 1wt% dispersant, 70wt% FeNi, 10wt% FeCr, 2wt% high molecular hindered phenol 1010, 1wt% phosphite auxiliary antioxidant 168 and 1wt% calcium stearate were weighed and added into a high-speed mixer;

[0044] S2: high-speed mixer at 500 RPM and 80 °C for 30 min;

[0045] S3: pouring the evenly mixed powder into an extrusion casting machine;

[0046] S4: Extrusion to obtain a magnetic interference shielding film with a thickness of 0.7 mm.

[0047] In this embodiment, the prepared magnetic interference shielding film is cut into annular sheets with an outer diameter of 7 mm and an inner diameter of 3 mm. The magnetic permeability is 148 at 13.56 MHz tested using an EA4991 impedance meter.

[0048] See also Figure 3 , Embodiment 3, the present invention also provides a method for preparing a magnetic interference shielding film, comprising the following steps:

[0049] S1: 15wt% PA12 powder, 1wt% dispersant, 70wt% FeNi, 5wt% FeCr, 5wt% FeSiCr, 2wt% high molecular hindered phenol 1010, 1wt% phosphite auxiliary antioxidant 168 and 1wt% calcium stearate were weighed and added into a high-speed mixer;

[0050] S2: high-speed mixer at 500 RPM and 80 °C for 30 min;

[0051] S3: pouring the evenly mixed powder into an extrusion casting machine;

[0052] S4: Extrusion to obtain a magnetic interference shielding film with a thickness of 0.7 mm.

[0053] In this embodiment, the prepared magnetic interference shielding film is cut into annular sheets with an outer diameter of 7 mm and an inner diameter of 3 mm. The magnetic permeability is 153 at 13.56 MHz tested using an EA4991 impedance meter.

[0054] See also Figure 4 , Embodiment 4, the present invention also provides a method for preparing a magnetic interference shielding film, comprising the following steps:

[0055] S1: 12wt% PA12 powder, 1wt% dispersant, 73wt% FeNi, 5wt% FeCr, 5wt% FeSiCr, 2wt% high molecular hindered phenol 1010, 1wt% phosphite auxiliary antioxidant 168 and 1wt% calcium stearate were weighed and added into a high-speed mixer;

[0056] S2: high-speed mixer at 500 RPM and 80 °C for 30 min;

[0057] S3: pouring the evenly mixed powder into an extrusion casting machine;

[0058] S4: Extrusion to obtain a magnetic interference shielding film with a thickness of 0.7 mm.

[0059] In this embodiment, the prepared magnetic interference shielding film is cut into annular sheets with an outer diameter of 7 mm and an inner diameter of 3 mm. The magnetic permeability is 169 at 13.56 MHz tested using an EA4991 impedance meter.

[0060] See also Figure 5 , Embodiment 5, the present invention also provides a method for preparing a magnetic interference shielding film, comprising the following steps:

[0061] S1: 10wt% PA12 powder, 1wt% dispersant, 75wt% FeNi, 5wt% FeCr, 5wt% FeSiCr, 2wt% high molecular hindered phenol 1010, 1wt% phosphite auxiliary antioxidant 168 and 1wt% calcium stearate were weighed and added into a high-speed mixer;

[0062] S2: high-speed mixer at 500 RPM and 80 °C for 30 min;

[0063] S3: pouring the evenly mixed powder into an extrusion casting machine;

[0064] S4: Extrusion to obtain a magnetic interference shielding film with a thickness of 0.7 mm.

[0065] In this embodiment, the prepared magnetic interference shielding film is cut into annular sheets with an outer diameter of 7 mm and an inner diameter of 3 mm. The magnetic permeability is 178 at 13.56 MHz tested using an EA4991 impedance meter.

[0066] What is disclosed above is only a preferred embodiment of the present invention, and it certainly cannot be used to limit the scope of rights of the present invention. Ordinary technicians in this field can understand that all or part of the processes of the above embodiment and equivalent changes made according to the claims of the present invention still fall within the scope of the invention.

Claims

1. A magnetic interference shielding film, It is characterized in that The following quality scores are included: 70 wt% to 85 wt% of absorbent, 10 wt% to 15 wt% of polyester, 1 wt% to 3 wt% of antioxidant, 1 wt% to 2 wt% of dispersant and 1 wt% to 2 wt% of processing lubricant.

2. A magnetic interference shielding film as claimed in claim 1, It is characterized in that The absorbent is any one or more combinations of FeNi, FeCr and FeSiCr.

3. A magnetic interference shielding film as claimed in claim 1, It is characterized in that The polyester is PA12 powder.

4. A magnetic interference shielding film as claimed in claim 1, It is characterized in that The antioxidant is prepared by mixing high molecular hindered phenol 1010 and phosphite auxiliary antioxidant 168.

5. A magnetic interference shielding film as claimed in claim 1, It is characterized in that The processing lubricant is calcium stearate.

6. A magnetic interference shielding film as claimed in claim 1, It is characterized in that The thickness of the magnetic interference shielding film is 0.5-1.5 mm.

7. A method for preparing a magnetic interference shielding film, comprising preparing the magnetic interference shielding film as claimed in claim 1, It is characterized in that The steps include: Add the raw materials of each component into the high-speed mixer according to the proportion; The high-speed mixer was stirred at a speed of 1000 RPM and a temperature of 80°C for 30 min; Pour the evenly mixed powder into the extrusion casting machine; The thickness of the cast film is controlled to be between 0.7 and 1.0 mm, and the preparation of the magnetic interference shielding film is now completed.