Soft anticorrosive material

Through soft wax-based anticorrosion materials, the existing temporary protective materials have been solved, and the corrosion performance and insufficient self-healing ability of existing temporary protective materials in heavy salt spray environments are achieved, self-repair and durability improvement in marine environments are achieved, and the cleaning process is simplified. .

CN118931390APending Publication Date: 2024-11-12SUZHOU HIMAX AUTOMOBILE PROTECTION MATERIAL
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202411201618.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-29
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The existing temporary protective materials have poor corrosion performance in heavy salt spray environments, difficult to cover irregularly shaped parts, are flammable and explosive during construction, and are difficult to remove, and lack self-healing ability, which affects the safety and efficiency of cargo transportation.

Method used

Use soft wax-based anticorrosion materials, containing microcrystalline wax, refined paraffin, Fischer-Tropsch wax, anti-rust agent, emulsifier and ultraviolet absorber, to form a self-repairable soft wax layer, adapt to the marine environment, overcome the hard wax shell Risk of damaged peeling.

Benefits of technology

It achieves long-term anti-corrosion performance and self-repair capability in heavy salt spray environments, avoids the risk of hard wax peeling, improves durability and environmental adaptability, and simplifies the cleaning process.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118931390A_ABST
    Figure CN118931390A_ABST
Patent Text Reader

Abstract

The invention discloses a soft anticorrosive material which comprises the following raw materials in percentage by weight: 10-20% of wax, 5-10% of an antirust agent, 4-10.5% of a resin emulsion, 1-20% of an emulsifier, 1-5% of an ultraviolet light absorber and the balance of deionized water, and the wax is selected from microcrystalline wax, refined paraffin and Fischer-Tropsch wax. The soft anti-corrosion material provided by the invention is a soft wax-based anti-corrosion material, has good stability and environmental tolerance, is integrally soft in a daily state, can better adapt to a sea transportation environment, and is beneficial to maintaining the overall sealing property for a long time, so that the soft anti-corrosion material fully adapts to severe environments such as high salinity and high humidity under a sea transportation condition.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of protective coatings, and in particular relates to a soft anti-corrosion material. Background Art

[0002] Common ocean-going cargoes include containers, complete vehicles, and large metal parts. They often take several months to transport and are always in a heavy salt spray environment. This heavy salt spray environment has a great corrosive impact on the damaged corners of the container, the exposed parts of the vehicle, and the paint surface of the vehicle body. In addition, the exposed paint surface is also subject to corrosion such as aging by ultraviolet rays. Therefore, temporary anti-corrosion materials are usually sprayed on the cargo before transportation.

[0003] The currently used temporary protective materials usually include tearable polyolefin films, solvent-based temporary anti-corrosion materials, and reactive cross-linking varnish-like temporary protective coatings. Tearable polyolefin films are only used on flat areas and cannot cover special-shaped parts, corners, and gaps; solvent-based temporary anti-corrosion materials usually use volatile solvents such as kerosene and other alkanes as solvents, which have low flash points, are flammable and explosive during construction, and have potential quality risks for automobile paint, tire rubber and other parts; the anti-corrosion layer formed after the material is constructed also needs to be cleaned with kerosene and other solvents after reaching the client, and the entire cleaning process is complicated and time-consuming. After the cross-linking is completed, the reactive cross-linking varnish-like temporary protective coating forms a dense varnish-like protective film, but it is troublesome to remove and cannot be completely removed. In addition, the anti-corrosion performance of this type of material is extremely poor, and corrosion usually occurs within 24 hours of the salt spray test under laboratory conditions.

[0004] CN114773973A discloses a temporary protective coating and preparation method for the transportation of marine engineering equipment, which is prepared by adding SK (Ss-04) aliphatic asparagine handmade polyurea as a matrix, multifunctional anti-rust lubricant, zinc phosphate and PU active diluent PEC. The coating forms a tearable film that can be torn off after transportation. However, as mentioned above, although the coating can be sprayed to form a film, it is difficult to remove the film from hidden parts after it is formed. This type of material does not have the ability to self-heal after being scratched or damaged during transportation.

[0005] CN115851055A A water-based strippable coating and its preparation method provides a water-based strippable coating and its preparation method, which contains film-forming resin, thixotropic agent, leveling agent, bactericide, defoamer, deionized water and functional stripping agent; it also has the effect of rust prevention and is suitable for temporary protection of metal surfaces. This patent belongs to the category of water-based coatings, and there are also irregular shapes (such as gaps, cavities, etc.) that are difficult to remove after film formation, and there is no clear description of its anti-rust function (measured by neutral salt spray time).

[0006] CN112724828A discloses a method for preparing a temporary anti-rust liquid for color-coated plates. The anti-rust liquid prepared in this patent has excellent bonding with the topcoat. When applied to the cold-rolled steel plate, the conversion film formed has a certain self-repairing ability. However, the coating needs to be dried, which is not easy to operate on large parts and has high energy consumption.

[0007] Therefore, in view of the above technical problems, it is necessary to provide a soft anti-corrosion material.

[0008] The information disclosed in this background technology section is only intended to enhance the understanding of the overall background of the invention and should not be regarded as an acknowledgment or any form of suggestion that the information constitutes the prior art already known to a person skilled in the art. Summary of the invention

[0009] The purpose of the present invention is to provide a soft anti-corrosion material.

[0010] In order to achieve the above object, a technical solution provided by a specific embodiment of the present invention is as follows:

[0011] The soft anti-corrosion material comprises raw materials in weight percent: 10-20% wax, 5-10% rust inhibitor, 4-10.5% resin emulsion, 1-20% emulsifier, 1-5% ultraviolet absorber, and the balance deionized water, wherein the wax is selected from microcrystalline wax, refined paraffin wax, and Fischer-Tropsch wax.

[0012] In one or more embodiments of the present invention, the microcrystalline wax is selected from: 65#, 70#, 75#, 80# and 90#. Preferably, the composition of the microcrystalline wax includes, by weight: 65# 50-85%; the remainder is the first wax component, and the first wax component is selected from 80# and 90#.

[0013] In one or more embodiments of the present invention, the Fischer-Tropsch wax is selected from Sasolwax5803 and Qihong oxidized Fischer-Tropsch wax F608A.

[0014] In one or more embodiments of the present invention, the refined paraffin is selected from fully refined paraffin 56#, 58#, and 60#.

[0015] In one or more embodiments of the present invention, the rust inhibitor is selected from: sodium petroleum sulfonate, calcium petroleum sulfonate, lithium-based grease, and benzotriazole.

[0016] In one or more embodiments of the present invention, the emulsifier is selected from: anionic emulsifiers and nonionic emulsifiers.

[0017] In one or more embodiments of the present invention, the anionic emulsifier is selected from ammonia soap of fatty acids. Sodium potassium soaps are too water-soluble and have poor anti-emulsification properties, which are not conducive to forming a soft wax layer tightly bonded to the surface, while the amino groups of ammonia soaps can bond with the active groups on the surface of the material after coating, or they can undergo an amino substitution reaction after coating and the emulsifier can further bond with the active groups to form a good bonding state, which is conducive to playing a protective state similar to that of hard wax under soft conditions.

[0018] In one or more embodiments of the present invention, the raw material fatty acid of the fatty acid soap is selected from: myristic acid, stearic acid, lauric acid, rosin acid, coconut acid, oleic acid. The neutralizing agent of the ammonia soap is preferably DMEA.

[0019] In one or more embodiments of the present invention, the anionic emulsifier is selected from a mixture of myristic acid soap and stearic acid soap.

[0020] In one or more embodiments of the present invention, the nonionic emulsifier is selected from polyoxyethylene ether H(OCH2CH2) n OH, wherein n is 4-12.

[0021] In one or more embodiments of the present invention, the UV absorber is selected from the group consisting of butyl methoxybenzophenone methane, salicylates, benzophenones, benzotriazoles, substituted acrylonitriles, and triazines.

[0022] In one or more embodiments of the present invention, the resin emulsion is selected from: Dow HG100 acrylic emulsion, Guangzhou Tongdes 3EA0661Y alkyd emulsion, Shandong Tongxu Chemical XQS-100 styrene-butadiene emulsion, Jiangsu Fuqisen 3330 epoxy ester emulsion.

[0023] Compared with the prior art, the soft anti-corrosion material of the present invention provides a wax-based anti-corrosion material in a soft form, which has good stability and environmental tolerance. It is soft as a whole in daily state and can adapt to the marine environment well. At the same time, this soft form can also be used to self-repair the damaged coating under the effects of gravity, light, self-tension, etc. when it is partially damaged, isolating the erosion in the marine environment. And the soft anti-corrosion structure effectively overcomes the risk of damage and peeling of the hard wax shell, and has better durability. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments recorded in the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0025] Figure 1 This is a photo of the properties of a wax-based anticorrosive material in one embodiment of the present invention;

[0026] Figure 2 This is a photograph of the wax-based anticorrosive material in one embodiment of the present invention after 480 hours of neutral salt spray test. DETAILED DESCRIPTION

[0027] In order to enable those skilled in the art to better understand the technical solutions in the present invention, the technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work should fall within the scope of protection of the present invention.

[0028] Neutral Salt Spray Test (NSS: Neutral Salt Spray Test): GB / T10125-2021 "Artificial atmosphere corrosion test salt spray test".

[0029] Needle penetration test: The depth of a standard cone loaded with 150 grams sinking into a sample wax specimen kept at 25°C within 5 seconds, the unit is 1 / 10 mm.

[0030] Recovery test: Use a 10cm long and 1cm diameter round-headed copper rod to scratch the surface of the test piece with a wax layer at a natural angle of 45 degrees, and then observe the state of the wax layer and the corrosion situation under the neutral salt spray test.

[0031] The preparation method of the anti-corrosion material in the following embodiment is: first, heat the uniform wax to 90-95°C, then add the rust inhibitor, emulsifier and ultraviolet absorber to completely dissolve them and then maintain 90°C for 10 minutes, add deionized water and stir evenly, and when it is cooled to below 80°C, add acrylic emulsion, stir well to emulsify it evenly, and cool it naturally to room temperature.

[0032] Example 1

[0033] The raw materials of the soft anti-corrosion material of this embodiment include, by weight: wax 10%, rust inhibitor sodium petroleum sulfonate 5%, resin emulsion Dow HG100 acrylic emulsion 4%, stearic acid dimethylethanolamine (obtained by reacting stearic acid and dimethylethanolamine DMEA as raw materials in a 1:1 molar ratio) 1%, ultraviolet absorber butyl methoxybenzophenone methane 1%, and deionized water as the balance, wherein the wax is 90# microcrystalline wax.

[0034] After one spraying, the sample of this embodiment forms a soft wax layer of about 5 μm thick on the surface, and the wax layer has a needle penetration of 262; it is resistant to neutral salt spray for 480 hours without corrosion; in the recovery test, the wax layer recovers to be basically flat without significant grooves after 12 hours, and the specimen is not corroded. In the 200-hour UV (band 290-390, 200W, 1m distance irradiation) aging test, the wax layer thickness has no significant change, the surface has no significant blistering or looseness, and has good adhesion to the surface of the specimen.

[0035] Example 2

[0036] The raw materials of the soft anti-corrosion material of this embodiment include, by weight: 15% wax, 8% rust inhibitor sodium petroleum sulfonate, 7.5% Dow HG100 acrylic emulsion resin emulsion, 10% stearic acid dimethylethanolamine (obtained by reacting stearic acid and dimethylethanolamine DMEA as raw materials in a 1:1 molar ratio), 3% ultraviolet absorber butyl methoxybenzophenone methane, and the balance deionized water, wherein the wax is refined paraffin wax 58#.

[0037] After one spraying, the sample of this embodiment forms a soft wax layer of about 5 μm thick on the surface, and the wax layer has a needle penetration of 264; it is resistant to neutral salt spray for 480 hours without corrosion; in the recovery test, the wax layer recovers to be basically flat without significant grooves in 12 hours, and the specimen is not corroded. In the 200-hour UV (band 290-390, 200W, 1m distance irradiation) aging test, the wax layer thickness has no significant change, the surface has no significant blistering or looseness, and has good adhesion to the surface of the specimen.

[0038] Example 3

[0039] The raw materials of the soft anti-corrosion material of this embodiment include, by weight: 20% wax, 10% rust inhibitor sodium petroleum sulfonate, 10.5% Dow HG100 acrylic emulsion resin emulsion, 20% dimethylethanolamine stearate (obtained by reacting stearic acid and dimethylethanolamine DMEA as raw materials in a 1:1 molar ratio), 5% ultraviolet absorber butyl methoxybenzophenone methane, and the balance deionized water, wherein the wax is Fischer-Tropsch wax Sasolwax5803.

[0040] After one spraying, the sample of this embodiment forms a 5μm thick soft wax layer on the surface, and the wax layer has a needle penetration of 263; it is resistant to neutral salt spray for 480 hours without corrosion; in the recovery test, the wax layer recovers to be basically flat without significant grooves in 12 hours, and the specimen is not corroded. In the 200-hour UV (band 290-390, 200W, 1m distance irradiation) aging test, the wax layer thickness has no significant change, the surface has no significant blistering or looseness, and has good adhesion to the surface of the specimen.

[0041] Example 4

[0042] The raw materials of the soft anti-corrosion material of this embodiment include, by weight: 13% wax, 8.13% rust inhibitor lithium grease, 6.25% resin emulsion Jiangsu Fuqisen 3330 epoxy ester emulsion, 12.3% stearic acid dimethylethanolamine (obtained by reacting stearic acid and dimethylethanolamine DMEA as raw materials in a 1:1 molar ratio), 1.75% ultraviolet absorber phenyl salicylate, and the balance deionized water, wherein the wax is a mixture of 50% 65# microcrystalline wax and the balance 80# microcrystalline wax.

[0043] After one spraying, the sample of this embodiment forms a 5μm thick soft wax layer on the surface, and the wax layer has a needle penetration of 273; it is resistant to neutral salt spray for 480 hours without corrosion; in the recovery test, the wax layer recovers to be basically flat without significant grooves in 12 hours, and the specimen is not corroded. In the 200-hour UV (band 290-390, 200W, 1m distance irradiation) aging test, the wax layer thickness has no significant change, the surface has no significant blistering or looseness, and has good adhesion to the surface of the specimen.

[0044] Example 5

[0045] The raw materials of the soft anti-corrosion material of this embodiment include, by weight: 13% wax, 8.13% rust inhibitor lithium grease, 6.25% resin emulsion Jiangsu Fuqisen 3330 epoxy ester emulsion, 12.3% stearic acid dimethylethanolamine (obtained by reacting stearic acid and dimethylethanolamine DMEA as raw materials in a 1:1 molar ratio), 1.75% ultraviolet absorber phenyl salicylate, and the balance deionized water, wherein the wax is 72% 65# microcrystalline wax and the balance is 80# microcrystalline wax.

[0046] After one spraying, the sample of this embodiment forms a 5μm thick soft wax layer on the surface, and the wax layer has a needle penetration of 275; it is resistant to neutral salt spray for 480 hours without corrosion; in the recovery test, the wax layer recovers to be basically flat without significant grooves in 12 hours, and the specimen is not corroded. In the 200-hour UV (band 290-390, 200W, 1m distance irradiation) aging test, the wax layer thickness has no significant change, the surface has no significant blistering or looseness, and has good adhesion to the surface of the specimen.

[0047] Example 6

[0048] The raw materials of the soft anti-corrosion material of this embodiment include, by weight: 13% wax, 8.13% rust inhibitor lithium grease, 6.25% resin emulsion Jiangsu Fuqisen 3330 epoxy ester emulsion, 12.3% stearic acid dimethylethanolamine (obtained by reacting stearic acid and dimethylethanolamine DMEA as raw materials in a 1:1 molar ratio), 1.75% ultraviolet absorber phenyl salicylate, and the balance deionized water, wherein the wax is 85% 65# microcrystalline wax and the balance is 80# microcrystalline wax.

[0049] After one spraying, the sample of this embodiment forms a 5μm thick soft wax layer on the surface, and the wax layer has a needle penetration of 272; it is resistant to neutral salt spray for 480 hours without corrosion; in the recovery test, the wax layer recovers to be basically flat without significant grooves in 12 hours, and the specimen is not corroded. In the 200-hour UV (band 290-390, 200W, 1m distance irradiation) aging test, the wax layer thickness has no significant change, the surface has no significant blistering or looseness, and has good adhesion to the surface of the specimen.

[0050] Example 7

[0051] The raw materials of the soft anti-corrosion material of this embodiment include, by weight: 13% wax, 8.13% rust inhibitor lithium grease, 6.25% resin emulsion Jiangsu Fuqisen 3330 epoxy ester emulsion, 12.3% stearic acid dimethylethanolamine (obtained by reacting stearic acid and dimethylethanolamine DMEA as raw materials in a 1:1 molar ratio), 1.75% ultraviolet absorber phenyl salicylate, and the rest deionized water, wherein the wax is 75% 80# microcrystalline wax and the rest is Qihong oxidized Fischer-Tropsch wax F608A.

[0052] After one spraying, the sample of this embodiment forms a 5μm thick soft wax layer on the surface, and the wax layer has a needle penetration of 274; it is resistant to neutral salt spray for 480 hours without corrosion; in the recovery test, the wax layer recovers to be basically flat without significant grooves in 12 hours, and the specimen is not corroded. In the 200-hour UV (band 290-390, 200W, 1m distance irradiation) aging test, the wax layer thickness has no significant change, the surface has no significant blistering or looseness, and has good adhesion to the surface of the specimen.

[0053] Example 8

[0054] The raw materials of the soft anti-corrosion material of this embodiment include, by weight: 13% wax, 8.13% rust inhibitor lithium grease, 6.25% resin emulsion Jiangsu Fuqisen 3330 epoxy ester emulsion, 12.3% stearic acid dimethylethanolamine (obtained by reacting stearic acid and dimethylethanolamine DMEA as raw materials in a 1:1 molar ratio), 1.75% ultraviolet absorber phenyl salicylate, and the balance deionized water, wherein the wax is 75% 80# microcrystalline wax and the balance is 58# fully refined paraffin wax.

[0055] After one spraying, the sample of this embodiment forms a 5μm thick soft wax layer on the surface, and the wax layer has a needle penetration of 275; it is resistant to neutral salt spray for 480 hours without corrosion; in the recovery test, the wax layer recovers to be basically flat without significant grooves in 12 hours, and the specimen is not corroded. In the 200-hour UV (band 290-390, 200W, 1m distance irradiation) aging test, the wax layer thickness has no significant change, the surface has no significant blistering or looseness, and has good adhesion to the surface of the specimen.

[0056] The surface of the parts has good adhesion.

[0057] Example 9

[0058] The raw materials of the soft anti-corrosion material of this embodiment include, by weight: 13% wax, 8.13% rust inhibitor lithium grease, 6.25% resin emulsion Jiangsu Fuqisen 3330 epoxy ester emulsion, 12.3% dimethylethanolamine rosin acid (obtained by reacting rosin acid and dimethylethanolamine DMEA as raw materials in a 1:1 molar ratio), 1.75% ultraviolet absorber phenyl salicylate, and the balance deionized water, wherein the wax is 75% 80# microcrystalline wax and the balance is 58# fully refined paraffin wax.

[0059] After one spraying, the sample of this embodiment forms a 5μm thick soft wax layer on the surface, the wax layer has a needle penetration of 282, and is resistant to neutral salt spray for 480 hours without corrosion; in the recovery test, the wax layer recovers to be basically flat without significant grooves in 12 hours, and the specimen is not corroded. In the 200-hour UV (band 290-390, 200W, 1m distance irradiation) aging test, the wax layer thickness has no significant change, the surface has no significant blistering or looseness, and has good adhesion to the surface of the specimen.

[0060] Example 10

[0061] The raw materials of the soft anti-corrosion material of this embodiment include, by weight: 13% wax, 8.13% rust inhibitor lithium grease, 6.25% resin emulsion Jiangsu Fuqisen 3330 epoxy ester emulsion, 12.3% polyoxyethylene ether H(OCH2CH2)8OH, 1.75% ultraviolet absorber phenyl salicylate, and the balance deionized water, wherein the wax is 85% 65# microcrystalline wax and the balance is 80# microcrystalline wax.

[0062] After one spraying, the sample of this embodiment forms a 5μm thick soft wax layer on the surface, and the wax layer has a needle penetration of 287; it is resistant to neutral salt spray for 480 hours without corrosion; in the recovery test, the wax layer recovers to be basically flat without significant grooves in 12 hours, and the specimen is not corroded. In the 200-hour UV (band 290-390, 200W, 1m distance irradiation) aging test, the wax layer thickness has no significant change, the surface has no significant blistering or looseness, and has good adhesion to the surface of the specimen.

[0063] Embodiment 11

[0064] The raw materials of the soft anti-corrosion material of this embodiment include, by weight: 13% wax, 8.13% rust inhibitor lithium grease, 6.25% resin emulsion Jiangsu Fuqisen 3330 epoxy ester emulsion, 12.3% polyoxyethylene ether H(OCH2CH2)8OH, 1.75% ultraviolet absorber phenyl salicylate, and the balance deionized water, wherein the wax is 75% 80# microcrystalline wax and the balance is Qihong oxidized Fischer-Tropsch wax F608A.

[0065] After one spraying, the sample of this embodiment forms a 5μm thick soft wax layer on the surface, and the wax layer has a needle penetration of 284; it is resistant to neutral salt spray for 480 hours without corrosion; in the recovery test, the wax layer recovers to be basically flat without significant grooves after 12 hours, and the specimen is not corroded. In the 200-hour UV (band 290-390, 200W, 1m distance irradiation) aging test, the wax layer thickness has no significant change, the surface has no significant blistering or looseness, and has good adhesion to the surface of the specimen.

[0066] Example 12

[0067] The raw materials of the soft anti-corrosion material of this embodiment include, by weight: 13% wax, 8.13% rust inhibitor lithium grease, 6.25% resin emulsion Jiangsu Fuqisen 3330 epoxy ester emulsion, 12.3% polyoxyethylene ether H(OCH2CH2)8OH, 1.75% ultraviolet absorber phenyl salicylate, and the balance deionized water, wherein the wax is 75% 80# microcrystalline wax and the balance is 58# fully refined paraffin wax.

[0068] After one spraying, the sample of this embodiment forms a 5μm thick soft wax layer on the surface, and the wax layer has a needle penetration of 286; it is resistant to neutral salt spray for 480 hours without corrosion; in the recovery test, the wax layer recovers to be basically flat without significant grooves after 12 hours, and the specimen is not corroded. In the 200-hour UV (band 290-390, 200W, 1m distance irradiation) aging test, the wax layer thickness has no significant change, the surface has no significant blistering or looseness, and has good adhesion to the surface of the specimen.

[0069] Embodiment 13

[0070] The raw materials of the soft anti-corrosion material of this embodiment include, by weight: 13% wax, 8.13% rust inhibitor lithium grease, 6.25% resin emulsion Jiangsu Fuqisen 3330 epoxy ester emulsion, 12.3% mixture of dimethylethanolamine myristic acid (obtained by reacting myristic acid and dimethylethanolamine DMEA as raw materials in a 1:1 molar ratio) and dimethylethanolamine stearate (obtained by reacting stearic acid and dimethylethanolamine DMEA as raw materials in a 1:1 molar ratio) in a mass ratio of 1:0.5, 1.75% ultraviolet absorber phenyl salicylate, and the balance deionized water, wherein the wax is 75% 80# microcrystalline wax and the balance is 58# fully refined paraffin wax.

[0071] After one spraying, the sample of this embodiment forms a 5μm thick soft wax layer on the surface, and the wax layer has a needle penetration of 271; it is resistant to neutral salt spray for 480 hours without corrosion; in the recovery test, the wax layer recovers to be basically flat without significant grooves in 12 hours, and the specimen is not corroded. In the 200-hour UV (band 290-390, 200W, 1m distance irradiation) aging test, the wax layer thickness has no significant change, the surface has no significant blistering or looseness, and has good adhesion to the surface of the specimen.

[0072] Embodiment 14

[0073] The raw materials of the soft anti-corrosion material of this embodiment include, by weight: 13% wax, 8.13% rust inhibitor lithium grease, 6.25% resin emulsion Jiangsu Fuqisen 3330 epoxy ester emulsion, 12.3% polyoxyethylene ether H(OCH2CH2)8OH, 1.75% ultraviolet absorber benzotriazole, and the balance deionized water, wherein the wax is 85% 65# microcrystalline wax and the balance is 80# microcrystalline wax.

[0074] After one spraying, the sample of this embodiment forms a 5μm thick soft wax layer on the surface, and the wax layer has a needle penetration of 283; it is resistant to neutral salt spray for 480 hours without corrosion; in the recovery test, the wax layer recovers to be basically flat without significant grooves in 12 hours, and the specimen is not corroded. In the 200-hour UV (band 290-390, 200W, 1m distance irradiation) aging test, the wax layer thickness has no significant change, the surface has no significant blistering or looseness, and has good adhesion to the surface of the specimen.

[0075] Embodiment 15

[0076] The raw materials of the soft anti-corrosion material of this embodiment include, by weight: 13% wax, 8.13% rust inhibitor lithium grease, 6.25% resin emulsion Jiangsu Fuqisen 3330 epoxy ester emulsion, 12.3% polyoxyethylene ether H(OCH2CH2)8OH, 1.75% ultraviolet absorber benzotriazole, and the balance deionized water, wherein the wax is 75% 80# microcrystalline wax and the balance is Qihong oxidized Fischer-Tropsch wax F608A.

[0077] The samples in this example are Figure 1 As shown in the paste form, after one spraying, a 5μm thick soft wax layer is formed on the surface, and the wax layer penetration is 298; it is resistant to neutral salt spray for 480 hours without corrosion. Figure 2 As shown in the figure, in the recovery test, the wax layer recovered to be basically flat without obvious grooves in 12 hours, and the specimen was not corroded. In the 200-hour UV (band 290-390, 200W, 1m distance irradiation) aging test, the wax layer thickness did not change significantly, the surface did not have obvious blistering or looseness, and it had good adhesion to the specimen surface.

[0078] Example 16

[0079] The raw materials of the soft anti-corrosion material of this embodiment include, by weight: 13% wax, 8.13% rust inhibitor lithium grease, 6.25% resin emulsion Jiangsu Fuqisen 3330 epoxy ester emulsion, 12.3% polyoxyethylene ether H(OCH2CH2)8OH, 1.75% ultraviolet absorber benzotriazole, and the balance deionized water, wherein the wax is 75% 80# microcrystalline wax and the balance is 58# fully refined paraffin wax.

[0080] After one spraying, the sample of this embodiment forms a 5μm thick soft wax layer on the surface, and the wax layer has a needle penetration of 285; it is resistant to neutral salt spray for 480 hours without corrosion; in the recovery test, the wax layer recovers to be basically flat without significant grooves in 12 hours, and the specimen is not corroded. In the 200-hour UV (band 290-390, 200W, 1m distance irradiation) aging test, the wax layer thickness has no significant change, the surface has no significant blistering or looseness, and has good adhesion to the surface of the specimen.

[0081] It will be apparent to those skilled in the art that the invention is not limited to the details of the exemplary embodiments described above and that the invention can be implemented in other specific forms without departing from the spirit or essential features of the invention. Therefore, the embodiments should be considered exemplary and non-limiting in all respects, and the scope of the invention is defined by the appended claims rather than the foregoing description, and it is intended that all variations falling within the meaning and scope of the equivalent elements of the claims be included in the invention. Any reference numeral in a claim should not be considered as limiting the claim to which it relates.

[0082] In addition, it should be understood that although the present specification is described according to implementation modes, not every implementation mode contains only one independent technical solution. This description of the specification is only for the sake of clarity. Those skilled in the art should regard the specification as a whole. The technical solutions in each embodiment may also be appropriately combined to form other implementation modes that can be understood by those skilled in the art.

Claims

1. A soft anti-corrosion material, whose raw materials include, by weight: 10-20% wax, 5-10% rust inhibitor, 4-10.5% resin emulsion, 1-20% emulsifier, 1-5% ultraviolet absorber, and the balance deionized water, wherein the wax is selected from microcrystalline wax, refined paraffin wax, and Fischer-Tropsch wax.

2. The soft anti-corrosion material according to claim 1, characterized in that: The microcrystalline wax is selected from: 65#, 70#, 75#, 80# and 90#.

3. The soft anti-corrosion material according to claim 2, characterized in that: The composition of the microcrystalline wax includes, by weight: 65# 50-85%; the remainder is the first wax component, and the first wax component is selected from 80# and 90#.

4. The soft anti-corrosion material according to claim 1, characterized in that: The rust inhibitor is selected from: sodium petroleum sulfonate, calcium petroleum sulfonate, lithium-based grease, and benzotriazole.

5. The soft anti-corrosion material according to claim 1, characterized in that: The emulsifier is selected from: anionic emulsifier and nonionic emulsifier.

6. The soft anti-corrosion material according to claim 5, characterized in that: The anionic emulsifier is selected from ammonia soaps of fatty acids.

7. The soft anti-corrosion material according to claim 6, characterized in that: The raw material fatty acid of the fatty acid soap is selected from the group consisting of myristic acid, stearic acid, lauric acid, rosin acid, coconut acid and oleic acid.

8. The soft anti-corrosion material according to claim 6, characterized in that: The anionic emulsifier is selected from a mixture of myristic acid soap and stearic acid soap.

9. The soft anti-corrosion material according to claim 5, characterized in that: The nonionic emulsifier is selected from polyoxyethylene ether H(OCH2CH2) n OH, wherein n is 4-12.

10. The soft anti-corrosion material according to claim 1, characterized in that: The resin emulsion is selected from: Dow HG100 acrylic emulsion, Guangzhou Tongdes 3EA0661Y alkyd emulsion, Shandong Tongxu Chemical XQS-100 styrene-butadiene emulsion, Jiangsu Fuqisen 3330 epoxy ester emulsion.

Citation Information

Patent Citations

  • Anti-rusting emulsifying wax and preparation method thereof

    CN104789126A

  • Bicontinuous anti-rust emulsion and preparation method thereof

    CN106244309A

  • Water-based anticorrosive wax composition and application thereof

    CN106800784A

  • Corrosion-resistant water-based paint as well as preparation method and application thereof

    CN116875127A

  • Paraffin emulsion waterproof agent

    CN117887355A