Composite phase change material for solar heat storage as well as preparation method and application of composite phase change material
By combining modified expanded graphite with sodium silicate and xanthan gum, the thermal conductivity and light absorption performance of sodium acetate trihydrate is solved, and an efficient solar thermal storage material is achieved, with excellent thermal conductivity and light storage. Heat capability, low cost.
Patent Information
- Application Number
- CN202411007910.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-25
- Publication Date
- 2024-11-12
AI Technical Summary
Sodium acetate trihydrate has low thermal conductivity, supercooling and phase separation in solar heat recovery, and poor light absorption performance, which affects its application effect.
Modified expanded graphite is used as a thermal/light absorption additive, and modified expanded graphite is combined with sodium silicate and xanthan gum through polydopamine and copper nanoparticles to form a composite phase change material, which improves thermal conductivity and light absorption performance, and then passes the The honeycomb mesh structure of modified expanded graphite reduces fluidity during melting.
Composite phase change materials with low supercooling and phase-free separation have increased the thermal conductivity from 0.59 W/(m·K) to 2.984 W/(m·K), maintaining high latent heat, and having excellent photo-storage heat Low cost.
Smart Images

Figure CN118931502A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of phase change materials, and in particular to a composite phase change material for solar heat storage, a preparation method and an application thereof. Background Art
[0002] The information disclosed in the background of the invention is only intended to enhance the understanding of the overall background of the invention and should not be necessarily regarded as an acknowledgment or any form of suggestion that the information constitutes the prior art already known to a person skilled in the art.
[0003] As a clean and renewable energy, solar energy has the important significance of reducing greenhouse gas emissions, reducing dependence on fossil fuels, and promoting energy independence and security. However, solar energy has the disadvantages of intermittent and unstable applications, which limits its scope of use. Latent heat storage has become one of the important ways of solar heat storage due to its advantages such as high energy density and stable heat release.
[0004] Hydrated salt is one of the important components of inorganic phase change materials. Among them, sodium acetate trihydrate has a phase change temperature of 58°C and a latent heat of 271kJ / kg, which is very suitable for the field of solar thermal recovery. It is also one of the representative materials among hydrated salt phase change materials. The disadvantages of sodium acetate trihydrate are also very obvious, such as its low thermal conductivity, the melting process is accompanied by phase separation and supercooling, and its extremely low light absorption performance seriously affects its application in solar thermal recovery.
[0005] Carbon nanotubes and graphene are commonly used light-absorbing materials, but their preparation process is complicated, the cost is high, and the thermal conductivity is poor; metal nanoparticles such as silver nanoparticles have good thermal conductivity, but their light absorption capacity is relatively poorer than that of carbon materials. In the prior art, the two are usually combined to simultaneously improve the thermal conductivity and light absorption performance of phase change materials, but this undoubtedly increases the cost, and the prior art generally adds them to the phase change material in the form of doping, and there will still be certain gaps between the thermal conductive particles at the microscopic or even macroscopic level, which will affect the heat transfer process.
[0006] Therefore, how to provide a method that can solve the problems of high supercooling and phase separation of sodium acetate trihydrate, while achieving simultaneous improvement of the thermal conductivity and light absorption performance of sodium acetate trihydrate at a lower cost, so as to make it suitable for solar thermal storage, is an urgent problem to be solved. Summary of the invention
[0007] In view of this, the present invention provides a composite phase change material for solar heat storage and a preparation method and application thereof, which can simultaneously solve the problems of poor solar light absorption capacity, poor thermal conductivity, high supercooling and phase separation of sodium acetate trihydrate.
[0008] In a first aspect, the present invention provides a composite phase change material for solar thermal storage, comprising, by mass fraction:
[0009] Sodium silicate nonahydrate 1-2wt%;
[0010] Xanthan gum 0.8-1.2wt%;
[0011] Modified expanded graphite 3-5wt%;
[0012] The balance is sodium acetate trihydrate;
[0013] The modified expanded graphite is obtained by sequentially modifying the surface of expanded graphite with polydopamine and copper nanoparticles.
[0014] Preferably, the preparation method of the modified expanded graphite is as follows:
[0015] S1. dispersing expanded graphite and dopamine hydrochloride in a solvent, and in-situ synthesizing polydopamine on the surface of the expanded graphite under alkaline conditions;
[0016] S2. Add the expanded graphite modified with polydopamine to a mixed aqueous solution of copper salt, boric acid and disodium ethylenediaminetetraacetate, heat and stir, then add dimethylamine borane solution dropwise, and after the reaction is completed, filter, wash and dry in sequence to obtain the product.
[0017] Preferably, the mass ratio of the expanded graphite to dopamine hydrochloride is (3-5):1.
[0018] Preferably, the solvent in step S1 is a mixed solvent of water and ethanol, and the volume ratio of water to ethanol is 3:(0.5-2).
[0019] Preferably, in the step of in-situ synthesizing polydopamine on the surface of expanded graphite under alkaline conditions, the pH is 8 to 9.5, the alkaline regulator is tris(hydroxymethyl)aminomethane, the synthesis temperature is 40 to 50° C., and the synthesis time is 20 to 30 hours.
[0020] Preferably, in step S2, in the mixed solution of copper salt, boric acid and disodium ethylenediaminetetraacetate, the dosage ratio of copper salt, boric acid, disodium ethylenediaminetetraacetate and water is (0.003-0.01) mol: (0.03-0.1) mol: (0.003-0.01) mol: (40-60) mL; the mass ratio of the polydopamine-modified expanded graphite and the copper salt is 1: (2-5).
[0021] Preferably, the pH of the mixed solution of the copper salt, boric acid and disodium ethylenediaminetetraacetate is 7.5-8.5, and the copper salt is selected from cupric chloride dihydrate.
[0022] Preferably, in step S2, the heating and stirring process is specifically as follows: first stirring at room temperature for 8 to 15 minutes, then heating to 35 to 45° C., and continuing stirring for 50 to 70 minutes.
[0023] Preferably, the concentration of the dimethylamine borane solution is 70-100 g / L, the volume ratio of the dimethylamine borane solution to the mixed solution of the copper salt, boric acid and disodium ethylenediaminetetraacetate is (10-30):50; the solvent of the dimethylamine borane solution is water and ethanol, and the volume ratio of water to ethanol is 1:(0.5-2); the dripping speed of the dimethylamine borane solution is 50-70 drops / min.
[0024] Preferably, after the dimethylamine borane solution is added dropwise, the reaction is carried out for 15 to 30 minutes.
[0025] In a second aspect, the present invention provides a method for preparing the composite phase change material for solar thermal storage, comprising the following steps:
[0026] Heat and melt sodium acetate trihydrate, add sodium silicate nonahydrate and xanthan gum in proportion, stir for 20 to 40 minutes, and then place at room temperature to solidify;
[0027] The solidified material is ground into powder, then evenly mixed with modified expanded graphite, heated to a molten state, stirred for 50 to 70 minutes, and then vacuumed in the molten state for 3 to 8 minutes to obtain the product.
[0028] In a third aspect, the present invention provides the use of the above-mentioned composite phase change material for solar heat storage or the composite phase change material for solar heat storage prepared by the above-mentioned preparation method in solar heat storage.
[0029] Compared with the prior art, the present invention has achieved the following beneficial effects:
[0030] (1) The composite phase change material for solar heat storage provided by the present invention has a low degree of supercooling and no phase separation phenomenon, and has excellent light heat storage capacity. The thermal conductivity can be increased from 0.59 W / (m·K) to 2.984 W / (m·K), and the latent heat can be maintained up to 233 kJ / kg;
[0031] (2) The present invention uses expanded graphite modified with polydopamine and copper nanoparticles as a thermal conductive / light absorbing additive. Compared with unmodified expanded graphite, it has better light absorption performance and higher thermal conductivity, and the composite phase change material prepared by adding it has a faster phase change response speed under light conditions; compared with graphene, carbon nanotubes, silver nanoparticles, etc., the thermal conductive / light absorbing additive of the present invention has lower cost. BRIEF DESCRIPTION OF THE DRAWINGS
[0032] The drawings constituting part of the present invention are used to provide a further understanding of the present invention. The exemplary embodiments of the present invention and their description are used to explain the present invention and do not constitute an improper limitation of the present invention. Obviously, for those skilled in the art, other drawings can be obtained based on these drawings without creative work.
[0033] Figure 1 It is an infrared test image of EP prepared in Example 1 of the present invention and unmodified expanded graphite (EG);
[0034] Figure 2 It is the XPS test total energy spectrum of EP and unmodified expanded graphite (EG) and EPCu prepared in Example 1 of the present invention;
[0035] Figure 3 It is the C1s decomposition diagram of EP prepared in Example 1 of the present invention (a) and the Cu2P decomposition diagram of EPCu (b);
[0036] Figure 4 is a step cooling curve of the composite phase change material of Example 2 of the present invention;
[0037] Figure 5 is a step cooling curve of the composite phase change material of Example 3 of the present invention;
[0038] Figure 6 is a step cooling curve of the composite phase change material of Example 4 of the present invention;
[0039] Figure 7 1 is a SEM image of the unmodified expanded graphite (EG) of the present invention, the ECu of this comparative example, and the EPCu of Example 1;
[0040] Figure 8 It is the UV-vis test graph of the unmodified expanded graphite (EG) of the present invention, the ECu of this comparative example and the EPCu of Example 1;
[0041] Fig. 9 is a step cooling curve of the composite phase change material of Comparative Example 2 of the present invention;
[0042] Fig.10 It is a light temperature curve diagram of each sample of the composite phase change material of Example 3 (PCM / EPCu) of the present invention and Comparative Example 5 (PCM / ECu) and pure sodium acetate trihydrate (SAT);
[0043] Fig.11 This is a picture of the sample (PCM / EPCu) of Example 3 of the present invention taken with an infrared camera under sunlight. DETAILED DESCRIPTION
[0044] It should be noted that the following detailed descriptions are exemplary and are intended to provide further explanation of the present invention. Unless otherwise specified, all technical and scientific terms used herein have the same meanings as those commonly understood by those skilled in the art to which the present invention belongs.
[0045] The present invention provides a composite phase change material for solar heat storage, which comprises, by mass fraction:
[0046] Sodium silicate nonahydrate 1-2wt%;
[0047] Xanthan gum 0.8-1.2wt%;
[0048] Modified expanded graphite 3-5wt%;
[0049] The balance is sodium acetate trihydrate;
[0050] The modified expanded graphite is obtained by sequentially modifying the surface of expanded graphite with polydopamine and copper nanoparticles.
[0051] The composite phase change material of the present invention uses sodium acetate trihydrate as the main phase change material. The phase change temperature of sodium acetate trihydrate (SAT) is 58°C, the supercooling degree is 25-30°C, the phase change latent heat is 271kJ / kg, and the thermal conductivity is 0.59W / (m·K). In order to improve the supercooling and phase separation phenomenon of sodium acetate trihydrate and improve its light absorption and thermal conductivity, the present invention uses sodium silicate nonahydrate (SMN) as a nucleating agent. The appropriate addition of SMN can improve the supercooling phenomenon of SAT, but excessive addition can reduce the latent heat value of the material. Too little addition can hardly achieve a good supercooling improvement effect. Xanthan gum (XG) is used as a thickener. The appropriate addition of SMN can solve the problem of phase separation. Too little addition cannot completely solve the phase separation phenomenon. Too much addition can cause the agglomeration of the thickener and affect the latent heat. At the same time, xanthan gum also has a certain effect on improving the supercooling problem. Modified expanded graphite is used as an enhanced light absorber, thermal conductive particle and adsorption skeleton. It has a good honeycomb network structure and can provide good attachment sites. Therefore, while improving the SAT thermal conductivity, it can also reduce the fluidity during melting and alleviate the leakage problem of the composite phase change material after melting.
[0052] Expanded graphite itself has a certain absorption capacity for sunlight, but its performance is poor, especially in the near-ultraviolet region, while copper has better absorption in the near-ultraviolet region. However, the binding ability between copper and expanded graphite is poor, so the present invention introduces polydopamine to connect expanded graphite and copper nanoparticles. The polydopamine (PDA) in the modified expanded graphite of the present invention is rich in a large number of O-containing and N-containing groups, which can be connected to the expanded graphite and the copper nanoparticles by covalent bonds in a coordinated manner, and the combination is very strong; at the same time, it also has a structure similar to the melanin constituent molecule, so that it has a wide light band absorption characteristic and a strong light heat storage capacity, and its coupling with copper can further improve the light absorption capacity. Copper nanoparticles and silver nanoparticles are metal elements of the same family, and have excellent thermal conductivity, but the preparation cost of copper nanoparticles is much lower than that of silver nanoparticles; at the same time, copper will produce a plasma resonance effect after illumination, and can also produce a certain illumination effect.
[0053] The composite phase change material finally obtained by using the above formula of the present invention has a supercooling degree of less than 7°C, no phase separation phenomenon, and still has a latent heat of 233 kJ / kg. At the same time, it has excellent light heat storage capacity, and the thermal conductivity can be increased from 0.59 W / (m·K) to 2.984 W / (m·K).
[0054] In the present invention, the preparation method of the modified expanded graphite is as follows:
[0055] S1. dispersing expanded graphite and dopamine hydrochloride in a solvent, and in-situ synthesizing polydopamine on the surface of the expanded graphite under alkaline conditions;
[0056] S2. Add the expanded graphite modified with polydopamine to a mixed aqueous solution of copper salt, boric acid and disodium ethylenediaminetetraacetate, heat and stir, then add dimethylamine borane solution dropwise, and after the reaction is completed, filter, wash and dry in sequence to obtain the product.
[0057] In step S1 of the present invention, the mass ratio of the expanded graphite to dopamine hydrochloride is (3-5):1; the solvent is a mixed solvent of water and ethanol, and the volume ratio of water to ethanol is 3:(0.5-2). The present invention does not impose any special restrictions on the amount of the solvent, as long as the in-situ synthesis of polydopamine can be achieved.
[0058] In the step of in-situ synthesizing polydopamine on the surface of expanded graphite under alkaline conditions of the present invention, the pH is 8-9.5, the alkaline regulator is tris(hydroxymethyl)aminomethane, the synthesis temperature is 40-50° C., and the synthesis time is 20-30 hours. Dopamine can undergo self-polymerization under alkaline conditions, thereby loading polydopamine on the surface of expanded graphite.
[0059] The present invention further comprises filtering and drying steps after the step of synthesizing polydopamine in situ on the surface of expanded graphite under alkaline conditions. The present invention does not impose any special restrictions on the filtering and drying steps, and the filtering and drying methods commonly used in the art can be used.
[0060] In step S2 of the present invention, in the mixed solution of copper salt, boric acid and disodium ethylenediaminetetraacetate, the dosage ratio of copper salt, boric acid, disodium ethylenediaminetetraacetate and water is (0.003-0.01) mol: (0.03-0.1) mol: (0.003-0.01) mol: (40-60) mL; the mass ratio of the polydopamine-modified expanded graphite and copper salt is 1: (2-5). Among them, copper salt provides copper ions, boric acid is used as a buffer to maintain the pH value of the solution, and disodium ethylenediaminetetraacetate (EDTA-2Na) forms a stable chelate with a variety of metal ions; in the process of reducing copper, EDTA-2Na can chelate impurity metal ions in the solution to prevent them from interfering with the reduction reaction, thereby improving the efficiency and effect of the reduction reaction.
[0061] In the present invention, the pH of the mixed solution of the copper salt, boric acid and disodium ethylenediaminetetraacetate is 7.5-8.5, and the copper salt is selected from cupric chloride dihydrate.
[0062] In the present invention, in step S2, the heating and stirring process is specifically to first stir at room temperature for 8 to 15 minutes, then heat to 35 to 45° C., and continue stirring for 50 to 70 minutes.
[0063] In the present invention, the concentration of the dimethylamine borane solution is 70-100 g / L, the volume ratio of the dimethylamine borane solution to the mixed solution of the copper salt, boric acid and disodium ethylenediaminetetraacetate is (10-30):50; the solvent of the dimethylamine borane solution is water and ethanol, and the volume ratio of water to ethanol is 1:(0.5-2); the dripping speed of the dimethylamine borane solution is 50-70 drops / min. Dimethylamine borane can accelerate the reduction of copper ions into copper element, thereby forming copper nanoparticles.
[0064] In the present invention, after the dimethylamine borane solution is added dropwise, the reaction is carried out for 15 to 30 minutes.
[0065] The present invention does not impose any special restrictions on the filtering, washing and drying steps after the reaction is completed, and the filtering, washing and drying methods commonly used in the art can be used.
[0066] The present invention also provides a method for preparing the composite phase change material for solar heat storage, comprising the following steps:
[0067] Heat and melt sodium acetate trihydrate, add sodium silicate nonahydrate and xanthan gum in proportion, stir for 20 to 40 minutes, and then place at room temperature to solidify;
[0068] The solidified material is ground into powder, then evenly mixed with modified expanded graphite, heated to a molten state, stirred for 50 to 70 minutes, and then vacuumed in the molten state for 3 to 8 minutes to obtain the product.
[0069] The stirring after adding the modified expanded graphite is to ensure uniform mixing between the phase change material and the modified expanded graphite. At the same time, because there is an intermolecular force between the modified expanded graphite and the phase change material, the modified expanded graphite can absorb the phase change material into its pores. The subsequent placement in a vacuum environment is to further allow the phase change material to enter the pores of the modified expanded graphite.
[0070] The present invention also provides the use of the composite phase change material for solar heat storage or the composite phase change material for solar heat storage prepared by the above preparation method in solar heat storage. The composite phase change material for solar heat storage described in the present invention has a suitable phase change temperature, a small degree of supercooling and no phase separation phenomenon, a high latent heat, and excellent light heat storage performance, so it is easy to use in solar heat storage.
[0071] The technical solution of the present invention is further described below in conjunction with specific embodiments.
[0072] Example 1
[0073] This embodiment provides a method for preparing modified expanded graphite EPCu.
[0074] (1) A portion of 0.2 g expanded graphite (EG) was placed in a 250 ml beaker, and then dopamine hydrochloride (DOP·HCl) was added at a rate of 0.25 times the mass of EG, followed by 50 ml of anhydrous ethanol and 150 ml of deionized water. After stirring for 20 min, the pH value was adjusted to 8.0 using tris(hydroxymethyl)aminomethane. Finally, the mixture was stirred in a water bath at 45°C for 24 h, and the suspension was filtered and dried to obtain polydopamine-modified expanded graphite, which was recorded as EP.
[0075] (2) 1.73 g of dimethylamine borane (DMAB, 0.029 mol) was dissolved in a mixed solution of 10 ml of deionized water and 10 ml of anhydrous ethanol, and ultrasonicated until DMAB was completely dissolved to obtain a DMAB solution.
[0076] (3) 3.1 g of H3BO3 (50 mmol) and 1.75 g of EDTA-2Na (4.7 mol) were dissolved in 50 ml of deionized water and stirred at room temperature until the solids were almost completely dissolved. Then, 0.8 g of CuCl2·2H2O (4.7 mmol) was added to the mixed solution, and the pH of the solution was adjusted to 8.0 with NaOH. At this time, 0.2 g of EP prepared in step (1) was added to the mixed solution, and stirred at room temperature for 10 min, and then placed in a 40°C environment and stirred for 1 h to ensure that EP and Cu in the solution were completely dissolved. 2 +Full contact.
[0077] (4) The DMAB solution prepared in step (2) is dripped into the mixed solution at 40° C. at a rate of one drop per second, and stirred continuously. When a reddish-brown luster appears on the surface of the black graphite and the blue solution turns into a light yellow solution (about 20 minutes), the suspension is quickly filtered and washed with deionized water and anhydrous ethanol three times each. Finally, the filtered sample is vacuum dried for 24 hours, and then sieved with a 100-mesh screen to filter out free copper nanoparticles, thereby obtaining modified expanded graphite, which is recorded as EPCu.
[0078] Figure 1 The infrared test graphs of the EP prepared in this example and the unmodified expanded graphite (EG) show different absorption peaks, which proves that PDA is successfully generated on the surface of the expanded graphite.
[0079] Figure 2 The XPS total energy spectra of the EP and unmodified expanded graphite (EG) and EPCu prepared in this embodiment are shown in FIG. Figure 3 These are the C1s dehesion diagrams for EP and the Cu2P dehesion diagrams for EPCu. The obvious increase in the N element content in the total energy spectrum of EP and the carbon bonds dehesioned from C1s also prove the formation of PDA, while the Cu2P diagram proves that the valence state of the generated Cu is 0, and it is a single substance.
[0080] Example 2
[0081] This embodiment provides a composite phase change material, including: 1wt% of sodium silicate nonahydrate; 1wt% of xanthan gum; 4wt% of the modified expanded graphite of embodiment 1; and the balance is sodium acetate trihydrate.
[0082] The preparation method is as follows:
[0083] (1) Place sodium acetate trihydrate crystals in a small glass bottle and place in a constant temperature water bath at 75°C for 60 minutes until completely melted.
[0084] (2) Add sodium silicate nonahydrate and xanthan gum to the melted sodium acetate trihydrate solution to obtain a mixed solution.
[0085] (3) The mixed solution was placed in a beaker and a rotor was added to the mixed solution. The beaker was placed in a water bath with a magnetic stirrer for mechanical stirring. The rotor mass was 2 g and the rotation speed was 750 r / min. After stirring for 30 min, the mixture was placed at room temperature to solidify.
[0086] (4) Grind the solidified material into powder, then mix it evenly with modified expanded graphite, heat it to a molten state, stir it for 60 minutes, and then evacuate the molten state for 5 minutes to obtain the product.
[0087] The cooling curve of the composite phase change material of this embodiment is as follows: Figure 4 shown.
[0088] Example 3
[0089] The present embodiment is different from the embodiment 2 in that the content of sodium silicate nonahydrate in the composite phase change material of the present embodiment is 1.5 wt %.
[0090] The cooling curve of the composite phase change material of this embodiment is as follows: Figure 5 shown.
[0091] Example 4
[0092] The difference between this embodiment and embodiment 2 is that the content of sodium silicate nonahydrate in the composite phase change material of this embodiment is 2 wt %.
[0093] The cooling curve of the composite phase change material of this embodiment is as follows: Figure 6 shown.
[0094] Comparative Example 1
[0095] This comparative example provides the preparation of modified expanded graphite ECu.
[0096] (1) Dissolve 1.73 g of dimethylamine borane (DMAB) in a mixed solution of 10 ml of deionized water and 10 ml of anhydrous ethanol, and perform ultrasonic treatment until DMAB is completely dissolved to obtain a DMAB solution.
[0097] (2) 3.1 g of H3BO3 and 1.75 g of EDTA-2Na were dissolved in 50 ml of deionized water and stirred at room temperature until the solids were almost completely dissolved. Then, 0.8 g of CuCl2·2H2O was added to the mixed solution and the pH of the solution was adjusted to 8.0 by using NaOH. At this time, 0.2 g of unmodified expanded graphite (EG) was added to the mixed solution and stirred at room temperature for 10 min. Then, the mixture was placed in a 40°C environment and stirred for 1 h to ensure that EG and Cu in the solution were completely dissolved. 2 +Full contact.
[0098] (3) The DMAB solution prepared in step (1) is dripped into the mixed solution at 40° C. at a rate of one drop per second, and stirred continuously. When a reddish-brown luster appears on the surface of the black graphite and the blue solution turns into a light yellow solution (about 20 minutes), the suspension is quickly filtered and washed with deionized water and anhydrous ethanol three times each. Finally, the filtered sample is vacuum dried for 24 hours, and then sieved with a 100-mesh sieve to filter out free copper nanoparticles, thereby obtaining copper nanoparticle-modified expanded graphite, which is recorded as ECu.
[0099] Figure 7 The SEM images of unmodified expanded graphite (EG), ECu of this comparative example, and EPCu of Example 1 show that there is little copper on the surface of ECu, while there is a lot of copper on the surface of EPCu and it is very dense.
[0100] Figure 8 The UV-vis test graphs of unmodified expanded graphite (EG), ECu of this comparative example, and EPCu of Example 1 show that the addition of PDA can improve the light absorption capacity of EG, while the addition of copper further improves the performance.
[0101] Comparative Example 2
[0102] The difference between this comparative example and Example 2 is that the composite phase change material in this comparative example includes: 0.5wt% sodium silicate nonahydrate, and the balance is sodium acetate trihydrate.
[0103] The cooling curve of the composite phase change material of this comparative example is as follows: Fig. 9 shown.
[0104] Comparative Example 3
[0105] The difference between this comparative example and Example 3 is that the xanthan gum in the composite phase change material of this comparative example is 1.5 wt %.
[0106] Comparative Example 4
[0107] The difference between this comparative example and Example 3 is that the xanthan gum in the composite phase change material of this comparative example is 0.5 wt %.
[0108] Comparative Example 5
[0109] The difference between this comparative example and Example 3 is that the modified expanded graphite used in the composite phase change material of this comparative example is the copper nanoparticle modified expanded graphite (ECu) prepared in Comparative Example 1.
[0110] Comparative Example 6
[0111] The difference between this comparative example and Example 3 is that unmodified expanded graphite is used in the composite phase change material of this comparative example.
[0112] Test example
[0113] 1. Determination of supercooling, phase separation, latent heat and thermal conductivity:
[0114] The supercooling and phase separation measurement results of sodium acetate trihydrate (SAT), Examples 2 to 4, and Comparative Examples 2 to 4 are shown in Table 1.
[0115] Table 1 Supercooling and phase separation test results of SAT, Examples 2 to 4, and Comparative Examples 2 to 4
[0116] Example / Comparative Example Subcooling(℃) Phase separation Example 2 6.69 No phase separation Example 3 5.86 No phase separation Example 4 5.8 No phase separation Comparative Example 2 No nucleation Obvious phase separation Comparative Example 3 - Agglomeration occurs Comparative Example 4 - Phase separation SAT No nucleation Obvious phase separation
[0117] Note: “-” in Table 1 means not determined.
[0118] As can be seen from Table 1, the addition of an appropriate amount of sodium silicate nonahydrate (SMN) can greatly improve the supercooling phenomenon of SAT and reduce the supercooling degree, but excessive addition will lead to a decrease in the latent heat value of the composite phase change material. The heat release is most stable at a ratio of 1.5wt% (Example 3), and the phase change platform lasts for a long time (such as Figure 5 As shown). Adding an appropriate amount of xanthan gum (XG) can effectively disperse SAT evenly, thereby completely solving the phase separation phenomenon; excessive addition will reduce the latent heat value of the material and cause XG to agglomerate (Comparative Example 3); if the addition amount is insufficient, the effect of completely solving the phase separation cannot be achieved (Comparative Example 4).
[0119] The latent heat and thermal conductivity of sodium acetate trihydrate (SAT), Example 3, and Comparative Examples 5 to 6 are shown in Table 2.
[0120] Table 2 Latent heat and thermal conductivity test results of Example 3, Comparative Examples 5-6 and SAT
[0121] Example / Comparative Example Latent heat (kJ / kg) Thermal conductivity (W / (m·K)) Example 3 233 2.984 Comparative Example 5 241 2.472 Comparative Example 6 - 1.432 SAT 271 0.590
[0122] Note: “-” in Table 2 means not determined.
[0123] From the comparison between Example 3 and Comparative Examples 5 and 6 in Table 2, it can be seen that the expanded graphite modified by PDA and copper nanoparticles can greatly improve the thermal conductivity of the composite phase change material. Since the copper ion loading of ECu used in Comparative Example 5 is low, its thermal conductivity is not much improved compared with the unmodified EG.
[0124] 2. Photothermal storage test
[0125] 1.2 g of the composite phase change materials of Example 3 (PCM / EPCu) and Comparative Example 5 (PCM / ECu) and pure sodium acetate trihydrate (SAT) were weighed respectively, and then pressed into tablets at a pressure of 7 MPa. The pressed tablets were then placed in an incubator and heated at 120 mW / cm 2The simulated sunlight was used to conduct the light heat storage experiment, and the temperature changes were recorded using a data logger. Fig.10 The light temperature curve of each sample shows that pure SAT is difficult to undergo phase change under light, while the samples with modified expanded graphite can undergo phase change, among which ECu takes a longer time and EPCu takes a slightly shorter time, indicating that EPCu has good solar heat storage capacity.
[0126] Fig.11 This is a picture taken by an infrared camera of the sample of Example 3 (PCM / EPCu) under sunlight. It can be seen that it still has good solar heat storage capacity under the irradiation of actual sunlight.
[0127] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A composite phase change material for solar heat storage, characterized in that: By quality score, including: Sodium silicate nonahydrate 1-2wt%; Xanthan gum 0.8-1.2wt%; Modified expanded graphite 3-5wt%; The balance is sodium acetate trihydrate; The modified expanded graphite is obtained by sequentially modifying the surface of expanded graphite with polydopamine and copper nanoparticles.
2. The composite phase change material according to claim 1, characterized in that: The preparation method of the modified expanded graphite is as follows: S1. dispersing expanded graphite and dopamine hydrochloride in a solvent, and in-situ synthesizing polydopamine on the surface of the expanded graphite under alkaline conditions; S2. Add the expanded graphite modified with polydopamine to a mixed aqueous solution of copper salt, boric acid and disodium ethylenediaminetetraacetate, heat and stir, then add dimethylamine borane solution dropwise, and after the reaction is completed, filter, wash and dry in sequence to obtain the product.
3. The composite phase change material according to claim 2, characterized in that: The mass ratio of the expanded graphite to dopamine hydrochloride is (3-5):1; the solvent in step S1 is a mixed solvent of water and ethanol, and the volume ratio of water to ethanol is 3:(0.5-2).
4. The composite phase change material according to claim 2, characterized in that: In the step of in-situ synthesizing polydopamine on the surface of expanded graphite under alkaline conditions, the pH is 8-9.5, the alkaline regulator is tris(hydroxymethyl)aminomethane, the synthesis temperature is 40-50° C., and the synthesis time is 20-30 hours.
5. The composite phase change material according to claim 2, characterized in that: In step S2, in the mixed solution of copper salt, boric acid and disodium ethylenediaminetetraacetate, the dosage ratio of copper salt, boric acid, disodium ethylenediaminetetraacetate and water is (0.003-0.01) mol: (0.03-0.1) mol: (0.003-0.01) mol: (40-60) mL; the mass ratio of the polydopamine-modified expanded graphite and the copper salt is 1: (2-5).
6. The composite phase change material according to claim 2, characterized in that: The pH of the mixed solution of the copper salt, boric acid and disodium ethylenediaminetetraacetate is 7.5-8.5, and the copper salt is selected from copper chloride dihydrate.
7. The composite phase change material according to claim 2, characterized in that: In step S2, the heating and stirring process is specifically as follows: first stirring at room temperature for 8 to 15 minutes, then heating to 35 to 45°C, and continuing stirring for 50 to 70 minutes.
8. The composite phase change material according to claim 2, characterized in that: The concentration of the dimethylamine borane solution is 70-100 g / L, and the volume ratio of the dimethylamine borane solution to the mixed solution of the copper salt, boric acid and disodium ethylenediaminetetraacetate is (10-30):50; the solvent of the dimethylamine borane solution is water and ethanol, and the volume ratio of water to ethanol is 1:(0.5-2); the dropping speed of the dimethylamine borane solution is 50-70 drops / min; after the dimethylamine borane solution is added dropwise, the reaction is carried out for 15-30 minutes.
9. The method for preparing a composite phase change material for solar thermal storage according to any one of claims 1 to 8, characterized in that: Heat and melt sodium acetate trihydrate, add sodium silicate nonahydrate and xanthan gum in proportion, stir for 20 to 40 minutes, and then place at room temperature to solidify; The solidified material is ground into powder, then evenly mixed with modified expanded graphite, heated to a molten state, stirred for 50 to 70 minutes, and then vacuumed in the molten state for 3 to 8 minutes to obtain the product.
10. Use of the composite phase change material for solar thermal storage according to any one of claims 1 to 8 or the composite phase change material for solar thermal storage prepared by the preparation method according to claim 9 in solar thermal storage.
Citation Information
Cited By
Spherical sodium acetate trihydrate composite phase change material and microfluidics preparation method thereof