Heat treatment method of foreign high-strength steel rail
Patent Information
- Application Number
- CN202410943925.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-15
- Publication Date
- 2024-11-12
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
[0014] After heat treatment, the finished rails were subjected to detailed testing of conventional tensile properties, tread hardness and other indicators in accordance with the AREMA-2020 standard strength carbon rail requirements. The testing results showed that all conventional and special properties met the standard requirements.
Smart Images

Figure CN118932158A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of metallurgical materials, and in particular relates to a heat treatment method for high-strength steel rails used abroad. Background Art
[0002] America is a region with developed heavy-haul railways and is at the forefront of the world in terms of heavy-haul transportation technology. It has a complete and developed railway network, and large-scale lines were completed around 2000. By 2009, the total operating mileage of heavy-haul railways in North America reached 224,000 kilometers. Australia is a country with relatively developed railway transportation, with a railway operating line of 43,000 km. The railway system has a high status in the national economy, with a freight turnover of 150 billion t·km. Railways account for more than 35% of the total domestic transportation volume. 80% of Australia's iron ore, 70% of coal and 20% of grain are exported by rail. The heavy-haul train operated by BHP Billiton Iron Ore Company of Australia on the Newman Mountain-Port Hedland railway line set the world record for the longest and heaviest train. In addition, in terms of market demand, many heavy-haul railways will be built in the future, and the demand for American standard high-strength rails will expand. By developing rail head tread hardness above 370HB and R p0.2 ≥120.0ks i(820MPa), R m High-strength rails with a strength of ≥171.0ksi (1180MPa) and an elongation of not less than 10% can enhance the market competitiveness of Baosteel products, fill the gap in rail varieties, increase economic benefits, and meet the demand for rail exports to America. Summary of the invention
[0003] The purpose of the present invention is to provide a heat treatment method for high-strength rails for foreign use, and all conventional and special properties meet standard requirements.
[0004] In order to solve the above technical problems, the present invention adopts the following technical solutions:
[0005] The invention discloses a heat treatment method for a high-strength steel rail for use abroad, comprising: inlet temperature: 730±5°C; outlet temperature 485±5°C; track speed 1.1-1.3m / s; 1-5# wind pressure 7KPa-8KPa, 6-7# wind pressure 9KPa-10KPa, 8-14# wind pressure 10KPa-11 KPa.
[0006] Furthermore, the chemical composition of the high-strength rail includes, by mass percentage, C: 0.75-0.85; Si: 0.45-0.6; Mn: 1.0-1.2; P≤0.020; S≤0.020; Cr: 0.2-0.3%, and the rest is Fe and unavoidable impurities.
[0007] Furthermore, inlet temperature: 730°C; outlet temperature 485°C.
[0008] Furthermore, the track speed is 1.2 m / s.
[0009] Furthermore, the production method of the high-strength rail includes: smelting, heating, rolling, and heat treatment; wherein:
[0010] The heating temperature is 1200℃; the furnace temperature is not less than 1100℃; the rolling temperature is 1100℃-1150℃, and the final rolling temperature is less than 940℃.
[0011] Furthermore, the specific cooling temperature of the rail heat treatment is shown in the following table:
[0012]
[0013] Compared with the prior art, the beneficial technical effects of the present invention are:
[0014] After heat treatment, the finished rails were subjected to detailed testing of various indicators such as conventional tensile properties and tread hardness in accordance with the requirements of AREMA-2020 standard strength carbon rails. The test results showed that all conventional and special properties met the standard requirements. BRIEF DESCRIPTION OF THE DRAWINGS
[0015] The present invention will be further described below in conjunction with the accompanying drawings.
[0016] Figure 1 Organize photos for Example 1;
[0017] Figure 2 Organize photos for Example 2;
[0018] Figure 3 This is a photo of the interlamellar spacing of Example 1;
[0019] Figure 4 This is a photo of the interlamellar spacing of Example 2. DETAILED DESCRIPTION
[0020] The present invention will be further described below in conjunction with the embodiments.
[0021] A method for producing high-strength rails for foreign use, comprising:
[0022] 1) Hot metal pretreatment: Hot metal must be pretreated with desulfurization, with requirements of [P] ≤ 0.12%, [S] ≤ 0.0.030%, and other raw materials must meet the corresponding standard requirements.
[0023] 2) Converter smelting: endpoint control C ≥ 0.06%, steel tapping temperature T (℃) > 1610, silicon manganese, ferromanganese and ferrosilicon alloys are used for in-tank deoxidation and alloying, and heavy rail carburizer is used for converter carburization.
[0024] 3) LF furnace refining: After the refined slag is added, there must be enough heating time to ensure that the slag is completely melted and foam slag is formed as soon as possible to achieve submerged arc operation and achieve the goal of white slag operation. Slag basicity control ≥2.0
[0025] 4) VD vacuum degassing: deep vacuum time ≥ 15min, vacuum degree less than 0.1KPa, soft blowing time after vacuum treatment is greater than or equal to 15min, and the molten steel must not be exposed during soft blowing.
[0026] 5) Continuous casting: The casting process is to achieve automatic liquid level control, and electromagnetic stirring is used normally. Liquidus temperature of steel grade: 1451 (℃) The superheat of continuous casting molten steel is between 15℃-25℃, and the fluctuation range is small, not more than 30℃, and constant casting speed is adopted. Specific composition is shown in Table 2
[0027] Table 1. Composition content of continuous casting products
[0028] C / % Si / % Mn / % P / % S / % Cr / % Example 1 0.8100 0.5200 1.1500 0.0190 0.0030 0.17 Example 2 0.8300 0.5200 1.1500 0.0190 0.0040 0.28
[0029] 6) Billet heating: The total heating time is more than 50 minutes, and the heating temperature of each section is shown in Table 2.
[0030] Table 2 American Standard Carbon Rail Heating Process
[0031] Preheating section Heating 1 stage Heating 2 stages Heat soaking section temperature ≤800℃ 1150-1280℃ ≤1200℃ 1150-1260℃
[0032] 7) Rolling temperature: The ingot is rolled into rails by a universal rolling mill. The starting rolling temperature is 1060-1135°C. The final rolling temperature is based on the second rolling temperature. The target final rolling temperature of the rail is less than 930°C.
[0033] The heat treatment process is further described below in conjunction with specific embodiments;
[0034] After rolling, the rails are heat treated. The specific heat treatment process is shown in the following table:
[0035] Table 3 Heat treatment process of HH rail
[0036]
[0037] Table 4 Cooling temperature of heat treatment of HH rail
[0038]
[0039]
[0040] After heat treatment, the finished rails from the two furnaces were tested in detail for various indicators such as conventional tensile properties and tread hardness according to the requirements of AREMA-2020 standard strength carbon rails. The test results show that all conventional and special properties meet the standard requirements. The specific test results are shown in Tables 5 and 6.
[0041] Table 5 Test results of rail tensile properties
[0042]
[0043] Table 6 Hardness and elongation test results of rails
[0044]
[0045] Comparing the test results of Example 1 and Example 2, the rail performance results, structure, and interlamellar spacing of Example 2 are more ideal and meet the standard requirements.
[0046] The embodiments described above are only descriptions of the preferred modes of the present invention, and are not intended to limit the scope of the present invention. Without departing from the design spirit of the present invention, various modifications and improvements made to the technical solutions of the present invention by ordinary technicians in this field should all fall within the protection scope determined by the claims of the present invention.
Claims
1. A heat treatment method for high-strength rails used abroad, characterized in that: Including: inlet temperature: 730±5℃; outlet temperature 485±5℃; track speed 1.1-1.3m / s; 1-5# wind pressure 7KPa-8KPa, 6-7# wind pressure 9KPa-10KPa, 8-14# wind pressure 10KPa-11 KPa.
2. The heat treatment method for high-strength rails for overseas use according to claim 1, characterized in that: The chemical composition of the high-strength rail includes, by mass percentage, C: 0.75-0.85; Si: 0.45-0.6; Mn: 1.0-1.2; P≤0.020; S≤0.020; Cr: 0.2-0.3%, and the rest is Fe and unavoidable impurities.
3. The heat treatment method for high-strength rails for overseas use according to claim 2, characterized in that: Inlet temperature: 730℃; outlet temperature 485℃.
4. The heat treatment method for high-strength rails for overseas use according to claim 2, characterized in that: Track speed 1.2m / s.
5. The heat treatment method for high-strength rails for overseas use according to claim 1, characterized in that: The production method of the high-strength rail includes: smelting, heating, rolling, and heat treatment; wherein: The heating temperature is 1200℃; the furnace temperature is not less than 1100℃; the rolling temperature is 1100℃-1150℃, and the final rolling temperature is less than 940℃.
6. The heat treatment method for high-strength rails for overseas use according to claim 3, characterized in that: The specific cooling temperature of rail heat treatment is shown in the following table:
Citation Information
Patent Citations
Production method of heavy haul railway large-radius curve heat treatment steel rail
CN115971239A
Rolling method of American-standard medium-strength steel rail
CN116371908A
Production method for eliminating abnormal structure of decarburized layer of pearlite steel rail
CN117683985A
Continuous hardening heat treatment method for head of rail with special section, and heat treatment apparatus
JP2006336043A
Cited By
Rolling method of export high-hardness steel rail
CN120362244A