Ornament surface processing method and structure

By controlling the parameters of ion bombardment, sputtering deposition and arc deposition steps, using stainless steel metal substrates and colored nitride ions to form a surface with high hardness, low roughness and color close to 18K gold, solving the color difference in vacuum coating technology and The problem of uneven deposits has achieved a cost-effective and efficient 18K gold imitation effect.

CN118932279APending Publication Date: 2024-11-12INPARK INT LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410095290.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2023-05-12
Filing Date
2024-01-23
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The existing vacuum coating technology cannot truly achieve 18K gold color without precious metals, and the deposition rate is low and the thickness is uneven when sputtering coating is plating, and the surface roughness is high and the deposition time is long when plating.

Method used

By controlling the parameters of the ion bombardment, sputtering deposition and arc deposition steps, using stainless steel metal substrates for ion bombardment, implanting color nitride ions and forming non-precious metal ions, adjusting color and hardness to achieve the LAB value color closest to 18K gold Parameters and low roughness.

Benefits of technology

It is achieved without using precious metals to form a surface with high hardness, low roughness and color close to 18K gold, solving the problems of color differences, low deposition rate and high surface roughness in vacuum coating technology.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118932279A_ABST
    Figure CN118932279A_ABST
Patent Text Reader

Abstract

The invention discloses an ornament surface processing method and structure, which mainly comprises the following steps of: sequentially performing an ion bombardment step, a sputtering deposition step and an electric arc deposition step on the surface of a stainless steel metal substrate, and strictly controlling various parameters in the steps, in the sputtering deposition step, colored nitride ions are arranged on the surface of the stainless steel metal substrate and the concave parts of the substrate so as to fade the color of the substrate and increase the hardness of the substrate to 1800HV-2000HV, so that the surface roughness of the stainless steel metal substrate is reduced. The first non-ferrous metal ion and the second non-ferrous metal ion are sequentially arranged on the surface of the colored nitride ion through arc deposition, so that the final roughness is reduced to 0.01-0.1 mu m, and the color parameter of the final LAB value forms a state closest to 18K gold, so that a luxurious metal style is generated under the condition that precious metal is not used.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a method and structure for processing the surface of an ornament with high hardness, low roughness and a color closest to 18K gold by controlling various step parameters. Background Art

[0002] Consumers' purchasing desire is usually enhanced by trendy designs, and the practice of satisfying consumers' aesthetic needs through color design is more common in the labels of branded accessories.

[0003] The three-color gold of precious metals is often used in jewelry itself or as inlay metal for jewelry. If distinguished by color, it can be simply divided into silver "white gold", gold "yellow gold", and pink gold "rose gold". The main component of the three is gold, and the difference in color mainly comes from the alloy ratio with other metals. Pure gold is 24K gold, and 75% gold plus 25% other metal alloys are called 18K gold. For example, "18K white gold" is mostly made of 75% gold and 25% palladium; "rose gold" is made of 75% gold and 25% copper. However, the reason why it is called precious metals is that this type of metal is very expensive.

[0004] It is known in the market that vacuum coating technology is used to coat a layer of gold on the surface of general metals. This gold color is said to have the color of gold, but no precious metals are used. Therefore, it can reduce costs while still having a golden surface. However, the performance of this type of gold plating in terms of brightness, surface roughness and hardness is unsatisfactory.

[0005] The above vacuum coating technology has the following problems and deficiencies that need to be improved when used:

[0006] First, the color is said to be the color of gold, but once compared with gold, the difference can still be seen with the naked eye, and it is impossible to truly achieve 18K gold that does not contain precious metals.

[0007] Second, when sputtering is used for gold plating, the deposition rate is generally low because the bombardment target area of ​​ion beam sputtering is too small, and ion beam sputtering deposition is not suitable for depositing large-area thin films with uniform thickness. Therefore, the thickness or hardness of metal films deposited by sputtering is relatively low.

[0008] Third, when using arc plating for gold plating, if the surface of the original material is not smooth enough, the particles attached during the deposition process will be uneven, which can easily cause the surface to be rough. In addition, although this step can achieve color control, if the color of the substrate is too dark, it will lead to a longer deposition time and a larger amount of target material.

[0009] Therefore, how to solve the above-mentioned problems and deficiencies in conventional use is the direction that the applicant of the present invention and related manufacturers engaged in this industry are eager to study and improve. Summary of the invention

[0010] Therefore, in view of the above-mentioned deficiencies, the present invention provides a method and structure for surface processing of jewelry, by controlling various step parameters, a method and structure for surface processing of jewelry with high hardness, low roughness and a color closest to 18K gold is formed on the surface of the jewelry.

[0011] One object of the present invention is to provide a method for surface processing of jewelry, which controls the step parameters of ion bombardment step, sputtering deposition step, and arc deposition step individually, so that the final roughness is reduced to 0.01μm~0.1μm, and the color parameters of the final LAB value are formed to be closest to 18K gold, so as to create a luxurious metal style without using precious metals.

[0012] To achieve the above-mentioned purpose, another object of the present invention is to provide a surface processing structure for jewelry, the main structure of which includes: a stainless steel metal substrate, a plurality of substrate recesses formed on the stainless steel metal substrate, a plurality of colored nitride ions arranged on the surface of the plurality of substrate recesses and the stainless steel metal substrate, a plurality of first colored metal ions arranged on the surface of the colored nitride ions, and a plurality of second colored metal ions arranged on the surface of the first colored metal ions.

[0013] The present invention further provides a method for processing the surface of an ornament, the main steps of which include: during processing, first taking a stainless steel metal substrate, performing ion bombardment on the stainless steel metal substrate to remove oxides on the surface of the stainless steel metal substrate, and exposing a plurality of substrate concave portions, which is conducive to reducing the surface roughness of the subsequent deposition process to 0.01 μm to 0.1 μm, then performing sputter deposition on the stainless steel metal substrate to implant colored nitride ions in the substrate concave portions and the surface of the stainless steel metal substrate to dilute the color of the substrate and increase the hardness of the substrate to 1800 HV to 2000 HV, and finally performing arc deposition on the stainless steel metal substrate. Deposition) is performed to form a first colored metal ion on the surface of the colored nitride ion, and a second colored metal ion is formed on the surface of the first colored metal ion. At this time, a non-precious metal is selected as the target material, and the plasma is used to control the color to be the closest to the LAB value color parameters of 18K gold (L is 72-93, A is 2.5-8, and B is 15-35). The step parameters of ion bombardment include: controlling the ambient pressure to -1 Torr with a pressure value of 0 Torr to -1 Torr, the ambient temperature to 200°C to 300°C, the voltage to 300kv to 400kv, and the energy density to 106W / cm 2 Up to 109W / cm 2 , power density is 105W / cm 2 Up to 1011W / cm 2 , and the holding time is 200 seconds to 400 seconds; the step parameters of sputtering deposition include: controlling the ambient pressure to -2 Torr with a pressure value of 1 Torr to -1 Torr, the ambient temperature is 150°C to 400°C, the voltage is 350kv to 400kv, and the holding time is 550 seconds to 1000 seconds; the step parameters of arc deposition include: controlling the ambient pressure to -3 Torr with a pressure value of 1 Torr to -1 Torr, the ambient temperature is 125°C to 300°C, the voltage is 500kv to 550kv, the current intensity is 400A to 430A, and the current density is 106A / cm 2 Up to 1012A / cm 2 , arc voltage is 10V to 40V, arc movement speed is 90m / s to 110m / s, instantaneous discharge time is 10ns to 1000ns, and maintenance time is 200 seconds to 400 seconds.

[0014] By means of the above technology, it is possible to overcome the problems existing in the commonly used vacuum coating technology, such as the difference between the imitation gold color and the 18K gold color can still be seen with the naked eye, the thickness or hardness of the metal film coated by sputtering is low, the final coating surface roughness is too high, the target material consumption is large, and the deposition time is long, so as to achieve the practical progress of the above advantages. BRIEF DESCRIPTION OF THE DRAWINGS

[0015] Figure 1 Flow chart of the steps of a preferred embodiment of the present invention.

[0016] Figure 2 It is a stereogram of a preferred embodiment of the present invention.

[0017] Figure 3 It is a structural schematic diagram of a preferred embodiment of the present invention.

[0018] Figure 4 FIG. 4 is a schematic diagram of ion bombardment according to a preferred embodiment of the present invention.

[0019] Figure 5 FIG. 4 is a schematic diagram of sputtering deposition according to a preferred embodiment of the present invention.

[0020] Figure 6 Schematic diagram of arc deposition according to a preferred embodiment of the present invention.

[0021] Figure 7 The figure is a flow chart of another preferred embodiment of the present invention.

[0022] Description of the accompanying drawings: stainless steel metal substrate-1; substrate recess-11; colored nitride ions-2; first non-ferrous metal ions-3; second non-ferrous metal ions-4. DETAILED DESCRIPTION

[0023] In order to achieve the above-mentioned purpose and effect, the technical means and structure adopted by the present invention are illustrated in detail with reference to the preferred embodiment of the present invention, and its features and functions are as follows for a complete understanding.

[0024] See also Figures 1 to 3 As shown, it is a step flow chart and a structural schematic diagram of a preferred embodiment of the present invention. It can be clearly seen from the figure that the main steps of the present invention include:

[0025] (A) Selecting the jewelry to be processed: Take a stainless steel metal substrate 1;

[0026] (B) Preparing for ion bombardment: performing ion bombardment on the stainless steel metal substrate 1 to remove oxides on the surface of the stainless steel metal substrate 1 and expose a plurality of substrate recesses 11;

[0027] (C) Parameter setting of the ion bombardment step: the pressure value is 0 Torr to -1 Torr, the ambient pressure of the ion bombardment step is controlled to be -1 Torr, the ambient temperature of the ion bombardment step is controlled to be 200°C to 300°C, and the voltage of the ion bombardment is controlled to be 300 kV to 400 kV, and the energy density is controlled to be 106 W / cm 2 Up to 109W / cm2 , and power density is 105W / cm 2 Up to 1011W / cm 2 , maintain for 200 to 400 seconds;

[0028] (D) Preparing for sputtering deposition: performing sputtering deposition on the stainless steel metal substrate 1 to implant colored nitride ions 2 into a plurality of the substrate recesses 11 and the surface of the stainless steel metal substrate 1;

[0029] (E) parameter setting of the sputtering deposition step: controlling the ambient pressure of the sputtering deposition step to -2 Torr with a gas pressure value of 1 Torr to -1 Torr, controlling the ambient temperature of the sputtering deposition step to 150° C. to 400° C., and controlling the voltage of the sputtering deposition to 350 kV to 400 kV for 550 seconds to 1000 seconds;

[0030] (F) Preparing for arc deposition: arc deposition is performed on the stainless steel metal substrate 1 to form first colored metal ions 3 on the surface of the colored nitride ions 2, and then second colored metal ions 4 are formed on the surface of the first colored metal ions 3;

[0031] (G) Parameter setting of the arc deposition step: the ambient pressure of the arc deposition step is controlled to be -3 Torr with a gas pressure value of 1 Torr to -1 Torr, the ambient temperature of the arc deposition step is controlled to be 125°C to 300°C, and the voltage of the arc deposition is controlled to be 500 kV to 550 kV, the current intensity is 400 A to 430 A, and the current density is 106 A / cm 2 Up to 1012A / cm 2 , arc voltage is 10V to 40V, arc movement speed is 90m / s to 110m / s, and instantaneous discharge time is 10ns to 1000ns, maintained for 200 seconds to 400 seconds; and

[0032] (H) The processing of 18K gold imitation gold jewelry with high hardness and low roughness is completed: using the colored nitride ions 2, the first colored metal ions 3 and the second colored metal ions 4, the surface hardness is controlled at 1800HV to 2000HV, the roughness is controlled at 0.01μm to 0.1μm, and the color parameter LAB values ​​are L 72~93, A 2.5~8, and B 15~35 respectively.

[0033] Therefore, the surface processing structure of the jewelry of the present invention mainly comprises:

[0034] A stainless steel metal substrate 1;

[0035] A plurality of substrate recesses 11 are formed on the stainless steel metal substrate 1;

[0036] A plurality of colored nitride ions 2 are disposed on a plurality of the substrate recesses 11 and on the surface of the stainless steel metal substrate 1;

[0037] A plurality of first colored metal ions 3 are disposed on the surface of the colored nitride ions 2; and

[0038] A plurality of second colored metal ions 4 are disposed on the surface of the first colored metal ions 3, and the first colored metal ions 3 and the second colored metal ions 4 have the same composition, but the amount of gas can be controlled to change according to the steps to cause different purities and thicknesses.

[0039] The colored nitride ions 2, the first colored metal ions 3 and the second colored metal ions 4 are used to control the surface hardness to 1800HV to 2000HV, the roughness to 0.01μm to 0.1μm, and the color parameter LAB values ​​are L 72-93, A 2.5-8, and B 15-35 respectively.

[0040] Through the above description, the structure of this technology can be understood. According to the corresponding coordination of this structure, various step parameters can be controlled to achieve the advantages of high hardness, low roughness and the color closest to 18K gold on the surface of the jewelry. The detailed explanation will be described below.

[0041] Please also refer to Figures 1 to 6 As shown, it is a flow chart of the steps of the preferred embodiment of the present invention to the schematic diagram of arc deposition. By assembling the above components, it can be clearly seen from the figure that during processing, a stainless steel metal substrate 1 is first taken. In this embodiment, a metal with a LOGO appearance is used as an example. The roughness of the original material is 0.03μm to 0.2μm, and the color parameter LAB values ​​are L 70-82, A 0.3-0.5, and B 4.0-7.2, which is roughly a silver-gray metal with particles that can be touched by hand. The stainless steel metal substrate 1 is subjected to ion bombardment. The parameters of the ion bombardment step include: controlling the ambient pressure to -1 Torr with a pressure value of 0 Torr to -1 Torr, the ambient temperature is 200℃ to 300℃, the voltage is 300kv to 400kv, and the energy density is 106W / cm 2 Up to 109W / cm 2 , power density is 105W / cm 2 Up to 1011W / cm 2, and maintaining time of 200 seconds to 400 seconds, thereby removing oxides on the surface of the stainless steel metal substrate 1 and exposing a plurality of substrate recesses 11, so that the surface of the stainless steel metal substrate 1 except for its own pores (substrate recesses 11) is smooth, which is beneficial to reduce the surface roughness of the subsequent deposition step to 0.01μm to 0.1μm.

[0042] Next, the stainless steel metal substrate 1 is subjected to sputter deposition to implant colored nitride ions 2 into a plurality of the substrate recesses 11 and the surface of the stainless steel metal substrate 1. The parameters of the sputter deposition step include: controlling the ambient pressure to -2 Torr with a pressure value of 1 Torr to -1 Torr, the ambient temperature to 150°C to 400°C, the voltage to 350kv to 400kv, and the maintenance time to 550 seconds to 1000 seconds. The colored nitride ions 2 are one of silicon nitride, aluminum nitride or boron nitride, and the colored nitride ions 2 are components of synthetic ceramics, thereby diluting the color of the substrate to facilitate color control in the arc deposition step and increase the substrate hardness to 1800HV to 2000HV.

[0043] Finally, arc deposition is performed on the stainless steel metal substrate 1 to form first colored metal ions 3 on the surface of the colored nitride ions 2, and second colored metal ions 4 on the surface of the first colored metal ions 3. The parameters of the arc deposition step include: controlling the ambient pressure to -3 Torr with a pressure value of 1 Torr to -1 Torr, the ambient temperature to 125° C. to 300° C., the voltage to 500 kV to 550 kV, the current intensity to 400 A to 430 A, and the current density to 106 A / cm 2 Up to 1012A / cm 2, arc voltage of 10V to 40V, arc movement rate of 90m / s to 110m / s, instantaneous discharge time of 10ns to 1000ns, and maintenance time of 200 seconds to 400 seconds. The first non-ferrous metal ions 3 and the second non-ferrous metal ions 4 are both from a target material such as nickel, chromium, zirconium, or titanium. The first non-ferrous metal ions 3 and the second non-ferrous metal ions 4 are not precious metals, and the cost of obtaining them is relatively low. They themselves have a little red, blue, yellow, or gray. Since the color of the colored nitride ions 2 is close to white, the specified color can be accurately formulated in conjunction with the control of the plasma, which is not affected by the color of the substrate, thereby avoiding the waste of target materials and avoiding lengthy deposition time. According to the principle of light refraction, the light is refracted to the first non-ferrous metal ions 3 and the second non-ferrous metal ions 4 of the same material but different thicknesses during the production process, which is different from simply increasing the thickness of the single layer. Then, through the superposition of colors and the influence of roughness, the required color tone can be obtained. The main purpose of the present invention is to adjust the LAB color parameters closest to 18K gold (L is 72-93, A is 2.5-8, B is 15-35). And because the ion bombardment step has made the surface smooth, the particles generated by the arc step can minimize the impact on the surface roughness.

[0044] Please also refer to Figure 7 As shown in FIG. 1 , it is a flow chart of steps of another preferred embodiment of the present invention. It can be clearly seen from the figure that this embodiment is similar to the above-mentioned embodiment. Only before the ion bombardment step, the surface of the stainless steel metal substrate is cleaned by a plasma cleaning step at a high temperature of 150° C. to 250° C. and a low pressure of 1.5 torr to 2.5 torr. This action can initially remove large particles attached to the surface of the stainless steel metal substrate, reducing the surface roughness to 0.04 μm to 0.1 μm, reducing the burden of the subsequent ion bombardment step, thereby reducing the cost of the ion bombardment step and improving the effectiveness of the ion bombardment step. The specific steps of this embodiment are as follows:

[0045] (A) Select the jewelry to be processed: Take a stainless steel metal base;

[0046] (A1) Plasma cleaning step: Plasma cleaning the stainless steel metal substrate;

[0047] (B) preparing for ion bombardment: performing ion bombardment on the stainless steel metal substrate to remove oxides on the surface of the stainless steel metal substrate and expose a plurality of substrate recesses;

[0048] (C) Parameter setting of the ion bombardment step: the pressure value is 0 Torr to -1 Torr, the ambient pressure of the ion bombardment step is controlled to be -1 Torr, the ambient temperature of the ion bombardment step is controlled to be 200°C to 300°C, and the voltage of the ion bombardment is controlled to be 300 kV to 400 kV, and the energy density is controlled to be 106 W / cm 2 Up to 109W / cm 2 , and power density is 105W / cm 2 Up to 1011W / cm 2 , maintain for 200 to 400 seconds;

[0049] (D) preparing for sputtering deposition: performing sputtering deposition on the stainless steel metal substrate to implant colored nitride ions into a plurality of the substrate recesses and the surface of the stainless steel metal substrate;

[0050] (E) parameter setting of the sputtering deposition step: controlling the ambient pressure of the sputtering deposition step to -2 Torr with a gas pressure value of 1 Torr to -1 Torr, controlling the ambient temperature of the sputtering deposition step to 150° C. to 400° C., and controlling the voltage of the sputtering deposition to 350 kV to 400 kV for 550 seconds to 1000 seconds;

[0051] (F) preparing for arc deposition: performing arc deposition on the stainless steel metal substrate to form first colored metal ions on the surface of the colored nitride ions, and then forming second colored metal ions on the surface of the first colored metal ions;

[0052] (G) Parameter setting of the arc deposition step: the ambient pressure of the arc deposition step is controlled to be -3 Torr with a gas pressure value of 1 Torr to -1 Torr, the ambient temperature of the arc deposition step is controlled to be 125°C to 300°C, and the voltage of the arc deposition is controlled to be 500 kV to 550 kV, the current intensity is 400 A to 430 A, and the current density is 106 A / cm 2 Up to 1012A / cm 2 , arc voltage is 10V to 40V, arc movement speed is 90m / s to 110m / s, and instantaneous discharge time is 10ns to 1000ns, maintained for 200 seconds to 400 seconds; and

[0053] (H) The processing of 18K gold imitation gold jewelry with high hardness and low roughness is completed: using the colored nitride ions, the first colored metal ions and the second colored metal ions, the surface hardness is controlled at 1800HV to 2000HV, the roughness is controlled at 0.01μm to 0.1μm, and the color parameter LAB values ​​are respectively L is 72 to 93, A is 2.5 to 8, and B is 15 to 35.

[0054] The above description is only a preferred embodiment of the present invention, and does not limit the patent scope of the present invention. Therefore, all simple modifications and equivalent structural changes made by using the contents of the present invention description and drawings should be included in the patent scope of the present invention.

Claims

1. A method for surface processing of jewelry, characterized in that: The main steps include: (A) Take a stainless steel metal substrate; (B) performing ion bombardment on the stainless steel metal substrate to remove oxides on the surface of the stainless steel metal substrate and expose a plurality of substrate recesses; (C) controlling the ambient pressure of the ion bombardment step to -1 Torr with a pressure value of 0 Torr to -1 Torr, controlling the ambient temperature of the ion bombardment step to 200° C. to 300° C., and controlling the voltage of the ion bombardment to 300 kV to 400 kV and the energy density to 106 W / cm 2 Up to 109W / cm 2 , and power density is 105W / cm 2 Up to 1011W / cm 2 , maintain for 200 to 400 seconds; (D) performing sputter deposition on the stainless steel metal substrate to implant colored nitride ions into a plurality of the substrate recesses and the surface of the stainless steel metal substrate; (E) controlling the ambient pressure of the sputtering deposition step to -2 Torr at a pressure value of 1 Torr to -1 Torr, controlling the ambient temperature of the sputtering deposition step to 150° C. to 400° C., and controlling the voltage of the sputtering deposition to 350 kV to 400 kV for 550 seconds to 1000 seconds; (F) performing arc deposition on the stainless steel metal substrate to form first colored metal ions on the surface of the colored nitride ions, and then forming second colored metal ions on the surface of the first colored metal ions; (G) controlling the ambient pressure of the arc deposition step to -3 Torr with a gas pressure value of 1 Torr to -1 Torr, controlling the ambient temperature of the arc deposition step to 125°C to 300°C, and controlling the voltage of the arc deposition to 500 kV to 550 kV, the current intensity to 400 A to 430 A, and the current density to 106 A / cm 2 Up to 1012A / cm 2 , arc voltage is 10V to 40V, arc movement speed is 90m / s to 110m / s, and instantaneous discharge time is 10ns to 1000ns, maintained for 200 seconds to 400 seconds; and (H) The colored nitride ions, the first colored metal ions and the second colored metal ions are used to control the surface hardness to 1800 HV to 2000 HV, the roughness to 0.01 μm to 0.1 μm, and the color parameter LAB values ​​are respectively L: 72 to 93, A: 2.5 to 8, and B: 15 to 35.

2. The method for surface processing of jewelry according to claim 1, characterized in that: The roughness of the stainless steel metal substrate raw material is 0.03 μm to 0.2 μm, and the color parameter LAB values ​​are respectively L is 70-82, A is 0.3-0.5, and B is 4.0-7.

2.

3. The method for surface processing of jewelry according to claim 1, characterized in that: Before step (B), step (A1) is performed to perform plasma cleaning on the stainless steel metal substrate.

4. The method for surface processing of accessories according to claim 3, characterized in that: The plasma cleaning step has an operating temperature of 150° C. to 250° C. and an operating pressure of 1.5 torr to 2.5 torr.

5. The method for surface processing of jewelry according to claim 1, characterized in that: The colored nitride ions are one of silicon nitride, aluminum nitride or boron nitride.

6. The method for surface processing of accessories according to claim 1, characterized in that: The first non-ferrous metal ion and the second non-ferrous metal ion are one of nickel, chromium, zirconium, or titanium.

7. A surface processing structure for jewelry, characterized in that: Mainly include: A stainless steel metal substrate; A plurality of substrate recesses are formed on the stainless steel metal substrate; A plurality of colored nitride ions are disposed on a plurality of the substrate recesses and on the surface of the stainless steel metal substrate; A plurality of first colored metal ions are disposed on the surface of the colored nitride ions; and A plurality of second non-ferrous metal ions are arranged on the surface of the first non-ferrous metal ions, and the surface hardness is controlled within 1800HV to 2000HV and the roughness is controlled within 0.01μm to 0.1μm by utilizing the colored nitride ions, the first non-ferrous metal ions and the second non-ferrous metal ions, and the color parameter LAB values ​​are L 72 to 93, A 2.5 to 8, and B 15 to 35 respectively.

8. The surface treatment structure for ornaments according to claim 7, characterized in that: The roughness of the stainless steel metal substrate raw material is 0.03 μm to 0.2 μm, and the color parameter LAB values ​​are respectively L is 70-82, A is 0.3-0.5, and B is 4.0-7.

2.

9. The surface treatment structure for ornaments according to claim 7, characterized in that: The colored nitride ions are one of silicon nitride, aluminum nitride or boron nitride.

10. The surface treatment structure for ornaments according to claim 7, characterized in that: The first non-ferrous metal ion and the second non-ferrous metal ion are one of nickel, chromium, zirconium, or titanium.