Method for repairing damaged inner wall of TA series titanium alloy thin-wall pipe fitting through laser cladding additive

By using TA15 powder and special pipe fitting deformation control fixtures in the inner wall repair of TA-based titanium alloy thin-wall pipe fittings, the deformation and forming problems during the inner wall repair process are solved, and efficient repair and resistance of the inner wall of TA-based titanium alloy thin-wall pipe fittings is achieved. Improved grinding performance.

CN118932329APending Publication Date: 2024-11-12WUHU STATE-OWNED FACTORY OF MACHINING
View PDF 0 Cites 3 Cited by

Patent Information

Application Number
CN202410901182.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-05
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The lack of research on laser cladding repair of inner wall of TA-based titanium alloy thin-walled pipe fittings in the prior art, resulting in the problem of deformation and poor cladding layer forming during the repair process, and there is a difference from the outer wall repair, making it difficult to effectively control the inner wall repair.

Method used

TA15 powder is used for laser cladding repair. By determining the damage area size and planning the repair path, selecting appropriate laser cladding parameters, and designing special pipe fitting deformation control fixtures to control the deformation of pipe fittings to ensure the smooth progress of the inner wall repair process.

Benefits of technology

It has achieved good forming and repair of the inner wall of the TA-based titanium alloy thin-walled pipe fittings, improved the wear resistance of the repair area, and met the repair needs in actual production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118932329A_ABST
    Figure CN118932329A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of titanium alloy additive manufacturing repair, in particular to a method for repairing the inner wall of a damaged TA series titanium alloy thin-wall pipe fitting through laser cladding additive, which comprises the following steps of: 1, determining the size of a damaged area, and cleaning the damaged area; secondly, an additive repairing path is planned, and laser cladding parameters are determined; thirdly, laser cladding is conducted in the argon protection environment, and a damaged area is repaired; and 4, carrying out post-treatment on the damaged area. According to the method, the inner wall of the damaged TA series titanium alloy pipe fitting is repaired by adopting TA15 powder with good performance and compatibility, in the repairing process, a repairing path is planned according to the size of a damaged area, and cladding parameters are determined. In the repairing process, a specially-designed clamp is used for controlling deformation of the thin-wall pipe fitting, repairing steps and characteristics of the damaged inner wall of the TA-series pipe fitting are defined, and good forming and repairing of the damaged inner wall of the TA-series titanium alloy thin-wall pipe fitting can be achieved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of titanium alloy additive manufacturing and repair, and specifically to a method for repairing the inner wall of a damaged TA series titanium alloy thin-wall pipe by laser cladding additive manufacturing. Background Art

[0002] TA series titanium alloy is a single-phase alloy composed of α-phase solid solution. Compared with TB series and TC series titanium alloys, it has good high-temperature strength and thermal stability and is widely used in the preparation of aircraft structural parts. However, since the TA series titanium alloy structure is mainly α-Ti, its hardness is low and its wear resistance is poor. It is prone to defects such as wear and tear, and there is a large demand for repair. Laser cladding is a common metal material damage repair technology that uses a high-energy laser beam to melt powder and substrate to repair damaged parts. Due to the high energy density of the laser and the low heat input, the molten pool cools quickly (the cooling rate can reach 10 4 -10 5 K / s), the formed cladding layer has fine structure, so after the damaged area is repaired, the area can also have good wear resistance.

[0003] In the past, scholars have mainly focused on the outer wall of pipe fittings in the laser cladding repair research, and there are fewer studies on the inner wall repair. Since the wall thickness of thin-walled pipe fittings is small, they are easily deformed by heat during the laser processing process, and measures need to be taken to control the deformation of pipe fittings. At the same time, the thermal conductivity of TA series titanium alloys is very different from that of other metal materials, which makes the laser cladding weld bead formation of TA series titanium alloys very different from that of other alloys. However, there is currently a lack of research data on TA series laser cladding repair formation. The large number of TA series repair needs in actual production urgently need research guidance in this area, so this study on the laser additive repair of the inner wall damage of TA series alloy thin-walled pipe fittings is very necessary.

[0004] Compared with the outer wall repair of pipe fittings, the special feature of the inner wall repair is that, on the one hand, the cladding head easily interferes with the end face of the pipe fitting, limiting the scope of the repair area. On the other hand, when repairing the outer wall, the laser is always at the top of the outer wall, and the laser forms a molten pool on the convex surface of the pipe wall, while when repairing the inner wall, the laser is always at the bottom of the inner wall, and the laser forms a molten pool on the concave surface of the pipe wall. At the same time, when repairing the inner wall, the laser has a certain inclination angle, which makes the molten pool morphology and thermal characteristics formed during the outer wall repair different, which leads to differences in the formation of the cladding layer. It is necessary to study the inner wall repair process and the characteristics of the cladding layer.

[0005] In response to the above problems, this patent proposes to use TA15 powder as raw material (a material commonly used in the repair process of TA alloys with good comprehensive properties) and use laser cladding technology to repair damaged TA pipe fittings. The relationship between laser cladding process parameters (power, powder feeding speed, rotation speed) and weld bead formation under the inner wall repair environment is studied, and the repair steps and characteristics of damaged inner walls of TA pipe fittings are clarified. At the same time, special tooling and fixtures are designed to control the deformation of thin-walled pipe fittings during additive repair, which has high engineering application value. Summary of the invention

[0006] In order to solve the above technical problems, the present invention proposes a method for repairing the inner wall of a damaged TA series titanium alloy thin-walled pipe by laser cladding additive, which can repair the inner wall of a damaged TA series titanium alloy pipe and control the deformation of the thin-walled pipe during the cladding repair process.

[0007] The technical problem to be solved by the present invention is achieved by adopting the following technical solutions:

[0008] The method for repairing the damaged inner wall of a TA series titanium alloy thin-walled pipe by laser cladding additive includes the following steps:

[0009] 1. Determine the size of the damaged area and clean the damaged area:

[0010] Measure the width of the damaged area on the pipe to be repaired perpendicular to the end face of the pipe and the maximum depth of the damaged area, then polish and clean the damaged area with acetone to make it smooth and oil-free;

[0011] 2. Plan the additive repair path and determine the laser cladding parameters:

[0012] According to the corresponding relationship between the width and height of the cladding layer during laser single-layer single-pass cladding and the laser power, the inner wall linear speed of the pipe, the powder feeding speed, and the width and depth of the damaged area, the laser cladding parameters are selected. When the cladding layer width is greater than the damaged area width, the single-layer single-pass cladding is used to complete the repair. When the damaged area width is greater than the single-pass width of the cladding layer, the repair is performed by overlapping, and the overlapping rate is between 35% and 60%.

[0013] 3. Perform laser cladding in an argon gas protection environment to repair the damaged area:

[0014] Clamp the designed pipe deformation control fixture on the pipe to be repaired, install the pipe to be repaired on the three-jaw chuck, connect the three-jaw chuck to the rotating motor, set the rotating motor speed, drive the pipe to be repaired to do a rotary motion, and tilt the laser beam and the powder beam at a certain angle so that the powder convergence point of the cladding head is located in the damaged area, and the cladding head does not interfere with the end face of the pipe to be repaired;

[0015] 4. Post-processing of damaged area:

[0016] The excess height of the cladding layer in the repair area is removed by machining, and the damaged pipe is restored to the original size and the same roughness of the inner wall of the pipe to complete the repair.

[0017] Preferably, in step 1, the wall thickness of the titanium alloy thin-walled pipe is 1 mm-2 mm, the diameter is 50 mm-200 mm, and the maximum depth of the damaged area does not exceed one quarter of the wall thickness of the titanium alloy thin-walled pipe.

[0018] Preferably, the corresponding relationship between the width and height of the cladding layer during the laser single-layer single-pass cladding in step 2 and the laser power, the linear velocity of the inner wall of the pipe, and the powder feeding speed is:

[0019] Cladding layer width = 2.74017 + 0.00272 * laser power - 0.17505 * inner wall linear velocity - 0.17029 * powder feeding speed;

[0020] Cladding layer height = 0.07966 + 0.000263 * laser power - 0.05178 * inner wall linear velocity + 0.12725 * powder feeding speed.

[0021] Preferably, the calculation formula of the linear velocity of the inner wall of the pipe is:

[0022] The linear velocity of the inner wall of the pipe = 2π*the radius of the inner wall of the pipe*the rotation speed of the pipe;

[0023] The pipe rotation speed is the rotation speed of the rotating motor.

[0024] Preferably, the laser cladding parameters in step 2 include: laser power of 1000W-2000W, linear velocity of the inner wall of the pipe of 5mm / s-20mm / s, and powder feeding speed of 3g / min-7g / min.

[0025] Preferably, the pipe deformation control fixture is made of red copper.

[0026] Preferably, the wall thickness of the pipe deformation control fixture is 3 mm, the inner diameter is consistent with the outer diameter of the pipe to be repaired, and the length is 5 mm*damaged area width-10 mm*damaged area width.

[0027] Preferably, the inclination angle between the laser beam and the powder beam does not exceed 30°.

[0028] The beneficial effects of the present invention are:

[0029] The present invention uses TA15 powder with good performance and compatibility to repair the damaged inner wall of TA series titanium alloy pipe fittings. During the repair process, the repair path is planned according to the size of the damaged area, and the cladding parameters are determined. During the repair process, a specially designed fixture is used to control the deformation of the thin-walled pipe fittings, and the repair steps and characteristics of the damaged inner wall of the TA series pipe fittings are clarified, so that the damaged inner wall of the TA series titanium alloy thin-walled pipe fittings can be well formed and repaired. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] The present invention is further described below in conjunction with the accompanying drawings and embodiments:

[0031] Figure 1 Schematic diagram of the repair process;

[0032] Figure 2 It is a three-dimensional structural schematic diagram of the pipe deformation control fixture;

[0033] Figure 3 It is a front view structural schematic diagram of the pipe deformation control fixture;

[0034] Figure 4 This is a schematic diagram of the tissue morphology of the repaired area after single-layer single-channel repair;

[0035] Figure 5 Schematic diagram of the tissue morphology of the repair area after single-layer multi-pass repair.

[0036] In the figure: 1. Rotating motor; 2. Pipe to be repaired; 3. Laser beam and powder beam; 4. Pipe deformation control fixture; 5. Three-jaw chuck. DETAILED DESCRIPTION

[0037] In order to make the technical means, creative features, objectives and effects achieved by the present invention easy to understand, the present invention is further described below with reference to the accompanying drawings and embodiments.

[0038] The method for repairing the damaged inner wall of a TA series titanium alloy thin-walled pipe by laser cladding additive includes the following steps:

[0039] 1. Determine the size of the damaged area and clean the damaged area.

[0040] The width of the damaged area on the pipe 2 to be repaired perpendicular to the end face of the pipe and the maximum depth of the damaged area are measured, and then the damaged area is polished and cleaned with acetone to make it flat and oil-free.

[0041] The wall thickness of titanium alloy thin-walled pipes is 1mm-2mm, the diameter is 50mm-200mm, and the maximum depth of the damaged area does not exceed one-fourth of the wall thickness of titanium alloy thin-walled pipes. The filling powder used for repair is TA15, and the powder particle size is between 53-150μm. The additive repair process is completed in an argon protection environment, and the powder feeding gas is argon with a purity of 99.99%-99.999%.

[0042] 2. Plan the additive repair path and determine the laser cladding parameters.

[0043] The laser cladding parameters are selected according to the corresponding relationship between the width and height of the cladding layer during laser single-layer single-pass cladding and the laser power, the linear velocity of the inner wall of the pipe, the powder feeding speed, and the width and depth of the damaged area.

[0044] The corresponding relationship between the width and height of the cladding layer during laser single-layer single-pass cladding and the laser power, the linear velocity of the inner wall of the pipe, and the powder feeding speed is:

[0045] Cladding layer width = 2.74017 + 0.00272 * laser power - 0.17505 * inner wall linear velocity - 0.17029 * powder feeding speed; Cladding layer height = 0.07966 + 0.000263 * laser power - 0.05178 * inner wall linear velocity + 0.12725 * powder feeding speed.

[0046] The calculation formula of the linear velocity of the inner wall of the pipe is:

[0047] The linear velocity of the inner wall of the pipe fitting=2π*the radius of the inner wall of the pipe fitting*the rotating speed of the pipe fitting, wherein the rotating speed of the pipe fitting is the rotating speed of the rotating motor 1 .

[0048] Laser cladding parameters include: laser power of 1000W-2000W, linear speed of the inner wall of the pipe of 5mm / s-20mm / s, and powder feeding speed of 3g / min-7g / min.

[0049] When the width of the cladding layer is greater than the width of the damaged area, the repair is completed by cladding a single layer and a single pass. When the width of the damaged area is greater than the width of a single pass of the cladding layer, the repair is carried out by overlapping, and the overlapping rate is between 35% and 60%.

[0050] 3. Perform laser cladding in an argon protection environment to repair the damaged area.

[0051] like Figure 1As shown, the designed pipe deformation control fixture 4 is clamped on the pipe 2 to be repaired, and the pipe 2 to be repaired is installed on the three-jaw chuck 5. The three-jaw chuck 5 is connected to the rotating motor 1. The rotating speed of the rotating motor 1 is set to drive the pipe 2 to be repaired to make a rotary motion. The laser beam and the powder beam 3 are tilted at a certain angle, and the tilt angle does not exceed 30°. The powder convergence point of the cladding head is located in the damaged area, and the cladding head does not interfere with the end face of the pipe 2 to be repaired.

[0052] like Figure 2 and Figure 3 As shown, the pipe deformation control fixture 4 is made of red copper, the wall thickness of the pipe deformation control fixture 4 is 3 mm, the inner diameter is consistent with the outer diameter of the pipe 2 to be repaired, and the length is 5 mm*damage area width-10 mm*damage area width.

[0053] 4. Post-processing of damaged area.

[0054] The excess height of the cladding layer in the repair area is removed by machining, and the damaged pipe is restored to the original size and the same roughness of the inner wall of the pipe to complete the repair.

[0055] Embodiment 1

[0056] In this embodiment, specifically, the titanium alloy thin-walled pipe is a TA15 pipe with an inner diameter of 78 mm and a wall thickness of 2 mm. The maximum depth of the damaged area is 0.44 mm, the width is 3.2 mm, and the damaged area is 17 mm away from the end face of the pipe.

[0057] In this embodiment, specifically, the inner diameter of the pipe deformation control fixture 4 is 82 mm, the thickness is 3 mm, and the width is 30 mm.

[0058] In this embodiment, specifically, the laser power is 1300W, the linear velocity of the inner wall of the tube is 10mm / s, and the powder feeding speed is 5.2g / min.

[0059] According to the calculation formula, the height of the cladding layer is 0.56 mm, and the width of the cladding layer is 3.6 mm. At this time, the width of the cladding layer is greater than the width of the damaged area, that is, 3.6 mm>3.2 mm. Single-layer single-pass cladding can meet the repair requirements under low heat input conditions.

[0060] Specifically: the pipe deformation control fixture 4 is clamped on the outer diameter area of ​​the pipe damage area, and then the damaged area is clad. After the cladding is completed, it is found that the height of the cladding area is slightly higher than the inner diameter surface by about 0.1mm, and then the area is ground and polished to complete the repair of the damaged area.

[0061] like Figure 3As shown, it can be seen that the cladding zone structure is mainly composed of fine needle-shaped martensite phase, and the hardness of the cladding zone is 431HV, which is higher than the hardness of the pipe base material of 330HV. While achieving good repair and forming of the pipe, the wear resistance of the repair zone is improved.

[0062] Embodiment 2

[0063] In this embodiment, specifically, the titanium alloy thin-walled pipe is a TA15 pipe with an inner diameter of 96 mm and a wall thickness of 2 mm. The maximum depth of the damaged area is 0.36 mm, the width is 12.7 mm, and the damaged area is 11 mm away from the end face of the pipe.

[0064] In this embodiment, specifically, the inner diameter of the pipe deformation control fixture 4 is 100 mm, the thickness is 3 mm, and the width is 127 mm.

[0065] In this embodiment, specifically, the laser power is 800W, the linear velocity of the inner wall of the pipe is 5mm / s, the powder feeding speed is 3.4g / min, and the height of the cladding layer can be calculated based on the formula. The height of the cladding layer is 0.47mm, and the width of the cladding layer is 3.46mm. At this time, the width of the damaged area is greater than the single-pass width of the cladding layer, that is, 12.7mm>3.46mm. The overlapping method, that is, single-pass and multiple-pass cladding, can meet the repair needs under low heat input conditions. The overlap rate is 50%, and a total of six overlaps are performed to complete the cladding of the damaged area. After repair, the height of the cladding area is slightly higher than the inner diameter surface by about 0.14mm. The area is then ground and polished to complete the repair of the damaged area. Figure 4 As shown, it can also be seen that the cladding zone structure is mainly composed of fine needle-shaped martensite phase, and the hardness of the cladding zone is 423HV, which is higher than the hardness of the pipe base material by 330HV. While achieving good repair and forming of the pipe, the wear resistance of the repair zone is improved.

[0066] The above shows and describes the basic principles, main features and advantages of the present invention. Those skilled in the art should understand that the present invention is not limited to the above embodiments. The above embodiments and descriptions only describe the principles of the present invention. Without departing from the spirit and scope of the present invention, the present invention may have various changes and improvements, which fall within the scope of the present invention. The scope of protection of the present invention is defined by the attached claims and their equivalents.

Claims

1. Laser cladding additive repair method for the inner wall of damaged TA series titanium alloy thin-walled pipes. Features: The following steps are involved:

1. Determine the size of the damaged area and clean the damaged area: Measuring the width of the damaged area on the pipe to be repaired (2) perpendicular to the end face of the pipe and the maximum depth of the damaged area, then polishing and cleaning the damaged area with acetone to make it smooth and free of oil stains; 2. Plan the additive repair path and determine the laser cladding parameters: According to the corresponding relationship between the width and height of the cladding layer during laser single-layer single-pass cladding and the laser power, the inner wall linear speed of the pipe, the powder feeding speed, and the width and depth of the damaged area, the laser cladding parameters are selected. When the cladding layer width is greater than the damaged area width, the single-layer single-pass cladding is used to complete the repair. When the damaged area width is greater than the single-pass width of the cladding layer, the repair is performed by overlapping, and the overlapping rate is between 35% and 60%.

3. Perform laser cladding in an argon gas protection environment to repair the damaged area: The designed pipe deformation control fixture (4) is clamped on the pipe to be repaired (2), and the pipe to be repaired (2) is installed on the three-jaw chuck (5). The three-jaw chuck (5) is connected to the rotating motor (1), and the rotation speed of the rotating motor (1) is set to drive the pipe to be repaired (2) to perform a rotary motion. The laser beam and the powder beam (3) are tilted at a certain angle so that the powder convergence point of the cladding head is located in the damaged area, and at the same time, the cladding head does not interfere with the end face of the pipe to be repaired (2); 4. Post-processing of damaged area: The excess height of the cladding layer in the repair area is removed by machining, and the damaged pipe is restored to the original size and the same roughness of the inner wall of the pipe to complete the repair.

2. The method for repairing the damaged inner wall of a TA series titanium alloy thin-walled pipe by laser cladding additive according to claim 1, Features: In step 1, the wall thickness of the titanium alloy thin-walled pipe is 1mm-2mm, the diameter is 50mm-200mm, and the maximum depth of the damaged area does not exceed one quarter of the wall thickness of the titanium alloy thin-walled pipe.

3. The method for repairing the inner wall of a damaged TA series titanium alloy thin-walled pipe by laser cladding additive according to claim 1, Features: The corresponding relationship between the width and height of the cladding layer during laser single-layer single-pass cladding in step 2 and the laser power, the linear velocity of the inner wall of the pipe, and the powder feeding speed is: Cladding layer width = 2.74017 + 0.00272 * laser power - 0.17505 * inner wall linear velocity - 0.17029 * powder feeding speed; Cladding layer height = 0.07966 + 0.000263 * laser power - 0.05178 * inner wall linear velocity + 0.12725 * powder feeding speed.

4. The method for repairing the inner wall of a damaged TA series titanium alloy thin-walled pipe by laser cladding additive according to claim 3, Features: The calculation formula of the linear velocity of the inner wall of the pipe is: The linear velocity of the inner wall of the pipe = 2π*the radius of the inner wall of the pipe*the rotation speed of the pipe; The rotation speed of the pipe is the rotation speed of the rotating motor (1).

5. The method for repairing the damaged inner wall of a TA series titanium alloy thin-walled pipe by laser cladding additive according to claim 4, Features: The laser cladding parameters in step 2 include: laser power of 1000W-2000W, linear speed of the inner wall of the pipe of 5mm / s-20mm / s, and powder feeding speed of 3g / min-7g / min.

6. The method for repairing the inner wall of a damaged TA series titanium alloy thin-walled pipe by laser cladding additive according to claim 1, Features: The pipe deformation control fixture (4) is made of red copper.

7. The method for repairing the damaged inner wall of a TA series titanium alloy thin-walled pipe by laser cladding additive according to claim 1, Features: The wall thickness of the pipe deformation control fixture (4) is 3 mm, the inner diameter is consistent with the outer diameter of the pipe to be repaired (2), and the length is 5 mm*damaged area width-10 mm*damaged area width.

8. The method for repairing the damaged inner wall of a TA series titanium alloy thin-walled pipe by laser cladding additive according to claim 1, Features: The inclination angle between the laser beam and the powder beam (3) does not exceed 30°.

Citation Information

Cited By

  • Method for repairing 30CrMnSiNi2A annular clamp for aviation through high-speed laser cladding additive

    CN119932558A

  • Method for repairing 1Cr11Ni2W2MoV stainless steel gear shaft for aviation through high-speed laser cladding additive

    CN119956349A

  • Cylinder part side wall damage repairing method

    CN121402969A