Method for strengthening and repairing nickel-plated composite coating of spline electric brush

The nanoparticle dispersant and electrochemical principles were prepared by sol-gel method, combined with heat treatment and alternating brush methods, the performance limitation of nanoparticle composite brush plating under dynamic load conditions was solved, and the binding force of the plating was significantly improved and wear resistance.

CN118932444AInactive Publication Date: 2024-11-12GUANGDONG UNIV OF TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411210046.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-30
Publication Date
2024-11-12
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The performance of nanoparticle composite brush plating is limited under dynamic load conditions, mainly due to the brittleness of ceramic-enhanced particles and the interface problems caused by differences in physical and chemical properties with the matrix materials, which affects the binding force and wear resistance of the plating.

Method used

The nanoparticle dispersant was prepared by the sol-gel method. The stability and dispersion of the plating solution were enhanced through electrochemical principles and heat treatment, and the surface was treated before plating. The coating was constructed by alternating brushes, including the bottom nickel- Alternating brushing method of copper-bright nickel-composite nickel-bright nickel.

Benefits of technology

The binding force and wear resistance of the coating are improved, the stability and performance of the coating are enhanced, the problem of poor binding force of the nanocomposite coating is avoided, and the wear rate of the coating is significantly improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118932444A_ABST
    Figure CN118932444A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of surface engineering, and particularly discloses a method for strengthening and repairing a spline electric brush nickel-based composite coating, which comprises the following steps of plating solution preparation, spline pretreatment, electric brush plating process and plating layer performance test. According to the method, a dispersing agent of nano-particles is selected by adopting a sol-gel method and an electrochemical principle, the plating solution is subjected to sufficient stirring and low-temperature ultrasonic oscillation, the stability and dispersity of the plating solution are enhanced, the binding force between a matrix and a plating layer is improved through spline pretreatment, metal ions are more easily deposited on the matrix, and the plating quality is improved. And meanwhile, the interface bonding force is further improved through heat treatment after bottom nickel brush plating, the defect that the bonding force of the nano-composite coating is poor is effectively overcome through the alternate electric brushing mode that bottom nickel, copper plating, bright nickel, composite nickel and bright nickel form one group, and the wear rate is also improved to some extent.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of surface engineering, and in particular relates to a method for strengthening and repairing a spline brush-plated nickel-based composite coating. Background Art

[0002] As an important branch of electrodeposition technology, brush plating occupies an important position in the field of surface engineering technology. This technology deposits metal or performs metallization treatment on the specific surface of the plated parts through electrochemical methods to strengthen and improve the surface performance of the workpiece. Brush plating has significant advantages such as simple equipment, flexible operation, low cost, controllable coating thickness and suitability for surface treatment of complex-shaped workpieces, so it has been widely used in industry.

[0003] Although the traditional brush-plated nickel layer has certain hardness, wear resistance and corrosion resistance, its performance is still difficult to meet the requirements under certain extreme working conditions. In order to further improve the performance of nickel plating, researchers began to explore adding other alloy elements or particles to nickel plating to form alloy plating or composite plating. For example, by adding nanoparticles such as diamond, graphite, SiC, Al2O3, SiO2, etc. to nickel plating, the hardness, strength, wear resistance and corrosion resistance of the coating can be significantly improved.

[0004] However, although the nanoparticle composite brush-plated coating exhibits good mechanical, chemical and friction and wear properties under static conditions, its performance is often limited during dynamic load service. This is mainly due to the large brittleness and poor toughness of ceramic reinforcing particles (such as nano-Al2O3), which are quite different from the physical and chemical properties of the coating alloy or matrix material, resulting in excessive compound generation, chemical incompatibility, and low connection strength at the interface. These problems directly affect the bonding force, thickness and wear resistance of the coating, limiting the widespread promotion of nano-composite coatings in practical industrial applications. Summary of the invention

[0005] The object of the present invention is to provide a method for strengthening and repairing a spline brush-plated nickel-based composite coating to solve the problems raised in the above-mentioned background technology.

[0006] To achieve the above object, the present invention provides the following technical solutions:

[0007] A method for preparing a reinforced and repaired brush-plated nickel-based composite coating.

[0008] S1. Prepare plating solution and activation solution.

[0009] S2. Remove oil stains from the surface of the spline and make it smooth;

[0010] S3, using direct current or pulse current as power source, first use the graphite plating pen as cathode and the workpiece surface as anode to activate the spline surface; then use the graphite plating pen as anode and the workpiece surface as cathode to brush-plate bottom nickel on the spline surface, and then place the spline at 450°C for dehydrogenation heat treatment;

[0011] S4. The spline surface is successively plated with bright copper, bright nickel, nickel-based composite plating solution, and finally with bright nickel.

[0012] S5. Coating performance test: hardness, wear rate and roughness test of coating samples.

[0013] Preferably, the coating for strengthening and repairing the spline brush is not limited to the nickel-based composite coating.

[0014] Preferably, the method for strengthening and repairing the spline brush-plated nickel-based composite coating includes but is not limited to the nickel-based composite coating and carburized 9310 steel, and also includes medium carbon steel, alloy steel, stainless steel spline steel, chromium-based, cobalt-based, copper-based brush-plated metals.

[0015] Compared with the prior art, the present invention has the following beneficial effects:

[0016] (1) The sol-gel method and electrochemical principle are used to select the dispersant of nanoparticles. The plating solution is fully stirred and subjected to low-temperature ultrasonic oscillation, and the stability and dispersibility of the plating solution are enhanced.

[0017] (2) The spline surface is pre-treated before plating to remove surface oil stains, improve the bonding strength between the substrate and the coating, and make it easier for metal ions to deposit on the substrate.

[0018] (3) The splines after brush-plating with nickel are heat-treated. On the one hand, the internal stress and hydrogen ions in the coating are reduced, and on the other hand, the thermal motion between molecules is accelerated, so that a small amount of the coating and the substrate can penetrate into each other, further improving the interface bonding strength.

[0019] (4) The alternating brushing method of base nickel-copper plating-bright nickel-composite nickel-bright nickel is adopted to effectively avoid the disadvantage of poor bonding strength of the nano-composite coating and improve the wear rate. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] Figure 1 This is a schematic diagram of the wear rate of mainstream brush plating on the market;

[0021] Figure 2 The cross-sectional SEM morphology and composition distribution of the coating in the embodiment of the present invention;

[0022] Figure 3 It is a schematic diagram of the structure of the substrate and the nickel-based composite coating of the present invention. DETAILED DESCRIPTION

[0023] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0024] Embodiment 1:

[0025] A method for preparing a reinforced and repaired brush-plated nickel-based composite coating.

[0026] 1. Plating solution configuration

[0027] Preparation of nanoparticle dispersion by sol-gel method:

[0028] Ethanol was selected as the solvent, and nickel salt and nano-Al2O3 particles (particle size 20 nm) were dissolved in the ethanol to form a mixed solution.

[0029] Deionized water and ammonia water were slowly added dropwise to adjust the pH value of the solution to 4.3-4.7, so as to promote the hydrolysis and polycondensation reaction of the nickel salt and the nanoparticles to form a sol.

[0030] Hexadecyltrimethylammonium bromide was added to the sol as a dispersant, and a magnetic stirrer was used to fully stir the sol to ensure that the nanoparticles were evenly dispersed.

[0031] The mixed solution is placed in an ultrasonic cleaning machine for low-temperature ultrasonic oscillation treatment to further enhance the stability and dispersibility of the sol.

[0032] Basic plating solution configuration:

[0033] According to the requirements of the electroplating process, appropriate amounts of pure nickel plating solution and nickel-based composite plating solution are prepared. The basic plating solution contains necessary ingredients such as nickel salt, buffer, and complexing agent, while the composite plating solution is additionally added with nanoparticle dispersion.

[0034] 2. Spline pre-processing

[0035] Use sandpaper to sand the spline surface in stages until the surface is smooth and free of scratches.

[0036] Polishing: Apply an appropriate amount of polishing paste and polish the spline surface with a polishing cloth until it reaches a mirror effect.

[0037] Degreasing treatment: First wipe the surface with acetone to remove most of the oil stains, and then use electrochemical degreasing method (electrocleaning method) to further clean the surface.

[0038] Dehydration treatment: Clean the spline surface with anhydrous ethanol to ensure that there is no residual moisture.

[0039] Certain pre-treatment of the splines to remove oil stains on the surface and make it smooth can make the substrate and the coating bond more firmly, and the metal ions are more likely to crystallize and deposit on the substrate.

[0040] 3. Brush plating process

[0041] Activation treatment: Place the spline in the electroplating tank, use direct current or pulse current as the power source, use the graphite plating pen as the cathode, and the workpiece surface as the anode. Add an activator under a constant voltage of 11V to etch the spline surface for 20 seconds.

[0042] Rinse: Rinse the spline surface with 45°C deionized water to remove residual activator.

[0043] Brush plating bottom nickel: switch the electrode polarity, use the graphite plating pen as the anode and the workpiece surface as the cathode, and brush plate the bottom nickel under a constant voltage of 12V for 30 seconds.

[0044] Heat treatment: Place the spline after brush-plating with base nickel in a 450°C environment for dehydrogenation heat treatment and keep it warm for 3 hours to remove hydrogen ion bubbles and internal stress in the coating and promote the bonding of the coating to the substrate.

[0045] Dehydrogenation heat treatment is carried out at 450°C, which is beneficial to accelerate the thermal motion between molecules so that a small amount of coating and substrate can penetrate into each other to improve the bonding strength.

[0046] Alternating brush plating: on the heat-treated spline surface, brush plate bright copper (1 minute), bright nickel (1 minute), nickel-based composite plating solution (5 minutes), and finally brush plate bright nickel again (1 minute). Rinse with 45℃ deionized water between each layer of brush plating.

[0047] 4. Post-plating consolidation treatment

[0048] According to needs, the coating is post-treated, such as passivation, sealing, etc., to improve the corrosion resistance and wear resistance of the coating.

[0049] 5. Performance testing

[0050] Coating performance testing

[0051] Hardness test: Hardness indicates the resistance of the material to fixed deformation caused by indentation. Due to the high hardness of brush-plated coating, Brinell and Rockwell hardness should not be used, but Vickers hardness should be used for testing. To prevent the indenter from pressing through the coating, the coating thickness and the diagonal of the indentation should meet a relationship of 0.4 times.

[0052] Roughness test: The roughness of the sample surface has a significant impact on the friction and wear properties of the sample. Therefore, it is necessary to measure the roughness of the sample and keep it below Ra≤1.6.

[0053] Tribological performance test: Tribological performance is the most important indicator of coating. The coating sample is placed on a reciprocating friction and wear tester. Zirconia is used as a friction pair to grind with it, with a load of 100N, a sliding friction speed of 200r / min, and a friction time of 15min. The weight loss method and the wear scar volume measurement method are used to test the wear resistance. The sample is cleaned and dried before and after friction, and the weight difference △W is weighed; the wear scar volume and sliding distance are obtained in a laser confocal microscope, and the wear rate is calculated using the formula.

[0054] Optimized process parameters of composite NiAl2O3 nanoparticle coating on 9310 steel surface

[0055]

[0056] The above table shows the test results of alternating brush-plated nickel-based composite coatings.

[0057] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A method for strengthening and repairing a spline brush-plated nickel-based composite coating, characterized in that: The following steps are involved: S1, prepare plating solution and activation solution; S2. Remove oil stains from the surface of the spline and make it smooth; S3, using direct current or pulse current as power source, first use the graphite plating pen as cathode and the workpiece surface as anode to activate the spline surface; then use the graphite plating pen as anode and the workpiece surface as cathode to brush-plate bottom nickel on the spline surface, and then place the spline at 450°C for dehydrogenation heat treatment; S4, brush-plating the spline surface with bright copper, bright nickel, nickel-based composite plating solution in sequence, and finally brush-plating the surface with bright nickel; S5. Coating performance test: hardness, wear rate and roughness test of coating samples.

2. A method for strengthening and repairing a spline brush-plated nickel-based composite coating according to claim 1, characterized in that: The coating for strengthening and repairing the spline brush is not limited to the nickel-based composite coating.

3. The method for strengthening and repairing a spline brush-plated nickel-based composite coating according to claim 1, characterized in that: The method for strengthening and repairing the spline brush-plated nickel-based composite coating includes but is not limited to the nickel-based composite coating and carburized 9310 steel, and also includes medium carbon steel, alloy steel, stainless steel spline steel, chromium-based, cobalt-based, copper-based brush-plated metals.