Application of polytellurooxane in non-chemically amplified photoresist

By using the Te-O chain structure of polytelluroxane in photoresist, the problem of absorption and pattern resolution of photoresist in extreme ultraviolet lithography is solved, and light with high sensitivity and low line edge roughness is achieved The performance simplifies the process flow and reduces costs.

CN118938603AActive Publication Date: 2024-11-12TSINGHUA UNIVERSITY +1

Patent Information

Application Number
CN202411296105.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-14
Publication Date
2024-11-12
Estimated Expiration
2044-09-14

AI Technical Summary

Technical Problem

Existing photoresist has low absorption, poor pattern resolution and line edge roughness in extreme ultraviolet lithography, making it difficult to meet the needs of high sensitivity and high resolution.

Method used

Using a non-chemical amplified photoresist based on polytelluroxane, the Te element and Te-O main chain are used to improve the absorption rate of extreme ultraviolet light, and the lithographic performance with high sensitivity and low linear edge roughness is achieved.

Benefits of technology

It significantly improves the absorption capacity of photoresist to extreme ultraviolet light, simplifies the lithography process, reduces costs, and achieves patterning effects of high resolution and low line edge roughness.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005047480410000021
    Figure BDA0005047480410000021
  • Figure BDA0005047480410000031
    Figure BDA0005047480410000031
  • Figure BDA0005047480410000161
    Figure BDA0005047480410000161
Patent Text Reader

Abstract

The invention discloses an application of poly (tellurium oxyalkane) in a non-chemical amplification photoresist. The poly (tellurium oxyalkane) is provided with a Te-O chain. Wherein the Te element has high absorption on EUV and a special Te-O main chain, so that excellent UV photoetching (I-line, KrF, ArF and the like), electron beam photoetching and EUV photoetching performances are realized, and particularly, the problem of EUV photoresist with high sensitivity, high resolution and low line edge roughness is solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of photoresists, and in particular to the application of polytelluroxane in non-chemically amplified photoresists. Background Art

[0002] Photolithography is the foundation of the semiconductor industry. Its essence is a technology that uses photochemical reactions to produce micro-nano structures. The solubility of the photoresist changes through exposure. The solubility difference between the exposed part and the unexposed part is developed in a specific organic solvent or aqueous solution to obtain the corresponding micro-nano structure. The exposed part that dissolves is called positive photoresist, and the exposed part that dissolves is called negative photoresist.

[0003] With the continuous advancement of Moore's Law, the demand for the continuous miniaturization of feature sizes in integrated circuits has promoted the development of photolithography technology. The exposure wavelength of photolithography technology has experienced G-line (436nm), I-line (365nm), KrF (248nm), ArF (193nm), and gradually developed towards shorter wavelengths. In recent years, extreme ultraviolet (EUV, 13.5nm) lithography technology has greatly promoted the iteration of the chip manufacturing industry and has become the most promising nanoscale manufacturing technology. However, the limited EUV light source power and the energy loss of the multi-layer mirror system place high demands on the sensitivity of the photoresist. In addition, EUV's high-resolution patterning requires the photoresist material to also have good resolution and line edge roughness. Therefore, the development of new photoresists suitable for EUV lithography remains a huge challenge.

[0004] Conventional ultraviolet (UV) lithography generally uses chemically amplified photoresists (CARs), which contain an acid-sensitive polymer host and a photoacid generator. For example, in polystyrene-based CARs, the photoacid generator generates protons in situ after exposure, which can catalyze the deprotection reaction to release the phenol structure, which is easily soluble in alkaline solution. CARs have been used in extreme ultraviolet (EUV) lithography, but their shortcomings become more obvious as the feature size decreases. CARs are mainly composed of low-period elements, which have poor absorption of EUV at 13.5nm; at the same time, as the pattern size decreases, the thickness of the photoresist film also decreases, and the problem of poor absorption becomes more significant. In addition, the complex working mechanism and multiple components of CARs mean that the randomness of the position and amount of each component will cause significant chemical noise, resulting in rough patterns, unclear structures, size variations and pattern defects. This requires us to develop photoresist materials and working modes that are more suitable for EUV lithography.

[0005] In recent years, in order to avoid the above problems, non-chemical amplification photoresists (non-CARs) have gradually received attention, such as polymer-based main-chain scission type photoresists with good film-forming properties and stability. The principle is that EUV is absorbed by the photoresist to generate secondary electrons, which can cut the polymer main chain and crack to produce small molecules with better solubility, thereby developing and removing the exposed area. Main-chain scission type photoresists do not need to introduce photoacid generators, so there are fewer components, less chemical noise, and may reduce line edge roughness. The earliest main-chain scission type photoresist, and also the earliest photoresist used in EUV lithography, is polymethyl methacrylate (PMMA). After exposure, the main chain CC bond or ester bond will break, producing organic small molecules or oligomers, the latter of which have greater solubility and are more soluble in the developer. However, since the main-chain scission type photoresist is not assisted by the chemical amplification process and the polymer main chain bond energy is relatively large, it requires a large exposure dose, which limits its application in high-sensitivity EUV lithography. Therefore, solving the problem of weak EUV absorption of photoresist is the key to developing main chain break type photoresist. Summary of the invention

[0006] The inventors have found that metal-based EUV photoresists have appeared in the prior art. These systems generally have higher absorption rates than CARs, but they are all negative photoresists. For specific pattern types, positive photoresists with high EUV absorption rates are still required.

[0007] In order to solve the above-mentioned related technical problems, the main purpose of the present invention is to provide a non-chemically amplified photoresist based on polytelluroxane, which utilizes the high absorption of EUV by the Te element and the special Te-O main chain to achieve excellent UV lithography (I-line, KrF, ArF, etc.), electron beam lithography and EUV lithography performance, especially to solve the problem of EUV photoresist with high sensitivity, high resolution and low line edge roughness.

[0008] In one aspect of the present invention, the present invention proposes the use of polytelluroxane in non-chemical amplification photoresist. According to an embodiment of the present invention, the polytelluroxane has a Te-O chain. The non-chemical amplification photoresist utilizes the high absorption of EUV by the Te element therein and the special Te-O main chain, aiming to achieve excellent UV lithography (I-line, KrF, ArF, etc.), electron beam lithography and EUV lithography performance, especially to solve the EUV photoresist problem of high sensitivity, high resolution and low line edge roughness.

[0009] According to an embodiment of the present invention, the above application may further include at least one of the following additional technical features:

[0010] According to an embodiment of the present invention, the polytelluroxane is a polymer composed of monomers having a structure as shown in formula (V),

[0011]

[0012] wherein R1 and R2 are independently selected from hydrogen, hydroxyl, amino, thiol, optionally substituted C1-C 20 Alkyl, optionally substituted C2-C 20 Alkenyl, optionally substituted C2-C 20 Alkynyl, optionally substituted C1-C 20 Heteroalkyl, optionally substituted C2-C 20 Heteroalkenyl, optionally substituted C2-C 20 heteroalkynyl, optionally substituted aryl, or having a structure represented by general formula (II),

[0013]

[0014] R3 is selected from hydroxyl, amino, cyano, and optionally substituted aryl, and x is any integer between 1 and 20;

[0015] or R1 and R2 are connected together to form a monomer having a structure represented by general formula (VI),

[0016] R4 is selected from optionally substituted optionally substituted C1-C8 alkyl, optionally substituted C2-C8 alkenyl, optionally substituted C2-C8 alkynyl, optionally substituted C1-C8 heteroalkyl, optionally substituted C2-C8 heteroalkenyl, optionally substituted C2-C8 heteroalkynyl.

[0017] According to an embodiment of the present invention, the polytelluroxane has a structure as shown in formula (I):

[0018] n is any integer between 2 and 5000.

[0019] According to an embodiment of the present invention, the polytelluroxane has a structure as shown in formula (III):

[0020] n is any integer between 2 and 5000.

[0021] According to an embodiment of the present invention, the polytelluroxane may be a copolymerization product of two or more monomers, that is, R1 and R2 in different repeating units are also independently selected from the above groups and are not necessarily completely the same. Taking the copolymerization of two monomers as an example, according to an embodiment of the present invention, the polytelluroxane has a structure as shown in formula (IV):

[0022] wherein R1′ and R1″ are independently selected from R1, R2′ and R2″ are independently selected from R2, and m and p are independently any integer between 1 and 5000.

[0023] According to the embodiments of the present invention, the above-mentioned polytelluroxane structural formulas (I), (III), and (IV) are only schematic diagrams for convenience of explanation and are not used to limit the protection scope of the present invention. Since the Te-O chain is the core of the performance of the non-chemically amplified photoresist described in the present invention, copolymerizing and blending the Te-O chain structure with other components can also improve the performance of the photoresist. Therefore, for those skilled in the art, the present invention can have various changes, modifications and improvements based on the above-mentioned polytelluroxane.

[0024] According to an embodiment of the present invention, R1 and R2 are independently selected from optionally substituted C1-C 12 Alkyl, optionally substituted C2-C 12 Alkenyl, optionally substituted C2-C 12 alkynyl or optionally substituted aryl.

[0025] According to an embodiment of the present invention, R1 and R2 are independently selected from optionally substituted C1-C4 alkyl, optionally substituted C2-C4 alkenyl, optionally substituted C2-C4 alkynyl,

[0026] According to an embodiment of the present invention, R1 and R2 are independently selected from optionally substituted C1-C4 alkyl, optionally substituted C2-C4 alkenyl, and optionally substituted C2-C4 alkynyl.

[0027] According to an embodiment of the present invention, R1 is a phenyl group, and R2 is a C1-C4 alkyl group, a C2-C4 alkenyl group or a C2-C4 alkynyl group.

[0028] According to an embodiment of the present invention, the polytelluroxane is n is 150.

[0029] According to an embodiment of the present invention, the polytelluroxane is n is 150.

[0030] According to an embodiment of the present invention, the polytelluroxane is n is 150.

[0031] According to an embodiment of the present invention, the polytelluroxane is n is 50.

[0032] According to an embodiment of the present invention, the polytelluroxane is n is 50.

[0033] According to an embodiment of the present invention, the polytelluroxane is n is 50.

[0034] According to an embodiment of the present invention, the application is implemented in the following manner:

[0035] After cleaning the substrate, a solution of polytelluroxane is applied to the substrate, and the solvent is removed by baking. The substrate is subjected to UV lithography, electron beam lithography or EUV lithography, and then developed using a developer to obtain a corresponding pattern.

[0036] According to an embodiment of the present invention, the material of the substrate is germanium, silicon, silicon carbide, silicon nitride, gallium arsenide or gallium nitride.

[0037] According to an embodiment of the present invention, the cleaning of the substrate is performed by using acetone and ultrasound to clean the substrate.

[0038] According to an embodiment of the present invention, the solvent of the solution of polytelluroxane is one or more mixed solvents selected from ethyl acetate, dichloromethane, chloroform, tetrahydrofuran, 2-hexanone, dimethylformamide and anisole.

[0039] According to an embodiment of the present invention, the concentration of the polytelluroxane solution is 1-50 mg / mL.

[0040] According to an embodiment of the present invention, the concentration of the polytelluroxane solution is 6-20 mg / mL.

[0041] According to an embodiment of the present invention, the polytelluroxane solution is coated on the substrate by using a spin coating method and a coating machine to coat the polytelluroxane solution on the substrate.

[0042] According to an embodiment of the present invention, the spin coating method adopts a rotation speed of 2000-5000 rpm and a time of 20-60 s.

[0043] According to an embodiment of the present invention, the baking temperature is 60-120° C., and the baking time is 1-10 minutes.

[0044] According to an embodiment of the present invention, the UV lithography dose is 1-1000 mJ / cm 2 .

[0045] According to an embodiment of the present invention, the electron beam lithography dose is 1-500 μC / cm 2 .

[0046] According to an embodiment of the present invention, the EUV lithography dose is 1-100 mJ / cm 2 .

[0047] According to an embodiment of the present invention, the developer is one or more mixed solvents selected from isopropyl alcohol, ethanol, methanol and water.

[0048] Another aspect of the present invention provides a process and method for patterning polytelluroxane in UV lithography (I-line, KrF, ArF, etc.), electron beam lithography and EUV lithography, which can be used to transfer the pattern to a photoresist layer. The specific process and method are as follows:

[0049] After cleaning the substrate, a solution of polytelluroxane is applied to the substrate and baked to remove the solvent. The substrate is exposed to UV, electron beam or EUV light at a certain dose and then developed with a developer to obtain a corresponding pattern.

[0050] According to an embodiment of the present invention, acetone and ultrasound are used to clean the substrate.

[0051] According to an embodiment of the present invention, the solvent selected for the solution of polytelluroxane is a mixed solvent of one or more of ethyl acetate, dichloromethane, chloroform, tetrahydrofuran, 2-hexanone, dimethylformamide, and anisole.

[0052] According to an embodiment of the present invention, the concentration of the polytelluroxane solution is 1-50 mg / mL.

[0053] According to an embodiment of the present invention, the concentration of the polytelluroxane solution is 6-20 mg / mL.

[0054] According to an embodiment of the present invention, a spin coating method is adopted to coat the polytelluroxane solution on the substrate using a coating machine.

[0055] According to an embodiment of the present invention, the typical rotation speed used in the spin coating method is 2000-5000 rpm and the time is 20-60 s. Other rotation speeds can also be used to prepare films of different thicknesses.

[0056] According to an embodiment of the present invention, the baking temperature is 60-120° C., and the baking time is 1-10 minutes.

[0057] According to an embodiment of the present invention, the UV lithography (I-line, KrF, ArF, etc.) dose is 1-1000 mJ / cm 2 The electron beam lithography dose is 1-500 μC / cm 2 The EUV lithography dose is 1-100 mJ / cm 2 .

[0058] According to an embodiment of the present invention, the developer is one or more mixed solvents of isopropyl alcohol, ethanol, methanol, and water.

[0059] In another aspect of the present invention, the present invention also provides a method for preparing polytelluroxane:

[0060] One or more organic tellurium ethers are dissolved in an organic solvent, an aqueous hydrogen peroxide solution is added and stirred, and interfacial oxidative polymerization is performed to obtain polytelluroxane.

[0061] According to an embodiment of the present invention, the above method may further include at least one of the following additional technical features:

[0062] According to an embodiment of the present invention, the organic tellurium ether has a structure shown in the general formula (X):

[0063] R1-Te-R2 (X), wherein R1 and R2 are as defined above;

[0064] According to an embodiment of the present invention, R1 and R2 may be connected end to end to form a ring having a structure shown in the general formula (XI):

[0065] Wherein, R4 is the same as defined above.

[0066] According to an embodiment of the present invention, the organic solvent is a mixed solvent of one or more of ethyl acetate, dichloromethane, chloroform and tetrahydrofuran.

[0067] According to an embodiment of the present invention, the concentration of the organic tellurium ether in the organic solvent is 0.1-2 mol / L.

[0068] According to an embodiment of the present invention, the concentration of the aqueous hydrogen peroxide solution is 0.1-5 mol / L.

[0069] According to an embodiment of the present invention, the interface oxidative polymerization reaction temperature is 0-40° C., and the reaction time is 0.5-7 days.

[0070] According to an embodiment of the present invention, the product is separated by dropping an organic solution of the product into a large amount of methanol for precipitation, and methanol is used as a washing agent.

[0071] According to an embodiment of the present invention, the use of a polytelluroxane in a non-chemically amplified photoresist provided by the present invention has at least one of the following characteristics and beneficial effects:

[0072] According to an embodiment of the present invention, compared with the commonly used non-chemically amplified photoresist system, such as PMMA, hydrogenated silsesquioxane HSQ, etc., the non-chemically amplified photoresist based on polytelluroxane introduces the tellurium element with strong EUV absorption capacity into the system, which theoretically greatly increases the material's absorption of EUV, thereby having higher sensitivity. In addition, polytelluroxane has two adjustable side chains R1 and R2, and the polymer structure can be optimized according to the needs of the lithography process, thereby obtaining better lithography performance. For example, the rigid benzene ring is directly introduced to the Te atom, which can increase the rigidity of the Te-O high molecular weight as a whole and reduce the entanglement between the chains, which improves the chain entanglement problem between the exposed part and the unexposed part in the development process.

[0073] The present invention provides a process flow and method for patterning polytelluroxane in UV lithography (I-line, KrF, ArF, etc.), electron beam lithography and EUV lithography, which has at least one of the following characteristics and beneficial effects:

[0074] According to an embodiment of the present invention, the photolithography process based on polytelluroxane is simple and easy to operate. Compared with the traditional chemical amplification photoresist system, there is no complicated pre-baking and post-baking process flow, which greatly shortens the overall time consumption of photolithography and reduces the cost of photolithography process. In addition, the photoresist system based on polytelluroxane can be composed of at least one component, and maintains the good molding and film-forming properties of the polymer. Compared with multi-component photoresist systems such as chemical amplification and metal nanoparticle type, polytelluroxane can more easily obtain a uniform and flat photoresist structure, reducing the generation of random defects. In addition, polytelluroxane is simple to prepare and the raw materials are easily available, so the overall process cost is low and has the application potential of large-scale production.

[0075] Definition and explanation of terms

[0076] Unless otherwise specified, the definitions of groups and terms recorded in the specification and claims of this application, including their definitions as examples, exemplary definitions, preferred definitions, definitions recorded in tables, definitions of specific compounds in examples, etc., can be arbitrarily combined and combined with each other. The definitions of groups and compound structures after such combinations and combinations should be understood to be within the scope of the specification and / or claims of this application.

[0077] In this article, the term "optionally" means that the feature exists or does not exist, which means that the event described later can but does not necessarily occur, thus including two types of situations where the event occurs or does not occur. For example, "optionally a heterocyclic group substituted with an alkyl group" means that the alkyl group can but does not necessarily exist, thus including situations where the heterocyclic group is substituted with an alkyl group and a heterocyclic group is not substituted with an alkyl group.

[0078] As described herein, the compounds of the present invention may contain "optionally substituted" moieties. In general, the term "substituted", whether or not preceded by the term "optionally", means that one or more hydrogens of the specified moiety are replaced by suitable substituents. Unless otherwise indicated, an "optionally substituted" group may have a suitable substituent at each substitutable position of the group, and when multiple positions in any given structure may be substituted by multiple substituents selected from a specified group, the substituents at each position may be the same or different. The combination of substituents contemplated by the present invention is preferably a combination of substituents that allows the formation of stable or chemically feasible compounds. As used herein, the term "stable" refers to a compound that does not substantially change when subjected to conditions that allow it to be manufactured, detected, and in certain embodiments, recovered, purified, and used for one or more purposes disclosed herein.

[0079] Each optional substituent on a substitutable carbon is independently selected from the following monovalent substituents: =O; cyano; C 1-6 Alkyl; C 2-6 Alkenyl; C 2-6 Alkynyl; HaloC 1-6 Alkyl, C 1-6 Alkoxy; Halogen; -(CH2) 0-4 Ro; -(CH2) 0-4 ORo; -O(CH2) 0- 4Ro; -O-(CH2) 0-4 C(O)ORo; -(CH2) 0-4 CH(ORo)2; -(CH2) 0-4 SRo; -(CH2) 0-4 Ph, which may be substituted by Ro; -(CH2) 0-4 O(CH2) 0-1 Ph, which may be substituted by Ro; -CH=CHPh, which may be substituted by Ro; -(CH2) 0-4 O(CH2)0-1-pyridyl, which may be substituted by Ro; -NO2; -CN; -N3; ​​-(CH2) 0-4 N(Ro)2; -(CH2) 0-4 N(Ro)C(O)Ro;-N(Ro)C(S)Ro;-(CH2) 0-4 N(Ro)C(O)NRo2;-N(Ro)C(S)NRo2;-(CH2) 0-4 N(Ro)C(O)-ORo; -N(Ro)N(Ro)C(O)Ro; -N(Ro)N(Ro)C(O)NRo-2; -N(Ro)N(Ro)C(O)ORo; -(CH2) 0-4 C(O)Ro; -C(S)-Ro; -(CH-2) 0-4C(O)ORo; -(CH2) 0-4 C(O)SRo; -(CH2) 0-4 C(O)OSiRo3; -(CH2) 0-4 OC(O)Ro; -OC(O)-(CH-2) 0-4 SR-; SC(S)SRo; -(CH2) 0-4 SC(O)Ro;-(CH2) 0-4 C(O)NRo2;-C(S)NRo2;-C(S)SRo;-SC(S)-SRo;-(CH2) 0- 4OC(O)NRo2; -C(O)N(ORo)Ro; -C(O)C(O)Ro; -C(O)CH2C(O)Ro; -C(NORo)Ro; --(CH2) 0-4 SSRo; -(CH2) 0-4 S(O)2Ro;-(CH2) 0-4 S(O)2ORo; -(CH2) 0-4 OS(O)2Ro;-S(O)2NRo2;-S(O)-(NRo)Ro;-S(O)2NC(NRo2)2;-(CH2) 0-4 S(O)Ro; -N(Ro)S(O)2NRo2; -N(Ro)S(O)2Ro; -N(ORo)Ro; -C(NH)NRo2; -P(O)2Ro; -P(O)Ro2; -OP(O)Ro2; -OP(O)(ORo)2; SiRo3; -(C 1-4 -(straight or branched chain alkylene)ON(Ro)2; or -(C1-4 straight or branched chain alkylene)C(O)ON(Ro)2.

[0080] Each Ro is independently hydrogen, a C1-6 aliphatic group, -CH2Ph, -O(CH2)0-1Ph, -CH2-(5-6 membered heteroaromatic ring) or a 5-6 membered saturated, partially unsaturated or aromatic ring having 0-4 heteroatoms independently selected from nitrogen, oxygen or sulfur, or, regardless of the above definition, two individual occurrences of Ro together with one or more intervening atoms form a 3-12 membered saturated, partially unsaturated or aromatic monocyclic or bicyclic ring having 0-4 heteroatoms independently selected from nitrogen, oxygen or sulfur, which may be substituted on the saturated carbon atoms of Ro by a divalent substituent selected from =O and =S; or each Ro is optionally substituted by a monovalent substituent independently selected from the following: halogen, -(CH2) 0-2 R, -(halogen R), -(CH2) 0-2 OH, -(CH2) 0-2 OR, -(CH2) 0-2CH(OR)2, -CN, -N3, -O(halogen R), -(CH2) 0-2 C(O)R, -(CH2) 0-2 C(O)OH, -(CH2) 0-2 C(O)OR, -(CH2) 0-2 SR·, -(CH2) 0-2 SH, -(CH2) 0-2 NH2, -(CH2) 0-2 NHR, -(CH2) 0-2 NR2, -NO2, -SiR3, -OSiR3, -C(O)SR, -(C 1-4 Straight chain or branched alkylene) C(O)OR or -SSR.

[0081] each R is independently selected from a C1-4 aliphatic group, -CH2Ph, -O(CH2)0-1Ph, or a 5-6 membered saturated, partially unsaturated or aromatic ring having 0-4 heteroatoms independently selected from nitrogen, oxygen or sulfur, and wherein each R is unsubstituted or, in the case of a preceding halogen, is substituted only by one or more halogens; or wherein the optional substituents on the saturated carbon are divalent substituents independently selected from the following: =O, =S, =NNR*2, =NNHC(O)R*, =NNHC(O)OR*, =NNHS(O)2R*, =NR*, =NOR*, -O(C(R*2)) 2-3 O-, or -S(C(R*2)) 2-3 S-, or the divalent substituent attached to the adjacent substitutable carbon of the "optionally substituted" group is -O(CR*2) 2-3 O-, wherein each individual occurrence of R* is selected from hydrogen, C 1-6 an aliphatic group or an unsubstituted 5-6 membered saturated, partially unsaturated or aromatic ring having 0-4 heteroatoms independently selected from nitrogen, oxygen or sulfur.

[0082] When R* is C 1-6 When it is an aliphatic group, R* is optionally substituted by halogen, -R·, -(haloR·), -OH, -OR, -O(haloR), -CN, -C(O)OH, -C(O)OR·, -NH2, -NHR, -NR2 or -NO2, wherein each R· is independently selected from a C1-4 aliphatic group, -CH2Ph, -O(CH2)0-1Ph, or a 5-6-membered saturated, partially unsaturated or aromatic ring having 0-4 heteroatoms independently selected from nitrogen, oxygen or sulfur, and wherein each R· is unsubstituted or, in the case of a halogen group being preceded, is substituted only by one or more halogens.

[0083] Optional substituents on the substitutable nitrogen are independently:

[0084]

[0085] or

[0086] Among them is independently hydrogen, a C1-6 aliphatic group, unsubstituted -OPh, or an unsubstituted 5-6 membered saturated, partially unsaturated or aromatic ring having 0-4 heteroatoms independently selected from nitrogen, oxygen or sulfur, or two single occurrences of Together with one or more of its intervening atoms, it forms an unsubstituted 3-12 membered saturated, partially unsaturated or aromatic monocyclic or bicyclic ring having 0-4 heteroatoms independently selected from nitrogen, oxygen or sulfur; wherein when When it is a C1-6 aliphatic group, Optionally substituted by halogen, -R·, -(haloR·), -OH, -OR·, -O(haloR·), -CN, -C(O)OH, -C(O)OR·, -NH2, -NHR·, -NR·2 or -NO2, wherein each R· is independently selected from a C1-4 aliphatic group, -CH2Ph, -O(CH2)0-1Ph or a 5-6-membered saturated, partially unsaturated or aromatic ring having 0-4 heteroatoms independently selected from nitrogen, oxygen or sulfur, and wherein each R· is unsubstituted or, in the case of a halogen group being preceded, is substituted only by one or more halogens.

[0087] Unless otherwise specified, the numerical ranges recorded in this specification and claims are equivalent to recording at least each specific integer value therein. For example, the numerical range "1-12" is equivalent to recording each integer value in the numerical range "1-12", that is, 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12.

[0088] The term "C 1-20 The term "alkyl" is understood to mean straight-chain and branched alkyl groups having 1 to 20 carbon atoms. 1-12 "Alkyl" means straight chain and branched chain alkyl groups having 1, 2, 3, 4, 5, 6, 7, 8, 8, 9, 10, 11 or 12 carbon atoms. 1-8 "Alkyl" means straight chain and branched chain alkyl groups having 1, 2, 3, 4, 5, 6, 7 or 8 carbon atoms. 1-6 "Alkyl" means straight chain and branched chain alkyl groups having 1, 2, 3, 4, 5 or 6 carbon atoms. 1-4The term "alkyl" refers to straight-chain and branched alkyl groups having 1, 2, 3 or 4 carbon atoms. The alkyl group is, for example, methyl, ethyl, propyl, butyl, pentyl, hexyl, isopropyl, isobutyl, sec-butyl, tert-butyl, isopentyl, 2-methylbutyl, 1-methylbutyl, 1-ethylpropyl, 1,2-dimethylpropyl, neopentyl, 1,1-dimethylpropyl, 4-methylpentyl, 3-methylpentyl, 2-methylpentyl, 1-methylpentyl, 2-ethylbutyl, 1-ethylbutyl, 3,3-dimethylbutyl, 2,2-dimethylbutyl, 1,1-dimethylbutyl, 2,3-dimethylbutyl, 1,3-dimethylbutyl or 1,2-dimethylbutyl or the like or isomers thereof. It may be monovalent (e.g., CH3), divalent (CH2) or polyvalent (e.g., CH4). ).

[0089] The term "C 2-12 "Alkenyl" is understood to mean a linear or branched monovalent hydrocarbon radical containing one or more double bonds and having 2 to 12 carbon atoms. 2-6 "Alkenyl" is understood to mean optionally a linear or branched monovalent hydrocarbon radical containing one or more double bonds and having 2, 3, 4, 5, 6 carbon atoms, in particular 2 or 3 carbon atoms ("C 2-3"alkenyl"), it being understood that, in the case where the alkenyl contains more than one double bond, the double bonds may be separated from one another or conjugated. The alkenyl is, for example, vinyl, allyl, (E)-2-methylvinyl, (Z)-2-methylvinyl, (E)-but-2-enyl, (Z)-but-2-enyl, (E)-but-1-enyl, (Z)-but-1-enyl, pent-4-enyl, (E)-pent-3-enyl, (Z)-pent-3-enyl, -enyl, (E)-pent-2-enyl, (Z)-pent-2-enyl, (E)-pent-1-enyl, (Z)-pent-1-enyl, hex-5-enyl, (E)-hex-4-enyl, (Z)-hex-4-enyl, (E)-hex-3-enyl, (Z)-hex-3-enyl, (E)-hex-2-enyl, (Z)-hex-2-enyl, (E)-hex-1-enyl, (Z)-hex-1-enyl, isopropenyl, 2-hexenyl, (E)-pent-2-enyl, (Z)-pent-2-enyl, (E)-pent-1-enyl, (Z)-pent ...1-enyl, (Z)-pent-1-enyl, isopropenyl, 2-hexenyl, (E)-pent-2- -methylprop-2-enyl, 1-methylprop-2-enyl, 2-methylprop-1-enyl, (E)-1-methylprop-1-enyl, (Z)-1-methylprop-1-enyl, 3-methylbut-3-enyl, 2-methylbut-3-enyl, 1-methylbut-3-enyl, 3-methylbut-2-enyl, (E)-2-methylbut-2-enyl, (Z)-2-methylbut-2-enyl, (E)-1-methylbut-2-enyl The invention can be substituted with vinyl or 1-isopropylvinyl, or a mixture of vinyl and 1-isopropylvinyl. The invention can be substituted with vinyl or 1-isopropylvinyl, or a mixture of vinyl and 1-isopropylvinyl.

[0090] The term "C 2-12The term "alkynyl" is understood as meaning a linear or branched monovalent hydrocarbon radical which contains one or more triple bonds and has 2 to 12 carbon atoms, optionally a "C2-C6-alkynyl" radical. The term "C2-C6-alkynyl" is understood as optionally meaning a linear or branched monovalent hydrocarbon radical which contains one or more triple bonds and has 2, 3, 4, 5, 6 carbon atoms, in particular 2 or 3 carbon atoms ("C2-C3-alkynyl"). The alkynyl radical is, for example, ethynyl, prop-1-ynyl, prop-2-ynyl, but-1-ynyl, but-2-ynyl, but-3-ynyl, pent-1-ynyl, pent-2-ynyl, pent-3-ynyl, pent-4-ynyl, hex-1-ynyl, hex-2-ynyl, hex-3-ynyl, hex-4-ynyl, hex-5-ynyl, 1-methylprop-2-ynyl, 2-methylbut-3-ynyl, 1-methylbut-3-ynyl, 2-methyl -ynyl, 1-methylbut-2-ynyl, 3-methylbut-1-ynyl, 1-ethylprop-2-ynyl, 3-methylpent-4-ynyl, 2-methylpent-4-ynyl, 1-methylpent-4-ynyl, 2-methylpent-3-ynyl, 1-methylpent-3-ynyl, 4-methylpent-2-ynyl, 1-methylpent-2-ynyl, 4-methylpent-1-ynyl, 3-methylpent-1-ynyl, 2-methylpent-4-ynyl, 1-methylpent-4-ynyl, 2-methylpent-3-ynyl, 1-methylpent-3-ynyl, 4-methylpent-2-ynyl, 1-methylpent-2-ynyl, 4-methylpent-1-ynyl, 3-methylpent-1-ynyl, 2 In some embodiments, the alkynyl group is ethynyl, prop-1-ynyl or prop-2-ynyl.

[0091] The term "heteroalkyl" by itself or in combination with another term refers to a stable straight or branched alkyl radical or combination thereof consisting of a certain number of carbon atoms and at least one heteroatom or heteroatom group. In some embodiments, the heteroatom is selected from B, O, N and S, wherein the nitrogen and sulfur atoms are optionally oxidized and the nitrogen heteroatom is optionally quaternized. In other embodiments, the heteroatom group is selected from C(=O)O, C(=O), C(=S), S(=O), S(=O)2, C(=O)N(H), N(H), C(=NH), S(=O)2N(H) and S(=O)N(H). In some embodiments, the heteroalkyl is C 16 In other embodiments, the heteroalkyl group is C 13Heteroalkyl. The heteroatom or heteroatom group may be located at any interior position of the heteroalkyl group, including the position at which the alkyl group is attached to the rest of the molecule, but the terms "alkoxy", "alkylamino" and "alkylthio" (or thioalkoxy) are customary expressions and refer to those alkyl groups that are attached to the rest of the molecule via an oxygen atom, amino group or sulfur atom, respectively. Examples of heteroalkyl groups include, but are not limited to, OCH3, OCH2CH3, OCH2CH2CH3, OCH2(CH3)2, CH2CH2OCH3, NHCH3, N(CH3)2, NHCH2CH3, N(CH3)(CH2CH3), CH2CH2NH CH3, CH2 CH2N(CH3)CH3, SCH3, SCH2CH3, SCH2CH2CH3, SCH2(CH3)2,

[0092] CH2SCH2CH3, CH2CH2, S(=O)CH3, CH2CH2S(=O)2CH3. Up to two

[0093] The heteroatoms may be consecutive, for example CH2NHOCH3.

[0094] The term "heteroalkenyl" by itself or in combination with another term refers to a monovalent hydrocarbon radical consisting of a certain number of carbon atoms and at least one heteroatom or heteroatom group, a stable straight or branched chain alkyl radical or combinations thereof, containing one or more double bonds.

[0095] The term "heteroalkynyl" by itself or in combination with another term refers to a monovalent alkynyl radical of a stable straight or branched chain alkyl radical or combinations thereof consisting of a certain number of carbon atoms and at least one heteroatom or heteroatom group, which contains one or more triple bonds.

[0096] The term "aryl" means a cyclic aromatic hydrocarbon group having 1 to 3 aromatic rings (including monocyclic or bicyclic or tricyclic groups), such as phenyl, biphenyl or naphthyl. When containing two aromatic rings (bicyclic, etc.), the aromatic rings of the aryl group are optionally connected at a single point (e.g., biphenyl) or fused (e.g., naphthyl). The term "C 6-14 The term "aryl" is understood to mean a monovalent aromatic monocyclic, bicyclic or tricyclic hydrocarbon ring ("C 6-14 aryl"), optionally "C 6-12 "Aryl", especially a ring having 6 carbon atoms ("C6 aryl"), such as phenyl; or biphenyl, or a bicyclic ring having 10 carbon atoms ("C 10 aryl), such as naphthyl, or a tricyclic ring having 13 carbon atoms ("C 13 aryl), such as fluorenyl, or a tricyclic ring ("C14 "aryl"), for example anthracenyl. BRIEF DESCRIPTION OF THE DRAWINGS

[0097] The above and / or additional aspects and advantages of the present invention will become apparent and easily understood from the description of the embodiments in conjunction with the following drawings, in which:

[0098] Figure 1 A schematic diagram of the polytelluroxane proposed in the present invention and its application in photolithography;

[0099] Figure 2 1 is a scanning electron microscope image of the EUV lithography pattern of poly-n-butyltelluroxane in Example 1 of the present invention, wherein (a) is a low dose and (b) is a high dose;

[0100] Figure 3 1 is a scanning electron microscope image of the EUV lithography pattern of poly-n-propyltelluroxane in Example 2 of the present invention, wherein (a) is a low dose and (b) is a high dose;

[0101] Figure 4 1 is a scanning electron microscope image of the EUV lithography pattern of polyethyltelluroxane in Example 3 of the present invention, wherein (a) is a low dose and (b) is a high dose;

[0102] Figure 5 1 is a scanning electron microscope image of the EUV lithography pattern of polyphenyl n-butyltelluroxane in Example 4 of the present invention, wherein (a) is a low dose and (b) is a high dose;

[0103] Figure 6 1 is a scanning electron microscope image of the EUV lithography pattern of polyphenyl n-propyl telluroxane in Example 5 of the present invention, wherein (a) is a low dose and (b) is a high dose;

[0104] Figure 7 1 is a scanning electron microscope image of the EUV lithography pattern of polyphenylethyltelluroxane in Example 6 of the present invention, wherein (a) is a low dose and (b) is a high dose;

[0105] Figure 8 (a) Optical microscope image and (b) atomic force microscope image of the UV photolithography (I-line) pattern of polyphenyl n-butyltelluroxane in Example 7 of the present invention;

[0106] Fig. 9 (a) Scanning electron microscope image and (b) cross-sectional scanning electron microscope image of the electron beam lithography pattern of polyphenyl-n-butyltelluroxane in Example 8 of the present invention. DETAILED DESCRIPTION

[0107] The embodiments of the present application are described in detail below, and the examples of the embodiments are shown in the accompanying drawings. The embodiments described below with reference to the accompanying drawings are exemplary and are intended to be used to explain the present invention, and should not be construed as limiting the present invention. In addition, if not explicitly stated, all reagents used in the following embodiments are commercially available, or can be synthesized according to this article or known methods, and for the reaction conditions not listed, they are also easily available to those skilled in the art.

[0108] Example 1: EUV Lithography Patterning of Poly-n-Butyl Telluride

[0109] (1) Dissolve n-butyl telluride (200 mg, 0.827 mmol) in 1 mL of dichloromethane to obtain component A, and dilute 0.5 mL of 30% hydrogen peroxide solution by half to obtain component B. Mix component A and component B thoroughly in a reaction flask, the reaction releases a large amount of heat, and the organic phase changes from yellow to colorless. Continue the reaction for 2 days. After the reaction is completed, separate the organic phase and add it dropwise into 40 mL of methanol to produce a white precipitate. Wash the product with 10 mL of methanol and dry it in an oven at 60°C to obtain a white solid of poly-n-butyl telluroxane, the structure of which is as follows:

[0110] Where n is 150.

[0111] (2) Soak a 1cm*1cm*625μm silicon wafer in acetone, ultrasonically clean it for 10 minutes, blow it dry with nitrogen after cleaning, place it in a 110℃ oven to dry for 10 minutes, and cool it to room temperature for use. Dissolve 6mg of poly-n-butyltelluroxane in 1mL of chloroform and obtain a poly-n-butyltelluroxane film by spin coating. The spin coating speed is 2000-3000rpm and the time is 40 seconds. Dry it at 80℃ for 1 minute to remove the solvent, and obtain a poly-n-butyltelluroxane film with a thickness of 20-30nm.

[0112] (3) Expose the silicon wafer using EUV light with an exposure dose of 1-100 mJ / cm 2 After exposure, the image is developed in a methanol / water mixed solvent, the volume ratio of the developer methanol / water is 1:(0-0.3), and the development time is 45-120 seconds. After development, the corresponding pattern can be obtained.

[0113] Example 2: EUV Lithography Patterning of Poly-n-propyl Telluride

[0114] The difference from Example 1 is that the polytelluroxane has the following structure:

[0115] Where n is 150.

[0116] Example 3: EUV Lithography Patterning of Polyethyltelluroxane

[0117] The difference from Example 1 is that the polytelluroxane has the following structure:

[0118] Where n is 150.

[0119] Example 4: EUV Lithography Patterning of Polyphenyl-n-Butyl Telluride

[0120] The difference from Example 1 is that the polytelluroxane has the following structure:

[0121] Where n is 50.

[0122] Example 5: EUV Lithography Patterning of Polyphenyl-n-propyl Telluride

[0123] The difference from Example 1 is that the polytelluroxane has the following structure:

[0124] Where n is 50.

[0125] Example 6: EUV Lithography Patterning of Polyphenylethyl Telluroxane

[0126] The difference from Example 1 is that the polytelluroxane has the following structure:

[0127] Where n is 50.

[0128] Example 7: UV photolithography (I-line) patterning of polyphenyl n-butyl telluroxane

[0129] (1) Dissolve phenyl n-propyl telluride (200 mg, 0.827 mmol) in 1 mL of dichloromethane to obtain component A, and dilute 0.5 mL of 30% aqueous hydrogen peroxide solution to obtain component B. Mix component A and component B thoroughly in a reaction flask, the reaction releases a large amount of heat, and the organic phase changes from yellow to colorless. Continue the reaction for 2 days. After the reaction is completed, separate the organic phase and add it dropwise into 40 mL of methanol to produce a white precipitate. Wash the product with 10 mL of methanol and dry it in an oven at 60°C to obtain polyphenyl n-propyl telluride as a white solid with the following structure:

[0130] Where n is 50.

[0131] (2) Soak a 1cm*1cm*625μm silicon wafer in acetone, ultrasonically clean it for 10 minutes, blow it dry with nitrogen after cleaning, place it in a 110℃ oven to dry for 10 minutes, and cool it to room temperature for use. Dissolve 30mg of polyphenyl n-propyl telluroxane in 1mL of chloroform and obtain a polyphenyl n-propyl telluroxane film by spin coating. The spin coating speed is 2000-3000rpm and the time is 40 seconds. Dry it at 80℃ for 1 minute to remove the solvent, and obtain a polyphenyl n-propyl telluroxane film with a thickness of 80-100nm.

[0132] (3) Expose the silicon wafer using UV light (I-line) with an exposure dose of 100-1000 mJ / cm 2 After exposure, the image is developed in a methanol / water mixed solvent, the volume ratio of the developer methanol / water is 1:(0-0.3), and the development time is 45-120 seconds. After development, the corresponding pattern can be obtained.

[0133] Example 8: Electron beam lithography patterning of polyphenyl n-butyltelluroxane

[0134] (1) Dissolve phenyl n-propyl telluride (200 mg, 0.827 mmol) in 1 mL of dichloromethane to obtain component A, and dilute 0.5 mL of 30% aqueous hydrogen peroxide solution to obtain component B. Mix component A and component B thoroughly in a reaction flask, the reaction releases a large amount of heat, and the organic phase changes from yellow to colorless. Continue the reaction for 2 days. After the reaction is completed, separate the organic phase and add it dropwise into 40 mL of methanol to produce a white precipitate. Wash the product with 10 mL of methanol and dry it in an oven at 60°C to obtain polyphenyl n-propyl telluride as a white solid with the following structure:

[0135] Where n is 50.

[0136] (2) Soak a 1cm*1cm*625μm silicon wafer in acetone, ultrasonically clean it for 10 minutes, blow it dry with nitrogen after cleaning, place it in a 110℃ oven to dry for 10 minutes, and cool it to room temperature for use. Dissolve 12mg of polyphenyl n-propyl telluroxane in 1mL of chloroform and use spin coating to obtain a polyphenyl n-propyl telluroxane film. The spin coating speed is 2000-3000rpm and the time is 40 seconds. Dry it at 80℃ for 1 minute to remove the solvent, and obtain a polyphenyl n-propyl telluroxane film with a thickness of 40-60nm.

[0137] (3) Expose the silicon wafer using an electron beam with an exposure dose of 1-500 μC / cm 2 After exposure, the image is developed in a methanol / water mixed solvent, the volume ratio of the developer methanol / water is 1:(0-0.3), and the development time is 45-120 seconds. After development, the corresponding pattern can be obtained.

[0138] Analysis of EUV lithography pattern sensitivity and resolution of polytelluroxane:

[0139] The sensitivity of the photoresist can be described by the exposure dose, and the lower the exposure dose, the higher the sensitivity; the resolution of the photoresist can be described by the minimum line width, and the smaller the minimum line width, the higher the resolution. The exposure dose and minimum line width of the EUV lithography patterns of Examples 1-6 are tabulated below, as shown in Table 1 below.

[0140] Table 1

[0141]

[0142] From the above analysis, it can be seen that the EUV exposure dose of the non-chemically amplified photoresist based on polytelluroxane of the present invention is 7.58-32.6 mJ / cm 2 The minimum line width is between 16-30nm. It can be further found that the minimum exposure dose of the non-chemically amplified photoresist based on polytelluroxane described in the present invention is only 7.58mJ / cm 2 Compared with commercial non-chemical amplification photoresist PMMA (about 20mJ / cm 2 ) has higher sensitivity. At the same time, the minimum line width of the non-chemically amplified photoresist based on polytelluroxane described in the present invention can reach 16nm, which has reached the performance of commercial photoresists, especially Examples 2 and 5, which achieve both high sensitivity and high resolution. At the same time, it can be observed that the line pattern has a lower line edge roughness.

[0143] Optical Microscopy and AFM Characterization of UV Lithographic Patterns of Polytelluroxane:

[0144] The UV photolithography (I-line) pattern results of Example 7 were characterized by optical microscopy and atomic force microscopy. The relevant results are as follows: Figure 8 a (UV photolithography (I-line) optical microscope image of polyphenyl n-butyl telluroxane), Figure 8 b (UV lithography (I-line) atomic force microscope image of poly(phenyl-n-butyltelluroxane)). The results show that poly(telluroxane) is feasible for UV lithography and has good UV lithography performance.

[0145] Scanning electron microscopy characterization of electron beam lithography patterns of polytelluroxane:

[0146] The electron beam lithography pattern results of Example 8 were characterized by scanning electron microscopy, and the relevant results are as follows: Fig. 9 a (Electron beam lithography scanning electron microscope image of polyphenyl n-butyl telluroxane), Fig. 9b (Scanning electron microscope image of the electron beam lithographed cross section of poly(phenyl-n-butyltelluroxane). The results show that poly(phenyl-n-butyltelluroxane) is feasible for electron beam lithography and has good electron beam lithography performance.

[0147] In the description of this specification, the description with reference to the terms "one embodiment", "some embodiments", "example", "specific example", or "some examples" etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representations of the above terms do not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described may be combined in any one or more embodiments or examples in a suitable manner. In addition, those skilled in the art may combine and combine the different embodiments or examples described in this specification and the features of the different embodiments or examples, without contradiction.

[0148] Although the embodiments of the present invention have been shown and described above, it is to be understood that the above embodiments are exemplary and are not to be construed as limitations of the present invention. A person skilled in the art may change, modify, replace and vary the above embodiments within the scope of the present invention.

Claims

1. Application of polytelluroxane in non-chemically amplified photoresist, It is characterized in that The polytelluroxane has a Te—O chain.

2. The use according to claim 1, It is characterized in that The polytelluroxane is a polymer composed of monomers having a structure as shown in formula (V), Among them, R 1 , R 2 are independently selected from hydrogen, hydroxyl, amino, thiol, optionally substituted C 1 -C 20 Alkyl, optionally substituted C 2 -C 20 Alkenyl, optionally substituted C 2 -C 20 Alkynyl, optionally substituted C 1 -C 20 Heteroalkyl, optionally substituted C 2 -C 20 Heteroalkenyl, optionally substituted C 2 -C 20 heteroalkynyl, optionally substituted aryl, or having a structure represented by general formula (II), R 3 is selected from hydroxy, amino, cyano, and optionally substituted aryl, and x is any integer between 1 and 20; or R 1 With R 2 are connected together to form a monomer having a structure shown in general formula (VI), R 4 Selected from optionally substituted optionally substituted C 1 -C 8 Alkyl, optionally substituted C 2 -C 8 Alkenyl, optionally substituted C 2 -C 8 Alkynyl, optionally substituted C 1 -C 8 Heteroalkyl, optionally substituted C 2 -C 8 Heteroalkenyl, optionally substituted C 2 -C 8 Heteroalkynyl.

3. The use according to claim 2, It is characterized in that The polytelluroxane has a structure as shown in formula (I): n is any integer between 2 and 5000.

4. The use according to claim 2, It is characterized in that The polytelluroxane has a structure as shown in formula (III): n is any integer between 2 and 5000.

5. The use according to claim 2, It is characterized in that The polytelluroxane has a structure as shown in formula (IV): Where R 1 '、R 1 " are independently selected from R 1 , R 2 '、R 2 " are independently selected from R 2 , m and p are independently any integer between 1 and 5000.

6. The use according to any one of claims 1 to 5, It is characterized in that R 1 , R 2 are independently selected from optionally substituted C 1 -C 12 Alkyl, optionally substituted C 2 -C 12 Alkenyl, optionally substituted C 2 -C 12 alkynyl or optionally substituted aryl; Optionally, R 1 , R 2 are independently selected from optionally substituted C 1 -C 4 Alkyl, optionally substituted C 2 -C 4 Alkenyl, optionally substituted C 2 -C 4 Alkynyl, Optionally, R 1 , R 2 are independently selected from optionally substituted C 1 -C 4 Alkyl, optionally substituted C 2 -C 4 Alkenyl, optionally substituted C 2 -C 4 Alkynyl; Optionally, R 1 is phenyl, R 2 C 1 -C 4 Alkyl, C 2 -C 4 Alkenyl or C 2 -C 4 Alkynyl.

7. The use according to any one of claims 1 to 6, It is characterized in that The polytelluroxide is n is 150; Optionally, the polytelluroxane is n is 150; Optionally, the polytelluroxane is n is 150; Optionally, the polytelluroxane is n is 50; Optionally, the polytelluroxane is n is 50; Optionally, the polytelluroxane is n is 50.

8. The use according to any one of claims 1 to 7, It is characterized in that The application is implemented in the following way: After cleaning the substrate, a solution of polytelluroxane is applied to the substrate, and the solvent is removed by baking. The substrate is subjected to UV lithography, electron beam lithography or EUV lithography, and then developed using a developer to obtain a corresponding pattern.

9. The use according to claim 8, It is characterized in that The material of the substrate is germanium, silicon, silicon carbide, silicon nitride, gallium arsenide or gallium nitride; Optionally, the cleaning of the substrate is performed by using acetone and ultrasound to clean the substrate; Optionally, the solvent of the solution of polytelluroxane is one or more mixed solvents selected from ethyl acetate, dichloromethane, chloroform, tetrahydrofuran, 2-hexanone, dimethylformamide and anisole; Optionally, the concentration of the polytelluroxane solution is 1-50 mg / mL; Preferably, the concentration of the polytelluroxane solution is 6-20 mg / mL.

10. The use according to claim 8, It is characterized in that The polytelluroxane solution is applied on the substrate by using a spin coating method and a coating machine to apply the polytelluroxane solution on the substrate; Optionally, the spin coating method uses a rotation speed of 2000-5000 rpm and a time of 20-60 s; Optionally, the baking temperature is 60-120° C. and the time is 1-10 minutes; Optionally, the UV photolithography dose is 1-1000 mJ / cm 2 ; Optionally, the electron beam lithography dose is 1-500 μC / cm 2 ; Optionally, the EUV lithography dose is 1-100 mJ / cm 2 ; Optionally, the developer is one or more mixed solvents selected from isopropyl alcohol, ethanol, methanol and water.

Citation Information

Patent Citations

  • Photosensitive composition

    JP1977019516A

  • Composition for forming resist underlayer film, lithography underlayer film using same, pattern forming method, compound, and method for producing same

    WO2017188450A1

  • Tellurium-containing polymer and compound

    WO2023214589A1

Cited By

  • Use of polytelluoxane in non-chemically amplified photoresist

    WO2026056241A1