Method for etching RF LDMOS Faraday shield dielectric layer
By using plasma bombardment and ashing processes to remove tungsten-containing polymers during the etching of the GSDO Faraday shielding cover dielectric layer, the problem of difficult polymer removal during overetching is solved, the risk of subsequent process is reduced and the loss of tungsten metal is avoided. A more stable process flow is achieved.
Patent Information
- Application Number
- CN202410958057.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-17
- Publication Date
- 2024-11-12
AI Technical Summary
During the etching of the GSDO Faraday shield, the large amount of W-containing polymers generated during overetching are difficult to remove, which affects the subsequent process process, and the chemical cleaning step using CF4 will lead to excessive W loss.
An RFLDMOS Faraday shielding cover dielectric layer etching method is adopted, including forming a gate structure and a Faraday shielding layer on the substrate, forming a shielding cover structure through photolithography and etching processes, and removing tungsten-containing polymerization using plasma bombardment and ashing processes. The substance is then subjected to a wet cleaning to remove by-products.
It effectively solves the problem that tungsten-containing polymers produced by overetching are difficult to remove, reduces the risk of subsequent process failure, and avoids excessive loss of tungsten metal.
Smart Images

Figure CN118943012A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of semiconductor technology, and in particular to a method for etching a dielectric layer of an RFLDMOS Faraday shield. Background Art
[0002] During the GSDO (Faraday shield interconnect oxide) etching process, the etching stops on W (tungsten). A large amount of W-containing polymers produced during the over-etching process are wrapped on the surface of the photoresist. The W-containing polymers cannot be removed by using ordinary O2 etching, resulting in the inability to remove the photoresist. The chemical cleaning step containing CF4 can remove the W-containing polymers, but it will cause excessive W loss.
[0003] In order to solve the above problems, it is necessary to propose a novel method for etching the dielectric layer of the RFLDMOS Faraday shield. Summary of the invention
[0004] In view of the above-mentioned shortcomings of the prior art, the purpose of the present invention is to provide a method for etching the dielectric layer of an RFLDMOS Faraday shield, which is used to solve the problem in the prior art that a large amount of W-containing polymer generated during the over-etching process is wrapped on the surface of the photoresist, which is difficult to remove and affects the subsequent process.
[0005] To achieve the above-mentioned object and other related objects, the present invention provides a method for etching a dielectric layer of a RFLDMOS Faraday shield, comprising:
[0006] Step 1: providing a substrate, wherein a drift region and a body region are provided in the substrate;
[0007] The drift region is provided with a drain region of the RFLDMOS, the body region is provided with a heavily doped region and a source region of the RFLDMOS, and the heavily doped region is connected to the source region of the RFLDMOS;
[0008] forming a gate structure of the RFLDMOS on the surface of the substrate; and forming a first dielectric layer covering the gate structure on the substrate;
[0009] forming a Faraday shielding layer above the dielectric layer, wherein the Faraday shielding layer comprises a tungsten metal layer;
[0010] Forming a Faraday shield structure by photolithography and etching processes, wherein the Faraday shield structure is located above a portion of the gate structure close to the drain region and above a portion of the drift region close to the gate structure;
[0011] forming a second dielectric layer on the substrate covering the Faraday shield structure and the first dielectric layer;
[0012] Step 2, forming an anti-reflection coating covering the two dielectric layers, forming a photoresist layer on the anti-reflection coating, and photolithographically opening the photoresist layer so that a portion of the anti-reflection coating below the photoresist layer is exposed, so as to define the position of a through hole for leading out the Faraday shield structure;
[0013] Step 3: etching the exposed anti-reflective coating layer and the second dielectric layer thereunder to the tungsten metal layer, so that a tungsten-containing polymer is formed on the upper surface of the photoresist layer and the side walls of the photoresist layer, the anti-reflective coating layer and the second dielectric layer after etching;
[0014] Step 4, bombarding the tungsten-containing polymer on the upper surface of the photoresist layer with plasma to make it loose;
[0015] Step 5: using an ashing process to remove the remaining anti-reflective coating and photoresist layer, and then using a wet cleaning method to remove the byproducts of the ashing process and the remaining tungsten polymer.
[0016] Preferably, the gate structure in step 1 is composed of a gate dielectric layer and a gate polysilicon layer stacked in sequence.
[0017] Preferably, the Faraday shielding layer in step 1 further includes a barrier layer located below the tungsten metal layer.
[0018] Preferably, the barrier layer in step one comprises titanium and titanium nitride.
[0019] Preferably, the method for forming the Faraday shielding layer in step 1 comprises: depositing a titanium metal layer on the second dielectric layer; depositing a titanium nitride layer; and depositing a tungsten metal layer.
[0020] Preferably, in step one, the substrate is P-type, the drift region is N-type, the body region is P-type, and the heavily doped region within the body region is N-type; or, the substrate is N-type, the drift region is P-type, the body region is N-type, and the heavily doped region within the body region is P-type.
[0021] Preferably, the substrate in step 1 comprises a bulk semiconductor substrate or a silicon-on-insulator (SOI) substrate.
[0022] Preferably, the through hole in step 2 is located above a portion of the gate structure close to the drain region.
[0023] Preferably, the etching in step three is dry etching, and the etching gas includes fluorine-containing gas and oxygen.
[0024] Preferably, in step three, the gas flow rate of the fluorine-containing gas is 5-20 sccm, and the gas flow rate of O2 is 5-20 sccm.
[0025] Preferably, the process conditions for loosening the tungsten-containing polymer on the upper surface of the photoresist layer by plasma bombardment in step 4 include: introducing Ar and O2 into the cavity, the gas flow rate of Ar is 300-600sccm, the gas flow rate of O2 is 10-50sccm, the power is 600-1500W, the cavity pressure is 20mT-40mT, and the processing time is 15-60s.
[0026] Preferably, the method of removing the remaining anti-reflective coating and photoresist layer by using an ashing process in step 4 includes: using O2 as an etching gas, the temperature of the ashing process is 130-180°C, and the processing time is 30-300s.
[0027] As described above, the method for etching the dielectric layer of the RFLDMOS Faraday shield of the present invention has the following beneficial effects:
[0028] The present invention can solve the problem that the subsequent process has a risk of failure due to the excessively heavy tungsten-containing polymer produced by etching. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] Figure 1 Shown is a schematic diagram of the process flow of the present invention;
[0030] Figure 2 It is a schematic diagram showing the formation position of a through hole defined by photolithography of the present invention;
[0031] Figure 3 It is a schematic diagram showing the etching method for forming a tungsten-containing polymer according to the present invention;
[0032] Figure 4 Shown is a schematic diagram of bombarding a tungsten-containing polymer according to the present invention;
[0033] Figure 5 Shown is a schematic diagram of the ashing process of the present invention;
[0034] Figure 6 Shown is a schematic diagram of wet cleaning of the present invention. DETAILED DESCRIPTION
[0035] The following describes the embodiments of the present invention through specific examples, and those skilled in the art can easily understand other advantages and effects of the present invention from the contents disclosed in this specification. The present invention can also be implemented or applied through other different specific embodiments, and the details in this specification can also be modified or changed in various ways based on different viewpoints and applications without departing from the spirit of the present invention.
[0036] See also Figure 1 The present invention provides a method for etching a dielectric layer of an RFLDMOS Faraday shield, comprising:
[0037] Step 1: providing a substrate 101, wherein the substrate 101 is provided with a drift region and a body region;
[0038] A drain region of the RFLDMOS is arranged in the drift region, a heavily doped region and a source region of the RFLDMOS are arranged in the body region, and the heavily doped region is connected to the source region of the RFLDMOS;
[0039] A gate structure 102 of RFLDMOS is formed on a surface of a substrate 101 ; a first dielectric layer 103 covering the gate structure 102 is formed on the substrate 101 ;
[0040] forming a Faraday shielding layer on the dielectric layer, wherein the Faraday shielding layer comprises a tungsten metal layer;
[0041] A Faraday shield structure 104 is formed by photolithography and etching processes, and the Faraday shield structure 104 is located above a portion of the gate structure 102 close to the drain region and above a portion of the drift region close to the gate structure 102;
[0042] A second dielectric layer 105 covering the Faraday shield structure 104 and the first dielectric layer 103 is formed on the substrate 101; the material of the second dielectric layer 105 of the first dielectric layer 103 may be an oxide layer;
[0043] In some embodiments, the gate structure 102 in step 1 is composed of a gate dielectric layer and a gate polysilicon layer stacked in sequence.
[0044] In some embodiments, the Faraday shielding layer in step 1 further includes a barrier layer located below the tungsten metal layer.
[0045] In some embodiments, the barrier layer in step one includes titanium and titanium nitride.
[0046] In some embodiments, the method for forming the Faraday shielding layer in step 1 includes: depositing a titanium metal layer on the second dielectric layer 105; depositing a titanium nitride layer; and depositing a tungsten metal layer.
[0047] In some embodiments, the substrate 101 in step one is P-type, the drift region is N-type, the body region is P-type, and the heavily doped region in the body region is N-type; or, the substrate 101 is N-type, the drift region is P-type, the body region is N-type, and the heavily doped region in the body region is P-type.
[0048] In some embodiments, the substrate 101 in step one includes a bulk semiconductor substrate or a silicon-on-insulator (SOI) substrate. The SOI substrate includes an insulator layer located below a thin semiconductor layer that is an active layer of the SOI substrate. The semiconductor of the active layer and the bulk semiconductor typically include crystalline semiconductor material silicon, but may also include one or more other semiconductor materials, such as germanium, silicon-germanium alloys, compound semiconductors (e.g., GaAs, AlAs, InAs, GaN, AlN, etc.) or their alloys (e.g., GaxAl1-xAs, GaxAl1-xN, InxGa1-xAs, etc.), oxide semiconductors (e.g., ZnO, SnO2, TiO2, Ga2O3, etc.) or combinations thereof. The semiconductor material may be doped or undoped. Other substrates that may be used include multilayer substrates, gradient substrates, or mixed orientation substrates.
[0049] Step 2: forming an anti-reflection coating 106 covering the second dielectric layer, forming a photoresist layer 107 on the anti-reflection coating 106, and photolithographically opening the photoresist layer 107 so that a portion of the anti-reflection coating 106 thereunder is exposed, so as to define the position of the through hole for leading out the Faraday shield structure 104;
[0050] In some embodiments, the through hole in step 2 is located above a portion of the gate structure 102 close to the drain region.
[0051] Step 3: Etching the exposed anti-reflective coating 106 and the second dielectric layer 105 thereunder to the tungsten metal layer, and forming a tungsten-containing polymer 108 on the upper surface of the photoresist layer 107 and the sidewalls of the photoresist layer 107, the anti-reflective coating 106, and the second dielectric layer 105 after etching;
[0052] In some embodiments, the etching in step three is dry etching, and the etching gas includes fluorine-containing gas and oxygen.
[0053] In some embodiments, the gas flow rate of the fluorine-containing gas in step three is 5-20 sccm, and the gas flow rate of O2 is 5-20 sccm.
[0054] Step 4: bombarding the tungsten-containing polymer 108 on the upper surface of the photoresist layer 107 with plasma to make it loose;
[0055] In some embodiments, the process conditions for loosening the tungsten-containing polymer 108 on the upper surface of the photoresist layer 107 by plasma bombardment in step four include: introducing Ar and O2 into the chamber, the gas flow rate of Ar is 300-600sccm, the gas flow rate of O2 is 10-50sccm, the power is 600-1500W, the chamber pressure is 20mT-40mT, and the processing time is 15-60s.
[0056] In some embodiments, the method of removing the remaining anti-reflective coating 106 and the photoresist layer 107 by a low-temperature ashing process in step 4 includes: using O2 as an etching gas, the ashing process temperature is 130-180°C, and the processing time is 30-300s.
[0057] Step 5: Use an ashing process to remove the remaining anti-reflective coating 106 and the photoresist layer 107, and then use a wet cleaning method to remove the byproducts of the ashing process and the remaining tungsten polymer.
[0058] It should be noted that the illustrations provided in this embodiment are only used to illustrate the basic concept of the present invention in a schematic manner. Therefore, the drawings only show components related to the present invention rather than being drawn according to the number, shape and size of components in actual implementation. In actual implementation, the type, quantity and proportion of each component may be changed arbitrarily, and the component layout may also be more complicated.
[0059] In summary, the present invention can solve the problem of the risk of failure of subsequent processes caused by etching producing excessively heavy tungsten-containing polymers. Therefore, the present invention effectively overcomes various shortcomings of the prior art and has high industrial utilization value.
[0060] The above embodiments are merely illustrative of the principles and effects of the present invention, and are not intended to limit the present invention. Anyone familiar with the art may modify or alter the above embodiments without departing from the spirit and scope of the present invention. Therefore, all equivalent modifications or alterations made by a person of ordinary skill in the art without departing from the spirit and technical concept disclosed by the present invention shall still be covered by the claims of the present invention.
Claims
1. A method for etching a dielectric layer of a RFLDMOS Faraday shield, It is characterized in that At least: Step 1, providing a substrate, wherein a drift region and a body region are provided in the substrate; The drift region is provided with a drain region of the RFLDMOS, the body region is provided with a heavily doped region and a source region of the RFLDMOS, and the heavily doped region is connected to the source region of the RFLDMOS; forming a gate structure of the RFLDMOS on the surface of the substrate; and forming a first dielectric layer covering the gate structure on the substrate; forming a Faraday shielding layer above the dielectric layer, wherein the Faraday shielding layer comprises a tungsten metal layer; Forming a Faraday shield structure by photolithography and etching processes, wherein the Faraday shield structure is located above a portion of the gate structure close to the drain region and above a portion of the drift region close to the gate structure; forming a second dielectric layer on the substrate covering the Faraday shield structure and the first dielectric layer; Step 2, forming an anti-reflection coating covering the two dielectric layers, forming a photoresist layer on the anti-reflection coating, and photolithographically opening the photoresist layer so that a portion of the anti-reflection coating below the photoresist layer is exposed, so as to define the position of a through hole for leading out the Faraday shield structure; Step 3: etching the exposed anti-reflective coating layer and the second dielectric layer thereunder to the tungsten metal layer, so that a tungsten-containing polymer is formed on the upper surface of the photoresist layer and the side walls of the photoresist layer, the anti-reflective coating layer and the second dielectric layer after etching; Step 4, bombarding the tungsten-containing polymer on the upper surface of the photoresist layer with plasma to make it loose; Step 5: using an ashing process to remove the remaining anti-reflective coating and photoresist layer, and then using a wet cleaning method to remove the byproducts of the ashing process and the remaining tungsten polymer.
2. The method for etching the dielectric layer of the RFLDMOS Faraday shield according to claim 1, Features: The gate structure in step 1 is composed of a gate dielectric layer and a gate polysilicon layer stacked in sequence.
3. The method for etching the dielectric layer of the RFLDMOS Faraday shield according to claim 1, Features: The Faraday shielding layer in step 1 further includes a barrier layer located below the tungsten metal layer.
4. The method for etching the dielectric layer of the RFLDMOS Faraday shield according to claim 3, Features: The barrier layer in step one includes titanium and titanium nitride.
5. The method for etching the dielectric layer of the RFLDMOS Faraday shield according to claim 4, Features: The method for forming the Faraday shielding layer in step 1 includes: depositing a titanium metal layer on the second dielectric layer; depositing a titanium nitride layer; and depositing a tungsten metal layer.
6. The method for etching the dielectric layer of the RFLDMOS Faraday shield according to claim 1, Features: In step 1, the substrate is P-type, the drift region is N-type, the body region is P-type, and the heavily doped region in the body region is N-type; or, the substrate is N-type, the drift region is P-type, the body region is N-type, and the heavily doped region in the body region is P-type.
7. The method for etching the dielectric layer of the RFLDMOS Faraday shield according to claim 1, Features: The substrate in step 1 includes a bulk semiconductor substrate or a silicon-on-insulator (SOI) substrate.
8. The method for etching the dielectric layer of the RFLDMOS Faraday shield according to claim 1, Features: The through hole in step 2 is located above a portion of the gate structure close to the drain region.
9. The method for etching the dielectric layer of the RFLDMOS Faraday shield according to claim 1, Features: The etching in step three is dry etching, and the etching gas includes fluorine-containing gas and oxygen.
10. The method for etching the dielectric layer of the RFLDMOS Faraday shield according to claim 9, Features: In step 3, the gas flow rate of the fluorine-containing gas is 5-20 sccm, and the gas flow rate of O2 is 5-20 sccm.
11. The method for etching the dielectric layer of the RFLDMOS Faraday shield according to claim 1, Features: The process conditions for loosening the tungsten-containing polymer on the upper surface of the photoresist layer by plasma bombardment in step 4 include: introducing Ar and O2 into the chamber, the gas flow rate of Ar is 300-600sccm, the gas flow rate of O2 is 10-50sccm, the power is 600-1500W, the chamber pressure is 20mT-40mT, and the processing time is 15-60s.
12. The method for etching the dielectric layer of the RFLDMOS Faraday shield according to claim 1, Features: The method of removing the remaining anti-reflective coating and photoresist layer by using an ashing process in step 4 includes: using O2 as an etching gas, the temperature of the ashing process is 130-180°C, and the processing time is 30-300s.