Solar cell preparation method, solar cell and photovoltaic module

By optimizing the angle position between silicon wafer and airflow in solar cells, a high-quality doped polysilicon layer and glass layer is formed, which solves the problem of poor alkali resistance of phosphorus silicon or borosilicon glass layers, and improves battery efficiency and resistance Corrosiveness reduces leakage.

CN118943251APending Publication Date: 2024-11-12LONGI GREEN ENERGY TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411018952.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-26
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

Existing solar cells have poor alkali resistance in the phosphorus silicon glass layer or borosilicate glass layer, which leads to corrosion of the polysilicon layer and affects battery efficiency and leakage problems.

Method used

By forming a tunnel oxide layer and an intrinsic amorphous silicon layer on the silicon wafer and performing a diffusion doping process at different locations, a doped polysilicon layer and glass layer are formed, and the glass layer is used as a mask for removal, so that the silicon wafer and The angle position of the airflow is to improve the density and corrosion resistance of the glass layer.

Benefits of technology

The corrosion resistance of the glass layer is improved, the quality of the doped polysilicon layer is ensured, the leakage is reduced, and the electrical performance and battery efficiency of the solar cell are significantly improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118943251A_ABST
    Figure CN118943251A_ABST
Patent Text Reader

Abstract

The invention discloses a solar cell preparation method, a solar cell and a photovoltaic module, and relates to the technical field of solar cells, and the solar cell preparation method comprises the steps: placing a silicon wafer at a first position, sequentially forming a tunneling oxide layer and an intrinsic amorphous silicon layer, and enabling the clamping degree of the silicon wafer relative to the horizontal plane to be alpha at the first position; and the silicon wafer is placed at a second position, diffusion doping is carried out on the intrinsic amorphous silicon layer to form a doped polycrystalline silicon layer and a glass layer, the clamping degree of the silicon wafer relative to the horizontal plane is beta at the second position, and alpha is smaller than beta. In the process of forming the intrinsic amorphous silicon layer, the placement of the silicon wafer is closer to the airflow flowing direction of the furnace tube, so that by-products of the intrinsic amorphous silicon layer can be conveniently extracted, and the film forming quality of the intrinsic amorphous silicon layer is improved. And in the diffusion doping process, the placement of the silicon wafer is closer to the direction perpendicular to the flowing direction of the airflow, so that the retention time of O2 on the surface in the oxidation process is longer, the compactness of the glass layer is increased, and the alkali corrosion resistance of the glass layer is remarkably enhanced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of solar cells, and in particular to a method for preparing a solar cell, a solar cell and a photovoltaic module. Background Art

[0002] For solar silicon cells such as AL-BSF (Aluminum Back Surface Field), PERC (Passivated Emitter and Rear Cell), and Topcon (Tunnel Oxide Passivated Contact), the phosphorus-silicon glass layer (PSG) produced during the phosphorus diffusion process or the borosilicate glass layer (BSG) produced during the boron diffusion process will be directly removed by pickling, while for BC (Back Contact) cells, the phosphorus-silicon glass layer or borosilicate glass layer can be used as a mask layer to shorten the process flow and cost. However, in the subsequent wet etching process, if the alkali resistance of PSG or BSG is poor, the underlying polysilicon layer (Polysilicon layer) will be corroded, resulting in cell efficiency loss and serious leakage. Therefore, it is crucial to improve the alkali resistance of PSG or BSG to improve the quality of the polysilicon layer. Summary of the invention

[0003] The object of the present invention is to provide a method for preparing a solar cell, a solar cell and a photovoltaic module, which can improve the corrosion resistance of a glass layer, thereby improving the quality of a polysilicon layer.

[0004] In order to achieve the above object, the present invention provides the following technical solutions:

[0005] In a first aspect, the present invention provides a method for preparing a solar cell, comprising:

[0006] Placing the silicon wafer in a first position to sequentially form a tunnel oxide layer and an intrinsic amorphous silicon layer; in the first position, the angle between the silicon wafer and the horizontal plane is α;

[0007] Placing the silicon wafer in a second position, diffusing the intrinsic amorphous silicon layer to form a doped polysilicon layer and a glass layer; in the second position, the angle between the silicon wafer and the horizontal plane is β; wherein α is less than β;

[0008] A portion of the glass layer is removed, and the remaining glass layer is used as a mask to remove the doped polysilicon layer not covered by the glass layer using an etching solution.

[0009] When the above technical solution is adopted, in the deposition process, the silicon wafer is placed in the first position, at which the angle of the silicon wafer relative to the horizontal plane is α, and a tunneling oxide layer and an intrinsic amorphous silicon layer are formed on the silicon wafer in sequence. After that, the silicon wafer is placed in the second position for processing in the diffusion doping process, at which the angle of the silicon wafer relative to the horizontal plane is β, and doping is performed to form a doped polysilicon layer and a glass layer. Finally, part of the glass layer is removed, and the remaining glass layer is used as a mask to remove the doped polysilicon layer not covered by the glass layer through an etching solution. During the entire process, α is less than β, so in the process of forming the intrinsic amorphous silicon layer, the silicon wafer is placed in the first position, which is closer to the airflow direction of the furnace tube, which is conducive to extracting the byproducts of the intrinsic amorphous silicon layer with poor adsorption in the deposition process, and improving the film quality of the intrinsic amorphous silicon layer. In the diffusion doping process, the silicon wafer is placed in the second position, which is closer to being arranged in the vertical airflow direction. At this time, the O 2 The longer the stay time on the silicon wafer surface, the more effectively the gaps in the glass layer, such as the PSG or BSG film layer, can be filled, thereby increasing the compactness of the glass layer and improving the corrosion resistance of the glass layer. In this way, when the glass layer is used as a mask to remove part of the polysilicon layer and the tunnel oxide layer using the etching liquid, due to the high film quality of the intrinsic amorphous silicon layer, that is, the high film quality of the formed doped polysilicon layer, and the improved corrosion resistance of the glass layer, the etching liquid can be prevented from destroying the doped polysilicon layer covered by the glass layer, ensuring that the quality of the doped polysilicon layer finally retained is high, thereby preventing leakage and improving battery efficiency.

[0010] Optionally, in the above-mentioned solar cell preparation method, 0°≤α≤30°; and / or, 60°≤β≤90°. In this way, the silicon wafer placed in the first position is arranged closer to the horizontal direction, and when the value of α is greater than this angle range, the silicon wafer contacts a larger air flow cross section in the furnace tube, which leads to the discharge of by-products that are not conducive to the intrinsic amorphous silicon layer, affecting the film formation quality of the intrinsic amorphous silicon layer. During the diffusion doping process, the silicon wafer placed in the second position is arranged closer to the vertical horizontal direction, and when the value of β is less than the angle range, the silicon wafer in the second position has poor verticality with the airflow, resulting in a reduction in the contact area between the silicon wafer and the airflow cross section, and the O in the received airflow is reduced. 2 becomes smaller, and the O 2 The residence time on the silicon wafer surface is too short, resulting in insufficient oxidation on the surface of the doped polysilicon layer, making it impossible to effectively fill the gaps in the PSG or BSG film layer, reducing the density of the glass layer and affecting the corrosion resistance. Therefore, considering the film quality of the intrinsic amorphous silicon layer and the corrosion resistance of the glass layer, 0°≤α≤30° and 60°≤β≤90° are selected.

[0011] Optionally, in the above-mentioned solar cell preparation method, 0°≤α≤10°; and / or, 80°≤β≤90°. By setting α within the angle range of 0°-10°, the silicon wafer arranged in the first position is closer to parallel with the airflow direction in the furnace tube, which is more conducive to improving the discharge of byproducts of the intrinsic amorphous silicon layer and improving the film formation quality of the intrinsic amorphous silicon layer. Setting β within the angle range of 80°-90° makes the silicon wafer placed in the second position more perpendicular to the airflow direction, further increasing the contact area between the silicon wafer and the airflow cross section, and further increasing the O 2 The longer residence time on the silicon wafer surface can more effectively fill the gaps in the PSG or BSG film layer, which is more conducive to improving the density of the glass layer and thus improving the corrosion resistance of the glass layer.

[0012] Optionally, in the above-mentioned solar cell preparation method, the silicon wafer is placed in the first position, and a tunneling oxide layer and an intrinsic amorphous silicon layer are sequentially formed by a low-pressure chemical vapor deposition process. In this way, a uniform, high-quality intrinsic amorphous silicon layer can be obtained at a lower temperature by a low-pressure chemical vapor deposition process, with a high deposition rate and high deposition accuracy.

[0013] Optionally, in the above-mentioned solar cell preparation method, placing the silicon wafer in the first position, and sequentially forming a tunneling oxide layer and an intrinsic amorphous silicon layer, comprises:

[0014] Inserting the silicon wafer into the wafer boat at the first position, and moving the wafer boat into a furnace tube of a low-pressure chemical vapor deposition device;

[0015] At a first preset temperature, a first preset volume flow rate of O is introduced into the furnace tube. 2 , so as to form a tunneling oxide layer on the surface of the silicon wafer;

[0016] A second preset volume flow rate of SiH2O2 is introduced into the furnace tube at a second preset temperature. 4 , so as to form an intrinsic amorphous silicon layer on the tunnel oxide layer.

[0017] In the case of adopting the above technical solution, the silicon wafer is inserted into the wafer carrier boat at the first position, the first position of the silicon wafer is fixed by the wafer carrier boat, and the silicon wafer is sent into the furnace tube of the low-pressure chemical vapor deposition equipment, and a tunneling oxide layer and an intrinsic amorphous silicon layer are sequentially formed on the silicon wafer. The silicon wafer is inserted in the wafer carrier boat in a manner that is approximately horizontal, so that the SiH 4 The decomposition reaction process is conducive to the extraction of byproducts of the intrinsic amorphous silicon layer with poor adsorption, so that the film formation quality of the intrinsic amorphous silicon layer is improved.

[0018] Optionally, in the above-mentioned solar cell preparation method, placing the silicon wafer at the second position, diffusing the intrinsic amorphous silicon layer to form the doped polysilicon layer and the glass layer, comprises:

[0019] Inserting the silicon wafer into a wafer boat at the second position, and moving the wafer boat into a furnace tube of a diffusion and doping device;

[0020] At a third preset temperature, a third preset volume flow rate of O is introduced into the furnace tube. 2 、N 2 and a diffusion doping source containing a doping element to be diffused;

[0021] At a fourth preset temperature, a fourth preset volume flow rate of O is introduced into the furnace tube. 2 , and controlling the cooling time to promote the diffusion doping source to continue to diffuse into the intrinsic amorphous silicon layer to form the doped polysilicon layer and the glass layer.

[0022] When the above technical solution is adopted, the silicon wafer is inserted into the wafer carrier boat at the second position, the second position of the silicon wafer is fixed by the wafer carrier boat, and the silicon wafer is sent to the furnace tube of the diffusion doping equipment, and the doped polysilicon layer is formed by diffusion doping and the glass layer is formed by simultaneous oxidation. By inserting the silicon wafer on the wafer carrier boat in a manner similar to vertical, the silicon wafer is arranged closer to the vertical airflow direction, and the oxidation process in the diffusion doping process is increased. 2 The residence time on the silicon wafer surface improves the density of the glass layer formed by oxidation, thereby improving the corrosion resistance of the glass layer.

[0023] In a second aspect, the present invention further provides a solar cell, comprising:

[0024] Silicon substrate;

[0025] A tunneling oxide layer is disposed on a partial area of ​​the silicon substrate;

[0026] A doped polysilicon layer is disposed on the tunnel oxide layer, wherein the doped polysilicon layer has micrometer-scale holes penetrating the doped polysilicon layer, and the average density of the holes is less than 5 / mm 2 .

[0027] Compared with the prior art, the doped polysilicon layer in the solar cell provided in the present application has a small hole density, so the molding quality is high, the corrosion resistance is strong, the defects are small, the carrier recombination is reduced, the conductivity and carrier lifetime are improved, the electrical performance of the solar cell is significantly improved, the battery efficiency is improved, and the leakage is reduced.

[0028] Optionally, in the above solar cell, the maximum size of the hole, that is, the distance between the two points on the hole that are farthest apart, is greater than 0 and less than 5 μm. It can be seen that the hole size formed is small, the defects are small, the carrier recombination is reduced, the conductivity and carrier life are improved, the electrical performance of the solar cell is significantly improved, the battery efficiency is improved, and the leakage is reduced.

[0029] Optionally, in the above solar cell, the maximum size range of the hole is 2um to 4um. In order to avoid the hole size being too small, which increases the difficulty of forming the hole, and to avoid the hole size being too large, which leads to serious carrier recombination, the embodiment of the present application chooses to set the maximum size range of the hole to 2um to 4um.

[0030] Optionally, in the above-mentioned solar cell, the depth of the hole ranges from 1 μm to 5 μm. It is understandable that if the depth of the hole is shallow, it only penetrates the doped polysilicon layer. If the depth of the hole is deep, it can penetrate the doped polysilicon layer and the tunnel oxide layer, and even extend into the surface of the silicon substrate. Considering that if the depth of the hole is small, it will increase the difficulty of forming the hole, and if the depth of the hole is large, the silicon substrate will be removed more, reducing the photoelectric conversion efficiency, the embodiment of the present application chooses to set the depth of the hole to range from 1 μm to 5 μm.

[0031] Optionally, in the above solar cell, the average density of the holes at the edge of the silicon substrate is greater than the average density of the holes at the middle of the silicon substrate. In this way, the average density of the holes at the edge of the silicon substrate is relatively large, which is beneficial to increase the contact area between the soldering ribbon and the battery cell when the soldering ribbon is welded at the edge of the silicon substrate, thereby increasing the welding strength between the soldering ribbon and the battery cell, and it is not easy for the soldering ribbon to separate from the battery cell.

[0032] Optionally, in the above-mentioned solar cell, the solar cell is a bifacial cell, and the tunneling oxide layer and the doped polysilicon layer are arranged on one side surface of the silicon substrate. For a bifacial cell, the tunneling oxide layer and the doped polysilicon layer formed on one side surface of the solar cell have the same structure as above, and the molding quality is good, thereby improving the cell efficiency of the bifacial cell and reducing leakage.

[0033] Optionally, in the above solar cell, the solar cell is a back contact cell, and the silicon substrate includes a first semiconductor region and a second semiconductor region of opposite conductivity types;

[0034] The tunneling oxide layer and the doped polysilicon layer are arranged in the first semiconductor region and / or the second semiconductor region.

[0035] When the above technical solution is adopted, for the back contact battery, the tunneling oxide layer and the doped polysilicon layer on the first semiconductor region and / or the second semiconductor region on the back have the same structure as above, with good molding quality and good corrosion resistance, thereby improving the battery efficiency of the back contact battery and reducing leakage. And the tunneling passivation contact structure composed of the tunneling oxide layer and the doped polysilicon layer in the first semiconductor region and / or the second semiconductor region has the advantages of high conversion efficiency, good stability and low Auger recombination.

[0036] In a third aspect, the present invention further provides a photovoltaic module, comprising a solar cell as described in any one of the above items.

[0037] Since the photovoltaic module adopts any of the solar cells described above, the photovoltaic module has the same beneficial effects as the above solar cells, which will not be described in detail here. BRIEF DESCRIPTION OF THE DRAWINGS

[0038] The drawings described herein are used to provide a further understanding of the present invention and constitute a part of the present invention. The exemplary embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute an improper limitation of the present invention. In the drawings:

[0039] Figure 1 It is a schematic diagram of the structure of inserting a silicon wafer in a first position in a low pressure chemical vapor deposition process disclosed in an embodiment of the present invention;

[0040] Figure 2 It is a structural schematic diagram of inserting a silicon wafer in a second position in the diffusion doping process disclosed in an embodiment of the present invention;

[0041] Figure 3 A distribution diagram of holes formed by etching the doped polysilicon layer in control group 1;

[0042] Figure 4 A distribution diagram of holes formed by etching the doped polysilicon layer in control group 2;

[0043] Figure 5 Schematic diagram of the distribution of holes formed by etching the doped polysilicon layer in the experimental group.

[0044] Reference numerals:

[0045] 100 is a film boat;

[0046] 200 is silicon wafer. DETAILED DESCRIPTION

[0047] In order to make the technical problems, technical solutions and beneficial effects to be solved by the present invention more clearly understood, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not intended to limit the present invention.

[0048] It should be noted that when an element is referred to as being "fixed to" or "disposed on" another element, it can be directly on the other element or indirectly on the other element. When an element is referred to as being "connected to" another element, it can be directly connected to the other element or indirectly connected to the other element.

[0049] In addition, the terms "first" and "second" are used for descriptive purposes only and should not be understood as indicating or implying relative importance or implicitly indicating the number of the indicated technical features. Therefore, the features defined as "first" and "second" may explicitly or implicitly include one or more of the features. In the description of the present invention, the meaning of "multiple" is two or more, unless otherwise clearly and specifically defined. The meaning of "several" is one or more, unless otherwise clearly and specifically defined.

[0050] In the description of the present invention, it is necessary to understand that the directions or positional relationships indicated by the terms "up", "down", "front", "back", "left", "right", etc. are based on the directions or positional relationships shown in the accompanying drawings, and are only for the convenience of describing the present invention and simplifying the description, rather than indicating or implying that the device or element referred to must have a specific direction, be constructed and operated in a specific direction, and therefore cannot be understood as a limitation on the present invention.

[0051] In the description of the present invention, it should be noted that, unless otherwise clearly specified and limited, the terms "installed", "connected", and "connected" should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection or an indirect connection through an intermediate medium, it can be the internal connection of two elements or the interaction relationship between two elements. For ordinary technicians in this field, the specific meanings of the above terms in the present invention can be understood according to specific circumstances.

[0052] The core of the present invention is to provide a method for preparing a solar cell, which can significantly improve the film-forming quality of a doped polysilicon layer and enhance the alkali corrosion resistance of a phosphosilicate glass layer or a borosilicate glass layer.

[0053] Another core of the present invention is to provide a solar cell and a photovoltaic module.

[0054] like Figure 1 and Figure 2 As shown, an embodiment of the present invention discloses a method for preparing a solar cell, comprising the following steps:

[0055] Step S100, placing the silicon wafer 200 in a first position, and sequentially forming a tunneling oxide layer and an intrinsic amorphous silicon layer on at least one side surface of the silicon wafer 200, wherein the angle between the silicon wafer 200 and the horizontal plane is α in the first position. That is, the silicon wafer 200 is inserted into the wafer boat 100 in the first position, and the angle between the silicon wafer 200 and the flow direction of the airflow in the furnace tube is α.

[0056] Step S200, placing the silicon wafer 200 in the second position, and performing diffusion doping on the intrinsic amorphous silicon layer to form a doped polysilicon layer and a glass layer. In the second position, the angle between the silicon wafer 200 and the horizontal plane is β, wherein α is less than β. That is to say, after the silicon wafer 200 is taken out after deposition to form the intrinsic amorphous silicon layer, a diffusion doping treatment is performed, and the angle between the silicon wafer 200 in the second position and the airflow direction in the furnace tube is β, and it should be noted that α in step S100 is less than β, so that the silicon wafer 200 placed in the first position in the process of forming the intrinsic amorphous silicon layer is closer to the airflow direction than the silicon wafer 200 placed in the second position in the diffusion doping process, while the silicon wafer 200 in the diffusion doping process is closer to being arranged along the vertical airflow direction.

[0057] Step S300, remove part of the glass layer, and use the remaining glass layer as a mask to remove the doped polysilicon layer not covered by the glass layer using an etching solution. By using the glass layer as a mask, the process of setting a separate mask can be saved, and the doped polysilicon layer and the glass layer are formed simultaneously in the same step, thereby simplifying the process.

[0058] As can be seen from the above, in the process of depositing the intrinsic amorphous silicon layer, the placement of the silicon wafer 200 is closer to the direction of the airflow in the furnace tube, which is conducive to extracting the byproducts of the intrinsic amorphous silicon layer with poor adsorption in the deposition process and improving the film quality of the intrinsic amorphous silicon layer. In the diffusion doping process, the placement of the silicon wafer 200 is closer to being arranged along the direction perpendicular to the airflow. At this time, the O 2 The longer the stay time on the surface of the silicon wafer 200, the more effectively fill the gaps in the glass layer, such as the PSG or BSG film layer, thereby increasing the compactness of the glass layer and improving the corrosion resistance of the glass layer. In this way, when the glass layer is used as a mask to remove part of the polysilicon layer and the tunnel oxide layer using the etching liquid, due to the high film quality of the intrinsic amorphous silicon layer, that is, the high film quality of the formed doped polysilicon layer, and the improved corrosion resistance of the glass layer, the etching liquid can be prevented from damaging the doped polysilicon layer covered by the glass layer, ensuring that the quality of the doped polysilicon layer finally retained is high, thereby preventing leakage and improving battery efficiency.

[0059] In some specific embodiments, the angle α between the silicon wafer 200 placed in the first position and the horizontal plane is in the range of 0°≤α≤30°. For example, α can be selected from 0°, 5°, 10°, 15°, 20°, 25°, 30°, etc., so that the silicon wafer 200 in the first position is arranged closer to the flow direction of the airflow, which is beneficial to extract the by-products of the intrinsic amorphous silicon layer with poor adsorption, thereby improving the film formation quality of the intrinsic amorphous silicon layer.

[0060] The angle β between the silicon wafer 200 placed at the second position and the horizontal plane in the diffusion doping process is in the range of 60°≤β≤90°. For example, β can be selected as 60°, 70°, 75°, 80°, 85° or 90°, so that the silicon wafer 200 at the second position is arranged closer to the vertical direction of the airflow, and the O 2 The silicon wafer 200 stays on the surface of the silicon wafer 200 for a longer time, and the gaps in the PSG or BSG film layer are filled more effectively, thereby enhancing the compactness of the film layer. If the value of β is less than the angle range during the diffusion doping process, the silicon wafer 200 at the second position is poorly perpendicular to the airflow, resulting in a decrease in the contact area between the silicon wafer 200 and the cross section of the airflow entering the furnace tube, and the O 2 becomes smaller, and the O 2 The residence time on the surface of the silicon wafer 200 is short, resulting in insufficient oxidation of the surface of the doped polysilicon layer, making it impossible to effectively fill the gaps in the PSG or BSG film layer, reducing the density of the glass layer and affecting the corrosion resistance. Therefore, considering the film quality of the intrinsic amorphous silicon layer and the corrosion resistance of the glass layer, 0°≤α≤30°, 60°≤β≤90° are selected.

[0061] Of course, it can be understood that in the process of forming the intrinsic amorphous silicon layer, the arrangement position of the silicon wafer 200 placed in the first position is closer to the horizontal direction, that is, along the flow direction of the gas flow, and the further value range of α is 0°≤α≤10°, which is more conducive to the timely extraction of the intrinsic amorphous silicon by-products with poor adsorption on the silicon wafer 200, and promotes the improvement of the film forming quality of the intrinsic amorphous silicon layer. The further value range of β is 80°≤β≤90°, that is, in the diffusion doping process, the silicon wafer 200 in the second position is arranged perpendicular to the flow direction of the gas flow, so that the O 2 Staying on the wafer surface for a longer time can more effectively fill the gaps in the PSG or BSG film layer to enhance the density of the film layer and thereby improve the corrosion resistance of the glass layer.

[0062] In a specific embodiment, a tunnel oxide layer and an intrinsic amorphous silicon layer are sequentially formed by a low pressure chemical vapor deposition process. In the low pressure chemical vapor deposition process, the silicon wafer 200 is placed in a first position, that is, the angle between the silicon wafer 200 and the horizontal plane is α. The low pressure chemical vapor deposition process can obtain a uniform and high quality intrinsic amorphous silicon layer at a lower temperature, with a high deposition rate and a high deposition accuracy. Of course, a plasma chemical vapor deposition process can also be used to sequentially form a tunnel oxide layer and an intrinsic amorphous silicon layer, as long as it can be placed in a plasma chemical vapor deposition device in the first position for deposition.

[0063] In some possible implementations, placing the silicon wafer 200 at the first position in step S100 to sequentially form a tunneling oxide layer and an intrinsic amorphous silicon layer specifically includes the following steps:

[0064] Step S110, insert the silicon wafer 200 into the wafer carrier boat 100 at the first position, and move the wafer carrier boat 100 into the furnace tube of the low-pressure chemical vapor deposition equipment. The wafer carrier boat 100 can be a quartz boat, and the wafer carrier boat 100 is used to insert and carry multiple silicon wafers 200. The wafer carrier boat 100 is usually a rectangular parallelepiped frame. The length direction of the wafer carrier boat 100 is parallel to the axis of the furnace tube and placed into the furnace tube. The axis of the furnace tube is a horizontal axis. Therefore, the angle α of the silicon wafer 200 relative to the horizontal plane can be understood as the angle of the silicon wafer 200 relative to the axis of the furnace tube or the angle of the silicon wafer 200 relative to the bottom surface of the wafer carrier boat 100. In the first position, the insertion method of the silicon wafer 200 on the wafer carrier boat 100 can be understood as horizontal insertion.

[0065] Step S120: introducing a first preset volume flow rate of O into the furnace tube at a first preset temperature. 2 , so that a tunneling oxide layer is formed on the surface of the silicon wafer 200.

[0066] Step S130: introducing SiH2O2 at a second preset volume flow rate into the furnace tube at a second preset temperature. 4 , an intrinsic amorphous silicon layer is formed on the tunnel oxide layer.

[0067] Step S140: Finally, N is introduced into the furnace tube. 2 The temperature is lowered, and then the wafer boat 100 with the silicon wafer 200 inserted therein is withdrawn from the furnace tube. Alternatively, those skilled in the art may introduce inert gas such as helium, argon, or neon into the furnace tube according to actual needs.

[0068] By adopting the above process, the silicon wafer 200 is inserted into the wafer carrier boat 100 at the first position, and the first position of the silicon wafer 200 is fixed by the wafer carrier boat 100, and the silicon wafer 200 is sent into the furnace tube of the low-pressure chemical vapor deposition equipment, and a tunneling oxide layer and an intrinsic amorphous silicon layer are sequentially formed on the silicon wafer 200. By inserting the silicon wafer 200 on the wafer carrier boat 100 in a manner that is approximately horizontal, the SiH 4 The decomposition reaction process is conducive to extracting the byproducts of the intrinsic amorphous silicon layer with poor adsorption, so that the film formation quality of the intrinsic amorphous silicon layer is improved.

[0069] It should be noted that the tunnel oxide layer can also be formed by other methods, for example, inserting the silicon wafer 200 into the wafer boat 100 at the first position, placing the wafer boat 100 in a plasma chemical vapor deposition device, and passing N 2O is used as a gas source, and a plasma chemical vapor deposition process is used to ionize and form a tunnel oxide layer on the silicon wafer 200, and then the intrinsic amorphous silicon layer is prepared. Alternatively, the tunnel oxide layer can be formed on the silicon wafer first, and then the silicon wafer with the tunnel oxide layer is inserted into a wafer carrier boat at the first position and placed in a furnace tube of a low-pressure chemical vapor deposition device to continue preparing the intrinsic amorphous silicon layer. For example, the tunnel oxide layer can be irradiated with UV light in the O 3 The surface of the silicon wafer is oxidized to form a tunneling oxide layer, or through HNO 3 The surface of the silicon wafer is wet chemically oxidized to form a tunneling oxide layer.

[0070] In a specific embodiment, in the low pressure chemical vapor deposition process, in step S110, 2 The first preset volume flow rate ranges from 15000 sccm to 25000 sccm, and the first preset temperature ranges from 580° C. to 610° C. In step S120, SiH 4 The first preset volume flow rate ranges from 1000sccm to 1500sccm, the second preset temperature ranges from 590℃ to 620℃, and the first preset pressure range in the furnace tube is from 150mtorr to 250mtorr, thereby forming a tunneling oxide layer and an intrinsic amorphous silicon layer of good quality on the silicon wafer 200, which is beneficial to the molding quality of the silicon glass layer containing doped elements formed by subsequent diffusion doping and improving corrosion resistance.

[0071] It should be noted that the diffusion doping in step S200 can be phosphorus diffusion doping or boron diffusion doping. The corresponding phosphorus diffusion doping forms a phosphosilicate glass layer, and the corresponding boron diffusion doping forms a borosilicate glass layer. The methods in this application can improve the alkali corrosion resistance of the phosphosilicate glass layer or the borosilicate glass layer.

[0072] In some possible implementations, placing the silicon wafer 200 at the second position in step S200 and performing diffusion doping on the intrinsic amorphous silicon layer to form a doped polysilicon layer and a glass layer specifically includes the following steps:

[0073] Step S210, inserting the silicon wafer 200 into the wafer carrier boat 100 at the second position, and moving the wafer carrier boat 100 into the furnace tube of the diffusion doping equipment. It should be noted that after the low-pressure chemical vapor deposition in step S100 is completed, the wafer carrier boat 100 needs to be taken out of the furnace tube, and the deposited silicon wafer 200 is taken off the wafer carrier boat 100, and the wafer carrier boat 100 is reinserted at the second position. The wafer carrier boat 100 at this time can be a new wafer carrier boat 100, so as to reduce the contamination of the wafer carrier boat 100 used during the deposition to the silicon wafer 200 during the diffusion. Similarly, the wafer carrier boat 100 is placed in the furnace tube with its length direction parallel to the axis of the furnace tube of the diffusion and doping equipment, and the axis of the furnace tube is a horizontal axis. Therefore, the angle β of the silicon wafer 200 relative to the horizontal plane is also understood as the angle of the silicon wafer 200 relative to the axis of the furnace tube or the angle of the silicon wafer 200 relative to the bottom surface of the wafer carrier boat 100, and the angle β is greater than the angle α, that is, the silicon wafer 200 in the second position tends to be arranged in a direction perpendicular to the horizontal plane relative to the silicon wafer 200 in the first position in step S110. At this time, the insertion method of the silicon wafer 200 on the wafer carrier boat 100 can be understood as vertical insertion.

[0074] Step S220: introducing a third preset volume flow rate of O into the furnace tube at a third preset temperature. 2 、N 2 and a diffusion doping source containing the doping elements to be diffused.

[0075] Step S230: introducing a fourth preset volume flow rate of O into the furnace tube at a fourth preset temperature. 2 , and controlling the cooling time, high temperature advancement and oxidation are performed to promote the diffusion doping source to continue to diffuse into the intrinsic amorphous silicon layer, forming a doped polysilicon layer and a glass layer, such as a phosphosilicate glass layer, or a borosilicate glass layer.

[0076] Step S240: Finally, N is introduced into the furnace tube in the same manner. 2 The temperature is lowered, and the wafer boat 100 with the silicon wafer 200 inserted therein is withdrawn from the furnace tube. Through the above steps, the diffusion doping source is introduced, and the diffusion doping source continues to diffuse inward under the high temperature promotion and oxidation action to finally form a phosphorus silicon glass layer or a borosilicate glass layer.

[0077] When the above technical solution is adopted, the silicon wafer 200 is inserted into the wafer carrier boat 100 at the second position, and the second position of the silicon wafer 200 is fixed by the wafer carrier boat 100, and then sent to the furnace tube of the diffusion doping equipment, and the doped polysilicon layer is formed by diffusion doping and the glass layer is formed by simultaneous oxidation. By inserting the silicon wafer 200 on the wafer carrier boat 100 in a manner close to being vertical, it is arranged more in the direction perpendicular to the air flow, and the oxidation process in the diffusion doping process is increased. 2 The residence time on the surface of the silicon wafer 200 improves the compactness of the glass layer formed by oxidation, thereby improving the corrosion resistance of the glass layer.

[0078] The diffusion doping is phosphorus diffusion doping to form a phosphosilicate glass layer, and the compound containing the element to be diffused is N 2 -POCl 3 When , then in step S210, 2 The third preset volume flow rate range is 700 sccm to 900 sccm. 2 -POCl 3 The third preset volume flow rate ranges from 1600 sccm to 1900 sccm, N 2 The third preset volume flow rate ranges from 2000 sccm to 2500 sccm, the third preset temperature ranges from 780° C. to 810° C., and the second preset pressure in the furnace tube is from 130 mbar to 160 mbar, thereby forming a phosphorus diffusion doping source.

[0079] In step S220, 2 The fourth preset volume flow rate ranges from 10000sccm to 15000sccm, the fourth preset temperature ranges from 860°C to 880°C, the third preset pressure in the furnace tube is 300mbar to 600mbar, and the cooling time control range is 20mins to 30mins, thereby finally forming a phosphorus silicon glass layer. Of course, it can be understood that when the doping element is boron, the above parameters can be adjusted in time according to the process requirements, and this article will not repeat them.

[0080] In some specific embodiments, during the low pressure chemical vapor deposition process, the angle α between the silicon wafer 200 placed at the first position and the horizontal plane is selected as 0°, during the diffusion doping process, the angle β between the silicon wafer 200 placed at the second position and the horizontal plane is selected as 90°, and phosphorus diffusion doping is performed. The specific steps of the solar cell preparation method provided in this embodiment are as follows:

[0081] Step S110, insert the silicon wafer 200 into the wafer boat 100 at the first position, push the wafer boat 100 with the silicon wafer 200 inserted into the furnace tube, at this time, the angle between the silicon wafer 200 in the furnace tube and the horizontal plane is 0°, and the silicon wafer 200 is arranged along the flow direction of the airflow, that is, in a horizontal insertion manner. 2 The air in the furnace tube is removed to prevent the interference of the messy substances in the air with the subsequent process.

[0082] Step S120: introducing O into the furnace tube 2 , and at this time O 2 The first preset volume flow rate is 20000 sccm, and the temperature is increased. The first preset heating temperature is 600° C., so that a tunneling oxide layer is formed on the surface of the silicon wafer 200.

[0083] Step S130: After tunneling through the oxide layer, SiH 4 , SiH 4 The second preset volume flow rate is 1300 sccm, and the second preset temperature is 610° C., and the first preset pressure in the furnace tube can be set to 200 mtorr, thereby forming an intrinsic amorphous silicon layer.

[0084] Step S140: After the tunnel oxide layer and the intrinsic amorphous silicon layer are formed, N is introduced into the furnace tube again. 2 The temperature is lowered, and when the temperature drops to a preset value, the wafer boat 100 with the silicon wafer 200 inserted therein is withdrawn from the furnace tube, and then enters the phosphorus diffusion doping process.

[0085] Step S210, insert the silicon wafer 200 into the wafer boat 100 at the second position, push the wafer boat 100 with the silicon wafer 200 inserted into the furnace tube, at this time, the angle between the silicon wafer 200 in the furnace tube and the horizontal plane is 90°, and the silicon wafer 200 is arranged perpendicular to the flow direction of the airflow, that is, the vertical insertion method. Similarly, N is introduced into the furnace tube. 2 The air in the furnace tube is removed to prevent the interference of the messy substances in the air with the subsequent process.

[0086] Step S220: introducing O into the furnace tube 2 、N 2 -POCl 3 and N 2 , where O 2 The third preset volume flow rate is 800 sccm, N 2 -POCl 3 The third preset volume flow rate is controlled at 1800 sccm, N 2 The third preset volume flow rate is set to 2300 sccm, and the third preset temperature is set to 800° C., and the second preset pressure in the furnace tube can be set to 150 mbar to form a phosphorus diffusion doping source.

[0087] Step S230: High temperature driving and oxidation treatment of the phosphorus diffusion doping source, and introducing O into the furnace tube. 2 , at this time O 2 The fourth preset volume flow rate can be set to 13000 sccm, the fourth preset temperature is set to 870°C, the third preset pressure in the furnace tube is set to 500 mbar, and during the cooling process, the cooling time is 25 minutes, and finally a phosphosilicate glass layer is obtained.

[0088] Step S240: Finally, N is introduced into the furnace tube. 2 After the temperature in the furnace tube drops to a preset value, the wafer boat 100 with the silicon wafer 200 inserted therein is withdrawn from the furnace tube.

[0089] In a specific embodiment, as shown in Table 1, two control groups and one experimental group according to the solar cell preparation method provided in this embodiment were set up for testing. The experimental group adopted the solar cell preparation method provided in this embodiment, that is, Figure 2 As shown, the silicon wafer 200 is placed in a first position for low-pressure chemical vapor deposition. In the first position, the angle between the silicon wafer 200 and the horizontal plane is α, and the selected value of α is 0°. Figure 1 As shown, the silicon wafer 200 is placed in the second position for diffusion doping. In the second position, the angle between the silicon wafer 200 and the horizontal plane is β, and the selected value of β is about 90°.

[0090] Table 1 Silicon wafer insertion methods for the control group and experimental group

[0091] NO LPCVD insert method Phosphorus expansion plug-in method Control group 1 Vertical Insert( Figure 1 ) Vertical Insert( Figure 1 ) Control group 2 Horizontal insertion Figure 2 ) Horizontal insertion Figure 2 ) Experimental Group Horizontal insertion Figure 2 ) Vertical Insert( Figure 1 )

[0092] Experiment 1: After the low pressure chemical vapor deposition process and diffusion doping treatment were completed for the control group and experimental group set in Table 1, the control group 1, the control group 2 and the experimental group were treated with the same alkali solution and time. The alkali solution formula is as follows: 18LH 2 O、750ML H 2 O 2 and 100ML KOH, and the solution temperature is 60℃, the control group and the experimental group are immersed in this solution for 60s, the thickness of the PSG film layer of the control group 1, the control group 2 and the experimental group before and after the experiment is measured and recorded, and the results are summarized in Table 2. From the data results in Table 2, it can be concluded that the thinning amount of the PSG film layer in the experimental group accounts for 28.46%, that is, compared with the control group 1 and the control group 2, the least, and the experimental group has the best alkali resistance protection.

[0093] Table 2 Alkali resistance test

[0094]

[0095] The embodiment of the present invention also discloses a solar cell, comprising a silicon substrate, a tunneling oxide layer and a doped polysilicon layer, wherein the tunneling oxide layer is arranged on a partial area of ​​the silicon substrate, the doped polysilicon layer is arranged on the tunneling oxide layer, the doped polysilicon layer has micrometer-level holes penetrating the doped polysilicon layer, and the average density of the holes is less than 5 / mm 2 For example, the average density of holes can be 1 / mm 2 , 2 pieces / mm 2 , 3 pieces / mm 2 , 4 pieces / mm 2 The solar cell can be prepared by the above-mentioned solar cell preparation method, or by other preparation methods.

[0096] For example, the surface of the silicon substrate can be a polished surface or a velvet surface. The velvet surface has a light trapping effect and can improve the light collection efficiency. If it is a velvet surface, the tunneling oxide layer and the doped polysilicon layer are conformally formed on the velvet surface, which is also a velvet structure.

[0097] For example, the cross-sectional shape of the hole can be a circular hole, an elliptical hole, a polygonal hole (such as a triangular hole, a trapezoidal hole, a rectangular hole, a pentagonal hole, etc.), a curved hole (such as a waist-shaped hole, a dumbbell-shaped hole, an S-shaped hole, etc.) or an irregular hole. The cross-sections of the hole along the depth direction can be of equal size or unequal size, and the cross-sections can be the same or different.

[0098] The doped polysilicon layer in the solar cell provided in the present application has a small pore density, so the molding quality is high, the corrosion resistance is strong, the defects are small, the carrier recombination is reduced, the conductivity and carrier lifetime are improved, the electrical performance of the solar cell is significantly improved, the battery efficiency is improved, and the leakage is reduced.

[0099] For example, when the insert is in single-insertion mode, that is, the silicon wafers in the furnace tube are arranged at intervals, and tunneling oxide layers and doped polysilicon layers are formed on both sides of the silicon substrate. When the insert is in double-insertion mode, that is, two silicon wafers bonded to each other are grouped together, and multiple groups are inserted into the furnace tube at intervals. At this time, the tunneling oxide layer and the doped polysilicon layer are arranged on the side of the silicon substrate facing away from the bonding surface.

[0100] After the control group and experimental group set in Table 1 completed the low-pressure chemical vapor deposition process, diffusion doping treatment, and then texturing treatment, in the alkaline etching process of battery production, the PSG film layer was used as a mask to etch part of the doped polysilicon layer, and the holes formed on the doped polysilicon layer were observed, as shown in FIG. Figure 3 , Figure 4 and Figure 5 As shown, Figure 3 This is a diagram showing the distribution of holes formed by etching the doped polysilicon layer in control group 1. Figure 4 This is a diagram showing the distribution of holes formed by etching the doped polysilicon layer in control group 2. Figure 5 Schematic diagram of the distribution of holes formed by etching the doped polysilicon layer in the experimental group.

[0101] The hole density of comparison group 1 was 10 to 24 holes / mm 2 The hole density of the comparison group 2 was 6 to 12 per mm 2 , while the hole density of the experimental group was only 5 / mm 2 It can be seen that the experimental group has better film quality.

[0102] In some embodiments of the present application, the maximum size of the hole, that is, the distance between the two points on the hole that are farthest apart, is greater than 0 and less than 5 μm, and can be specifically 0.1 μm, 1 μm, 2 μm, 3 μm, 4 μm, 4.5 μm, etc. The formed hole size is small and the defects are small, which reduces carrier recombination, improves conductivity and carrier lifetime, significantly improves the electrical performance of solar cells, improves battery efficiency, and reduces leakage.

[0103] In some examples, the maximum size range of the hole can be 2um-4um, that is, the maximum size range of the hole is greater than or equal to 2um and less than or equal to 4um. In order to avoid the hole size being too small, which increases the difficulty of forming the hole, and to avoid the hole size being too large, which leads to serious carrier recombination, some embodiments of the present application choose to set the maximum size range of the hole to 2um~4um.

[0104] The solar cell preparation method provided in this embodiment can be applied to the preparation of any battery that requires etching of part of the doped polysilicon layer and the tunneling oxide layer, such as Topcon batteries, TBC (Topcon+BC, back contact tunneling oxide passivation batteries) batteries, Topcon and crystalline silicon stacked batteries, composite passivated back contact solar cells, batteries with partial Topcon structures, etc.

[0105] In some embodiments, the depth of the hole ranges from 1 μm to 5 μm. Considering that if the depth of the hole is small, the process difficulty of forming the hole will increase, and if the depth of the hole is large, the silicon substrate will be removed more, reducing the photoelectric conversion efficiency, the embodiment of the present application chooses to set the depth of the hole to be 1 μm to 5 μm. The depth of the hole can be specifically 1 μm, 2 μm, 3 μm, 4 μm, 5 μm, etc. When the depth of the hole is shallow, for example, 1 μm to 3 μm, the hole only penetrates the doped polysilicon layer. When the depth of the hole is deep, for example, 3 μm to 5 μm, the hole can penetrate the doped polysilicon layer and the tunnel oxide layer, and even the hole can extend into the surface of the silicon substrate, forming a pit on the surface of the silicon substrate. For a silicon substrate with a velvet structure, for example, the velvet structure is a pyramid structure, a prism structure, etc., if the hole is located on the top of the pyramid structure, the position of the top of the pyramid corresponding to the hole will form a pit or crack structure.

[0106] In some embodiments, the average density of holes at the edge of the silicon substrate is greater than the average density of holes at the middle of the silicon substrate. For example, the average density of holes at the edge of the silicon substrate is 3 to 5 holes / mm. 2 The average density of holes in the middle of the silicon substrate is 1 to 2 holes / mm 2With such arrangement, the average density of the holes at the edge of the silicon substrate is relatively large, which is beneficial for increasing the contact area between the soldering ribbon and the battery cell when soldering the soldering ribbon at the edge of the silicon substrate, thereby increasing the soldering strength between the soldering ribbon and the battery cell, and preventing the soldering ribbon from being separated from the battery cell.

[0107] In some embodiments, the solar cell further includes a passivation layer covering the doped polysilicon layer, and the passivation layer fills the hole. If the hole only penetrates the doped polysilicon layer, the passivation layer fills the hole and then covers the tunneling oxide layer. If the hole penetrates the doped polysilicon layer and the tunneling oxide layer, the passivation layer fills the hole and then covers the surface of the silicon substrate. By providing the passivation layer, the passivation layer and the tunneling oxide layer play a passivation effect together, further improving the passivation effect on the silicon substrate, reducing the surface defects of the silicon substrate, and improving the photoelectric conversion efficiency of the solar cell.

[0108] In some embodiments, the solar cell further comprises an electrode disposed on the passivation layer, the electrode penetrating the passivation layer and contacting the doped polysilicon layer. The electrode may be made of metal paste and may be prepared by screen printing. For burn-through metal paste, the metal paste burns through the passivation layer and contacts the doped polysilicon layer to form an electrode for collecting carriers. The material of the electrode may be one or more of silver, aluminum, copper, tin, gold, lead, and nickel.

[0109] When the solar cell is a bifacial cell, the tunneling oxide layer and the doped polysilicon layer can be arranged on one side surface of the silicon substrate. For example, the entire surface of one side surface of the silicon substrate is provided with the tunneling oxide layer and the doped polysilicon layer, and the other side surface of the silicon substrate is not provided with the tunneling oxide layer and the doped polysilicon layer; for another example, the entire surface of one side surface of the silicon substrate is provided with the tunneling oxide layer and the doped polysilicon layer, and the tunneling oxide layer and the doped polysilicon layer are provided in a partial area of ​​the other side surface of the silicon substrate, for example, the tunneling oxide layer and the doped polysilicon layer are only provided at the position directly opposite to the electrode.

[0110] When the solar cell is a back contact cell, one side surface of the silicon substrate includes a first semiconductor region and a second semiconductor region of opposite conductivity types, the first semiconductor region may correspond to the first of the P region and the N region, and the second semiconductor region corresponds to the other of the P region and the N region. The tunneling oxide layer and the doped polysilicon layer are arranged in the first semiconductor region and / or the second semiconductor region. That is, the tunneling oxide layer and the doped polysilicon layer may be arranged only in the first semiconductor region or the second semiconductor region, and the tunneling oxide layer and the doped polysilicon layer on the first semiconductor region or the second semiconductor region have the same structure as the above embodiment, with good molding quality and good corrosion resistance, thereby improving the battery efficiency of the back contact cell and reducing leakage. And the first semiconductor region or the second semiconductor region is a tunneling passivation contact structure composed of a tunneling oxide layer and a doped polysilicon layer, which has the advantages of high conversion efficiency, good stability and low Auger recombination.

[0111] Of course, it is understandable that on the basis of the tunneling oxide layer and the doped polysilicon layer being provided in the first semiconductor region, the tunneling oxide layer and the doped polysilicon layer can also be provided in the second semiconductor region to form a TBC battery in which both the first semiconductor region and the second semiconductor region are tunneling passivation contact structures. The tunneling oxide layer and the doped polysilicon layer on the second semiconductor region have the same structure as the above-mentioned embodiment, with good molding quality and good corrosion resistance, thereby improving the battery efficiency of the back contact battery and reducing leakage. It should be noted that the type of doping element of the doped polysilicon layer on the first semiconductor region is different from the type of doping element of the doped polysilicon layer on the second semiconductor region to achieve different conductivity types.

[0112] Of course, on the basis that one of the first semiconductor region and the second semiconductor region is provided with a tunneling oxide layer and a doped polysilicon layer, the other may also be other structures, such as a heterojunction or a PERC structure. When one of them is a heterojunction structure, a hybrid back contact cell is formed in which one of the first semiconductor region and the second semiconductor region is a tunneling passivation contact structure and the other is a heterojunction structure; when one of them is a PERC structure, that is, a passivation layer is formed in the region, and the electrode contacts the silicon substrate through the passivation layer, forming a hybrid back contact cell in which one of the first semiconductor region and the second semiconductor region is a tunneling passivation contact structure and the other is a PERC structure.

[0113] Experiment 3: The cell production was completed by using the insert processing methods of the control group and the experimental group in Table 1, and following the processes of silicon wafer polishing, low-pressure chemical vapor deposition, phosphorus diffusion doping, acid etching, texturing, ALD (Atomic layer deposition), PECVD (Plasma Enhanced Chemical Vaper Deposition) positive film, PECVD back film, and screen printing sintering. The efficiency and leakage data of the cells produced by the control group and the experimental group were tested and compared, as shown in Table 3:

[0114] Table 3 Battery efficiency and leakage data

[0115] Group Count Voc(V) Isc(A) Rs(Ω) Rsh(Ω) FF(%) Eff(%) Leakage @-13V Control group 1 796 BSL BSL BSL BSL BSL BSL BSL Control group 2 791 +0.04% +0.01% -2.32% +0.19% +0.09% +0.10% -20.00% Experimental Group 795 +0.16% +0.01% -4.86% +0.34% +0.28% +0.44% -37.33%

[0116] From the test results in Table 3, it can be concluded that the battery efficiency of the experimental group is better than that of the two control groups, especially in Voc and FF.

[0117] Based on the solar cell described in any one of the above embodiments, an embodiment of the present invention further provides a photovoltaic assembly, comprising the solar cell described in any one of the above embodiments.

[0118] Since the photovoltaic module adopts the solar cell described in any of the above embodiments, the photovoltaic module has the same beneficial effects as the above solar cell, which will not be described in detail here.

[0119] In the description of the above embodiments, specific features, structures, materials or characteristics may be combined in a suitable manner in any one or more embodiments or examples.

[0120] The above is only a specific embodiment of the present invention, but the protection scope of the present invention is not limited thereto. Any person skilled in the art can easily think of changes or substitutions within the technical scope disclosed by the present invention, which should be included in the protection scope of the present invention. Therefore, the protection scope of the present invention should be based on the protection scope of the claims.

Claims

1. A method for preparing a solar cell, characterized in that: include: placing the silicon wafer in a first position, and sequentially forming a tunneling oxide layer and an intrinsic amorphous silicon layer; In the first position, the angle between the silicon wafer and the horizontal plane is α; The silicon wafer is placed in a second position, and the intrinsic amorphous silicon layer is diffused to form a doped polysilicon layer and a glass layer; in the second position, the angle between the silicon wafer and the horizontal plane is β; wherein α is less than β; A portion of the glass layer is removed, and the remaining glass layer is used as a mask to remove the doped polysilicon layer not covered by the glass layer using an etching solution.

2. The method for preparing a solar cell according to claim 1, characterized in that: 0°≤α≤30°; And / or, 60°≤β≤90°.

3. The method for preparing a solar cell according to claim 2, characterized in that: 0°≤α≤10°; and / or, 80°≤β≤90°.

4. The method for preparing a solar cell according to claim 1, characterized in that: The silicon wafer is placed at a first position, and the tunnel oxide layer and the intrinsic amorphous silicon layer are formed by a low pressure chemical vapor deposition process.

5. The method for preparing a solar cell according to claim 1, characterized in that: Placing the silicon wafer at the first position to sequentially form the tunneling oxide layer and the intrinsic amorphous silicon layer comprises: Inserting the silicon wafer into a wafer boat at the first position, and moving the wafer boat into a furnace tube of a low-pressure chemical vapor deposition device; introducing a first preset volume flow rate of O2 into the furnace tube at a first preset temperature to form the tunneling oxide layer on the surface of the silicon wafer; A second preset volume flow rate of SiH4 is introduced into the furnace tube at a second preset temperature to form the intrinsic amorphous silicon layer on the tunneling oxide layer.

6. The method for preparing a solar cell according to claim 1, characterized in that: Placing the silicon wafer at the second position and diffusing the intrinsic amorphous silicon layer to form the doped polysilicon layer and the glass layer includes: Inserting the silicon wafer into a wafer boat at the second position, and moving the wafer boat into a furnace tube of a diffusion and doping device; At a third preset temperature, a third preset volume flow rate of O2, N2 and a diffusion doping source containing a doping element to be diffused are introduced into the furnace tube; A fourth preset volume flow rate of O2 is introduced into the furnace tube at a fourth preset temperature, and the cooling time is controlled to promote the diffusion doping source to continue to diffuse into the intrinsic amorphous silicon layer to form the doped polysilicon layer and the glass layer.

7. A solar cell, characterized in that: include: Silicon substrate; A tunneling oxide layer is disposed on a partial area of ​​the silicon substrate; A doped polysilicon layer is disposed on the tunnel oxide layer, the doped polysilicon layer has micrometer-scale holes penetrating the doped polysilicon layer, and the average density of the holes is less than 5 / mm 2 .

8. The solar cell according to claim 7, characterized in that: The maximum size range of the holes is greater than 0 and less than 5 um.

9. The solar cell according to claim 8, characterized in that The maximum size range of the holes is 2um to 4um.

10. The solar cell according to any one of claims 7 to 9, characterized in that: The depth of the holes ranges from 1um to 5um.

11. The solar cell according to any one of claims 7 to 9, characterized in that: An average density of the holes located at the edge of the silicon substrate is greater than an average density of the holes located at the middle of the silicon substrate.

12. A photovoltaic module, characterized in that: Comprising a solar cell as described in any one of claims 7 to 11.