Compositions for non-aqueous battery electrolyte formulations

By using improved non-aqueous electrolyte formulas in lithium-ion batteries, including dioxolane and metal salts, the problems of electrolyte flammability and chemical stability are solved, and the cycle performance and safety of the battery are improved, achieving more efficient Charge transfer and environmentally friendly battery operation.

CN118943494APending Publication Date: 2024-11-12MEXICHEM FLUOR S A DE CV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410928230.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2020-05-06
Filing Date
2020-10-09
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The electrolyte solvents of existing lithium-ion batteries are flammable and have poor chemical stability, resulting in safety hazards and environmental problems, and it is difficult to maintain good ion fluidity and charge transfer efficiency at high temperatures.

Method used

Using a non-aqueous electrolyte formulation containing dioxolane compounds and metal salts such as LiPF6, the electrolyte is designed through specific synthetic methods and compositions to reduce the flammability and overpotential of the electrolyte, improve its stability at high temperatures and Electrochemical properties.

Benefits of technology

It significantly reduces the flammability and overpotential of the electrolyte, improves the circulation capacity and capacity retention rate of lithium-ion batteries, enhances compatibility with electrodes, and reduces the risk of self-discharge and environmental pollution of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118943494A_ABST
    Figure CN118943494A_ABST
Patent Text Reader

Abstract

The present invention relates to a composition and the use of a compound of formula (1): # imgabs0 # wherein R is H, F, Cl, CF3, alkyl or fluoroalkyl in a non-aqueous battery electrolyte formulation.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] This application is a divisional application of the Chinese patent application with an application date of October 9, 2020, application number "202080070684.6", and invention name "Composition". The original application is the Chinese national phase application of international application PCT / GB2020 / 052526. Technical Field

[0002] The present disclosure relates to non-aqueous electrolytic solutions for energy storage devices including batteries and capacitors, particularly for secondary batteries and devices known as supercapacitors. Background Art

[0003] There are two main types of batteries: primary batteries and secondary batteries. Primary batteries are also called non-rechargeable batteries. Secondary batteries are also called rechargeable batteries. One well-known type of rechargeable battery is the lithium-ion battery. Lithium-ion batteries have high energy density, no memory effect, and low self-discharge.

[0004] Lithium-ion batteries are commonly used in portable electronics and electric vehicles. In the battery, lithium ions move from the negative electrode to the positive electrode during discharge and back during charging.

[0005] Typically, the electrolytic solution comprises a non-aqueous solvent and an electrolyte salt and an additive. The electrolyte is typically a mixture of an organic carbonate such as ethylene carbonate, propylene carbonate, fluoroethylene carbonate, dialkyl carbonate (such as ethyl methyl carbonate) and ethers and polyethers (such as dimethoxyethane) containing a lithium ion electrolyte salt. Many lithium salts can be used as electrolyte salts, common examples of which include lithium hexafluorophosphate (LiPF6), lithium bis(fluorosulfonyl) imide (LiFSI) and lithium bis(trifluoromethanesulfonyl) imide (LiTFSI).

[0006] The electrolyte solution must perform many different roles within a battery.

[0007] The main function of the electrolyte is to facilitate the flow of charge carriers between the positive and negative electrodes. This occurs by transporting metal ions within the battery to and / or from one or both of the negative and positive electrodes, thereby releasing / adopting charge based on chemical reduction or oxidation.

[0008] Therefore, the electrolyte needs to provide a medium capable of solvating and / or loading the metal ions.

[0009] The electrolytes are typically non-aqueous due to the use of lithium electrolyte salts and the exchange of lithium ions with lithium metal, which is highly reactive with water and other battery components are also sensitive to water.

[0010] Additionally, the electrolyte must have suitable rheology to allow / enhance the flow of ions therein at the typical operating temperatures to which the battery is exposed and expected to operate.

[0011] In addition, the electrolyte must be as chemically inert as possible. In the context of the expected life of the battery, this is particularly relevant to internal corrosion within the battery (e.g., of the electrodes and housing) and battery leakage issues. Flammability is also important in light of chemical stability. Unfortunately, typical electrolyte solvents can pose safety risks because they often contain flammable materials.

[0012] This can be problematic because the battery can build up heat during operation when discharging or being discharged. This is particularly true for high density batteries such as lithium ion batteries. Therefore, it is desirable for the electrolyte to exhibit low flammability, as well as other related properties such as a high flash point.

[0013] It is also desirable that the electrolyte not present environmental issues regarding disposability after use, or other environmental issues such as global warming potential.

[0014] “Regioselectivity in addition reactions of some binucleophilic reagents to (trifluoromethyl)acetylene” Stepanova et al., Zhurnal Organicheskoi Khimii (1988), 24 (4), 692-9 describe the preparation of dioxolanes having a CF3CH2 group with a relatively low level of selectivity.

[0015] The listing or discussion of an independent prior-published document in this specification should not necessarily be taken as an admission that the document is part of the state of the art or is common general knowledge. Summary of the invention

[0016] It is an object of the present invention to provide a non-aqueous electrolytic solution which provides improved properties compared to prior art non-aqueous electrolytic solutions.

[0017] Another object of the present invention is to provide an improved process for producing the dioxolanes used according to the invention.

[0018] Usage

[0019] According to a first aspect of the present invention, there is provided a use of a compound of formula 1 in a non-aqueous battery electrolyte formulation.

[0020] According to a second aspect of the present invention, there is provided a use of a non-aqueous battery electrolyte formulation comprising a compound of Formula 1 in a battery.

[0021] Composition / device aspects

[0022] According to a third aspect of the present invention, a battery electrolyte formulation is provided, which comprises a compound of Formula 1.

[0023] According to a fourth aspect of the present invention, there is provided a formulation comprising a metal ion and a compound of formula 1, optionally in combination with a solvent.

[0024] According to a fifth aspect of the present invention, a battery is provided, which comprises a battery electrolyte formulation containing a compound of Formula 1.

[0025] Methodology

[0026] According to a sixth aspect of the present invention, there is provided a method of reducing the flash point of a battery and / or battery electrolyte formulation, comprising adding a formulation comprising a compound of Formula 1.

[0027] According to a seventh aspect of the present invention, there is provided a method of powering an article, comprising using a battery comprising a battery electrolyte formulation containing a compound of Formula 1.

[0028] According to an eighth aspect of the present invention, a method for modifying a battery electrolyte formulation is provided, comprising (a) at least partially replacing the battery electrolyte with a battery electrolyte formulation comprising a compound of Formula 1, and / or (b) supplementing the battery electrolyte with a battery electrolyte formulation comprising a compound of Formula 1.

[0029] According to a ninth aspect of the present invention, there is provided a method for preparing a battery electrolyte formulation, comprising mixing a compound of Formula 1 with a lithium-containing salt and other solvents or co-solvents.

[0030] According to a tenth aspect of the present invention, there is provided a method for preparing a battery electrolyte formulation, comprising mixing a composition comprising a compound of Formula 1 with a lithium-containing compound.

[0031] According to an eleventh aspect of the present invention, there is provided a method for improving battery capacity / charge transfer within a battery / battery lifespan, etc. by using the compound of Formula 1.

[0032] According to a twelfth aspect of the present invention, there is provided a method of reducing an overpotential generated at one or both electrodes of a battery during cycling by using a compound of Formula 1.

[0033] Process

[0034] According to the thirteenth aspect, there is provided a method for preparing a compound of formula 1

[0035] Compound of Formula 1

[0036] With respect to all aspects of the present invention, preferred embodiments of formula (1) are as follows:

[0037]

[0038] Wherein R=H, F, CF3 alkyl or fluoroalkyl.

[0039] "Regioselectivity in addition reactions of some binucleophilic reagents to (trifluoromethyl)acetylene" Stepanova et al., Zhurnal Organicheskoi Khimii (1988), 24 (4), 692-9 describe the preparation of a dioxolane of formula 1, in which all 4 R = H, as a minor byproduct in the reaction of a compound of formula RNH2 (in which R = ethyl or phenyl) and trifluoromethylacetylene with a base and ethylene glycol solvent. Trifluoromethylacetylene is condensed in a potassium hydroxide / methanediol solution at -70°C, then warmed to room temperature and then heated to 80°C for 5 hours. The reaction product is said to contain the linear adduct 2-(3,3,3-trifluoro-1H-propenyloxy)ethanol and the cyclic adduct 2-(2,2,2-trifluoroethyl)-1,3-dioxolane in a ratio of 4:1.

[0040] Suitable dioxolanes can also be prepared by the methods described in this application.

[0041] We have surprisingly found that high yields of the cyclic adduct can be obtained in this reaction if the trifluoromethylacetylene (TFMA) component is maintained under positive pressure in the reaction vessel.

[0042] Therefore, in another aspect of the present invention, there is provided a method for preparing a compound of Formula 1 by reacting a diol with trifluoromethylacetylene under a positive pressure under basic conditions.

[0043] Preferably, the reaction is carried out at a temperature of 0° C. or above, suitably 20° C. or above, suitably at about 40° C. Preferably, the base is KOH.

[0044] Suitably, the diol is reacted with TFMA for a period of at least 1 hour, preferably at least 5 hours, preferably at least 9-10 hours. Ideally, the reaction time should be less than 5 days. We have found that a suitable reaction time is about 72 hours.

[0045] The pressure during the reaction is preferably at least 2 barg, preferably at least 4 barg, preferably at least 6 barg. We have found that a suitable pressure for the reaction is from 8 to 12 barg, preferably about 10 barg. In a preferred embodiment, the gas pressure is monitored and maintained during the reaction and, if necessary, TFMA is replenished to the reaction vessel during the reaction.

[0046] We have also surprisingly found that if a diol or diols are condensed with an aldehyde, a cyclic adduct can be obtained in high yields:

[0047]

[0048] Therefore, in another aspect of the present invention, there is provided a process for preparing a compound of formula 1 by reacting a diol or a diol with an aldehyde.

[0049] Preferably, the diol or glycol is a compound of formula 2a:

[0050]

[0051] In the compound of Formula 2a, each R group may independently comprise a functional group including H, F, Cl, CF3, alkyl, fluoroalkyl, and the like.

[0052] Preferably, the aldehyde is a compound of formula 2b:

[0053]

[0054] In the compounds of Formula 1 and Formula 2b, R' may include functional groups including F, Cl, CF3, alkyl, fluoroalkyl, etc. Suitably, R' is the same as R. In a preferred embodiment, R' is CH2CF3; in a further preferred embodiment, R is H and / or CF3. Suitably, R' is CH2CF3 and R is H and / or CF3.

[0055] The following table includes some examples of preferred diols, aldehydes and their condensation reaction products:

[0056]

[0057]

[0058] The products of these reactions include all stereoisomers, some of which may have different properties, such as melting points, boiling points, or electrochemical properties.

[0059] Suitably, the diol or diol is reacted with the aldehyde for a period of at least 12 hours, preferably at least 24 hours, preferably at least 48 hours. Ideally, the reaction time should be less than 5 days. We have found that a suitable reaction time is about 48 hours.

[0060] The productive rate of reaction can be improved by continuously removing the formed water by-product. The reaction can be carried out at any suitable temperature and pressure so that the water by-product can be effectively removed. Alternatively, the reaction can be carried out in the presence of a reagent (such as molecular sieve or zeolite, sulfuric acid or thionyl chloride) removing the formed water.

[0061] The diol and aldehyde may be present in equal amounts or one may be used in excess of the other. A reaction solvent may advantageously be used to ensure good contact between the diol and the aldehyde. An example of a suitable reaction solvent is dichloromethane.

[0062] Catalysts can be used to increase the reaction rate and improve yield and selectivity. Preferably, the catalyst is an acid, such as p-toluenesulfonic acid.

[0063] For use in battery electrolyte compositions, it is important that the preparation procedure is high yielding and selective, making it possible to recover the compound of formula 1 and purify it to above 95%, for example above 99%.

[0064] Therefore, another object of the present application is to improve the known methods for preparing compounds of formula 1, recovering these compounds and purifying them to a purity of more than 95%, for example more than 99%. The compounds of formula 1 can be prepared in high yield and selectively by reacting TFMA with a diol compound of preferably formula 2 under alkaline conditions and pressure and heating, wherein the pressure in the reactor is maintained by repeated addition of TFMA:

[0065]

[0066] In one embodiment, the alkyl or fluoroalkyl group may have a carbon chain length of C1-C6.

[0067] Preferably, the so-called "alkyl" refers to C1-C6. The so-called "fluorinated alkyl" refers to a partially or fully fluorinated alkyl.

[0068] In a preferred embodiment, at least one R group may be CF3. Suitably, one, two, three or four R groups may be CF3.

[0069] Compounds of formula 1 can also be prepared in high yield and selectively by reacting an aldehyde with a diol compound, preferably of formula 2a, under acidic and dehydrating conditions:

[0070]

[0071] Formula 2a

[0072] In one embodiment, the alkyl or fluoroalkyl group may have a carbon chain length of C1-C6.

[0073] Preferably, the so-called "alkyl" refers to C1-C6. The so-called "fluorinated alkyl" refers to a partially or fully fluorinated alkyl.

[0074] In a preferred embodiment, at least one R group may be CF3. Suitably, one, two, three or four R groups may be CF3.

[0075] advantage

[0076] In various aspects of the present invention, this electrolyte formulation has been found to be surprisingly advantageous.

[0077] The advantages of using compounds of Formula 1 in electrolyte solvent compositions are manifested in many ways. Their presence can reduce the flammability of the electrolyte composition (such as when measured, for example, by flash point). Their oxidative stability makes them useful in batteries that require operation under harsh conditions and high temperatures, and they are compatible with common electrode chemistries and can even enhance the performance of these electrodes through their interactions.

[0078] In addition, the electrolyte composition comprising the compound of Formula 1 can have excellent physical properties, including low viscosity and low melting point, as well as high boiling point, with the associated advantage of little or no gas generation during use. The electrolyte formulation can wet and spread very well on surfaces, especially fluorinated surfaces; this is believed to be due to the favorable relationship between its adhesive and cohesive forces, resulting in a low contact angle.

[0079] In addition, the electrolyte composition comprising the compound of Formula 1 can have excellent electrochemical properties, including improved capacity retention, reduced overpotential generation at one or both electrodes during cycling, improved cycling ability and capacity retention, improved compatibility with other battery components (e.g., separators and current collectors) and with all types of positive and negative electrode chemicals, including systems that operate at a range of voltages and especially high voltages and contain additives such as silicon. In addition, the electrolyte formulation shows good solvation of metal (e.g., lithium) salts and interaction with any other electrolyte solvents present.

[0080] Preferred features associated with various aspects of the invention are as follows. Unless the context indicates otherwise, preferences and options for a given aspect, feature or parameter of the invention should be considered disclosed in any and all combinations of preferences and options for all aspects, features and parameters of the invention.

[0081] Preferred compounds

[0082] The compound of Formula 1 has the following structure:

[0083]

[0084] Wherein R and R'=H, F, Cl, CF3 alkyl or fluoroalkyl.

[0085] In a further preferred embodiment, at least one H group may be replaced by a CF3 group, for example one, two or three H groups may be CF3.

[0086] Preferably, the compound of formula 1 is prepared by a process that facilitates its recovery and purification to greater than 95%, such as greater than 99%.

[0087] Preferably, the compound of Formula 1 has the following structure:

[0088]

[0089] Wherein R=H, F, CF3 alkyl or fluoroalkyl.

[0090] In a preferred embodiment, the compound of Formula 1 is:

[0091]

[0092] In a further preferred embodiment, at least one R group may be CF3. Suitably, one, two, three or four R groups may be CF3.

[0093] Preferably, the compound of formula 1 is prepared by a process that facilitates its recovery and purification to greater than 95%, such as greater than 99%.

[0094] Electrolyte Formula

[0095] The electrolyte formulation will preferably comprise from 0.1 wt% to 99.9 wt% of the compound of formula 1 , suitably from 90.0 wt% to 99.9 wt% of the compound of formula 1 .

[0096] Metal Salts

[0097] The non-aqueous electrolyte solution also includes a metal electrolyte salt, which is generally present in an amount of 0.1 wt % to 20 wt % relative to the total mass of the non-aqueous electrolyte formulation.

[0098] Metal salts typically include salts of lithium, sodium, magnesium, calcium, lead, zinc or nickel.

[0099] Preferably, the metal salt comprises a salt of lithium, such as those selected from the group comprising lithium hexafluorophosphate (LiPF6), lithium hexafluoroarsenate monohydrate (LiAsF6), lithium perchlorate (LiClO4), lithium tetrafluoroborate (LiBF4), lithium trifluoromethanesulfonate (LiSO3CF3), lithium bis(fluorosulfonyl)imide (LiFSI, Li(FSO2)2N) and lithium bis(trifluoromethanesulfonyl)imide (LiTFSI, Li(CF3SO2)2N).

[0100] Most preferably, the metal salt comprises LiPF6, LiFSI or LiTFSI. Thus, in a most preferred variant of the fourth aspect of the invention, a formulation is provided comprising LiPF6, LiFSI, LiTFSI and a compound of formula 1, optionally in combination with one or more co-solvents.

[0101] Solvents

[0102] The non-aqueous electrolytic solution may contain a solvent. Preferred examples of the solvent include fluoroethylene carbonate (FEC) and / or propylene carbonate (PC), dimethyl carbonate (DMC), ethyl methyl carbonate (EMC), ethylene carbonate (EC) or dimethoxyethane (DME).

[0103] When present, the additional solvent comprises from 0.1 wt % to 99.9 wt % of the liquid component of the electrolyte.

[0104] additive

[0105] The non-aqueous electrolytic solution may contain additives.

[0106] Suitable additives can be used as surface film formers, which form an ion permeable film on the surface of the positive electrode or the negative electrode. This can prevent the decomposition reaction of the non-aqueous electrolytic solution and the electrolyte salt occurring on the electrode surface in advance, thereby preventing the decomposition reaction of the non-aqueous electrolytic solution on the electrode surface.

[0107] Examples of the film former additive include vinylene carbonate (VC), vinyl sulfite (ES), lithium bis(oxalato)borate (LiBOB), cyclohexylbenzene (CHB), and o-terphenyl (OTP). The additives may be used alone or in combination of two or more.

[0108] When present, the additive is present in an amount of 0.1 wt % to 3 wt % relative to the total mass of the non-aqueous electrolyte formulation.

[0109] Battery

[0110] Primary battery / Secondary battery

[0111] The battery may comprise a primary battery (non-rechargeable) or a secondary battery (rechargeable).Most preferably, the battery comprises a secondary battery.

[0112] Batteries containing non-aqueous electrolytic solutions typically contain several elements. The elements that make up a preferred non-aqueous electrolyte secondary battery are described below. It is understood that other battery elements (such as temperature sensors) may be present; the following list of battery components is not intended to be exhaustive.

[0113] electrode

[0114] Batteries typically include a positive electrode and a negative electrode. Typically, the electrodes are porous and allow metal ions (lithium ions) to enter and exit their structure through a process called insertion (intercalation) or extraction (deintercalation).

[0115] For rechargeable batteries (secondary batteries), the term "positive electrode" refers to the electrode that undergoes reduction during the discharge cycle. For lithium-ion batteries, the positive electrode ("cathode") is lithium-based.

[0116] Positive electrode (anode)

[0117] The positive electrode is typically comprised of a positive electrode current collector such as a metal foil, optionally with a positive electrode active material layer disposed on the positive electrode current collector.

[0118] The positive electrode current collector may be a metal foil that is stable within the potential range applied to the positive electrode, or a film having a metal surface layer that is stable within the potential range applied to the positive electrode. Aluminum (Al) is ideal as a metal that is stable within the potential range applied to the positive electrode.

[0119] The positive electrode active material layer generally contains the positive electrode active material and other components such as a conductive agent and a binder. This is generally obtained by mixing the components in a solvent, applying the mixture to a positive electrode current collector, followed by drying and roll pressing.

[0120] The positive electrode active material may be lithium (Li) or a lithium-containing transition metal oxide. The transition metal element may be at least one selected from the group consisting of scandium (Sc), manganese (Mn), iron (Fe), cobalt (Co), nickel (Ni), copper (Cu) and yttrium (Y). Among these transition metal elements, manganese, cobalt and nickel are most preferred.

[0121] Furthermore, in certain embodiments, transition metal fluorides may be preferred.

[0122] Some transition metal atoms in the transition metal oxide can be replaced by atoms of non-transition metal elements. The non-transition element can be selected from the group consisting of magnesium (Mg), aluminum (Al), lead (Pb), antimony (Sb) and boron (B). Among these non-transition metal elements, magnesium and aluminum are most preferred.

[0123] Preferred examples of the positive electrode active material include lithium-containing transition metal oxides such as LiCoO2, LiNiO2, LiMn2O4, LiMnO2, LiNi 1-y Co y O2(0 <y<1)、LiNi 1-y-z Co y Mn zO2 (0 < y + z < 1) and LiNi 1-y-z Co y Al z O2 (0 < y + z < 1). From the perspective of cost and specific capacity, LiNi containing nickel in a proportion of not less than 50 mol% relative to all transition metals 1-y-z Co y Mn z O2 (0 < y + z < 0.5) and LiNi 1-y-z Co y Al z O2 (0 < y + z < 0.5) is ideal. These positive electrode active materials contain a large amount of alkaline components, thus accelerating the decomposition of the non-aqueous electrolyte solution, resulting in reduced durability. However, the non-aqueous electrolyte solution of the present disclosure is resistant to decomposition even when used in combination with these positive electrode active materials.

[0124] The positive electrode active material may be a lithium (Li)-containing transition metal fluoride. The transition metal element may be at least one selected from the group consisting of scandium (Sc), manganese (Mn), iron (Fe), cobalt (Co), nickel (Ni), copper (Cu), and yttrium (Y). Among these transition metal elements, manganese, cobalt, and nickel are most preferred.

[0125] Some transition metal atoms in the transition metal fluoride may be replaced by atoms of non-transition metal elements. The non-transition elements may be selected from the group consisting of magnesium (Mg), aluminum (Al), lead (Pb), antimony (Sb), and boron (B). Among these non-transition metal elements, magnesium and aluminum are most preferred.

[0126] A conductive agent may be used to increase the electron conductivity of the positive electrode active material layer. Preferred examples of the conductive agent include conductive carbon materials, metal powders, and organic materials. Specific examples include carbon materials such as acetylene black, Ketjen black, and graphite, metal powders such as aluminum powder, and organic materials such as phenyl derivatives.

[0127] An adhesive may be used to ensure good contact between the positive electrode active material and the conductive agent, and to increase the adhesion of components such as the positive electrode active material to the surface of the positive electrode current collector. Preferred examples of the adhesive include fluorine-containing polymers and rubber polymers, such as polytetrafluoroethylene (PTFE), polyvinylidene fluoride (PVdF), ethylene-propylene-isoprene copolymer, and ethylene-propylene-butadiene copolymer. The adhesive may be used in combination with a thickener such as carboxymethyl cellulose (CMC) or polyethylene oxide (PEO).

[0128] Negative electrode (cathode)

[0129] The negative electrode is usually composed of a negative electrode current collector such as a metal foil, optionally having a negative electrode active material layer provided on the negative electrode current collector.

[0130] The negative electrode current collector may be a metal foil. Copper (without lithium) is suitable as the metal. Copper is easy to process at low cost and has good electronic conductivity.

[0131] Typically, the negative electrode comprises carbon, such as graphite or graphene, or lithium metal. In a preferred embodiment, the negative electrode is lithium metal.

[0132] Silicon-based materials may also be used for the negative electrode. A preferred form of silicon is in the form of nanowires, which are preferably present on a support material. The support material may include a metal (such as steel) or a non-metal such as carbon.

[0133] The negative electrode may include an active material layer. When present, the active material layer comprises the negative electrode active material and other components such as a binder. This is typically obtained by mixing the components in a solvent, applying the mixture to the positive electrode current collector, followed by drying and rolling.

[0134] There is no particular limitation on the negative electrode active material, provided that these materials can store and release lithium ions. Examples of suitable negative electrode active materials include carbon materials, metals, alloys, metal oxides, metal nitrides, and lithium intercalated carbon and silicon. Examples of carbon materials include natural / artificial graphite and pitch-based carbon fibers. Preferred examples of metals include lithium (Li), silicon (Si), tin (Sn), germanium (Ge), indium (In), gallium (Ga), titanium (Ti), lithium alloys, silicon alloys, and tin alloys. Examples of lithium-based materials include lithium titanate (Li2TiO3).

[0135] The active materials can be in many forms, such as thin films, foils, or supported on a three-dimensional matrix.

[0136] As with the positive electrode, the binder may be a fluorine-containing polymer or a rubber polymer, and is desirably a rubbery polymer such as styrene-butadiene copolymer (SBR). The binder may be used in combination with a thickener.

[0137] In a preferred embodiment, in a secondary battery, the negative electrode is lithium metal; suitably, in such embodiments, but also in other embodiments with other negative electrodes and in other battery types, the electrolyte comprises LiTFSI and / or LiFSI, dimethoxyethane and a compound of formula 1.

[0138] Diaphragm

[0139] The separator is preferably present between the positive electrode and the negative electrode. The separator has insulating properties. The separator may include a porous membrane having ion permeability. Examples of porous membranes include microporous films, woven fabrics, and nonwoven fabrics. Suitable materials for the separator are polyolefins, such as polyethylene and polypropylene.

[0140] case

[0141] The battery components are preferably disposed within a protective housing.

[0142] The housing may comprise any suitable material that is resilient to provide support for the battery and electrical contact to the device being powered.

[0143] In one embodiment, the housing comprises a metal material, preferably in sheet form, molded into the shape of the battery. The metal material preferably comprises a plurality of parts adapted to fit together (e.g. by push fit) in battery assembly. Preferably, the housing comprises an iron / steel based material.

[0144] In another embodiment, the housing comprises a plastic material molded into the shape of a battery. The plastic material preferably comprises a plurality of parts suitable for being connected together (e.g., by push fit / adhesion) in the battery assembly. Preferably, the housing comprises a polymer such as polystyrene, polyethylene, polyvinyl chloride, polyvinylidene chloride, or polymonochlorofluoroethylene. The housing may also include other additives for the plastic material, such as fillers or plasticizers. In this embodiment where the housing for the battery comprises primarily plastic material, a portion of the housing may additionally include a conductive / metal material to establish electrical contact with a device powered by the battery.

[0145] Layout

[0146] The positive electrode and the negative electrode may be wound or stacked together through a separator. They are contained in a casing together with a non-aqueous electrolytic solution. The positive electrode and the negative electrode are electrically connected to the casing as separate parts.

[0147] Module / Battery Pack

[0148] Many / multiple battery cells can constitute a battery module. In a battery module, the battery cells can be organized in series and / or in parallel. Typically, these are packaged in a mechanical structure.

[0149] A battery pack can be assembled by connecting multiple modules in series or in parallel. Typically, the battery pack includes further features such as sensors and controllers, including a battery management system and a thermal management system. The battery pack usually includes a packaging shell structure to form the final battery pack product.

[0150] End Use

[0151] The batteries of the present invention (in the form of individual batteries / cells, modules and / or packs (and their electrolyte formulations)) are intended for use in one or more of a variety of end products.

[0152] Preferred examples of end products include portable electronic devices such as GPS navigation devices, cameras, laptops, tablet computers and mobile phones. Other preferred examples of end products include vehicle devices (powering the propulsion system and / or any electrical system or device present therein) such as electric bicycles and motorcycles and automotive applications (including hybrid and pure electric vehicles).

[0153] Unless the context dictates otherwise, preferences and options for a given aspect, feature or parameter of the invention should be considered disclosed in any and all combinations with preferences and options for all other aspects, features and parameters of the invention. BRIEF DESCRIPTION OF THE DRAWINGS

[0154] Figure 1 Figures a to c show the reaction of LiPF6 and 2-(2,2,2-trifluoroethyl)-1,3-dioxolane in propylene carbonate. 19 F NMR spectrum. Figure 1 The invention relates to a composition comprising LiPF6 / 2-(2,2,2-trifluoroethyl)-1,3-dioxolane / propylene carbonate.

[0155] Figures 2a to 2c show the reaction of LiPF6 and 2-(2,2,2-trifluoroethyl)-1,3-dioxolane in propylene carbonate (90%) and fluoroethylene carbonate (10%). 19 F NMR spectrum. Figures 2a to 2c relate to compositions comprising LiPF6 / 2-(2,2,2-trifluoroethyl)-1,3-dioxolane / propylene carbonate and fluoroethylene carbonate.

[0156] Figures 3a to 3c show the reaction of LiPF6 and 2-(2,2,2-trifluoroethyl)-1,3-dioxolane in ethylene carbonate (30%) and ethyl methyl carbonate (70%). 19 F NMR spectrum. Figures 3a to 3c relate to compositions comprising LiPF6 / 2-(2,2,2-trifluoroethyl)-1,3-dioxolane / ethylene carbonate and ethyl methyl carbonate.

[0157] Figures 4a to 4c show the reaction of LiFSI and 2-(2,2,2-trifluoroethyl)-1,3-dioxolane in propylene carbonate. 19 F NMR spectrum. Figures 4a to 4c relate to compositions comprising LiFSI / 2-(2,2,2-trifluoroethyl)-1,3-dioxolane / propylene carbonate.

[0158] Figures 5a to 5c show the reaction of LiFSI and 2-(2,2,2-trifluoroethyl)-1,3-dioxolane in propylene carbonate (90%) and fluoroethylene carbonate (10%). 19F NMR spectrum. Figures 5a to 5c relate to compositions comprising LiFSI / 2-(2,2,2-trifluoroethyl)-1,3-dioxolane / propylene carbonate and fluoroethylene carbonate.

[0159] Figures 6a to 6c show the reaction of LiFSI and 2-(2,2,2-trifluoroethyl)-1,3-dioxolane in ethylene carbonate (30%) and ethyl methyl carbonate (70%). 19 F NMR spectrum. Figures 6a to 6c relate to a composition comprising LiFSI / 2-(2,2,2-trifluoroethyl)-1,3-dioxolane / ethylene carbonate and ethyl methyl carbonate.

[0160] Figure 7 The electrochemical performance of MEXI-20-cell chemistry 1 is shown.

[0161] Figure 8 The electrochemical performance of MEXI-20-cell chemistry 2 is shown.

[0162] Fig. 9 The electrochemical performance of MEXI-20-cell chemistry 1 is shown.

[0163] Fig.10 The electrochemical performance of MEXI-20-cell chemistry 2 is shown.

[0164] Fig.11 The electrochemical performance of the basic electrolyte in a symmetric Li / Li / Li cell is shown.

[0165] Fig.12 The electrochemical performance of the control electrolyte in a symmetric Li / Li / Li cell is shown.

[0166] Fig.13 The electrochemical performance of the basic electrolyte in Cu / Li is shown.

[0167] Fig.14 The electrochemical performance of the control electrolyte in a Cu / Li cell is shown.

[0168] Fig.15 The electrochemical performance of the control electrolyte in a symmetric Li / Li / Li cell is shown.

[0169] Fig.16 The electrochemical performance of the control electrolyte in a Cu / Li cell is shown. DETAILED DESCRIPTION

[0170] The invention will now be illustrated with reference to the following non-limiting examples.

[0171] Example

[0172] Example 1-Synthesis, separation and electrochemical measurement of 2-(2,2,2-trifluoroethyl)-1,3-dioxolane (Mexi-20) try

[0173]

[0174] Potassium hydroxide (4.02 g, 85 wt%) was dissolved in ethylene glycol (20 g) with stirring in a 100 ml pressure reaction vessel. Once dissolution was complete, the reaction vessel was sealed, purged with nitrogen and the contents were heated to 40°C with stirring and then pressurized to 8 barg with trifluoromethylacetylene (TFMA). After 52 minutes, the pressure dropped to 6.4 barg and was repressurized to 10 barg with more TFMA. This pressure loss and repressurization pattern was repeated several times over 6 hours before a final pressurization to 10 barg with TFMA. After further stirring at 40°C for 72 hours, the final pressure in the reaction vessel was 6.4 barg.

[0175] After cooling and decompression, the contents of the reactor were recovered as a viscous yellow oil. To this oil was added 21 g of water to achieve phase separation. The lower organic layer was recovered and repeatedly washed with 50 ml aliquots of water. The product was dried over anhydrous sodium sulfate to obtain 16.1 g of product.

[0176] The crude product was analyzed by GC-MS and shown to contain the desired product and an unsaturated ether byproduct identified as CF3CH=CHOCH2CH2OH in a ratio of 6.1:1.

[0177] The desired product is separated from the by-products in the crude product by distillation and 19 F NMR (56 MHz) δ-64.5 (t, J = 11.0 Hz) analysis. The mass spectrum of the desired product contained characteristic fragments at m / z 155, 126, 111, 73, 69, 45.

[0178] For preparative purposes, the procedure was scaled up. Therefore, KOH (40 g, 85%) was dissolved in ethylene glycol (200 g) and transferred to a 450 ml Hastelloy autoclave. The autoclave was sealed, pressure tested and purged with nitrogen, and the contents were then heated to 40°C with stirring. While at this temperature, the autoclave was pressurized to 9-10 Barg with TFMA. The pressure within the vessel dropped as the TFMA reacted. When the pressure dropped to about 3 barg, the vessel was re-pressurized with TFMA. This cycle of reaction and re-pressurization steps was continued until the rate of TFMA consumption became negligible. In a typical procedure, the reactor would be re-pressurized 5-6 times over the course of about 3 days.

[0179] Five batches of crude product were prepared. The crude product was separated from the reaction mixture by quenching with water, which resulted in product separation so that it could be recovered. The isolated crude product was further washed with water to remove trace amounts of potassium salts and then dried over sodium sulfate. The products from each batch were combined to obtain 269 g of a light yellow oil, which was analyzed by GCMS and found to contain 93% of the desired product 2-(2,2,2-trifluoroethyl)-1,3-dioxolane.

[0180] The crude product was further purified by distillation using a packed column to give the following fractions:

[0181]

[0182] Fractions 2-6 were combined and analyzed by a combination of GC-MS and multinuclear NMR spectroscopy:

[0183] Purity (GC-MS area %) 99.1

[0184] Mass spectrum m / z: 155, 126, 111, 91, 77, 73, 69, 57, 45, 43

[0185] 1 H NMR(60MHz)δ5.12(t,J=5.12Hz,1H),3.92(d,J=2.1Hz,4H),2.48(qd,J=10.9,4.8Hz,2H)

[0186] 19 F NMR(56MHz)δ-64.5(t,J=11.0Hz)

[0187] 13 C NMR(15MHz)δ125.97(q,j=276.2Hz),99.37(q,3.9Hz),65.46(s),39.47(q,27.6Hz)

[0188] The spectral information clearly confirmed that the purified product was the desired compound of Formula 1: 2-(2,2,2-trifluoroethyl)-1,3-dioxolane (Mexi-20). In addition, the data showed that it can be prepared in high yield and selectivity, so that it can be purified to above 99% and can therefore be used in lithium ion and lithium metal battery electrolyte compositions.

[0189] Compositions of the present invention (all in % w / w):

[0190] Table 1: Compositions containing 2-(2,2,2-trifluoroethyl)-1,3-dioxolane and lithium hexafluorophosphate (LiPF6)

[0191]

[0192] Table 2: Compositions containing 2-(2,2,2-trifluoroethyl)-1,3-dioxolane and lithium bis(fluorosulfonyl)imide (LiFSI)

[0193]

[0194] Flammability and safety testing

[0195] For convenience, 2-(2,2,2-trifluoroethyl)-1,3-dioxolane is hereinafter referred to as Mexi-20.

[0196] Flash point

[0197] Flash point was determined using a Miniflash FLP / H apparatus from Grabner Instruments according to ASTM D6450 standard method:

[0198]

[0199] These measurements show that the addition of the additive designated MEXI-20 increases the flash point of the standard electrolyte solution.

[0200] Self-extinguishing time

[0201] The self-extinguishing time was measured using a custom-made device consisting of an automatically controlled stopwatch connected to a UV detector. In this experiment, the electrolyte to be tested (500 μL) was applied to a Whatman GF / D The ignition source was transferred under the sample and held in this position for a preset time (1, 5 or 10 seconds) to ignite the sample. Ignition and combustion of the sample was detected using a UV light detector. The burning time / electrolyte weight [sg -1 ] The ignition time [s] was plotted and evaluated by extrapolating the linear regression line to the ignition time = 0s. Self-extinguishing time (sg -1 ) is the time required for the sample to stop burning from ignition.

[0202]

[0203] These measurements demonstrate that compound MEXI-20 has flame retardant properties.

[0204] Electrochemical testing

[0205] Lithium-ion battery

[0206] dry

[0207] Prior to testing, MEXI-20 was dried to less than 10 ppm water by treatment with preactivated type 4A molecular sieves.

[0208] Electrolyte preparation

[0209] Electrolyte preparation and storage were performed in an argon-filled glove box (H2O and O2 < 0.1 ppm). The base electrolyte was 1 M LiPF6 dissolved in ethylene carbonate: ethyl methyl carbonate (3:7 wt%) with MEXI-20 additive at concentrations of 2 wt%, 5 wt%, 10 wt%, and 30 wt%.

[0210] Battery chemistry and construction

[0211] The performance of each electrolyte formulation was tested over 50 cycles in multilayer pouch cells (2 cells per electrolyte):

[0212] Chemistry 1: Lithium-nickel-cobalt-manganese oxide (NCM622) positive electrode and artificial graphite (specific capacity: 350 mAh g -1 ) negative electrode. The areal capacities of NMC622 and graphite are 3.5 mAh cm -2 and 4.0mAh cm -2 . The N / P ratio is 115%.

[0213] Chemistry 2: Lithium-nickel-cobalt-manganese oxide (NCM622) positive electrode and SiO x / Graphite (Specific capacity: 550mAh g -1 ) Negative electrode. NMC622 and SiO x The area capacity of graphite is 3.5 mAh / cm -2 and 4.0mAh cm -2 . The N / P ratio is 115%.

[0214] The tested soft pack batteries have the following characteristics:

[0215] Nominal capacity 240mAh+ / -2%

[0216] Standard Deviation:

[0217] Capacity: ±0.6mAh

[0218] Coulombic efficiency (CE) 1st cycle: ±0.13%

[0219] Coulombic efficiency (CE) subsequent cycles: ±0.1%

[0220] Positive electrode: NMC-622

[0221] Active material content: 96.4%

[0222] Mass loading: 16.7 mg cm -2

[0223] Negative electrode: artificial graphite

[0224] Active material content: 94.8%

[0225] Mass loading: 10 mg cm -2

[0226] ·Separator: PE (16μm) + 4μm Al2O3

[0227] Balanced at 4.2V cut-off voltage

[0228] Negative electrode: artificial graphite + SiO

[0229] Active material content: 94.6%

[0230] Mass loading: 6.28 mg cm -2

[0231] ·Separator: PE (16μm) + 4μm Al2O3

[0232] Balanced at 4.2V cut-off voltage

[0233] After assembly, the following formation scheme was used (CC = constant current charge and CCCV = constant current constant voltage charge):

[0234] 1. Stage charge to 1.5V, followed by a 5-hour rest step (wetting step at 40°C)

[0235] 2.CCCV(C / 10,3.7V(I 极限 : 1 hour)) (pre-forming step)

[0236] 3. Resting step (6 hours)

[0237] 4.CCCV(C / 10,4.2V(I 极限 : 0.05C))Station step (20 minutes)

[0238] 5.CC discharge (C / 10, 3.8V), (battery degassing)

[0239] 6.CC discharge (C / 10, 2.8V)

[0240] After this formation step, the cells were tested as follows:

[0241] ·Station step (1.5V, 5 hours), CCCV (C / 10, 3.7V (1h))

[0242] Rest step (6 hours), CCCV (C / 10, 4.2 V (I 极限 :0.05C))

[0243] Rest step (20 minutes), CC discharge (C / 10, 3.8V)

[0244] Degassing step

[0245] Discharge (C / 10, 2.8V), rest step (5 hours)

[0246] CCCV(C / 3,4.2V(I 极限 : 0.05C)), rest step (20 minutes)

[0247] CC discharge (C / 3, 2.8V)

[0248] 50 cycles at 40°C or until 50% SOH is reached:

[0249] CCCV(C / 3,4.2V(I 极限 : 0.02C), rest step (20 min)

[0250] CC discharge (C / 3, 3.0V), rest step (20 minutes)

[0251] Test Results

[0252] The test results of MEXI-20 for additives in each battery chemistry are summarized in Figure 7-10 middle.

[0253] Lithium Metal Batteries

[0254] Symmetrical Li / Li / Li battery

[0255] Electrolyte preparation

[0256] Electrolyte solution preparation and storage were performed in an argon-filled glove box (H2O and O2 < 0.1 ppm):

[0257] Base electrolyte: 1M LiTFSI dissolved in dimethoxyethane (DME): dioxolane (DOL) (1:1 wt%)

[0258] Control electrolyte: 1M LiTFSI dissolved in DME:Mexi-20 (1:1 wt%)

[0259] Battery Construction, Testing and Chemistry

[0260] Symmetrical 3-electrode Li / electrolyte / Li cells ("Swagelok cells") were filled with base and control electrolytes and used for electrochemical testing and for determining their key performance indicators (5 cells per electrolyte, 10 cells in total).

[0261] This cell chemistry was chosen because it is considered a “state of the art” cell chemistry for measuring the stripping and plating behavior of metallic lithium and the evolution of overpotential during stripping and plating. A symmetric Li / Li / Li cell was charged at 0.1 mA / cm 2 Cycling. The charging and discharging times were 1 hour each (a cycle is defined as a charging step followed by a discharging step). The battery was cycled at 20°C for 25 days.

[0262] result

[0263] The results are as follows Fig.11 and Fig.12 shown.

[0264] For the base electrolyte, an exponential increase in the overpotential was observed during the continuous stripping and plating of lithium metal. In addition, a strong increase in the cell resistance was observed, which was caused by the extensive degradation of the electrolyte on the Li electrode. For the control electrolyte, a constant and lower overpotential was observed during the continuous stripping and plating of lithium metal. The overpotential remained stable throughout the measurements. The studied compound (MEXI-20) showed the ability to form or modify SEI on lithium at a concentration of 50 wt% and in combination with DME as a co-solvent.

[0265] These electrochemical test results of Li / Li / Li cells show that the cycling performance of the cells is positively affected by MEXI-20 at a concentration of 50 wt%. During the continuous stripping and plating of lithium metal, the electrolyte containing MEXI-20 shows a constant and fairly low overpotential. It is believed that this is because the electrolyte containing MEXI-20 forms a low-resistance passivation layer on the lithium metal, and therefore MEXI-20 can be beneficially used as a co-solvent in rechargeable lithium metal batteries.

[0266] Cu / Li battery

[0267] Electrolyte preparation

[0268] Electrolyte preparation and storage were performed in an argon-filled glove box (H2O and O2 < 0.1 ppm).

[0269] Base electrolyte: 1M LiTFSI dissolved in DME:DOL (1:1 wt%)

[0270] Control electrolyte: 1M LiTFSI dissolved in DME:Mexi-20 (1:1 wt%)

[0271] Battery Construction, Testing and Chemistry

[0272] Two-electrode Cu / electrolyte / Li cells (coin cells) filled with base electrolyte and control electrolyte were used for electrochemical testing and for determination of key performance indicators (5 cells per electrolyte, 10 cells in total).

[0273] This cell chemistry was chosen because it represents the “state of the art” cell chemistry used to measure the stripping and plating behavior of metallic lithium and the evolution of the Coulombic efficiency during cycling.

[0274] Cycling: For the charging process (lithium deposition), the battery was charged at 1 mA / cm 2 Cycle for 1 hour. For the discharge process (lithium dissolution), the battery was charged at 0.25 mA / cm 2 Cycling was performed until a Cu electrode cutoff voltage of 1 V was reached (a cycle is defined as one charging step followed by one discharging step). The cells were cycled for 100 cycles (approximately 25 days) at 20°C.

[0275] result

[0276] The test results are summarized in Figure 13-14 middle.

[0277] Fig.13 Test data for the following base electrolyte is shown: 1M LiTFSI dissolved in DME:DOL (1:1 wt %):

[0278] In the first 10 cycles, the battery Coulombic efficiency (CE) increased to about 88%

[0279] Increased fluctuations in discharge capacity and CE during continuous stripping and plating of lithium metal after 35 cycles

[0280] This strong increase is believed to be caused by the continuous degradation of the electrolyte and the formation of high surface area lithium metal on the Cu electrode.

[0281] The CE increase of more than 100% clearly indicates that the formation and growth of dendrites can cause small short circuits in the battery and lead to battery performance degradation.

[0282] Fig.14 Test data for the following control electrolyte is shown: 1M LiTFSI dissolved in DME:Mexi 20 (1:1 wt %):

[0283] Within the first 10 cycles, the CE of the battery increased to about 88%

[0284] The discharge capacity and CE evolution are stable during continuous stripping and plating of lithium metal

[0285] CE and discharge capacity show only limited decay over 100 cycles

[0286] This stable performance is indicative of a more efficient surface layer formation when Mexi-20 is present in the electrolyte

[0287] No evidence of dendrite formation or cell shorting

[0288] These results indicate that replacing DOL with Mexi-20 leads to more stable cycling performance and fewer parasitic reactions. There is no evidence of lithium metal dendrite formation and short circuits in the cells containing Mexi-20, and the electrolyte containing Mexi-20 leads to a strong increase in the first cycle CE.

[0289] These results further demonstrate the practicality of Mexi-20 in secondary (rechargeable) batteries with lithium metal anodes.

[0290] Example 2

[0291] Synthesis and Isolation of 5-Trifluoromethyl-2-(2,2,2-trifluoroethyl)-1,3-dioxolane (Mexi-19)

[0292] Preparation of Mexi-19 via cycloaddition of 3,3,3-trifluoropropanal and 3,3,3-trifluoropropane-1,2-diol:

[0293]

[0294] 3,3,3-trifluoropropanal is prepared by dehydrating 3,3,3-trifluoropropanal hydrate with phosphorus pentoxide and used immediately. 850 g of the newly prepared aldehyde is loaded into a 5-liter flask equipped with a magnetic stirrer, a heating jacket, an improved Dean-Stark trap and a reflux condenser. 930 g (7.15 mol) of 3,3,3-trifluoropropane-1,2-diol is added, followed by 2 liters of dichloromethane and 20 g of p-toluenesulfonic acid monohydrate catalyst. The mixture is vigorously refluxed for 48 hours while continuously removing the water produced by the reaction.

[0295] After cooling to room temperature, the reaction mixture was neutralized by washing in a separatory funnel with one liter of saturated aqueous sodium bicarbonate solution and then twice with one liter of water.

[0296] The organic (bottom) phase was dried over anhydrous magnesium sulfate and filtered. Dichloromethane and unreacted aldehyde were removed on a rotary evaporator. The crude product was fractionated using a rotating belt distillation column to give a product with a purity of >99.6% (GC area %) and a boiling point of 58°C-60°C at 25 mmHg. The two diastereomers were present in a ratio of about 5:1. The yield was 1,046 g (65% of theoretical based on the limited diol reactant).

[0297] The product Molecular sieve drying and passing 19 F NMR spectroscopy confirmed its structure: 19 F NMR (56MHz) δ-61.4, 61.7 (t, J = 10.6 Hz), 75.6, 76.7 (d, J = 6.2 Hz).

[0298] The flash point of Mexi-19 was determined as described above to be 138 ± 4°C.

[0299] The electrochemical performance of Mexi-19 in symmetric Li / Li / Li cells and Cu / Li was determined in the same manner as described above for Mexi-20, firstly drying it by treatment with 4A molecular sieves.

[0300] Electrochemical test results in symmetric Li / Li / Li battery

[0301] The test results are as follows Fig.15 as shown (and should be Fig.11 (For comparison). As in the case of Mexi-20, the cells constructed using the electrolyte containing Mexi-19 exhibited a constant and fairly low overpotential during the continuous stripping and plating of lithium metal. Moreover, the overpotential remained stable throughout the measurements. This behavior was found to be highly reproducible over multiple repetitions of the experiment.

[0302] Electrochemical test results in symmetric Cu / Li battery

[0303] The test results are as follows Fig.16 As shown (should be Fig.13 (Compare). Although Mexi-19 shows a lower CE for lithium stripping from and plating onto the Cu electrode compared to the base electrolyte, it is apparent that the discharge capacity and CE are more stable. In addition, there is little decay in CE and discharge capacity after 100 cycles. This stable performance indicates that a more effective surface layer is formed on Cu in the presence of Mexi-19. There is no evidence of lithium metal dendrites and short circuits formed in the cell during cycling.

Claims

1. Use of the compound of formula 1 in non-aqueous battery electrolyte formulations Where R and R' are H, F, Cl, CF 3 , alkyl or fluoroalkyl.

2. The use according to claim 1, wherein the alkyl group R and / or R' is a carbon chain length of C 1 To C 6 An alkyl or fluoroalkyl group.

3. Use according to claim 1 or 2, wherein the formulation comprises a metal electrolyte salt present in an amount of 0.1 wt% to 20 wt% relative to the total mass of the non-aqueous electrolyte formulation.

4. The use according to claim 3, wherein the metal salt is a salt of lithium, sodium, magnesium, calcium, lead, zinc or nickel.

5. The use according to claim 4, wherein the metal salt is selected from the group consisting of lithium hexafluorophosphate (LiPF 6 ), lithium tetrafluoroborate (LiBF 4 ), lithium perchlorate (LiClO 4 ), lithium trifluoromethanesulfonate (LiSO 3 CF3), Lithium Bis(Fluorosulfonyl)imide (LiFSI, Li(FSO 2 ) 2 N) and lithium bis(trifluoromethanesulfonyl)imide (LiTFSI, Li(CF3SO 2 ) 2 N) of the group consisting of lithium salts.

6. Use according to any one of claims 1 to 5, wherein the formulation comprises an additional solvent in an amount of 0.1% to 99.9% by weight of the liquid component of the formulation.

7. Use according to claim 6, wherein the additional solvent is selected from the group comprising fluoroethylene carbonate (FEC), propylene carbonate (PC) or ethylene carbonate, dimethoxyethane or thionyl chloride.

8. Use according to any one of the preceding claims, wherein the battery is a secondary battery, the negative electrode is lithium metal, and the electrolyte comprises a compound of formula 1, dimethoxyethane and lithium bis(fluorosulfonyl)imide and / or lithium bis(trifluoromethanesulfonyl)imide.

9. A battery electrolyte formulation comprising a compound of formula 1: Where R and R' are H, F, Cl, CF 3 , alkyl or fluoroalkyl.

10. A formulation comprising a metal ion and a compound of formula 1, optionally in combination with a solvent: Where R and R' are H, F, Cl, CF 3 , alkyl or fluoroalkyl.

11. A battery comprising a battery electrolyte formulation containing a compound of formula 1: Where R is H, F, Cl, CF 3 , alkyl or fluoroalkyl.

12. The formulation according to any one of claims 9 to 11, wherein the formulation comprises a metal electrolyte salt present in an amount of 0.1 wt% to 20 wt% relative to the total mass of the non-aqueous electrolyte formulation.

13. The formulation of claim 12, wherein the metal salt is a salt of lithium, sodium, magnesium, calcium, lead, zinc or nickel.

14. The formulation according to claim 13, wherein the metal salt is selected from the group consisting of lithium hexafluorophosphate (LiPF 6 ), lithium perchlorate (LiClO 4 ), lithium tetrafluoroborate (LiBF 4 ), lithium trifluoromethanesulfonate (LiSO 3 CF3), Lithium Bis(Fluorosulfonyl)imide (LiFSI, Li(FSO 2 ) 2 N) and lithium bis(trifluoromethanesulfonyl)imide (LiTFSI, Li(CF3SO 2 ) 2 N) of the group consisting of lithium salts.

15. A formulation according to any one of claims 9 to 14, wherein the formulation comprises an additional solvent in an amount of 0.1% to 99.9% by weight of the liquid component of the formulation.

16. The formulation according to claim 15, wherein the additional solvent is selected from the group comprising fluoroethylene carbonate (FEC), propylene carbonate (PC) and ethylene carbonate (EC), dimethoxyethane or thionyl chloride.

17. A method of reducing the flammability of a battery and / or battery electrolyte comprising adding a formulation comprising a compound of formula 1: Where R or R' is H, F, Cl, CF 3 , alkyl or fluoroalkyl.

18. A method of powering an article comprising using a battery comprising a battery electrolyte formulation comprising a compound of Formula 1: Where R or R' is H, F, Cl, CF 3 , alkyl or fluoroalkyl.

19. A method of modifying a battery electrolyte formulation, comprising (a) at least partially replacing the battery electrolyte with a battery electrolyte formulation comprising a compound of Formula 1 and / or (b) supplementing the battery electrolyte with a battery electrolyte formulation comprising a compound of Formula 1: Where R or R' is H, F, Cl, CF 3 , alkyl or fluoroalkyl.

20. A method of preparing a battery electrolyte formulation comprising mixing a compound of formula 1 with ethylene carbonate, propylene carbonate or fluoroethylene carbonate and lithium hexafluorophosphate.

21. A method for improving battery capacity / charge transfer within a battery / battery life, etc. by using the compound of formula 1.

22. The method of any one of claims 17 to 21, wherein the formulation comprises a metal electrolyte salt present in an amount of 0.1 wt% to 20 wt% relative to the total mass of the non-aqueous electrolyte formulation.

23. The method of claim 22, wherein the metal salt is a salt of lithium, sodium, magnesium, calcium, lead, zinc or nickel.

24. The method according to claim 23, wherein the metal salt is selected from the group consisting of lithium hexafluorophosphate (LiPF 6 ), lithium perchlorate (LiClO 4 ), lithium tetrafluoroborate (LiBF 4 ), lithium trifluoromethanesulfonate (LiSO 3 CF3), Lithium Bis(Fluorosulfonyl)imide (LiFSI, Li(FSO 2 ) 2 N) and lithium bis(trifluoromethanesulfonyl)imide (LiTFSI, Li(CF3SO 2 ) 2 N) of the group consisting of lithium salts.

25. A method according to any one of claims 17 to 24, wherein the formulation comprises additional solvent in an amount of from 0.1% to 99.9% by weight of the liquid component of the formulation.

26. The method according to claim 25, wherein the additional solvent is selected from the group comprising fluoroethylene carbonate (FEC), propylene carbonate (PC) and ethylene carbonate (EC), dimethoxyethane or thionyl chloride.

27. A method for preparing a compound of formula 1, preferably the following compound: Where R is H, F, CF 3 , alkyl or fluoroalkyl It involves reacting a diol with trifluoromethylacetylene under positive pressure and alkaline conditions.

28. The method according to claim 27, wherein the diol compound is a compound of Formula 2:

29. A process according to claim 27 or claim 28, wherein the reaction is carried out at above 0°C.

30. The method according to any one of claims 27 to 29, wherein the reaction is carried out for 9 to 10 hours.

31. A process according to any one of claims 27 to 30 wherein the reaction pressure is maintained at 8 to 12 barg.

32. A method for preparing a compound of formula 1: Where R and R' are H, Cl, F, CF 3 , alkyl or fluoroalkyl; This involves condensing a diol or glycol with an aldehyde.

33. The method of claim 32, wherein the diol compound is a compound of formula 2a: Each R may independently include H, F, Cl, CF 3 , alkyl or fluoroalkyl functional groups and optional similar functional groups, and preferably H, F, Cl, CF 3 Alkyl or fluoroalkyl.

34. A method according to claim 32 or claim 33, wherein the aldehyde is a compound of formula 3: Where R' can include F, Cl, CF 3 , alkyl or fluoroalkyl functional groups and optionally similar functional groups, and preferably F, Cl, CF 3 , alkyl or fluoroalkyl.

35. The process according to any one of claims 32 to 34, wherein the reaction is carried out in the presence of an acid catalyst.