Separator, secondary battery and electronic device
By coating organic cyanide with specific functional groups on the secondary battery separator, the problem of performance deterioration of high-energy-density secondary batteries at high temperatures is solved, and its thermal safety and high-temperature cycling performance is significantly improved, achieving higher energy density and stability.
Patent Information
- Application Number
- CN202411171725.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-26
- Publication Date
- 2024-11-12
AI Technical Summary
High-energy density secondary batteries are prone to performance deterioration at high temperatures, resulting in reduced safety performance and difficult to maintain stability.
The separator of the secondary battery is coated with organic cyanide with specific functional groups. By controlling its molar concentration and element content, the surface of the positive electrode material is stabilized, structural phase change is suppressed, and thermal safety performance and high-temperature circulation performance are improved.
It effectively improves the thermal safety performance and high-temperature circulation performance of secondary batteries, extends the service life of the battery, and improves the energy density.
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_3
Abstract
Description
Technical Field
[0001] The present application relates to the field of energy storage technology, and in particular to a diaphragm, a secondary battery and an electronic device. Background Art
[0002] With the popularization and application of smart products, people's demand for electronic products such as mobile phones, laptops, cameras, etc. has increased year by year. Secondary batteries have the advantages of long life, low self-discharge, no memory effect and environmental friendliness, and have become the most valued new energy storage battery. However, with the advancement of science and technology and the continuous improvement of living standards, people's requirements for the energy density of secondary batteries are also increasing.
[0003] However, high energy density secondary batteries are prone to high temperature performance degradation. Therefore, it is urgent to provide a high energy density secondary battery with good high temperature performance. Summary of the invention
[0004] In view of this, the embodiments of the present application provide a diaphragm, a secondary battery and an electronic device, which have good high-temperature performance on the basis of high energy density.
[0005] In a first aspect, an embodiment of the present application provides a diaphragm, the diaphragm comprising a base film and a first coating disposed on a surface of the base film for facing a positive electrode plate, the first coating comprising an organic cyanide having a first functional group, the first functional group comprising at least one of a cyano group, an isocyano group, an isocyanate group, or a melamine derivative. Based on the volume of the first coating, the molar concentration of the first functional group is Mfmol / μm 3 , 0.1≤M≤30.
[0006] Based on the diaphragm of the embodiment of the present application, the inventors found that as the charging voltage of the high energy density secondary battery increases, the oxygen atoms in the positive lithium layer lose their barrier and repel each other, and the lithium is continuously removed, causing gas overflow from the surface lattice, and the surface structure of the positive lithium cobalt oxide material decreases steadily, and an irreversible structural phase change gradually occurs, resulting in a decrease in safety performance. A specific concentration of organic cyanide is coated on the positive electrode side surface of the diaphragm, and the organic cyanide diffuses and contacts the surface of the positive electrode material, which can stabilize the metal atoms and the positive electrode crystal structure, reduce the release of active oxygen, and inhibit the structural phase change of materials such as lithium cobalt oxide that causes the electrochemical performance of the material to decay during high voltage charging and discharging, thereby improving the stability of the positive electrode, and thus improving the thermal safety performance and high temperature cycle performance of the secondary battery.
[0007] In some embodiments, the above-mentioned membrane satisfies the following condition: 1≤M≤10. Based on the above-mentioned embodiment, the membrane of the embodiment of the present application adjusts the molar concentration of the first functional group M fmol / μm 3 Within the above range, the thermal safety performance and high-temperature cycle performance of the secondary battery can be further improved.
[0008] In some of the embodiments, the organic cyanide includes at least one of polyacrylonitrile, nitrile rubber, 1,3,5-triazine-2,4,6-triamine, melamine cyanurate or melamine thiocyanate. Based on the above embodiments, the diaphragm of the embodiment of the present application uses the above organic cyanide to keep the amount of organic cyanide dissolved within a specific range, which can better stabilize the metal atoms and crystal structure on the surface of the positive electrode material, inhibit the structural phase change of the positive electrode material, and further improve the stability of the positive electrode, thereby further improving the thermal safety performance and high temperature cycle performance of the secondary battery.
[0009] In some embodiments, the first coating includes nitrogen and carbon. Based on the mass of the first coating, the mass percentage of nitrogen is J%, the mass percentage of carbon is K%, 0.3≤J / K≤2.2; and / or, 10.5≤J≤55. Based on the above embodiments, the diaphragm of the embodiment of the present application controls the mass percentage of nitrogen J% in the first coating and its ratio to the mass percentage of carbon K% within the above range, so that the content of each element in the first coating, especially the nitrogen content, is within a suitable range. This is more conducive to further improving the thermal safety performance and high-temperature cycle performance of the secondary battery, while taking into account the improvement of high-temperature storage performance.
[0010] In some embodiments, the first coating satisfies at least one of the following conditions: (1) 0.7 ≤ J / K ≤ 1.8; (2) 15 ≤ J ≤ 55; (3) 20 ≤ K ≤ 65. Based on the above embodiments, the separator of the embodiment of the present application can further improve the thermal safety performance and high temperature cycle performance of the secondary battery by further controlling the mass percentage content J% of the nitrogen element and the mass percentage content K% of the carbon element in the first coating and the ratio of the two within the above preferred range, while taking into account the improvement of the high temperature storage performance.
[0011] In some of the embodiments, the material of the base film is selected from at least one of polyethylene or polypropylene; and / or, the closed-cell temperature of the diaphragm is 120°C to 140°C; and / or, the first coating layer also includes an adhesive, and the adhesive includes at least one of polyacrylic acid, polyacrylate, lithium polyacrylate, polyvinylidene fluoride, styrene-butadiene rubber, polyacrylamide or sodium carboxymethyl cellulose. Based on the above embodiments, the diaphragm of the embodiment of the present application, by selecting the above polyolefin as the base film material, can close the pores at an appropriate temperature to block the interaction between the positive and negative electrodes; by selecting the above adhesive, the first coating layer can be evenly applied to the surface of the base film, thereby further improving the thermal safety performance and high-temperature cycle performance of the secondary battery, while also improving the high-temperature storage performance.
[0012] In some of the embodiments, the above-mentioned diaphragm further includes an adhesive layer, which is located between the first coating layer and the positive electrode plate, and the thickness of the adhesive layer is H μm, 0.1≤H≤3. Based on the above embodiments, the diaphragm of the embodiment of the present application can bond the battery cell into a whole by providing an adhesive layer between the first coating layer and the positive electrode plate, and controlling the thickness of the adhesive layer within the above range, and storing an appropriate amount of electrolyte between the diaphragm and the positive electrode, so that the organic cyanide in the first coating layer can be better diffused to the surface of the positive electrode material, thereby further improving the thermal safety performance and high-temperature cycle performance of the secondary battery, while also taking into account the improvement of high-temperature storage performance.
[0013] In some of the embodiments, in the above-mentioned adhesive layer, 0.2≤H≤2; and / or, the material of the adhesive layer includes at least one of styrene-butadiene rubber, polyacrylic acid, polyacrylate, lithium polyacrylate, polymethyl methacrylate, polyacrylonitrile or polyvinylidene fluoride. Based on the above-mentioned embodiments, the diaphragm of the embodiment of the present application, by further regulating the thickness of the above-mentioned adhesive layer within the above-mentioned preferred range, can make the diaphragm and the positive electrode store an appropriate amount of electrolyte while making the first coating contact with the positive electrode plate, so that the organic cyanide in the first coating can be better diffused to the surface of the positive electrode material; by selecting the above-mentioned adhesive, it has good resistance to electrolyte swelling, and can maintain the adhesion of the first coating to the positive electrode, thereby further improving the thermal safety performance and high-temperature cycle performance of the secondary battery, while taking into account the improvement of high-temperature storage performance.
[0014] In the second aspect, the embodiment of the present application provides a secondary battery, including a positive electrode plate, an electrolyte and the above-mentioned separator. The positive electrode plate includes a positive electrode current collector and a positive electrode material layer arranged on at least one surface of the positive electrode current collector, the positive electrode material layer includes a positive electrode active material, and the delithiation amount of the positive electrode active material is P, 0.5≤P≤0.9. Based on the above embodiment, in the secondary battery of the embodiment of the present application, when the delithiation amount P of the positive electrode active material is within the above range, the organic cyanide in the first coating can better diffuse to the surface of the positive electrode material, thereby improving the thermal safety performance and high temperature cycle performance of the secondary battery.
[0015] In some of the embodiments, in the above-mentioned positive electrode active material, 0.6≤P≤0.8. Based on the above-mentioned embodiments, in the secondary battery of the embodiment of the present application, when the lithium removal amount P of the positive electrode active material is within the above-mentioned preferred range, the organic cyanide in the first coating can be better diffused to the surface of the positive electrode material, further improving the thermal safety performance and high temperature cycle performance of the secondary battery.
[0016] In some of the embodiments, the positive electrode active material of the secondary battery includes at least one of lithium cobalt oxide, ternary positive electrode material, lithium iron phosphate or lithium-rich manganese-based material. Based on the above embodiments, the secondary battery of the embodiment of the present application uses the above positive electrode active material, so that the positive electrode has a large amount of lithium removal and the battery cell has a high energy density. At the same time, the organic cyanide in the first coating diffuses to the surface of the above positive electrode material, which can better improve the positive electrode stability and further improve the thermal safety performance and high temperature cycle performance of the secondary battery.
[0017] In some of the embodiments, the electrolyte includes fluoroethylene carbonate, and the mass percentage of fluoroethylene carbonate based on the total mass of the electrolyte is N%, 2≤N≤12. Based on the above embodiments, the secondary battery of the embodiment of the present application, the electrolyte contains the above content of fluoroethylene carbonate, which can help the negative electrode form a stable SEI film, thereby synergizing with the organic cyanide to enhance the stability of the positive and negative electrodes, making the positive and negative electrodes of the battery cell stable at high temperatures, reducing the overall heat generation of the battery cell, and further improving the thermal safety performance and high temperature cycle performance of the secondary battery.
[0018] In a third aspect, an embodiment of the present application provides an electronic device, which includes the secondary battery mentioned above. DETAILED DESCRIPTION
[0019] In order to make the purpose, technical solution and advantages of the present application more clear, the present application is further described in detail below in conjunction with the embodiments. It should be understood that the specific embodiments described here are only used to explain the present application and are not used to limit the present application.
[0020] An embodiment of the present application provides a secondary battery, including a separator, an electrolyte, a positive electrode plate, and a negative electrode plate.
[0021] Diaphragm In the present application, a diaphragm is usually provided between the positive electrode plate and the negative electrode plate, and the diaphragm is used to separate the positive electrode plate and the negative electrode plate to prevent internal short circuit of the secondary battery, allow electrolyte ions to pass freely, and do not affect the battery charging and discharging process.
[0022] In some embodiments, the separator includes a base film and a first coating disposed on a surface of the base film facing the positive electrode, the first coating including an organic cyanide having a first functional group, the first functional group including at least one of a cyano group (-C≡N), an isocyano group (-N≡C), an isocyanate group (-N=C=O), or a melamine derivative. Based on the volume of the first coating, the molar concentration of the first functional group is Mfmol / μm 3, 0.1≤M≤30, preferably 1≤M≤10. For example, the value of the molar concentration M of the first functional group can be 0.1, 0.5, 1, 5, 10, 15, 20, 30 or a value in the range formed by any two of these values. The present application regulates the value of the molar concentration M of the first functional group in the separator within the above range, which can improve the thermal safety performance and high temperature storage performance of the secondary battery.
[0023] In some embodiments, the organic cyanide includes at least one of polyacrylonitrile, nitrile rubber, 1,3,5-triazine-2,4,6-triamine, melamine cyanurate or melamine thiocyanate. The above organic cyanide is selected in the present application to further improve the thermal safety performance and high temperature storage performance of the secondary battery.
[0024] In some embodiments, the first coating on the diaphragm includes nitrogen and carbon. Based on the mass of the first coating, the mass percentage of nitrogen is J%, 10.5≤J≤55, preferably 15≤J≤55. For example, the value of J can be 10.5, 15, 31, 46, 55, or a value within the range of any two of these values. The mass percentage of carbon is K%, 20≤K≤65. For example, the value of K can be 20, 29, 35, 47, 51, 53, 60, 65, or a value within the range of any two of these values. 0.3≤J / K≤2.2, preferably 0.7≤J / K≤1.8. For example, the ratio of J to K can be 0.3, 0.5, 0.8, 1.2, 1.8, 2.2, or a value within the range of any two of these values. The present application controls the mass percentage content J% of nitrogen element, the mass percentage content K% of carbon element and the ratio of the two in the first coating layer within the above range, which can further improve the thermal safety performance and high-temperature cycle performance of the secondary battery while also improving the high-temperature storage performance.
[0025] In some embodiments, the material of the base film is selected from at least one of polyethylene or polypropylene. The present application selects the above polyolefin as the base film material, which can further improve the thermal safety performance and high temperature cycle performance of the secondary battery, while also improving the high temperature storage performance.
[0026] In some embodiments, the closed-cell temperature of the separator is 120°C to 140°C. For example, the closed-cell temperature of the separator can be 120, 123, 126, 132, 133, 135, 140, or a value in the range formed by any two of these values. The closed-cell temperature of the separator of the present application is within the above range, which can further improve the thermal safety performance and high-temperature cycle performance of the secondary battery, while also improving the high-temperature storage performance.
[0027] In some embodiments, the first coating on the separator further includes an adhesive, and the adhesive includes at least one of polyacrylic acid, polyacrylate, lithium polyacrylate, lithium polyacrylate polyvinylidene fluoride, styrene-butadiene rubber, polyacrylamide, or sodium carboxymethyl cellulose. The present application selects the above adhesive to further improve the thermal safety performance and high temperature cycle performance of the secondary battery, while also improving the high temperature storage performance.
[0028] In some embodiments, the separator further includes an adhesive layer, the adhesive layer is located between the first coating and the positive electrode sheet, and the thickness of the adhesive layer is H μm, 0.1≤H≤3, preferably 0.2≤H≤2. For example, the value of H can be 0.1, 0.2, 0.5, 1.0, 1.5, 2.0, 2.5, 3 or a value in the range of any two of these values. The thickness of the adhesive layer of the present application is within the above range, which can further improve the thermal safety performance and high temperature cycle performance of the secondary battery, while taking into account the improvement of high temperature storage performance.
[0029] In some embodiments, the material of the adhesive layer includes at least one of styrene-butadiene rubber, polyacrylic acid, polyacrylate, lithium polyacrylate, polymethyl methacrylate, polyacrylonitrile or polyvinylidene fluoride. The above adhesive layer materials are selected in the present application to further improve the thermal safety performance and high temperature cycle performance of the secondary battery, while also improving the high temperature storage performance.
[0030] The pore size of the diaphragm in the present application is 0.01 μm to 1 μm, and the thickness is 5 μm to 50 μm. In some embodiments, the thickness of the diaphragm is greater than 1 μm, greater than 5 μm, or greater than 8 μm. In some embodiments, the thickness of the diaphragm is less than 50 μm, less than 40 μm, or less than 30 μm. When the thickness of the diaphragm is within the above range, the insulation and mechanical strength can be ensured, and the rate characteristics and energy density of the secondary battery can be ensured.
[0031] Electrolyte The electrolyte used in the secondary battery of the embodiment of the present application is a non-aqueous electrolyte, which includes an electrolyte and a solvent that dissolves the electrolyte.
[0032] In some embodiments, the non-aqueous electrolyte of the present application includes fluoroethylene carbonate, and the mass percentage of fluoroethylene carbonate based on the total mass of the electrolyte is N%, 2≤N≤12. For example, N is 2, 3.1, 4.2, 5.4, 6.8, 7.2, 10.5, 12, or a value within the range consisting of any two of these values.
[0033] The electrolyte may also include lithium salts and non-aqueous solvents. The present application does not particularly limit the types of lithium salts, as long as the purpose of the present application can be achieved. For example, the lithium salt may include but is not limited to at least one of lithium hexafluorophosphate (LiPF6), lithium tetrafluoroborate (LiBF4), lithium difluorophosphate (LiPO2F2), lithium trifluoromethanesulfonyl imide (LiTFSI), lithium bis (fluorosulfonyl) imide (LiFSI), lithium bis oxalate borate (LiBOB) or lithium difluoro oxalate borate (LiDFOB). Based on the mass of the electrolyte, the mass percentage of the lithium salt may be 8% to 15%, for example, the mass percentage of the lithium salt may be 8%, 9%, 10%, 11%, 12.5%, 13%, 15% or a range consisting of any two of the values. The present application does not particularly limit the types of the above-mentioned non-aqueous solvents, as long as the purpose of the present application can be achieved. For example, it may include but is not limited to at least one of carbonate compounds, carboxylate compounds, ether compounds or other organic solvents. The above-mentioned carbonate compounds may include but are not limited to at least one of chain carbonate compounds or cyclic carbonate compounds. The above-mentioned linear carbonate compound may include but is not limited to at least one of dimethyl carbonate, diethyl carbonate, dipropyl carbonate, methyl propyl carbonate, ethyl propyl carbonate or ethyl methyl carbonate. The above-mentioned cyclic carbonate compound may include but is not limited to at least one of ethylene carbonate, propylene carbonate, butylene carbonate or vinyl ethylene carbonate.
[0034] The above-mentioned carboxylate compound may include but is not limited to at least one of methyl formate, methyl acetate, ethyl acetate, n-propyl acetate, tert-butyl acetate, methyl propionate, ethyl propionate, propyl propionate, γ-butyrolactone, decanolactone, valerolactone or caprolactone. The above-mentioned ether compound may include but is not limited to at least one of ethylene glycol dimethyl ether, dibutyl ether, tetraethylene glycol dimethyl ether, diethylene glycol dimethyl ether, 1,2-dimethoxyethane, 1,2-diethoxyethane, 1-ethoxy-1-methoxyethane, 2-methyltetrahydrofuran or tetrahydrofuran. The above-mentioned other organic solvents may include but are not limited to at least one of dimethyl sulfoxide, 1,2-dioxolane, cyclopentane, methyl cyclopentane, 1,3-dimethyl-2-imidazolidinone, N-methyl-2-pyrrolidone, dimethylformamide, acetonitrile, trimethyl phosphate, triethyl phosphate or trioctyl phosphate.
[0035] Positive electrode The positive electrode sheet includes a positive electrode current collector and a positive electrode material layer disposed on at least one surface of the positive electrode current collector, the positive electrode material layer includes a positive electrode active material, and the delithiation amount of the positive electrode active material is P, 0.5≤P≤0.9. Preferably, 0.6≤P≤0.8. For example, P is 0.5, 0.6, 0.7, 0.8, 0.9, or a value within the range of any two of these values.
[0036] In some embodiments, the positive electrode active material includes at least one of lithium cobalt oxide, a ternary positive electrode material, lithium iron phosphate, or a lithium-rich manganese-based material. For example, the positive electrode active material may be at least one of lithium cobalt oxide, lithium nickel cobalt manganese oxide NCM811, lithium nickel cobalt manganese oxide NCM523, lithium nickel cobalt manganese oxide NCM333, lithium iron phosphate, LiMnO·LiCoO, Li2MnO·LiNiCoO, and xLiMnO·(1-x)LiNi.Mn.O.
[0037] In some embodiments, the positive electrode material layer includes a positive electrode conductive material; the type of the positive electrode conductive material is not limited, and any known conductive material can be used. Examples of positive electrode conductive materials may include, but are not limited to, carbon black such as acetylene black and Super-P; amorphous carbon such as needle coke; carbon nanotubes; graphene, etc. The positive electrode conductive material may be used alone or in any combination.
[0038] In some embodiments, the positive electrode material layer includes a positive electrode binder; the type of the positive electrode binder is not particularly limited, and in the case of a coating method, any material that can be dissolved or dispersed in a liquid medium used in electrode manufacturing can be used. Examples of positive electrode binders may include, but are not limited to, one or more of the following: resin polymers such as polyethylene, polypropylene, polyethylene terephthalate, polymethyl methacrylate, polyimide, aromatic polyamide, cellulose, nitrocellulose, etc.; rubber polymers such as styrene-butadiene rubber, nitrile rubber, fluororubber, isoprene rubber, polybutadiene rubber, ethylene-propylene rubber, etc.; thermoplastic elastomer polymers such as styrene-butadiene-styrene block copolymers or their hydrides, ethylene-propylene-diene terpolymers, styrene-ethylene-butadiene-ethylene copolymers, styrene-isoprene-styrene block copolymers or their hydrides; soft resin polymers such as syndiotactic-1,2-polybutadiene, polyvinyl acetate, ethylene-vinyl acetate copolymers, propylene-α-olefin copolymers; fluorine polymers such as polyvinylidene fluoride, polytetrafluoroethylene, fluorinated polyvinylidene fluoride, polytetrafluoroethylene-ethylene copolymers; polymer compositions having ion conductivity of alkali metal ions, etc. The positive electrode binder may be used alone or in any combination.
[0039] There is no limitation on the type of solvent used to form the positive electrode slurry, as long as it is a solvent that can dissolve or disperse the positive electrode active material, the conductive material, the positive electrode binder, and the thickener used as needed. Examples of solvents used to form the positive electrode slurry may include any of aqueous solvents and organic solvents. Examples of aqueous media may include, but are not limited to, a mixed medium of alcohol and water or water, etc. Examples of organic media may include, but are not limited to, aliphatic hydrocarbons such as hexane; aromatic hydrocarbons such as benzene, toluene, xylene, methylnaphthalene; heterocyclic compounds such as quinoline and pyridine; ketones such as acetone, methyl ethyl ketone, and cyclohexanone; esters such as methyl acetate and methyl acrylate; amines such as diethylenetriamine and N,N-dimethylaminopropylamine; ethers such as diethyl ether, propylene oxide, and tetrahydrofuran; amides such as N-methylpyrrolidone, dimethylformamide, and dimethylacetamide; aprotic polar solvents such as hexamethylphosphoramide and dimethyl sulfoxide, etc.
[0040] Thickeners are generally used to adjust the viscosity of the slurry. In the case of using an aqueous medium, the thickener and styrene-butadiene rubber emulsion can be used for slurrying. The type of thickener is not particularly limited, and examples thereof may include, but are not limited to, carboxymethyl cellulose, methyl cellulose, hydroxymethyl cellulose, ethyl cellulose, polyvinyl alcohol, oxidized starch, phosphorylated starch, casein, and salts thereof. The thickener may be used alone or in any combination.
[0041] The type of positive electrode current collector is not particularly limited, and it can be any material known to be suitable for use as a positive electrode current collector. Examples of positive electrode current collectors may include, but are not limited to, metal materials such as aluminum, stainless steel, nickel plating, titanium, tantalum, and materials such as carbon cloth and carbon paper. In some embodiments, the positive electrode current collector is a metal material. In some embodiments, the positive electrode current collector is aluminum.
[0042] In order to reduce the electronic contact resistance between the positive electrode current collector and the positive electrode material layer, the surface of the positive electrode current collector may include a conductive additive or a conductive coating. Examples of conductive additives may include, but are not limited to, carbon and precious metals such as gold, platinum, and silver. Examples of conductive coatings may include a mixture layer containing an inorganic oxide, a conductive agent, and a binder.
[0043] Negative electrode The negative electrode comprises a negative electrode current collector and a negative electrode material layer disposed on at least one surface of the negative electrode current collector, wherein the negative electrode material layer comprises a negative electrode active material. In some embodiments, the chargeable capacity of the negative electrode active material is greater than the discharge capacity of the positive electrode active material to prevent lithium metal from being accidentally precipitated on the negative electrode during charging.
[0044] The negative electrode active material may include natural graphite, artificial graphite, mesophase microcarbon beads (MCMB), silicon, silicon-carbon composites, SiO x(0.5<x<1.6), Li-Sn alloy, Li-Sn-O alloy, Sn, SnO, SnO2, spinel structure lithium titanate Li4Ti5O 12 , Li-Al alloy or metallic lithium, etc. Optionally, the negative electrode active material may further include an amorphous carbon material, and the amorphous carbon may be soft carbon (low temperature calcined carbon), hard carbon, mesophase pitch carbide or calcined coke, etc.
[0045] The negative electrode material layer of the present application also includes a negative electrode binder. The negative electrode binder can improve the bonding between the negative electrode active material particles and the bonding between the negative electrode active material and the current collector. The type of negative electrode binder is not particularly limited, as long as it is a material that is stable to the solvent used in the electrolyte or electrode manufacturing. In some embodiments, the negative electrode binder includes a resin binder. Examples of resin binders include, but are not limited to, fluororesins, polyacrylonitrile (PAN), polyimide resins, acrylic resins, polyolefin resins, and the like. When an aqueous solvent is used to prepare the negative electrode mixture slurry, the negative electrode binder includes, but is not limited to, carboxymethyl cellulose (CMC) or its salt, styrene-butadiene rubber (SBR), polyacrylic acid (PAA) or its salt, polyvinyl alcohol, and the like.
[0046] The negative electrode material layer of the present application also includes a conductive agent. The present application has no particular restrictions on the type of the negative electrode conductive agent, as long as the purpose of the present application can be achieved. For example, the negative electrode conductive agent can be at least one of acetylene black, Ketjen black, carbon nanotubes, carbon fibers, carbon dots or graphene, and the carbon nanotubes can include but are not limited to at least one of single-walled carbon nanotubes or multi-walled carbon nanotubes.
[0047] The present application has no particular restrictions on the negative electrode current collector, as long as the purpose of the present application can be achieved. For example, the negative electrode current collector may include copper foil, aluminum foil, nickel foil, stainless steel foil, titanium foil, nickel foam, copper foam or a polymer substrate covered with a conductive metal, etc. Among them, the conductive metal includes but is not limited to copper, nickel or titanium, and the material of the polymer substrate includes but is not limited to at least one of polyethylene, polypropylene, ethylene propylene copolymer, polyethylene terephthalate, polyethylene naphthalate or poly(p-phenylene terephthalamide). In the present application, there is no particular restriction on the thickness of the negative electrode current collector and the negative electrode material layer, as long as the purpose of the present application can be achieved. For example, the thickness of the negative electrode current collector is 4μm to 12μm, and the thickness of the single-sided negative electrode material layer is 30μm to 160μm. In the present application, the negative electrode mixture layer can be arranged on one surface in the thickness direction of the negative electrode current collector, or on two surfaces in the thickness direction of the negative electrode current collector. It should be noted that the "surface" here can be the entire area of the negative electrode current collector or a partial area of the negative electrode current collector. This application has no special restrictions as long as the purpose of this application can be achieved.
[0048] The present application has no particular restrictions on the compaction density of the negative electrode sheet, as long as the purpose of the present application can be achieved. For example, the compaction density of the negative electrode sheet can be 1.0 g / cm 3 Up to 1.85g / cm 3 The present application has no particular limitation on the cold pressing pressure of the negative electrode sheet, as long as the purpose of the present application can be achieved. For example, the cold pressing pressure of the negative electrode sheet can be 3 tons to 30 tons.
[0049] Optionally, the negative electrode plate may further include a conductive layer, which is located between the negative electrode current collector and the negative electrode material layer. The present application has no particular restrictions on the composition of the conductive layer, which may be a conductive layer commonly used in the art. The conductive layer includes a conductive agent and a binder. The present application has no particular restrictions on the conductive agent and the binder in the conductive layer, which may be at least one of the conductive agent and the binder. The present application has no particular restrictions on the mass ratio of the conductive agent and the binder in the conductive layer, and those skilled in the art may choose according to actual needs, as long as the purpose of the present application can be achieved. The present application has no particular restrictions on the thickness of the conductive layer, as long as the purpose of the present application can be achieved, for example, the thickness of the conductive layer is 1 μm to 10 μm.
[0050] The secondary battery of the present application also includes a packaging bag for containing a positive electrode sheet, a separator, a negative electrode sheet and an electrolyte, as well as other components known in the art in the secondary battery, and the present application does not limit the above other components. The present application does not specifically limit the packaging bag, and it can be a packaging bag known in the art, as long as it can achieve the purpose of the present application.
[0051] The present application further provides an electronic device, which includes a secondary battery of an embodiment of the present application. The electronic device includes but is not limited to a laptop computer, a pen-input computer, a mobile computer, an electronic book player, a portable phone, a portable fax machine, a portable copier, a portable printer, a head-mounted stereo headset, a video recorder, an LCD TV, a portable cleaner, a portable CD player, a mini-disc, a transceiver, an electronic notepad, a calculator, a memory card, a portable recorder, a radio, a backup power supply, a motor, a car, a motorcycle, a power-assisted bicycle, a bicycle, a lighting fixture, a toy, a game console, a clock, an electric tool, a flashlight, a camera, a large household battery and a lithium-ion capacitor, etc.
[0052] Example Hereinafter, taking lithium-ion batteries as an example, examples and comparative examples are given to more specifically describe the implementation of the secondary battery of the present application. The preparation method described in the present application is only an example, and any other suitable preparation method is within the scope of the present application. In addition, unless otherwise specified, "part" and "%" are based on mass.
[0053] Example 1-1 <Preparation of lithium-ion batteries> (1) Preparation of positive electrode: The positive electrode active material lithium cobalt oxide, the conductive agent conductive carbon black and polyvinylidene fluoride (PVDF) are mixed in a mass ratio of 95:2:3, N-methylpyrrolidone (NMP) is added, and the mixture is stirred evenly under the action of a vacuum mixer to obtain a positive electrode slurry with a solid content of 70wt%. The positive electrode slurry is evenly coated on one surface of a positive electrode current collector aluminum foil with a thickness of 9μm, and dried to obtain a positive electrode sheet coated with a positive electrode mixture layer on one side. Repeat the above steps on the other surface of the positive electrode current collector aluminum foil to obtain a positive electrode sheet coated with a positive electrode mixture layer on both sides. After cold pressing, cutting, slitting and drying, a positive electrode sheet with a specification of 74mm×867mm is obtained.
[0054] (2) Preparation of non-aqueous electrolyte: In a dry argon atmosphere glove box, ethylene carbonate (EC), ethylene carbonate (PC) and diethyl carbonate (DEC) were mixed in a weight ratio of 1:3:6 as a base solvent, and then fluoroethylene carbonate and LiPF6 were dissolved in the above base solvent to obtain an electrolyte. Based on the total mass of the electrolyte, the mass percentage of LiPF6 is 12.5%, and the mass percentage of fluoroethylene carbonate is 5%.
[0055] (3) Preparation of negative electrode: artificial graphite is used as the negative electrode active material, and the negative electrode active material, styrene-butadiene rubber (SBR), polyacrylic acid (PAA), carbon nanotubes (CNT) and carboxymethyl cellulose (CMC) are mixed in a mass ratio of 95.8:2.4:0.5:0.5:0.8, and then deionized water is added as a solvent and stirred evenly to prepare a negative electrode slurry with a solid content of 45wt%. The negative electrode slurry is evenly coated on one surface of a negative electrode current collector copper foil with a thickness of 6μm, and dried to obtain a negative electrode sheet coated with a negative electrode mixture layer on one side. The above steps are repeated on the other surface of the negative electrode current collector copper foil to obtain a negative electrode sheet coated with a negative electrode mixture layer on both sides. After cold pressing, cutting, slitting and drying, a negative electrode sheet with a specification of 76.6mm×875mm is obtained.
[0056] (4) Preparation of diaphragm: The organic cyanide layer slurry is prepared by mixing polyacrylonitrile (C3H3N) n After grinding, the mixture is mixed with a binder, styrene-butadiene rubber and lithium polyacrylate, in a mass ratio of 94:5:1, and deionized water or an organic solvent is added and dispersed and stirred for 120 minutes to obtain an organic cyanide coating slurry.
[0057] The organic cyanide layer slurry is evenly coated on the surface of the porous polyethylene film of the substrate layer by transfer coating, and the moisture is dried in an oven. Then, an adhesive layer is coated on the surface of the organic cyanide layer. The adhesive layer is composed of acrylic polymer particles (D90≤1μm) mixed with sodium carboxymethyl cellulose in a mass ratio of 85:15, and deionized water is added to disperse them evenly to obtain the final diaphragm after drying.
[0058] (5) Preparation of lithium-ion batteries: stack the positive electrode sheet, separator, and negative electrode sheet in order, with the separator placed between the positive and negative electrode sheets to isolate them, and wind them to obtain a bare cell. Place the bare cell in a packaging bag, inject electrolyte, and package. After the formation, degassing, trimming, and capacity testing processes, a lithium-ion battery is obtained.
[0059] <Test Method> (1) Thermal safety performance test: Place the lithium-ion battery in a 25℃ constant temperature environment and let it stand for 30 minutes to allow the lithium-ion battery to reach a constant temperature. Charge at a constant current of 0.5C to the lithium depletion potential P, and then charge at a constant voltage to a current of 0.05C. Transfer the lithium-ion battery to a hot box, heat it to 130℃ at 5℃ / min, and keep it at a constant temperature for 60 minutes. The battery cell passes if it does not catch fire or explode. Test 20 lithium-ion battery samples in parallel and calculate the pass rate of the thermal safety test.
[0060] Thermal safety pass rate = number of samples passing the test / total number of samples × %.
[0061] (2) High temperature cycle performance test Place the lithium-ion battery in a 60℃ constant temperature test box and let it stand for 30 minutes to allow the lithium-ion battery to reach a constant temperature. Charge at a constant current of 0.5C to the lithium desorption potential P, charge at a constant voltage to a current of 0.05C, let it stand for 5 minutes, and discharge at a constant current of 0.5C to 3.0V, which is recorded as the initial discharge capacity C0. Repeat this step for 100 cycles, record the discharge capacity C1 after 100 cycles, and calculate the lithium-ion battery cycle capacity retention rate.
[0062] High temperature cycle capacity retention rate = C1 / C0×100%.
[0063] (3) High temperature storage performance test: Place the lithium-ion battery in a 25°C constant temperature environment and let it stand for 30 minutes to allow the lithium-ion battery to reach a constant temperature. Charge at a constant current of 0.5C to the lithium desorption potential P, and then charge at a constant voltage to a current of 0.05C. Record the thickness of the lithium-ion battery and record it as the initial thickness. Transfer the lithium-ion battery to an 80°C constant temperature box and store it for 42 hours. During this period, test and record the thickness of the lithium-ion battery every 7 hours. Record the test thickness after 42 hours as the storage thickness. Calculate the thickness expansion rate of the lithium-ion battery and use it as an indicator to evaluate the high-temperature storage performance of the lithium-ion battery.
[0064] High temperature storage expansion rate = (storage thickness - initial thickness) / initial thickness × 100%.
[0065] (4) Test of lithium removal amount and complete lithium removal amount The amount of completely de-lithiumed refers to the amount of lithium contained in the positive electrode after the battery cell is fully discharged and the lithium returns from the negative electrode to the positive electrode. The positive electrode plate is disassembled after full discharge, the electrolyte is cleaned with NMP, and the lithium content that can be completely de-lithiumed from the positive electrode is obtained by ICP elemental analysis.
[0066] The residual lithium content is the remaining lithium content in the positive electrode after the battery cell is fully charged. At this time, the lithium migrates from the positive electrode to the negative electrode. The fully charged positive electrode plate is disassembled, the electrolyte is cleaned with NMP, and the residual lithium content of the positive electrode is obtained by ICP elemental analysis.
[0067] After the battery cell is fully charged, the amount of lithium removed = (the amount of completely removed lithium - the lithium content in the positive electrode) / the amount of completely removed lithium.
[0068] (5) Molar concentration test of the first functional group The membrane coating with an area of S was cleaned and dried with NMP to obtain a coating with a weight of G, which was ground and mixed with potassium bromide powder and pressed into tablets with a total mass of 150 mg. The first functional group peak intensity I was obtained by infrared spectrometer (FTIR) testing; the weight of the external standard sample with a weight gradient of 0.1*G, G, 5*G, and 10*G was divided by the molecular weight M to obtain the corresponding molar amount, and a total of 150 mg of potassium bromide powder was used to make tablets, and the first functional group peak intensity was obtained by FTIR measurement. The molar amount of the external standard sample was fitted with the peak intensity of the first functional group, and the I value was substituted to obtain the molar amount Mg of the first functional group in the coating mass G, and the molar concentration = Mg / S.
[0069] (6) Nitrogen and carbon mass percentage test Remove the diaphragm from the battery cell and select the diaphragm at the head, tail or super anode area of the battery cell. The diaphragm here is not bonded to the pole piece, and the coating is not transferred to the pole piece surface. Use NMP to clean the diaphragm to remove the electrolyte and residual lithium salt. The coating falls off the surface of the base film and is dried. Use an elemental analyzer to obtain the quantitative carbon and nitrogen element ratio in the coating.
[0070] The lithium-ion batteries of the following embodiments or comparative examples differ from those of embodiment 1-1 only in that the type of positive electrode active material, the type of organic cyanide, the amount of lithium removed from the positive electrode active material P, and the molar concentration of the first functional group on the first coating Mfmol / μm are adjusted according to Table 1. 3 , and the mass percentage of fluoroethylene carbonate in the electrolyte N%. Wherein, the P value is adjusted by regulating the voltage of the positive electrode. The performance test results of the lithium ion batteries of various embodiments and comparative examples are shown in Table 1 below.
[0071] Table 1
[0072] *In the above table, P is the amount of lithium removed from the positive electrode active material, M is the molar concentration of the first functional group on the first coating, and N is the mass percentage of fluoroethylene carbonate in the electrolyte. Comprehensive performance = P 2 (Thermal safety pass rate + high temperature cycle capacity retention rate), the value is rounded to one decimal place, and “ / ” means that the substance is not contained.
[0073] As shown in Table 1, the molar concentration of the first functional group on the first coating layer of the lithium ion battery prepared in the embodiment of the present application is M fmol / μm 3 The value M satisfies 0.1≤M≤30, which can stabilize the metal atoms and the positive electrode crystal structure, reduce the release of active oxygen, inhibit the structural phase change of materials such as lithium cobalt oxide that causes the electrochemical performance of the material to decay during high-voltage charging and discharging, improve the positive electrode stability, and thus improve the thermal safety performance and high-temperature cycle performance of the secondary battery. Among them, when 1≤M≤10, the secondary battery can achieve a higher energy density while further improving the thermal safety performance and high-temperature cycle performance of the secondary battery.
[0074] In particular, when the value of the lithium removal amount P of the positive electrode active material is regulated to meet 0.5≤P≤0.9, the thermal safety performance and high temperature cycle performance of the secondary battery can be improved. Among them, when 0.6≤P≤0.8, the secondary battery can achieve a higher energy density while further improving the thermal safety performance and high temperature cycle performance of the secondary battery. In particular, when the value of the mass percentage content N% of fluoroethylene carbonate in the electrolyte is regulated to meet 2≤N≤12, the heat generation of the entire battery cell can be reduced, further improving the thermal safety performance and high temperature cycle performance of the secondary battery.
[0075] The lithium-ion batteries of the following Examples 2-1 to 2-32 differ from those of Example 1-24 only in that: when preparing the diaphragm, different types of base film materials, binders and bonding layer materials are selected, and the mass percentage of nitrogen element J%, the mass percentage of carbon element K% on the first coating layer, and the thickness of the bonding layer H μm are regulated, wherein when adjusting the mass percentage of nitrogen element, the molar concentration of the first functional group is controlled to remain unchanged.
[0076] Table 2
[0077] * In the above table, based on the mass of the first coating, J is the mass percentage of nitrogen J%, K is the mass percentage of carbon K%, and H is the thickness of the bonding layer Hμm. Comprehensive performance = 0.5*(thermal safety pass rate + high temperature cycle capacity retention rate)-high temperature storage expansion rate%, where the percentages of high temperature cycle capacity retention rate and high temperature storage expansion rate are integers, and the comprehensive performance score is rounded to one decimal place.
[0078] As can be seen from Table 2, the lithium-ion battery prepared in the embodiment of the present application, when the mass percentage of nitrogen element J% on the first coating is regulated to satisfy 10.5≤J≤55, and the ratio of the mass percentage of nitrogen element J% to the mass percentage of carbon element K% satisfies 0.3≤J / K≤2.2, the thermal safety performance and high temperature cycle performance of the secondary battery can be further improved, while the high temperature storage performance can be improved. In particular, by regulating 0.7≤J / K≤1.8, 15≤J≤55, and 20≤K≤65, the thermal safety performance and high temperature cycle performance of the secondary battery can be further improved, while the high temperature storage performance can be improved.
[0079] In particular, when the thickness Hμm of the adhesive layer is adjusted to satisfy 0.1≤H≤3, the thermal safety performance and high-temperature cycle performance of the secondary battery can be further improved while also improving the high-temperature storage performance.
[0080] The above description is only a preferred embodiment of the present application and is not intended to limit the present application. Any modifications, equivalent substitutions and improvements made within the principles of the present application should be included in the protection scope of the present application.
Claims
1. A diaphragm, It is characterized in that The separator includes a base film and a first coating disposed on a surface of the base film facing a positive electrode plate, wherein the first coating includes an organic cyanide having a first functional group, wherein the first functional group includes at least one of a cyano group, an isocyano group, an isocyanate group, or a melamine derivative; Based on the volume of the first coating, the molar concentration of the first functional group is Mfmol / μm 3 , 0.1≤M≤30.
2. The diaphragm according to claim 1, It is characterized in that The separator satisfies 1≤M≤10.
3. The diaphragm according to claim 1 or 2, It is characterized in that The organic cyanide comprises at least one of polyacrylonitrile, nitrile rubber, 1,3,5-triazine-2,4,6-triamine, melamine cyanurate or melamine thiocyanate.
4. The diaphragm according to claim 1 or 2, It is characterized in that The first coating layer includes nitrogen and carbon; Based on the mass of the first coating, the mass percentage of nitrogen is J%, the mass percentage of carbon is K%, and 0.3≤J / K≤2.2; and / or, 10.5≤J≤55。 5. The diaphragm according to claim 4, It is characterized in that The first coating satisfies at least one of the following conditions: (1) 0.7 ≤ J / K ≤ 1.8; (2)15≤J≤55; (3)20≤K≤65。 6. The diaphragm according to claim 1 or 2, It is characterized in that The material of the base film is selected from at least one of polyethylene and polypropylene; and / or, The diaphragm has a closed cell temperature of 120°C to 140°C; and / or, The first coating layer also includes an adhesive, and the adhesive includes at least one of polyacrylic acid, polyacrylate, lithium polyacrylate, polyvinylidene fluoride, styrene-butadiene rubber, polyacrylamide or sodium carboxymethyl cellulose.
7. The diaphragm according to claim 1 or 2, It is characterized in that The separator further includes an adhesive layer, wherein the adhesive layer is located between the first coating layer and the positive electrode plate, and the thickness of the adhesive layer is H μm, and 0.1≤H≤3.
8. The diaphragm according to claim 7, It is characterized in that In the adhesive layer, 0.2≤H≤2; and / or, The material of the adhesive layer includes at least one of styrene-butadiene rubber, polyacrylic acid, polyacrylate, lithium polyacrylate, polymethyl methacrylate, polyacrylonitrile or polyvinylidene fluoride.
9. A secondary battery comprising a positive electrode sheet, an electrolyte and the separator according to any one of claims 1 to 8; The positive electrode plate includes a positive electrode current collector and a positive electrode material layer disposed on at least one surface of the positive electrode current collector, the positive electrode material layer includes a positive electrode active material, and the delithiation amount of the positive electrode active material is P, 0.5≤P≤0.
9.
10. The secondary battery according to claim 9, It is characterized in that 0.6≤P≤0.8。 11. The secondary battery according to claim 9 or 10, It is characterized in that The positive electrode active material includes at least one of lithium cobalt oxide, a ternary positive electrode material, lithium iron phosphate or a lithium-rich manganese-based material.
12. The secondary battery according to claim 9 or 10, It is characterized in that The electrolyte includes fluoroethylene carbonate, and the mass percentage of the fluoroethylene carbonate is N% based on the total mass of the electrolyte, 2≤N≤12.
13. An electronic device, It is characterized in that A secondary battery comprising the secondary battery according to any one of claims 9 to 12.
Citation Information
Cited By
Coating composition, separator, electrochemical device, and electronic device
CN119231097A
Positive pole piece, electrochemical device and electronic device
CN119275395A
Coating, secondary battery, and electronic device
CN119331480A
Coatings, secondary batteries and electronic devices
CN119331480B
Secondary battery and electronic device
CN121011667A