Perovskite thin film and preparation method thereof

Through PVD technology, dihydrohalide is used in perovskite solar cells to form a moderate thickness upper and lower interface modification layer, which solves the complexity and harmful problems of interface modification in the traditional solution method, and improves the uniformity of perovskite film and the battery. performance, achieving higher photoelectric conversion efficiency.

CN118946171APending Publication Date: 2024-11-12TRINA SOLAR CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411024778.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-29
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

Traditional solution method interface modifications have problems such as complex process, high cost, low efficiency and harmful to the human body in perovskite solar cells, resulting in unstable film uniformity and affecting battery performance.

Method used

The upper and lower interfaces of perovskite films are double modified by physical vapor deposition (PVD) technology, using dihydrohalides such as 1,3-diaminopropane dihydroiodide and 1,3-diaminopropane dihydrochloride As the interface modification layer material, an upper and lower interface modification layer of moderate thickness is formed by PVD evaporation method to improve the uniformity of the perovskite film.

Benefits of technology

The process flow is simplified, the uniformity and battery performance of perovskite films are improved, and the short-circuit current, open-circuit voltage, fill factor and photoelectric conversion efficiency are significantly improved, while reducing the potential impact on the environment and human health.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118946171A_ABST
    Figure CN118946171A_ABST
Patent Text Reader

Abstract

The invention discloses a perovskite thin film, and relates to the technical field of solar cells. According to the embodiment of the invention, the perovskite thin film comprises a perovskite absorption layer; the upper interface modification layer is arranged on one side of the perovskite absorption layer; the lower interface modification layer is arranged on one side, far away from the upper interface modification layer, of the perovskite absorption layer; wherein the materials of the upper interface modification layer and the lower interface modification layer are independently selected from dihydrohalide respectively. Therefore, the uniformity of the perovskite thin film is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of solar cells, and in particular, to a perovskite film and a preparation method thereof, and further to a perovskite solar cell and an electrical device. Background Art

[0002] Perovskite solar cells have become a hot topic of research due to their high photoelectric conversion efficiency. The cell consists of an electron transport layer, a perovskite active layer, a hole transport layer and electrodes, of which the perovskite active layer is the key to determining the performance of the cell. Although the existing technology has improved the performance of the perovskite layer through organic chemical modification, component regulation and additive doping, the traditional solution method interface modification has the disadvantages of complex process, high cost, low efficiency and harm to the human body, and may lead to unstable uniformity of the thin film layer, affecting the overall performance of the cell.

[0003] Therefore, it is urgent to propose a new method for preparing perovskite films to modify the upper and lower interfaces of the perovskite films in order to improve the performance of perovskite solar cells. Summary of the invention

[0004] The present application aims to solve at least one of the technical problems existing in the prior art to a certain extent. To this end, the present application provides a perovskite film.

[0005] In the first aspect of the present application, the present application proposes a perovskite film. According to an embodiment of the present application, the perovskite film comprises: a perovskite absorption layer, an upper interface modification layer, the upper interface modification layer is arranged on one side of the perovskite absorption layer; a lower interface modification layer, the lower interface modification layer is arranged on the side of the perovskite absorption layer away from the upper interface modification layer; wherein the materials of the upper interface modification layer and the lower interface modification layer are independently selected from dihydrogen halides. Thus, the uniformity of the perovskite film is improved.

[0006] In some embodiments, the dihydrohalide comprises at least one of 1,3-diaminopropane dihydroiodide (PDADI) and 1,3-diaminopropane dihydrochloride (PDADC1).

[0007] In some embodiments, the thickness of the upper interface modification layer is 0.7-1.3 nm. Thus, the upper interface modification layer with moderate thickness can further improve the uniformity of the perovskite film, thereby improving the short-circuit current, open-circuit voltage, fill factor and photoelectric conversion efficiency of the perovskite solar cell.

[0008] In some embodiments, the thickness of the lower interface modification layer is 4.7 to 5.3 nm. Thus, the lower interface modification layer with moderate thickness can further improve the uniformity of the perovskite film, thereby improving the short-circuit current, open-circuit voltage, fill factor and photoelectric conversion efficiency of the perovskite solar cell.

[0009] In some embodiments, the thickness of the upper interface modification layer is 0.8-1.2 nm.

[0010] In some embodiments, the thickness of the lower interface modification layer is 4.8-5.2 nm.

[0011] In a second aspect of the present application, the present application proposes a method for preparing a perovskite film. According to an embodiment of the present application, the method includes modifying both sides of a perovskite absorption layer using a dihydrogen halide so as to form an upper interface modification layer on one side of the perovskite absorption layer and a lower interface modification layer on a side of the perovskite absorption layer away from the upper interface modification layer. Thus, the method can prepare a perovskite film with improved uniformity.

[0012] In some embodiments, the dihydrohalide comprises at least one of 1,3-diaminopropane dihydroiodide and 1,3-diaminopropane dihydrochloride.

[0013] In some embodiments, the thickness of the upper interface modification layer is 0.7-1.3 nm.

[0014] In some embodiments, the thickness of the lower interface modification layer is 4.7-5.3 nm.

[0015] In some embodiments, the modification treatment is performed by PVD evaporation, and the rate of the PVD evaporation is

[0017] In the third aspect of the present application, the present application proposes a perovskite solar cell. According to an embodiment of the present application, the perovskite solar cell comprises: a perovskite film layer, the perovskite film layer comprises the perovskite film described in the first aspect of the present application or the perovskite film prepared by the method described in the second aspect of the present application. As a result, the perovskite solar cell has a higher short-circuit current, a higher open-circuit voltage, a higher fill factor and a higher photoelectric conversion efficiency.

[0018] In a fourth aspect of the present application, the present application proposes an electrical device. According to an embodiment of the present application, the electrical device includes: the perovskite solar cell described in the third aspect of the present application.

[0019] Additional aspects and advantages of the present application will be given in part in the description below, and in part will become apparent from the description below, or will be learned through the practice of the present application. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] The above and / or additional aspects and advantages of the present application will become apparent and easily understood from the description of the embodiments in conjunction with the following drawings, in which:

[0021] Figure 1 Schematic diagram of the structure of a perovskite film according to an embodiment of the present application.

[0022] Figure 2 Schematic diagram of the structure of an inversion perovskite solar cell according to an embodiment of the present application.

[0023] Figure 3 Schematic diagram of the structure of a positive-type perovskite solar cell according to an embodiment of the present application.

[0024] Figure 4 4 is a flow chart of a method for laser scribing of a perovskite solar cell according to an embodiment of the present application.

[0025] Description of reference numerals:

[0026] Perovskite film 50; inverted perovskite solar cell 101; positive perovskite solar cell 102;

[0027] Perovskite absorption layer 01; upper interface modification layer 02; lower interface modification layer 03; hole transport layer 13; electrode 14; transparent conductive substrate 15. DETAILED DESCRIPTION

[0028] The embodiments of the present application are described in detail below. Examples of the embodiments are shown in the drawings, but unnecessary detailed descriptions may be omitted. For example, detailed descriptions of well-known matters and repeated descriptions of actually identical structures may be omitted. This is to avoid the following description from becoming unnecessarily lengthy and to facilitate understanding by those skilled in the art. In addition, the drawings and the following description are provided for those skilled in the art to fully understand the present application and are not intended to limit the subject matter described in the claims.

[0029] Unless otherwise defined, all technical and scientific terms used in this application have the same meanings as those commonly understood by technicians in the technical field to which this application belongs; the terms used in this application are only for the purpose of describing specific embodiments and are not intended to limit this application; unless otherwise specified, the numerical values ​​of the parameters mentioned in this application can be measured using various measurement methods commonly used in the art (for example, they can be tested according to the methods given in the embodiments of this application).

[0030] The terms "including" and "having" in the specification and claims of the present application and any modifications thereof are open expressions, that is, including the contents specified in the present application but not excluding other contents.

[0031] In the description of the present application, it should be understood that the terms "width", "thickness", etc. indicate orientation or positional relationships based on the orientation or positional relationships shown in the accompanying drawings, and are only for the convenience of describing the present application and simplifying the description, rather than indicating or implying that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore should not be understood as a limitation on the present application.

[0032] In the description of this application, the terms "first" and "second" are used for descriptive purposes only and should not be understood as indicating or implying relative importance or implicitly indicating the number of the indicated technical features. "First feature" and "second feature" may include one or more of the features.

[0033] In the description of the present application, it should be understood that the terms "center", "longitudinal", "lateral", "length", "width", "thickness", "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside", "outside", "clockwise", "counterclockwise", "axial", "radial", "circumferential" and the like indicate orientations or positional relationships based on the orientations or positional relationships shown in the accompanying drawings, and are only for the convenience of describing the present application and simplifying the description, and do not indicate or imply that the referred device or element must have a specific orientation, be constructed and operated in a specific orientation, and therefore should not be understood as a limitation on the present application.

[0034] In the description of the present application, unless otherwise clearly specified and limited, a first feature being “above” or “below” a second feature may mean that the first and second features are in direct contact, or the first and second features are in indirect contact through an intermediate medium. Moreover, a first feature being “above”, “above”, and “above” a second feature may mean that the first feature is directly above or obliquely above the second feature, or simply means that the first feature is higher in level than the second feature. A first feature being “below”, “below”, and “below” a second feature may mean that the first feature is directly below or obliquely below the second feature, or simply means that the first feature is lower in level than the second feature.

[0035] In the description of the present application, “plurality” means two or more.

[0036] In the description of the present application, "A and / or B" may include the case of A alone, the case of B alone, or any of the cases of A and B, where A and B are only used for examples and may be any technical feature connected by "and / or" in the present application.

[0037] Unless otherwise specified, all embodiments and optional embodiments of the present application can be combined with each other to form a new technical solution.

[0038] Organic-inorganic halide perovskite solar cells (PSCs) have become the forefront of solar technology due to their excellent optoelectronic properties and manufacturing cost advantages. These cells are composed of electron transport layers, perovskite active layers, hole transport layers and electrodes, among which the performance of the perovskite active layer is the key to the photoelectric conversion efficiency.

[0039] Existing technology uses a solution method to modify the interface of perovskite films to improve performance, but this method faces challenges such as complex process, high cost, and low efficiency when applied on a large scale. At the same time, the solution method may cause unstable uniformity of perovskite films, affecting battery performance, and the organic solvents used may have adverse effects on the environment and human health.

[0040] In response to these limitations, this application proposes an interface modification technology based on physical vapor deposition (PVD), which simplifies the process flow, improves the uniformity of the perovskite film, and reduces the potential impact on the environment and human health. The technical solution of this application double-modifies the interface of the perovskite film through specific compounds, optimizing the interface characteristics between the hole transport layer and the perovskite film and between the perovskite film and the electron transport layer. This modification not only maintains the structural integrity of the perovskite crystal, but also significantly improves the fill factor and short-circuit current of the battery by promoting uniform film formation and effective defect passivation, while increasing the open circuit voltage through surface passivation, comprehensively improving the overall performance of perovskite solar cells.

[0041] Based on this, in the first aspect of the present application, the present application proposes a perovskite film. According to the embodiments of the present application, referring to Figure 1 , the perovskite film 50 comprises:

[0042] Perovskite absorber layer 01;

[0043] An upper interface modification layer 02, wherein the upper interface modification layer 02 is disposed on one side of the perovskite absorption layer 01;

[0044] The lower interface modification layer 03 is disposed on a side of the perovskite absorption layer 01 away from the upper interface modification layer 02; wherein the materials of the upper interface modification layer and the lower interface modification layer are independently selected from dihydrogen halides. Thus, the uniformity of the perovskite film is improved.

[0045] In some embodiments, the dihydrohalide comprises at least one of 1,3-diaminopropane dihydroiodide and 1,3-diaminopropane dihydrochloride.

[0046] In some embodiments, the thickness of the upper interface modification layer is 0.7 to 1.3 nm, for example, it can be 0.7 nm, 0.75 nm, 0.8 nm, 0.85 nm, 0.9 nm, 0.95 nm, 1.0 nm, 1.05 nm, 1.1 nm, 1.15 nm, 1.2 nm, 1.25 nm, 1.3 nm and the range between any two points thereof, such as 0.7 to 1.2 nm, 0.7 to 1.15 nm, 0.7 to 1.1 nm and 0.7 to 1.05 nm. An upper interface modification layer with moderate thickness will reduce the absorption of light and increase the amount of light reaching the perovskite layer; at the same time, an upper interface modification layer with moderate thickness will increase the transmittance of the battery and improve the light capture and conversion efficiency; in addition, an upper interface modification layer with moderate thickness will reduce interface defects, reduce non-radiative recombination, and reduce the transmission impedance of electrons from the perovskite film layer to the electron transport layer; an upper interface modification layer with moderate thickness can fully cover and passivate interface defects and improve the stability and efficiency of the battery; at the same time, an upper interface modification layer with moderate thickness is mechanically stable enough to improve the adhesion of the upper interface modification layer. Therefore, an upper interface modification layer with moderate thickness can further improve the uniformity of the perovskite film, thereby improving the short-circuit current, open-circuit voltage, fill factor, and photoelectric conversion efficiency of perovskite solar cells.

[0047] In some embodiments, the thickness of the lower interface modification layer is 4.7 to 5.3 nm, for example, it can be 4.7 nm, 4.75 nm, 4.8 nm, 4.85 nm, 4.9 nm, 4.95 nm, 5.0 nm, 5.05 nm, 5.1 nm, 5.15 nm, 5.2 nm, 5.25 nm, 5.3 nm and the range between any two points thereof, such as 4.7 to 5.25 nm, 4.7 to 5.2 nm, 4.7 to 5.15 nm, 4.7 to 5.1 nm and 4.7 to 5.05 nm. A lower interface modification layer with moderate thickness helps reduce defects at the interface, which can capture charge and cause the battery performance to deteriorate. A modification layer with moderate thickness can cover the interface more effectively, thereby reducing these defects. A lower interface modification layer with moderate thickness can ensure that the modification layer covers the entire interface uniformly, prevent direct contact between the perovskite layer and the bottom layer, and reduce side reactions or unfavorable interface reactions. A lower interface modification layer with moderate thickness can regulate the stress between the perovskite layer and the bottom layer, reduce stress concentration, reduce the risk of cracks and fractures, and improve the uniformity of the film. Therefore, a lower interface modification layer with moderate thickness can further improve the uniformity of the perovskite film, thereby improving the short-circuit current, open-circuit voltage, fill factor, and photoelectric conversion efficiency of perovskite solar cells.

[0048] In some embodiments, the thickness of the upper interface modification layer is 0.8-1.2 nm.

[0049] In some embodiments, the thickness of the upper interface modification layer is 4.8-5.2 nm.

[0050] In some embodiments, the thickness of the perovskite absorption layer is 500-800nm, for example, it can be 500nm, 550nm, 600nm, 650nm, 700nm, 750nm, 760nm, 770nm, 780nm, 790nm, 800nm ​​and the range between any two of them, such as 500-790nm, 500-780nm and 500-770nm. Thus, the thickness of the perovskite absorption layer is moderate, which can further improve the uniformity of the perovskite film, thereby improving the short-circuit current, open-circuit voltage, fill factor and photoelectric conversion efficiency of the perovskite solar cell.

[0051] In some embodiments, the perovskite absorber layer is composed of ABX3; wherein A includes but is not limited to methylamine cation (FA + ), methylammonium cation (MA + ), cesium cation (Cs + ), rubidium cation (Rb + ), potassium cation (K + ) at least one of; B includes but is not limited to lead cations (Pb 2+ ), tin cation (Sn 2+ ), copper cation (Cu 2+ ), zinc cation (Zn 2+ ), gallium cation (Ga 2+ ), calcium cation (Ca 2+ ) at least one of; X includes but is not limited to fluoride anion (F - ), chloride anion (Cl - ), bromide anion (Br - ), iodide anion (I - )

[0052] In some embodiments, the ABX3 is Cs 0.05 FA 0.95 PbI3.

[0053] In a second aspect of the present application, the present application proposes a method for preparing a perovskite film. According to an embodiment of the present application, the method comprises: modifying both sides of a perovskite absorption layer using a dihydrogen halide so as to form an upper interface modification layer on one side of the perovskite absorption layer, and forming a lower interface modification layer on a side of the perovskite absorption layer away from the upper interface modification layer. Thus, the method can prepare a perovskite film with improved uniformity.

[0054] In some embodiments, the dihydrohalide comprises at least one of 1,3-diaminopropane dihydroiodide and 1,3-diaminopropane dihydrochloride.

[0055] In some embodiments, the thickness of the upper interface modification layer is 0.7 to 1.3 nm, for example, it can be 0.7 nm, 0.75 nm, 0.8 nm, 0.85 nm, 0.9 nm, 0.95 nm, 1.0 nm, 1.05 nm, 1.1 nm, 1.15 nm, 1.2 nm, 1.25 nm, 1.3 nm and the range between any two points thereof, such as 0.7 to 1.2 nm, 0.7 to 1.15 nm, 0.7 to 1.1 nm and 0.7 to 1.05 nm. An upper interface modification layer with moderate thickness will reduce the absorption of light and increase the amount of light reaching the perovskite layer; at the same time, an upper interface modification layer with moderate thickness will increase the transmittance of the battery and improve the light capture and conversion efficiency; in addition, an upper interface modification layer with moderate thickness will reduce interface defects, reduce non-radiative recombination, and reduce the transmission impedance of electrons from the perovskite film layer to the electron transport layer; an upper interface modification layer with moderate thickness can fully cover and passivate interface defects and improve the stability and efficiency of the battery; at the same time, an upper interface modification layer with moderate thickness is mechanically stable enough to improve the adhesion of the upper interface modification layer. Therefore, an upper interface modification layer with moderate thickness can prepare a perovskite film with improved uniformity, thereby improving the short-circuit current, open-circuit voltage, fill factor, and photoelectric conversion efficiency of perovskite solar cells.

[0056] In some embodiments, the thickness of the lower interface modification layer is 4.7 to 5.3 nm, for example, it can be 4.7 nm, 4.75 nm, 4.8 nm, 4.85 nm, 4.9 nm, 4.95 nm, 5.0 nm, 5.05 nm, 5.1 nm, 5.15 nm, 5.2 nm, 5.25 nm, 5.3 nm and the range between any two points thereof, such as 4.7 to 5.25 nm, 4.7 to 5.2 nm, 4.7 to 5.15 nm, 4.7 to 5.1 nm and 4.7 to 5.05 nm. A lower interface modification layer with moderate thickness helps reduce defects at the interface, which may capture charge and cause the battery performance to deteriorate. A modification layer with moderate thickness can cover the interface more effectively, thereby reducing these defects; a lower interface modification layer with moderate thickness can ensure that the modification layer covers the entire interface uniformly, prevent direct contact between the perovskite layer and the bottom layer, and reduce side reactions or unfavorable interface reactions; a lower interface modification layer with moderate thickness can regulate the stress between the perovskite layer and the bottom layer, reduce stress concentration, reduce the risk of cracks and fractures, and improve the uniformity of the film. Therefore, a lower interface modification layer with moderate thickness can prepare a perovskite film with improved uniformity, thereby improving the short-circuit current, open-circuit voltage, fill factor, and photoelectric conversion efficiency of perovskite solar cells.

[0057] In some embodiments, the thickness of the upper interface modification layer is 0.8-1.2 nm.

[0058] In some embodiments, the thickness of the lower interface modification layer is 4.8-5.2 nm.

[0059] In some embodiments, the modification treatment is performed by PVD evaporation, and the rate of the PVD evaporation is For example, And the range between any two of their point values, such as and The PVD evaporation method of the present application can simplify the process flow of double interface modification. Compared with solution spin coating or coating, it does not require complex templates or external structure guidance, which helps to reduce production steps; and the PVD method is suitable for the preparation of large-area perovskite solar cells, and can quickly and uniformly form thin films on a large area, improving production efficiency; the PVD evaporation method can reduce process steps and improve production efficiency, which helps to reduce overall production costs; and the PVD evaporation method can better control the thickness and uniformity of the upper interface modification layer and the lower interface modification layer, which is crucial to the performance of large-area perovskite solar cells. According to the embodiments of the present application, the perovskite solar cell is modified by the PVD evaporation method, which can improve the short-circuit current, open-circuit voltage, fill factor and photoelectric conversion efficiency of the perovskite solar cell; the rate of the PVD evaporation method has a significant effect on the interface modification, and the rate of the PVD evaporation method can affect the quality and uniformity of the film. A higher evaporation rate may cause defects such as pinholes and bubbles in the aforementioned upper interface modification layer and lower interface modification layer. For example, when the PVD evaporation rate is When the PVD deposition rate is , it will cause defects in the perovskite solar cell, thus reducing the efficiency of the perovskite solar cell. The slower evaporation rate will cause the upper and lower interface modification layers to be overcooled during the growth process, affecting the microstructure and performance. For example, when the PVD evaporation rate is Therefore, an appropriate PVD rate helps to form a uniform and dense upper and lower interface modification layers, thereby improving the short-circuit current, open-circuit voltage, fill factor and photoelectric conversion efficiency of perovskite solar cells.

[0060] In the third aspect of the present application, the present application proposes a perovskite solar cell.

[0061] According to an embodiment of the present application, the perovskite solar cell includes: the perovskite film described in the first aspect of the present application or a perovskite film prepared by the method described in the second aspect of the present application.

[0062] According to an embodiment of the present application, the perovskite solar cell includes but is not limited to an inverted perovskite solar cell, a normal perovskite solar cell, an intermediate perovskite solar cell and a tandem perovskite solar cell. Among them, the tandem perovskite solar cell includes a perovskite stacked cell.

[0063] According to the embodiments of the present application, reference Figure 2 , the inverted perovskite solar cell 101 comprises:

[0064] Electrode 14;

[0065] An electron transport layer 12, wherein the electron transport layer 12 is disposed on one side of the electrode 14;

[0066] The perovskite film 50 described in the first aspect of the present application or the perovskite film 50 prepared by the method described in the second aspect of the present application, wherein the perovskite film 50 is disposed on a side of the electron transport layer 12 away from the electrode 14;

[0067] The hole transport layer 13 is disposed on a side of the perovskite film 50 away from the electron transport layer 12. Thus, the perovskite solar cell has a higher short-circuit current, a higher open-circuit voltage, a higher fill factor and a higher photoelectric conversion efficiency.

[0068] The transparent conductive substrate 15 is disposed on a side of the hole transport layer 13 away from the perovskite film 50 .

[0069] The upper interface modification layer 02 of the perovskite film 50 is disposed on the side of the electron transport layer 12 away from the electrode 14; the lower interface modification layer 03 of the perovskite film 50 is disposed on the side of the hole transport layer 13 away from the transparent conductive substrate 15. Thus, the perovskite solar cell has a higher short-circuit current, a higher open-circuit voltage, a higher fill factor and a higher photoelectric conversion efficiency.

[0070] According to the embodiments of the present application, reference Figure 3 , the positive-type perovskite solar cell 102 comprises:

[0071] Electrode 14;

[0072] A hole transport layer 13, wherein the hole transport layer 13 is disposed on one side of the electrode 14;

[0073] The perovskite film 50 described in the first aspect of the present application or the perovskite film 50 prepared by the method described in the second aspect of the present application, wherein the perovskite film 50 is disposed on a side of the hole transport layer 13 away from the electrode 14;

[0074] The electron transport layer 12 is disposed on a side of the perovskite film 50 away from the hole transport layer 13 .

[0075] The transparent conductive substrate 15 is disposed on a side of the electron transport layer 12 away from the perovskite film 50 .

[0076] The upper interface modification layer 02 of the perovskite film 50 is disposed on the side of the electron transport layer 12 away from the transparent conductive substrate 15; the lower interface modification layer 03 of the perovskite film 50 is disposed on the side of the hole transport layer 13 away from the electrode 14. Thus, the perovskite solar cell has a higher short-circuit current, a higher open-circuit voltage, a higher fill factor and a higher photoelectric conversion efficiency.

[0077] According to an embodiment of the present application, it is preferred to combine two or more different band gaps such as Figure 2 The inverted perovskite solar cells shown are connected in series to construct a series perovskite solar cell to more effectively utilize the solar spectrum and improve the overall photoelectric efficiency. In order to connect the inverted perovskite solar cells in series, the present application uses Figure 4 The laser scribing method shown is used to separate and connect individual inversion perovskite solar cells.

[0078] S100: laser scribing P1 on the transparent conductive substrate, and then cleaning it;

[0079] S200: After cleaning and drying, slit coating is performed to prepare the perovskite film and its functional layers, and laser scribing is performed on the perovskite film and its functional layers P2;

[0080] S300: perform copper electrode evaporation and perform laser scribing P3 on the copper electrode.

[0081] In some embodiments, the thickness of the electron transport layer is 30-40 nm, for example, 30 nm, 31 nm, 32 nm, 33 nm, 34 nm, 35 nm, 36 nm, 37 nm, 38 nm, 39 nm, 40 nm and range values ​​between any two of them, such as 30-39 nm, 30-38 nm and 30-37 nm. Thus, the thickness of the electron transport layer is moderate, which is conducive to improving the short-circuit current, open-circuit voltage, fill factor and photoelectric conversion efficiency of the perovskite solar cell.

[0082] In some embodiments, the thickness of the hole transport layer is 20 to 80 nm, for example, 20 nm, 25 nm, 30 nm, 35 nm, 40 nm, 45 nm, 50 nm, 55 nm, 60 nm, 65 nm, 70 nm, 75 nm, 80 nm and ranges between any two of them, such as 20-75 nm, 20-70 nm and 20-65 nm. Thus, the thickness of the hole transport layer is moderate, which is beneficial to improving the short-circuit current, open-circuit voltage, fill factor and photoelectric conversion efficiency of the perovskite solar cell.

[0083] In some embodiments, the thickness of the electrode is 100-200 nm, for example, 100 nm, 110 nm, 120 nm, 130 nm, 140 nm, 150 nm, 160 nm, 170 nm, 180 nm, 190 nm, 200 nm and ranges between any two of them, such as 100-190 nm, 100-180 nm and 100-170 nm. Thus, the thickness of the electrode is moderate, which is beneficial to improving the short-circuit current, open-circuit voltage, fill factor and photoelectric conversion efficiency of the perovskite solar cell.

[0084] In some embodiments, the material of the electron transport layer includes but is not limited to at least one of titanium dioxide (TiO2), tin dioxide (SnO2), zinc oxide (ZnO), zirconium dioxide (ZrO2), gallium zinc oxide (GZO), indium zinc oxide (IZO), transparent conductive iron oxide (FTO), transparent conductive indium oxide (ITO), barium stannate (BaSnO3), fullerene C60 (C60), fullerene C70 (C70) and [6,6]-phenyl-C61-butyric acid methyl ester (PCBM).

[0085] In some embodiments, the electrode includes at least one of copper (Cu), silver (Ag), and gold (Au).

[0086] In some embodiments, the material of the hole transport layer includes [2-(9H-carbazole-9-yl)ethyl]phosphonic acid, [2-(3,6-dimethoxy-9H-carbazole-9-yl)ethyl]phosphonic acid, [4-(3,6-dimethyl-9H-carbazole-9-yl)butyl]phosphonic acid (Me-4PACZ), benzoic acid, 4-[bis(2,4-dimethoxybiphenyl-4-yl)amino]-biphenyl-4-carboxylic acid, 2,2',7,7'-tetrakis[N,N-di(4-methoxyphenyl)amino]-9,9'-spirobifluorene), poly(p-phenylene) Ethylene glycol dicarboxylate, poly(3-hexylthiophene) (P3HT), poly(3,4-ethylenedioxythiophene)-poly(styrenesulfonate) (PEDOT:PSS), spirobis(terthiophene)benzodithiophene (Spiro-TTB), tetrafluoro-7,7,8,8-tetracyanoquinolinium (F4-TCNQ), hexafluoro-7,7,8,8-tetracyanoquinodimethane (F6TCNNQ), 2,2'-(1,4-phenylene)bis-4-(2-ethylhexyloxy)phenyl-1-phenyloctanone (TAPC), nickel oxide (NiO x ), copper thiocyanate (CuSCN), copper aluminum oxide (CuAlO2), vanadium pentoxide (V2O5), cadmium sulfide (CdS), cadmium selenide (CdSe) and poly (9,9-di-n-decylfluorene) bromide (PFN-Br), and at least one of x is 0.5 to 1.5.

[0087] In some embodiments, the material of the electron transport layer includes C60.

[0088] In some embodiments, the material of the hole transport layer includes [4-(3,6-dimethyl-9H-carbazol-9-yl)butyl]phosphonic acid.

[0089] In some embodiments, the electrode comprises Cu.

[0090] In a fourth aspect of the present application, the present application proposes an electrical device. According to an embodiment of the present application, the electrical device includes: the perovskite solar cell described in the third aspect of the present application.

[0091] The scheme of the present application will be explained below in conjunction with the embodiments. It will be appreciated by those skilled in the art that the following embodiments are only used to illustrate the present application and should not be considered as limiting the scope of the present application. If no specific technology or conditions are indicated in the embodiments, the technology or conditions described in the literature in this area or the product specification are carried out. The reagents used or the instruments that do not indicate the manufacturer are all conventional products that can be obtained commercially.

[0092] Embodiment 1:

[0093] The perovskite solar cell prepared in this example is a reverse structure device, which consists of a transparent conductive substrate, a hole transport layer, a lower interface modification layer, a perovskite absorption layer, an upper interface modification layer, an electron transport layer, and a copper electrode from bottom to top. The conductive substrate is 10×10 cm 2 FTO; the hole transport layer is Me-4PACZ; the modification layer of the upper and lower interfaces is PDADI; the structure of the perovskite film layer is the most basic Cs 0.05 FA 0.95 PbI3; the electron transport layer is C60 / BCP; the electrode is a copper electrode.

[0094] (1) Provide a transparent conductive substrate FTO with a thickness of 2.18 mm.

[0095] (2) The preparation method of the hole transport layer is as follows: the prepared 0.5 mg / mL Me-4PACZ is dissolved in ethanol and stirred overnight, and then the hole transport layer is prepared on the FTO substrate using slit coating, and then annealed at 100°C for 10 min. The thickness of the hole transport layer is 10 nm.

[0096] (3) The preparation method of the lower interface modification layer is as follows: PDADI chemicals are placed in the evaporation chamber, and the pressure in the chamber is pumped down to 1×10 -4 , followed by The thickness of the lower interface modification layer is 5 nm.

[0097] (4) The preparation method of the perovskite absorption layer is as follows: a 1.5M concentration of Cs 0.05 FA 0.95 The perovskite solution of PbI3 was dissolved in a solvent of DMF:NMP at a ratio of 6:1 and stirred overnight. The perovskite film was then prepared on the PDADI modified layer using slit coating and annealed at 130°C for 20 minutes. The thickness of the perovskite absorption layer was 550nm.

[0098] (5) The preparation method of the upper interface modification layer is as follows: PDADI chemicals are placed in the evaporation chamber, and the pressure in the chamber is pumped down to 1×10 -4 , followed by The thickness of the upper interface modification layer is 1 nm.

[0099] (6) The preparation method of the electron transport layer is as follows: a C60 layer is prepared by thermal evaporation method, with a total thickness of 30 nm; a SnO2 layer is prepared by atomic layer deposition, with a thickness of 10 nm; wherein the C60 layer and the SnO2 layer constitute the electron transport layer of the perovskite solar cell.

[0100] (7) The preparation method of the copper electrode is as follows: on the surface of the hole transport layer, a copper electrode is deposited using a thermal evaporation evaporator, and the vacuum degree of the thermal evaporation chamber is 10-5 Pa, the metal evaporation rate is 5nm / min, and the thickness of the copper electrode is 110nm.

[0101] Example 2: This example is the same as Example 1, the main difference is that the upper and lower interface modification layers are The deposition is carried out at a speed of .

[0102] Example 3: This example is the same as Example 1, the main difference is that the upper and lower interface modification layers are The deposition is carried out at a speed of .

[0103] Example 4: The process of this example is the same as that of Example 1, the main difference being that the thickness of the upper interface modification layer is 0.8 nm.

[0104] Example 5: The process of this example is the same as that of Example 1, the main difference being that the thickness of the upper interface modification layer is 1.2 nm.

[0105] Example 6: The process of this example is the same as that of Example 1, the main difference being that the thickness of the upper interface modification layer is 0.7 nm.

[0106] Example 7: The process of this example is the same as that of Example 1, the main difference being that the thickness of the upper interface modification layer is 1.3 nm.

[0107] Example 8: The process of this example is the same as that of Example 1, the main difference being that the thickness of the lower interface modification layer is 4.8 nm.

[0108] Example 9: The process of this example is the same as that of Example 1, the main difference being that the thickness of the lower interface modification layer is 5.2 nm.

[0109] Example 10: The process of this example is the same as that of Example 1, the main difference being that the thickness of the lower interface modification layer is 4.7 nm.

[0110] Example 11: The process of this example is the same as that of Example 1, the main difference being that the thickness of the lower interface modification layer is 5.3 nm.

[0111] Comparative Example 1:

[0112] The experimental process of this comparative example is the same as that of Example 1, the main difference being that the upper and lower interface modifiers used in this comparative example are changed from PDADI to PDADC1.

[0113] Comparative Example 2:

[0114] The experimental process of this comparative example is the same as that of Example 1. The functional layers of the perovskite battery provided in this comparative example are basically the same as the functional layers of the perovskite battery in Example 1. Compared with Example 1, the main difference is that the lower interface modification layer is not prepared in this comparative example.

[0115] Test Example 1:

[0116] In order to test the effect of different evaporation rates of PDADI on the performance of perovskite devices, the present application tested the perovskite solar cell performance of PDADI after different evaporation rates in Examples 1 to 3, with the upper interface modification layer thickness of 1 nm and the lower interface modification layer thickness of 5 nm. The results are shown in Table 1.

[0117] Table 1

[0118]

[0119] The measured photovoltaic parameters open circuit voltage (V OC ), current density (I SC ), filling factor (FF) and PCE) are summarized in the table above. It can be seen from the table that when the evaporation rate is When the perovskite solar cells are prepared, the efficiency is further improved.

[0120] Test Example 2:

[0121] The performance of the perovskite solar cells prepared by Examples 1 to 11 and Comparative Examples 1 to 2 was compared, and the parameters thereof are shown in Table 2. It can be seen that the efficiency of the perovskite solar cells with upper and lower interface modification layers is significantly improved.

[0122] Table 2: Performance test:

[0123] Perovskite devices ISC(A) VOC(V) FF(%) PCE(%) Example 1 0.0881 10.46 80.29 20.55 Example 2 0.0876 10.26 77.44 19.32 Example 3 0.0849 10.35 78.90 19.25 Example 4 0.0879 10.39 80.11 20.32 Example 5 0.0877 10.42 80.09 20.27 Example 6 0.0873 10.32 79.87 19.98 Example 7 0.0876 10.28 79.98 20.01 Example 8 0.0874 10.43 79.67 20.27 Example 9 0.0882 10.44 79.81 20.41 Example 10 0.0879 10.42 78.21 19.88 Embodiment 11 0.0883 10.45 77.21 19.70 Comparative Example 1 0.0860 10.21 77.19 19.14 Comparative Example 2 0.0851 10.18 77.09 19.07

[0124] By comparing Example 1 with Comparative Example 1, it can be seen that the performance of the perovskite solar cell modified with PDADI is better than that of the perovskite solar cell modified with PDADCl, which is mainly reflected in the higher open circuit voltage of the perovskite solar cell. This shows that PDADI is more conducive to improving the short-circuit current, open circuit voltage, fill factor and photoelectric conversion efficiency of the perovskite solar cell.

[0125] Compared with Example 1 and Comparative Example 2, the short-circuit current, open-circuit voltage, fill factor and photoelectric conversion efficiency of the perovskite solar cell after both the upper and lower interfaces are modified are better than those of the perovskite solar cell with only a single layer of modification on the upper interface. This shows that modifying both the upper and lower interfaces of the perovskite solar cell is more conducive to improving the short-circuit current, open-circuit voltage, fill factor and photoelectric conversion efficiency of the perovskite solar cell than modifying only a single layer of the upper interface.

[0126] By comparing Example 1, Example 4, Example 5 and Examples 6 to 7, it can be seen that the short-circuit current, open-circuit voltage, fill factor and photoelectric conversion efficiency of the perovskite solar cells prepared in Example 1, Example 4 and Example 5 are higher.

[0127] By comparing Example 1, Example 8, Example 9 and Examples 10 to 11, it can be seen that the short-circuit current, open-circuit voltage, fill factor and photoelectric conversion efficiency of the perovskite solar cells prepared in Example 1, Example 8 and Example 9 are higher.

[0128] In the description of this specification, the description with reference to the terms "one embodiment", "some embodiments", "example", "specific example", or "some examples" etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present application. In this specification, the schematic representations of the above terms do not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described may be combined in any one or more embodiments or examples in a suitable manner. In addition, those skilled in the art may combine and combine the different embodiments or examples described in this specification and the features of the different embodiments or examples, without contradiction.

[0129] Although the embodiments of the present application have been shown and described above, it can be understood that the above embodiments are exemplary and cannot be understood as limitations on the present application. Ordinary technicians in this field can change, modify, replace and modify the above embodiments within the scope of the present application.

Claims

1. A perovskite film, characterized in that: include: Perovskite absorber layer; An upper interface modification layer, wherein the upper interface modification layer is disposed on one side of the perovskite absorption layer; A lower interface modification layer, wherein the lower interface modification layer is disposed on a side of the perovskite absorption layer away from the upper interface modification layer; Wherein, the materials of the upper interface modification layer and the lower interface modification layer are independently selected from dihydrogen halides.

2. The perovskite film according to claim 1, characterized in that The dihydrohalide includes at least one of 1,3-diaminopropane dihydroiodide and 1,3-diaminopropane dihydrochloride.

3. The perovskite film according to claim 1, characterized in that The thickness of the upper interface modification layer is 0.7 to 1.3 nm; And / or, the thickness of the lower interface modification layer is 4.7-5.3 nm.

4. The perovskite film according to claim 1, characterized in that The thickness of the upper interface modification layer is 0.8 to 1.2 nm; And / or, the thickness of the lower interface modification layer is 4.8-5.2 nm.

5. A method for preparing a perovskite film, characterized in that: Both sides of the perovskite absorption layer are modified by using dihydrogen halide so as to form an upper interface modification layer on one side of the perovskite absorption layer and a lower interface modification layer on a side of the perovskite absorption layer away from the upper interface modification layer.

6. The method according to claim 5, characterized in that The dihydrohalide includes at least one of 1,3-diaminopropane dihydroiodide and 1,3-diaminopropane dihydrochloride.

7. The method according to claim 6, characterized in that The thickness of the upper interface modification layer is 0.7-1.3 nm; and / or the thickness of the lower interface modification layer is 4.7-5.3 nm.

8. The method according to claim 5, characterized in that The modification treatment is carried out by PVD evaporation method, and the rate of PVD evaporation is 9. A perovskite solar cell, characterized in that: include: The perovskite film according to any one of claims 1 to 4 or the perovskite film prepared by the method according to any one of claims 5 to 8.

10. An electrical device, characterized in that: include: The perovskite solar cell according to claim 9.