Method for accurately regulating and controlling filling growth of perovskite in mesoporous layers of carbon-based mesoporous perovskite solar cell
By adopting a four-mesoporous layer architecture in perovskite solar cells, the characteristics of each mesoporous layer film are controlled, and the problems of mismatch between the energy levels of the perovskite film and the carbon electrode and the poor growth quality of the mesoporous layer are solved, and the photoelectricity is improved Conversion efficiency and stability promote the commercialization of perovskite solar cells.
Patent Information
- Application Number
- CN202310522256.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-10
- Publication Date
- 2024-11-12
AI Technical Summary
The photoelectric conversion efficiency of carbon-based mesoporous perovskite solar cells is low, and the main factors include the mismatch between the perovskite film and the carbon electrode energy level, the lack of close contact, the low carrier mobility, poor mesoporous layer growth quality and electrons Inadequate hole transmission.
The four-mesoporous layer architecture is adopted to control the porosity, thickness, surface roughness and orientation of TiO2, ZrO2, NiO and C films, and the filling and growth of perovskites in each mesoporous layer is regulated to improve the photoelectric conversion efficiency.
It significantly improves the photoelectric conversion efficiency of carbon-based mesoporous perovskite solar cells, enhances the stability and performance of the device, and promotes its commercial application.
Smart Images

Figure CN118946217A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of carbon-based mesoporous perovskite solar cell film preparation, and in particular to a method for accurately regulating the filling and growth of perovskite in each mesoporous layer of a carbon-based mesoporous perovskite solar cell. Background Art
[0002] The highest photoelectric efficiency of perovskite solar cells reported in current research has reached 25.7%. The efficiency of carbon-based mesoporous perovskite solar cells is only about 18%, but its advantage lies in the fact that it can work stably for more than 9,000 hours at the maximum power point, and its preparation process is simple and inexpensive. In order to achieve commercial large-scale production and application of carbon-based mesoporous perovskite solar cells, it is urgent to improve their photoelectric conversion efficiency. Studies have shown that the factors that restrict the photoelectric conversion efficiency of carbon-based mesoporous perovskite solar cells include: (1) the energy level of the perovskite film and the carbon electrode do not match, the contact is not tight, and the carbon electrode has poor conductivity and low carrier mobility; (2) the growth quality of the perovskite film crystal in the mesoporous layer is poor, there are many defect states, and the recombination is serious; (3) the perovskite film needs to be doped; (4) the electron and hole transport mesoporous layer film needs to be doped to improve the conductivity, and the morphology and structure of the film needs to be controlled; (5) interface engineering, etc. Summary of the invention
[0003] In order to solve the above technical problems, the present invention adopts a mesoporous perovskite solar cell with a four-mesoporous layer architecture, and controls the filling and growth of perovskite in the mesoporous layer by precisely adjusting the pore size, porosity, thickness, surface roughness and orientation of each mesoporous layer film, thereby improving the photoelectric conversion efficiency of carbon-based mesoporous perovskite solar cells. The present invention prepares mesoporous layer films with different morphologies, different porosities, different surface roughness and different orientation characteristics by respectively changing the solution particle size, film thickness, number of passes of the substrate under the flame and annealing temperature used in preparing four mesoporous layer films, thereby controlling the filling and growth of the perovskite film. In order to achieve the above purpose, the present invention adopts the following technical solutions: See also Figure 1When preparing TiO2 slurry, TiO2 nanoparticles of different particle sizes are used to control the porosity and pore size of the mesoporous electron transport layer TiO2 film. The pore size can control the filling effect of perovskite, and the porosity can control the filling amount of perovskite, thereby regulating the filling growth of perovskite in the TiO2 mesoporous electron transport layer; when preparing ZrO2 film, the mass ratio of pine alcohol and ZrO2 powder is changed, and other components remain unchanged, so as to achieve the effect of controlling the thickness of the mesoporous support layer ZrO2 film, thereby controlling the filling amount of perovskite, thereby regulating the growth of perovskite in ZrO2. Filling and growth of the mesoporous support layer; when preparing the NiO film, the number of times the substrate passes under the flame in the flame-assisted chemical vapor deposition method is changed to change the porosity, surface roughness, and crystallinity of the mesoporous hole transport layer NiO film, thereby controlling the filling effect and filling amount of the perovskite, thereby regulating the filling growth of the perovskite in the NiO mesoporous hole transport layer; when preparing the C film, the annealing temperature is changed to control the surface roughness of the back electrode C film and the orientation of the carbon layer, wherein the roughness and orientation will affect the filling effect of the perovskite, thereby regulating the filling growth of the perovskite in the C layer. BRIEF DESCRIPTION OF THE DRAWINGS
[0004] In order to explain the technical solution more clearly, the following briefly introduces the drawings required for use.
[0005] Figure 1 The figure is the overall flow chart of the preparation method.
[0006] Figure 2 This is a flow chart of the method for preparing mesoporous electron transport layer TiO2 thin film.
[0007] Figure 3 Flow chart of the method for preparing mesoporous support layer ZrO2 thin film.
[0008] Figure 4 Flow chart of the method for preparing mesoporous hole transport layer NiO film.
[0009] Figure 5 Flow chart of the method for preparing the back electrode C film.
[0010] Figure 6 Flowchart for the filling of the perovskite precursor solution.
[0011] Figure 7 Schematic diagram of the regulation of mesoporous film morphology, porosity, orientation and grain size. Implementation
[0012] The present invention will be further described in detail below in conjunction with the accompanying drawings and embodiments.
[0013] First, the mesoporous electron transport layer TiO2 film is prepared, see Figure 2The method includes steps S1 to S4.
[0014] S1: Prepare the slurry. Weigh an appropriate amount of TiO2 slurry in a glass bottle, add pine alcohol at a mass ratio of 1:4 and stir with a glass rod for 20 minutes. After stirring, perform ultrasonic dispersion for 24 hours. After the ultrasonic dispersion is completed, the TiO2 slurry for thin film printing can be obtained.
[0015] S2: Use TiO2 with different particle sizes to control the porosity and the size of its pores. Four types of TiO2 nanoparticles with particle sizes of 15nm, 20nm, 25nm and 30nm can be used to make the slurry.
[0016] S3: Use a screen printer to print TiO2 slurry on the surface of the FTO substrate with a dense TiO2 layer deposited thereon. After the slurry flows evenly and there are no bubbles on the surface, place the FTO substrate on a 70°C hot table for drying.
[0017] S4: After the TiO2 slurry is dried, the substrate is transferred to a titanium plate hot plate and the temperature is raised to 500°C. After sintering at 500°C for 40 minutes, the substrate is allowed to cool naturally to room temperature.
[0018] The filling and growth of perovskite in the mesoporous electron transport layer TiO2 thin film is regulated by controlling the powder particle size of TiO2. The porosity and pore size of the TiO2 layer are changed by controlling the powder particle size of TiO2, thereby affecting the filling and growth of perovskite. As the particle size of TiO2 nanoparticles increases, the pore size will also increase, which will make the filling of perovskite in the mesopores better, but when the size increases further, the porosity will decrease, which will lead to a decrease in the filling amount of perovskite in the mesoporous layer. Therefore, by controlling the powder particle size of TiO2, the filling of perovskite in the mesoporous electron transport layer TiO2 thin film can be precisely regulated.
[0019] Then the mesoporous support layer ZrO2 film is prepared, see Figure 3 The method includes steps S1 to S4.
[0020] S1: Prepare slurry, weigh 12g ZrO2 powder, 6g ethyl cellulose, 36g pinene alcohol, and 2mL acetic acid in a ball mill, wherein the mass ratio of pinene alcohol to ZrO2 powder is changed, and the amounts of other components remain unchanged to control the thickness of the ZrO2 film.
[0021] S2: Add an appropriate amount of anhydrous ethanol, stir evenly with a glass rod, and place it in a planetary ball mill for 48 hours. After the ball milling is completed, take out the slurry and perform rotary evaporation at 45°C to remove excess ethanol. After the rotary evaporation is completed, white ZrO2 slurry can be obtained.
[0022] S3: Use a screen printer to print ZrO2 slurry on the surface of the sintered TiO2 mesoporous layer.
[0023] S4: After the slurry flows evenly, the substrate is placed on a 70°C hot plate for drying. After drying, a white ZrO2 film can be obtained.
[0024] The filling and growth of perovskite in the mesoporous support layer ZrO2 film is regulated by controlling the thickness of the ZrO2 film. The ZrO2 film separates the TiO2 film and the NIO film to avoid direct contact. At the same time, the perovskite filled in the ZrO2 film will also absorb photons transmitted through the TiO2 / MAPbI3 composite film. The photogenerated electrons are transferred from MAPbI3 to TiO2, and the holes are transported to the NIO film and then to the carbon electrode. Therefore, it is particularly important to control the thickness of ZrO2. As the thickness of the film increases, more perovskite can be filled in the ZrO2 film layer, which can enhance the performance of the device. However, when the thickness is too thick, the performance of the device will be reduced due to the limitation of the carrier diffusion length. Secondly, the surface roughness of the ZrO2 film layer with different thicknesses is also different. The surface with high surface roughness can provide more perovskite penetration channels, so it will promote the filling and growth of perovskite, thereby enhancing the absorption of light by the device. Therefore, the filling and growth of perovskite in the mesoporous support layer ZrO2 film layer can be regulated by controlling the thickness of the ZrO2 film.
[0025] The second is the preparation of NiO thin film with mesoporous hole transport layer, see Figure 4 The method includes steps S1 to S3.
[0026] S1: Nickel nitrate hexahydrate is used as raw material to prepare a 0.05M nickel nitrate aqueous solution, with a nitrogen-containing gas flow rate of 2L*min -1 The product is delivered as an aerosol using an ultrasonic nebulizer.
[0027] S2: Precursor and 0.6 L *min - 1 Oxygen is added to the combustion gas upstream of the burner head (0.8 -1.0L*min - 1 Propane / 22-20L* min -1 air).
[0028] S3: The glass substrate is heated to 400°C and heated at a speed of 10 mm*s -1 The speed of the substrate is adjusted to control the number of times the substrate passes under the flame, so that the number of times the substrate passes under the flame ranges from 4 to 50.
[0029] The filling and growth of perovskite in the mesoporous hole transport layer NiO thin film layer is regulated by controlling the number of times the substrate passes under the flame when preparing the NiO thin film. When the number of passes increases, the crystallinity of NIO will be increased, thereby promoting the filling of perovskite in the NIO film, but too many times will lead to a decrease in crystallinity. Secondly, as the number of passes increases, the roughness of the NIO film will be reduced, which is not conducive to the filling of perovskite. In addition, when the number of passes increases, the porosity of the film will also increase at any time, making the filling of perovskite more compact, but when it is too much, it will cause the film to become dense, which will have an adverse effect on the filling and growth of perovskite, and will cause the perovskite to be unable to penetrate into the bracket, thereby reducing the performance of the battery. Therefore, for the NIO hole transport layer film, the roughness, crystallinity, and porosity of the NIO film can be regulated by controlling the number of times the substrate passes under the flame, thereby regulating the filling of perovskite in the NIO film, thereby affecting the performance of perovskite solar cells.
[0030] Finally, the back electrode C film is prepared, see Figure 5 The method includes steps S1 to S4.
[0031] S1: First, prepare the carbon slurry. Weigh 26 g of graphite and 8 g of carbon black into a ball mill. Then add 6.4 g of ZrO2 powder and 4.8 g of ethyl cellulose powder respectively. Add 90 g of pine alcohol and an appropriate amount of anhydrous ethanol. After mixing, place the ball mill in a planetary ball mill and mill for 24 hours.
[0032] S2: After sufficient ball milling, the ball-milled mixture is transferred to a rotary evaporator, and the added anhydrous ethanol is removed by rotary evaporation to obtain a carbon slurry.
[0033] S3: Printing the carbon paste on the surface of the dried NIO layer using a screen printer.
[0034] S4: During annealing, different annealing temperatures are used for annealing.
[0035] The filling growth of perovskite in the back electrode C film is regulated by controlling the annealing temperature when preparing the C film. When the annealing temperature increases from 100°C, the resistance decreases exponentially, which will affect the filling factor and power conversion efficiency of the battery, but further increasing the annealing temperature (above 300°C) will deform the carbon film, resulting in uneven filling of perovskite in the carbon electrode. In addition, when annealing at 100°C~400°C, the surface roughness increases with the increase of annealing temperature. The surface roughness will affect the filling of perovskite in the carbon layer, thereby affecting the performance of the battery. Secondly, different annealing temperatures will also cause different orientations of the carbon layer, and different orientations will also affect the filling of perovskite in the carbon layer. Therefore, the growth and filling of perovskite in the back electrode C film can be precisely regulated by controlling the annealing temperature of the carbon layer, thereby affecting the performance of perovskite solar cells.
[0036] After the mesoporous scaffold is prepared, the perovskite precursor solution is filled in. Figure 6 The method includes steps S1 to S4.
[0037] S1: When the sintered substrate is naturally cooled to about 100°C, the substrate is taken out.
[0038] S2: Cover the surface of the non-filled area with high-temperature tape, then use a pipette to absorb an appropriate amount of perovskite precursor solution and drop it on the edge of ZrO2.
[0039] S3: Let stand for 5 to 10 minutes until the solution diffuses throughout the mesoporous film.
[0040] S4: The substrate filled with the solution is transferred to a constant temperature convection oven and annealed at 50° C. for 2 hours. After the annealing is completed, the device is allowed to cool naturally to room temperature to obtain a device.
[0041] The mesoporous scaffolds prepared by this method can precisely control the filling and growth of perovskite in each mesoporous layer, see Figure 7 Schematic diagram, by controlling the pore size, porosity, thickness, surface roughness and orientation of each mesoporous layer film to accurately fill and grow perovskite in each mesoporous layer, thereby affecting the performance of the battery. This will provide theoretical and technical support for the study of the influence mechanism of stress relaxation, stability and photoelectric efficiency of carbon-based mesoporous perovskite solar cells, promote the basic research and commercialization process of perovskite solar cells, have important scientific significance and economic value, and can be widely used in photovoltaic power generation bases, aerospace, civil green energy, ocean navigation, emergency medical care, military and other fields.
Claims
1. A method for precisely controlling the filling and growth of perovskite in each mesoporous layer of a carbon-based mesoporous perovskite solar cell, characterized in that: include: Referring to Figure 1, when preparing TiO2 slurry, TiO2 nanoparticles of different particle sizes are used to control the porosity and pore size of the mesoporous electron transport layer TiO2 film. The pore size can control the filling effect of perovskite, and the porosity can control the filling amount of perovskite, thereby regulating the filling growth of perovskite in the TiO2 mesoporous electron transport layer; when preparing ZrO2 film, the mass ratio of pine alcohol and ZrO2 powder is changed, and other components remain unchanged, so as to achieve the effect of controlling the thickness of the mesoporous support layer ZrO2 film, thereby controlling the filling amount of perovskite, thereby regulating the growth of perovskite in Zr The filling and growth of the O2 mesoporous support layer; when preparing the NiO film, the number of times the substrate passes under the flame in the flame-assisted chemical vapor deposition method is changed to change the porosity, surface roughness, and crystallinity of the mesoporous hole transport layer NiO film, thereby controlling the filling effect and filling amount of the perovskite, thereby regulating the filling growth of the perovskite in the NiO mesoporous hole transport layer; when preparing the C film, the annealing temperature is changed to control the surface roughness of the back electrode C film and the orientation of the carbon layer, wherein the roughness and orientation will affect the filling effect of the perovskite, thereby regulating the filling growth of the perovskite in the C layer.