Composite material comprising void spaces and preparation and use thereof

By using composite materials with hole space in lithium-ion batteries, the structural deterioration caused by volume expansion of silicon particles during charging and discharging is solved, the cycle stability and capacity maintenance of lithium-ion batteries are improved, and the battery life is extended.

CN118946526APending Publication Date: 2024-11-12ASPEN AEROGELS INC
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380030436.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-07-20
Filing Date
2023-07-18
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

In the charging and discharging process of silicon particles in existing lithium-ion batteries, the structure deteriorates due to volume expansion, resulting in poor cycle stability and capacity degradation. Nano-sized silicon particles lead to structural cracks and crushing due to large surface area and high binding energy.

Method used

Using composite materials including hole space, by creating hole space between the outer surface of the silicon particles and the three-dimensional carbon network structure to accommodate the volume expansion of the silicon particles, the structural integrity of the material is improved and the direct exposure of silicon to the electrolyte is prevented.

Benefits of technology

It significantly improves the cycle stability and capacity maintenance of lithium-ion batteries, extends battery life, reduces capacity fading, and improves battery performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005059809920000141
    Figure BDA0005059809920000141
  • Figure HDA0005059809930000011
    Figure HDA0005059809930000011
  • Figure HDA0005059809930000012
    Figure HDA0005059809930000012
Patent Text Reader

Abstract

Provided herein are composites for use in electrical energy storage systems (e.g., high capacity batteries) and methods for making the composites. Composite materials of the present disclosure include silicon particles and a three-dimensional carbon network structure. The composite material further includes a void space between the outer surface of each silicon particle and the three-dimensional carbon network structure. The void space advantageously provides a space to accommodate changes in volume of the silicon particles during charging and discharging of the electrical energy storage system.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] CROSS-REFERENCE TO RELATED APPLICATIONS

[0002] This application claims priority to and the rights of U.S. Provisional Application No. 63 / 390,838, filed on July 20, 2022, the contents of which are incorporated herein by reference in their entirety. Technical Field

[0003] The present disclosure generally relates to composite materials for use in electrical energy storage systems (e.g., high-capacity batteries) including void spaces and methods for preparing the composite materials. More specifically, the present disclosure relates to materials and methods for producing composite materials including silicon particles and a three-dimensional carbon network structure, wherein the void spaces (e.g., pores) exist between the outer surface of the silicon particles and the three-dimensional carbon network structure. Background Art

[0004] High-capacity battery materials, such as lithium-ion batteries (LIBs), represent one of the most attractive energy storage systems and play an increasingly important role in modern society. They have conquered the market for portable electronics such as mobile phones, laptops and digital cameras. They have also been established as the preferred power source for electric vehicles and stationary energy storage. However, the current state-of-the-art technologies cannot meet the growing demands of electric vehicles and large-scale energy storage.

[0005] Silicon is one of the most promising anode materials for lithium-ion batteries because it has the highest known theoretical capacity and crustal abundance. Silicon has been shown to have a high theoretical gravimetric capacity of approximately 4200 mAh / g, while graphite has only 372 mAh / g. Therefore, silicon (Si) active materials have been viewed as promising candidates for next-generation lithium-ion battery (LIB) anodes.

[0006] Unfortunately, silicon is known to undergo significant "breathing effect" during insertion / extraction of lithium during continuous charge and discharge processes. This "breathing effect" causes severe structural degradation and leads to loss of specific capacity and increase in battery impedance. In other words, the volume of Si can expand by about 400% of its original size during lithiation (insertion of lithium ions into silicon) and then shrink to a different size during delithiation (extraction of lithium ions from silicon). Significant volume changes are a real challenge for Si electrodes to retain their morphology through cycling.

[0007] With each cycle, the expansion creates stress and strain on the silicon, causing cracks and fragmentation. The silicon fragmentation process is called comminution. Due to this comminution, the electrical isolation between silicon fragments causes loss of contact with adjacent fragments. In addition, the space caused by the expansion pushes the surrounding conductive material away from the active material, also causing loss of contact, resulting in low conductivity. Without strong electrical contact with the current collector, the silicon fragments will not lithiate and cannot contribute to the capacity of the battery. This behavior leads to low capacity stability and rapid capacity degradation after a large number of cycles. The reduction in capacity during charge and discharge cycles is called fading or continuous capacity reduction and is generally irreversible.

[0008] The particle size of the silicon particles may play a role in how quickly the battery performance degrades. Without being bound by theory, nano-sized silicon particles have better capacity in accommodating the volume change of Si due to its larger specific surface area and higher average binding energy per atom at the surface. These materials can therefore minimize the stress imposed on them when the volume changes and avoid cracks or shattering of their structure, and reduce irreversible capacity and enhance cycle stability.

[0009] In addition, the surrounding environment, chemical properties, surface properties and morphology of silicon particles may affect the mechanical stability, aggregation, processing and electrochemical properties of silicon particles.

[0010] Therefore, there is a need for improved methods for controlling, selecting, modifying or improving the surface properties and morphology of electroactive materials such as silicon. Summary of the invention

[0011] In order to eliminate or alleviate at least one disadvantage (e.g., cycle stability, battery life) of previous methods and materials for improving the performance of high-capacity batteries (such as, for example, lithium-ion batteries), the present technology provides a composite material comprising pore spaces (e.g., pores). The composite material provided herein further comprises silicon particles and a three-dimensional carbon network structure, wherein the pore space is between the outer surface of the silicon particles and the three-dimensional carbon network structure.

[0012] In one aspect, the multiple pores of the present technology provide several advantages, including providing space to accommodate the volume expansion of silicon particles during the charging process and stabilizing the composite material. Without wishing to be bound by theory, accommodating the volume expansion of silicon particles can delay the fracture of silicon particles due to continuous charge and discharge battery cycling.

[0013] The presence of pores can reserve space for Si particles during volume expansion as well as buffer the mechanical pressure of the three-dimensional carbon network structure (also called porous network structure or porous network composite), leading to significantly improved structural integrity and thus preventing Si from being directly exposed to the electrolyte.

[0014] The pore spaces sufficient to accommodate the volume expansion of the silicon particles provide free space for volume expansion accommodation.

[0015] In one aspect, the pore space between the outer surface of the silicon particles and the three-dimensional carbon network structure can lead to good dispersion and anti-aggregation of the silicon particles.

[0016] In one aspect, the materials provided in the present disclosure can advantageously prevent or mitigate rapid capacity fade (eg, over at least 10 cycles) of high capacity batteries.

[0017] The composite materials of the present technology can improve the performance of lithium-ion batteries relative to lithium-ion batteries having electrodes without the disclosed composite materials (eg, composite materials without pores).

[0018] Provided herein is a composite material including a void space, further comprising: silicon particles having a diameter of less than about 1000 nm; and a three-dimensional carbon network structure, wherein the void space is between the outer surface of the silicon particles and the three-dimensional carbon network structure. In other words, the void space surrounds or contains the silicon particles, providing isolation or space to accommodate the "breathing" of silicon. In some embodiments, the silicon particles have a diameter of less than about 300 nm.

[0019] Provided herein is a composite material including void spaces, further comprising: silicon particles having a diameter of about 50 nm to about 1000 nm, about 300 nm to 1000 nm; and a three-dimensional carbon network structure, wherein the void spaces are between the outer surface of the silicon particles and the three-dimensional carbon network structure.

[0020] In some embodiments, the volume of the pore space is between 1% and 80%, 1% and 70%, 1% and 60%, 1% and 50%, 1% and 40%, 1% and 30%, 1% and 20%, 3% and 80%, 3% and 60%, 3% and 40%, 3% and 40%, 3% and 30%, 3% and 20%, 3% and 10%, 3% and 20%, 3% and 50%, 3% and 100%, 3% and 200%, 3% and 250%, 5% and ... 40%, 5% to 20%, 5% to 15%, 10% to 20%, 20% to 40%, 20% to 50%, 20% to 60%, 20% to 80%, 20% to 100%, 50% to 100%, 20% to 120%, 20% to 140%, 20% to 160%, 20% to 180%, 20% to 200%, 20% to 250%, 50% to 200%, 80% to 200%, 100% to 200%, 50% to 250%. The present technology provides a design advantage of controllable pore space volume. In some embodiments, the pore volume is controlled by providing a sacrificial layer of known thickness surrounding the silicon particles. In some embodiments, the pore space is designed by controlling the number and / or distribution of silicon particles with a sacrificial layer.

[0021] In some embodiments, the three-dimensional carbon network structure includes a carbon aerogel derived from a polyimide. In some embodiments, the three-dimensional carbon network structure includes a carbon aerogel, a carbon xerogel, a carbon bigel, a carbon aerogel-xerogel hybrid material, a carbon aerogel-bigel hybrid material, a carbon aerogel-bigel-xerogel hybrid material, or a combination thereof. In some embodiments, the three-dimensional carbon network structure is in the form of a bead. In some embodiments, the bead is substantially spherical, with a diameter of about 100 nm to about 4 mm or about 5 μm to about 4 mm.

[0022] In some embodiments, the silicon particles are dispersed in the three-dimensional carbon network structure. In some embodiments, the silicon particles are unevenly dispersed throughout the three-dimensional carbon network structure. In some embodiments, about 10wt% to about 20wt%, about 10wt% to about 30wt%, about 10wt% to about 60wt%, about 20wt% to about 50wt% of the dispersed silicon particles are in an aggregated state. In some embodiments, less than about 20wt% of the dispersed silicon particles are in an aggregated state.

[0023] In some embodiments, the carbon network structure is a carbon network structure. In some embodiments, the pore structure of the three-dimensional carbon network structure includes a maximum peak of distribution at a pore size of about 150nm or less. In some embodiments, the three-dimensional carbon network structure has a total bead level pore volume of at least 0.3cc / g. In some embodiments, the three-dimensional carbon network structure has a total bead porosity level between about 10% and about 90%. In some embodiments, the three-dimensional carbon network structure has a porosity less than about 90%.

[0024] In some embodiments, the composite material has a capacity between about 500 mAh / g and about 3000 mAh / g. In some embodiments, the three-dimensional carbon network structure has a conductivity of at least about 1 S / cm.

[0025] In one aspect, an energy storage system is provided herein, comprising a composite material according to the present technology. In some embodiments, the energy storage system is a battery. In one embodiment, the battery is a rechargeable battery. In another embodiment, the rechargeable battery is a lithium-ion battery.

[0026] In another aspect, provided herein is a rechargeable battery comprising a composite material according to the present technology.

[0027] In one aspect, the present invention provides a method for preparing a composite material, the method comprising: a. providing silicon particles; b. oxidizing the surface of the silicon particles to obtain hydroxyl groups on the surface; c. forming a sacrificial layer on at least a portion of the surface of the silicon particles; d. providing a sol-gel solution, the sol-gel solution comprising a polar solvent and a precursor of a porous network structure; e. treating the silicon particles in the presence of the sol-gel solution to obtain a precursor bead, the precursor bead comprising silicon particles dispersed in the precursor bead, the precursor bead may include pores or optionally does not include pores; and f. pyrolyzing the precursor bead comprising silicon particles dispersed throughout the precursor bead to obtain a porous network composite material, the porous network composite material comprising a pore space. In some embodiments, the three-dimensional network structure is a porous network structure. In some embodiments, the silicon particles have a diameter of less than 1000nm. In some embodiments, the silicon particles have a diameter in the range of about 300nm to about 1000nm. In some embodiments, the silicon particles have a diameter of less than 300nm.

[0028] In some embodiments, the sacrificial layer is formed of a material selected from the group consisting of polymethyl methacrylate (PMMA), polyvinyl pyrrolidone (PVP), polyvinyl acetate (PVAc), polyvinyl alcohol (PVA), polyacrylonitrile (PAN), polyethylene oxide (PEO), polypropylene oxide (PPO), polyethyleneimine (PEI), polyurethane, poly(3,4-ethylenedioxythiophene) (PEDOT), polyvinyl butyral, polyethylene oxide copolymer, polypropylene oxide copolymer, polycarbonate (PC), polyvinyl chloride (PVC), polycaprolactone, polyvinylidene fluoride, polystyrene, or a combination thereof.

[0029] In some embodiments, the sacrificial layer has a thickness less than or equal to about 100 nm, or a thickness between about 100 nm and about 60 nm, or a thickness of about 60 nm to 0.3 nm. In some embodiments, the sacrificial layer has a thickness in the range of about 20% to about 0.01% of the diameter of the silicon particles.

[0030] In some embodiments, the sacrificial layer has a carbonization yield of less than about 20 wt%. In some embodiments, the chemical decomposition temperature of the sacrificial layer is in a range of about 130°C to about 850°C.

[0031] In some embodiments, the sacrificial layer is uniform over at least a portion of the surface of the silicon particles. In some embodiments, the sacrificial layer is continuous over at least a portion of the surface of the silicon particles. In some embodiments, at least a portion of the surface of the silicon particles is at least 70% of the surface of the silicon particles, at least 90% of the surface of the silicon particles, or at least 9% of the surface of the silicon particles.

[0032] In some embodiments, the composite material is in monolithic form, flake form, or particle form.

[0033] In some embodiments, the method further comprises a step of subcritical or supercritical drying after treating the silicon particles in the presence of the sol-gel solution and before pyrolyzing the precursor beads comprising the silicon particles.

[0034] In some embodiments, the porous network structure comprises an aerogel, a xerogel, a bigel, an aerogel-xerogel hybrid material, an aerogel-bigel hybrid material, an aerogel-bigel-xerogel hybrid material, or a combination thereof. In some embodiments, the porous network structure comprises a polyimide derivative. In some embodiments, the porous network structure is in the form of beads.

[0035] In some embodiments, the porous network structure has a carbonization yield greater than about 30 wt %.

[0036] In some embodiments, the precursor beads are pyrolytically carbonized to form a sacrificial layer. In some embodiments, the sacrificial layer has a carbonization yield of less than about 20 wt%.

[0037] In one aspect, the present invention provides a method for preparing a composite material, the method comprising: a. providing silicon particles; b. forming a sacrificial layer on at least a portion of the surface of the silicon particles; d. incorporating the silicon particles into a three-dimensional network structure; and e. processing the three-dimensional network structure to obtain a composite material including a pore space surrounding the silicon particles. In some embodiments, the three-dimensional network structure is a porous three-dimensional network structure.

[0038] In some embodiments, the at least a portion of the surface of the silicon particle is at least 70% of the surface of the silicon particle, at least 90% of the surface of the silicon particle, or at least 95% of the surface of the silicon particle.

[0039] In some embodiments, the three-dimensional network structure includes organic materials. In some embodiments, the step of processing the three-dimensional network structure includes heating the three-dimensional network structure to the carbonization temperature of the sacrificial layer. In some embodiments, the step of processing the three-dimensional network structure includes pyrolyzing the three-dimensional network structure. In some embodiments, the three-dimensional porous network structure has a carbonization yield greater than about 30wt%. In some embodiments, pyrolyzing the three-dimensional network structure carbonizes the sacrificial layer. In some embodiments, the sacrificial layer has a carbonization yield less than about 20wt%.

[0040] Provided herein is a composite material comprising void spaces surrounding silicon particles, which can be obtained by any of the methods described in the present technology.

[0041] In another aspect, a method of improving the performance of an energy storage system is provided herein, wherein the method comprises incorporating a composite material according to the present disclosure. BRIEF DESCRIPTION OF THE DRAWINGS

[0042] The present technology will be more fully understood from the following detailed description in conjunction with the accompanying drawings, in which:

[0043] Figure 1A Scanning electron microscope (SEM) photographs of exemplary composite materials according to the present disclosure are shown.

[0044] Figure 1B Shown is a graphical representation of an exemplary composite material according to the present disclosure.

[0045] Figure 2 Depicted are steps in a method of making an exemplary composite material according to an embodiment of the present disclosure.

[0046] Figure 3 Depicted are steps in a method of making an exemplary composite material according to an embodiment of the present disclosure.

[0047] Figure 4A and 4BA preparation scheme is shown for forming a sacrificial layer on at least a portion of a silicon particle surface, followed by pyrolysis to form an exemplary composite material according to the present disclosure.

[0048] Figure 5 Infrared radiation (IR) spectra showing pristine, oxidized and surface modified Si particles. DETAILED DESCRIPTION

[0049] Silicon (Si) is considered to be a promising alternative LIB anode material. It forms Li7Si3, Li 12 Si7、Li 13 Si4、Li 15 Si4 and Li 22 Si5 silicon-lithium alloy, in which Li 15 Si4 has 3579mAh g at room temperature -1 (2194Ah L -1 ), which is the highest known theoretical capacity of anode materials. Therefore, it is desirable to incorporate as much silicon as possible into the anode.

[0050] At the same time, the average voltage plateau of Si (0.4 V vs. Li / Li + ) is higher than graphite electrode (0.125V vs. Li / Li + ), which makes it possible to avoid lithium plating and dendritic lithium formation on the surface of the anode material during the lithiation process. As a result, the safety performance of the battery can be significantly improved. Moreover, Si has the advantages of abundant reserves in the earth's crust and low cost, which further stimulates the interest of the industry in using silicon in batteries.

[0051] Despite these advantages, silicon still has serious drawbacks when used as an electrode material. The core problem of using Si in LIBs is the huge volume expansion during lithiation. Si electrodes can expand up to 400%, which is much larger than the 10% expansion of graphite electrodes. First, Si particles are gradually crushed and lose electrical contact between the active material and other components (including conductive carbon and binder) due to repeated volume changes, which causes a sharp decrease in capacity and a rapid decline in cycle performance. Secondly, the volume change also gradually causes the active material to fall off from the current collector, resulting in a loss of electrical contact between the active material and the current collector, and a decrease in electrode capacity after the initial cycle. In addition, due to the expansion / contraction behavior of the Si electrode during the cycle, the solid electrolyte interphase (SEI) layer is broken and continuously reformed, resulting in a continuous exposure of fresh Si surfaces to the electrolyte. Therefore, electrolyte degradation occurs continuously on the highly reduced fresh lithiated Si surface, resulting in irreversible capacity loss and ultimately battery failure at each cycle. Both mechanical failure and electrolyte degradation can cause the Si electrode to lose its electrochemical activity very quickly during the cycle.

[0052] The composite material provided herein avoids or mitigates at least one defect of Si when used as an electrode material. Without being bound by theory, in general, the composite material provided herein may be able to accommodate the volume change of active Si material during battery operation. In general, the composite material of the present technology includes a cut or designed pore space that accommodates the volume change of silicon particles incorporated into the composite material.

[0053] In the following description, several embodiments are provided in the context of lithium-ion batteries because of the current prevalence and penetration of lithium-ion technology. However, it should be recognized that such embodiments are provided only to assist in the understanding and description of the underlying technology, and that these technologies can be similarly applied to various other metal ion batteries, such as Li + 、Na + Mg 2+ , Ca 2+ and Al 3+ , and other metal ion batteries. The disclosed composites can be used in other battery chemistries where the active particles undergo significant volume changes during their operation (eg, irreversible reduction-oxidation reactions), for example, batteries containing aqueous electrolytes.

[0054] definition

[0055] The articles "a" and "an" are used herein to refer to one or more than one (ie, to at least one) of the grammatical object of the article.

[0056] In the context of the present disclosure, the term "about" used throughout this specification is used to describe and illustrate small fluctuations. For example, the term "about" can refer to less than or equal to ±10%, or less than or equal to ±5%, such as less than or equal to ±2%, less than or equal to ±1%, less than or equal to ±0.5%, less than or equal to ±0.2%, less than or equal to ±0.1%, or less than or equal to ±0.05%. All numerical values ​​herein are modified by the term "about", whether or not explicitly stated. Values ​​modified by the term "about" certainly include the specific value. For example, "about 5.0" must include 5.0.

[0057] In the context of the present disclosure, the term "aerogel" or "aerogel material" refers to a solid object, regardless of shape or size, comprising a framework of interconnected solid structures, having a corresponding network of interconnected pores integrated within the framework, and containing a gas such as air as a dispersed interstitial medium. Thus, an aerogel (such as the carbon aerogel of the present application) is an open non-fluid colloid or polymer network expanded throughout the volume by a gas. Aerogels (e.g., carbon aerogels) are generally prepared by removing solvent from a gel (a solid network containing a solvent) in a manner such that gel shrinkage due to capillary forces at the gel pore walls is minimal or absent, in other words, by removing all of the swelling agent from the corresponding wet gel without substantial volume reduction or network compaction. Solvent removal methods include, but are not limited to, supercritical drying (or drying using a supercritical fluid such that the low surface tension of the supercritical fluid is exchanged with a transient solvent in the gel), exchanging a solvent with a supercritical fluid, exchanging a solvent with a fluid that subsequently transitions to a supercritical state, subcritical or near-critical fluid drying, and sublimating a frozen solvent in a freeze-drying process. See, for example, PCT patent application publication number WO2016127084A1.

[0058] Aerogels, such as carbon aerogels, include a highly porous network of micropores, mesopores, and macropores and are generally characterized by the following physical and structural properties attributable to aerogels (according to nitrogen porosity testing and helium pycnometer determination): (a) an average pore diameter in the range of about 2 nm to about 100 nm; (b) a total bead porosity level of at least 60% or greater, and (c) a specific surface area of ​​about 100 m2 as analyzed by nitrogen adsorption. 2 / g or more, such as about 100 to about 1000m 2 / g.

[0059] Thus, the aerogel materials of the present disclosure include any aerogel or other open-cell compound that satisfies the defining elements detailed in the preceding paragraphs.

[0060] As used herein, the terms "xerogel" and "bigel" refer to a gel comprising an open, non-fluid colloid or polymer network formed by removing all of the swelling agent from a corresponding wet gel without taking any precautions to avoid substantial volume reduction or compaction, such as drying at ambient pressure. In contrast to aerogels (e.g., carbon aerogels), xerogels such as carbon xerogels generally comprise a compacted structure. Xerogels undergo substantial volume reduction during ambient pressure drying and may have a lower surface area than aerogels, such as 0 to 100 m 2 / g or about 0 to about 20 m 2 / g, as measured by nitrogen adsorption analysis.

[0061] In the context of the present disclosure, the term "continuous" refers to a layer without voids, holes or any discontinuities. For example, a continuous layer does not include two (or more) constituent materials within the layer that are physically isolated (or spatially separated).

[0062] As used herein, the term "uniform" refers to a material (eg, a coating of the present disclosure) having a thickness that varies by less than about 10%, less than about 5%, or less than about 1%.

[0063] In the context of the present disclosure, the term "capacity" refers to the amount of specific energy or charge that a battery can store. Capacity is specifically measured as the discharge current per unit mass that a battery can deliver over time. It is typically provided as ampere-hours or milliampere-hours per gram of total active material mass (Ah / g or mAh / g). For example, a battery with a capacity of 1Ah can supply a current of one ampere for one hour or a current of 0.5 amperes for two hours, etc. Therefore, 1 ampere-hour (Ah) is equivalent to 3,600 coulombs of charge. Similarly, the term "milliampere-hour (mAh)" also refers to the storage capacity unit of a battery, and is 1 / 1,000 of an ampere-hour. The capacity of a battery (and in particular an anode) can be measured by methods known in the art, for example, including but not limited to: applying a fixed constant current load to a fully charged battery cell until the voltage of the battery cell reaches the discharge end voltage value; the time to reach the discharge end voltage multiplied by the constant current is the discharge capacity; the discharge capacity is divided by the electrode material weight or volume. In the context of this disclosure, unless otherwise specified, capacity measurements are obtained according to this method.Unless otherwise specified, capacity is reported at the 10th cycle of the battery.

[0064] As used herein, the term "electrode" refers to either a "cathode" or an "anode." As used herein, a "positive electrode" is used interchangeably with a cathode. Likewise, the term "negative electrode" is used interchangeably with an anode.

[0065] In the context of the present disclosure, the term "dispersion" refers to a dispersion in which one substance (the dispersed phase) is distributed in discrete units throughout a second substance (the continuous phase or medium). Generally speaking, the dispersed phase is substantially non-aggregated, but rather is spaced apart within the second substance. Although the dispersion includes some agglomerations or touches of particles (e.g., two, three, four, less than five), the particles are generally evenly spaced apart throughout the second medium.

[0066] In the context of the present disclosure, the term "framework" or "framework structure" refers to a network of interconnected oligomers, polymers or colloidal particles that form the solid structure of a gel or aerogel. The polymers or particles that make up the framework structure typically have a diameter of about 100 angstroms. However, the framework structure of the present disclosure may also include a network of interconnected oligomers, polymers or colloidal particles of all diameter sizes that form the solid structure within a gel or aerogel.

[0067] As used herein, "particle size D50" is the cumulative 50% particle size based on volume, which is the particle size at the 50% point on the cumulative curve (i.e., the particle diameter of the 50th percentile (median) of the particle volume) when a cumulative curve is plotted to obtain a volume-based particle size distribution and the entire volume is 100%.

[0068] Composite Materials

[0069] In one aspect, the composite materials provided herein deliver high lithium storage capacity with improved cyclability.

[0070] Figure 1A and Figure 1B Depicts an exemplary composite material of the present disclosure. Figure 1A and Figure 1B In one aspect, a composite material 100 comprising a void space 120 (e.g., a void 120) is provided herein. The composite material of the present disclosure comprises silicon particles 110 having a diameter less than about 300 nm; and a three-dimensional carbon network structure 130. The silicon particles are generally provided by the same source and have a known desired particle size, shape, porosity, and other substantially similar material properties. In some embodiments, the silicon particles have a diameter less than 1000 nm, less than 800 nm, less than 500 nm, less than 300 nm, less than 250 nm, less than 200 nm, less than 150 nm, or less than 100 nm. In some embodiments, the three-dimensional carbon network structure is a carbon aerogel or a carbon xerogel. Figure 1A and Figure 1B The pore space shown in is between the outer surface of the silicon particle and the three-dimensional carbon network structure. This is a pore that at least partially surrounds or covers the silicon particle and is therefore able to accommodate volume changes of the silicon particle.

[0071] In the context of the present disclosure, the term "pore" or "pore space" as used throughout this specification refers to "empty" space, ie, space that is not utilized by either silicon or the three-dimensional carbon network structure.

[0072] In some embodiments, the volume of the hole space is about 1% to about 20%, about 3% to about 15%, about 5% to about 15%, about 3% to about 10%, or about 5% to about 10% of the volume of the silicon particle. In the attempt to design the hole space of the present disclosure, a sacrificial layer is first produced on at least a portion of the outer surface of the silicon particle. The sacrificial layer of the present technology provides a design advantage of controllable hole space volume. In other words, the hole space between the outer surface of the silicon particle and the three-dimensional carbon network structure can be established by partially or completely removing the sacrificial layer. By adjusting the thickness of the sacrificial layer of the present technology, the volume of the hole space can be controlled.

[0073] In another embodiment, the volume of the void space can be adjusted by controlling the amount of sacrificial layer that is removed (e.g., decomposed) upon exposure to an external stimulus / agent. Without wishing to be bound by theory, as the amount of sacrificial layer removed increases, the volume of the void space becomes larger.

[0074] In some embodiments, the volume of the pore space is cut or controlled by controlling the distribution of the silicon particles. In certain embodiments, the volume of the pore space is cut or controlled by designing the number of silicon particles in the composite material (e.g., the volume percentage of the particles, or the volume percentage of the sacrificial layer component).

[0075] Generally speaking, silicon is at least partially contained in the pores of the porous network structure, that is, silicon is placed in the framework of the porous network structure. Silicon accepts lithium ions during charging and releases lithium ions during discharging. In certain embodiments, the porous network structure forms an interconnected structure surrounding silicon, and silicon is connected to the porous network structure at multiple points. In some embodiments, the three-dimensional network structure is a porous network structure.

[0076] Measurement of composite material properties

[0077] Composite materials can be characterized by properties such as pore volume, porosity, surface area, and pore size distribution. These properties and related terms are defined below, along with methods of measuring and / or calculating such properties.

[0078] In the context of the present disclosure, the term "pore volume" refers to the total volume of pores within a porous material sample. Pore volume is specifically measured as the volume of the void space within the porous material, where the void space may be measurable and / or accessible to another material (e.g., an electrochemically active material such as silicon particles). It is typically reported as cubic centimeters per gram (cm 3 / g or cc / g).

[0079] In the context of the present disclosure, the term "porosity" when used with respect to a polymer network structure or a composite material disclosed herein refers to the volume fraction of pores that do not contain another material (e.g., an electrochemically active material, such as silicon particles) bound to the pore walls. For clarity and description purposes, it should be noted that in the specific implementation of a silicon-doped polymer network structure (e.g., such as an aerogel as the primary anode material in a LIB), the porosity refers to the pore space after the silicon particles are included. Thus, the porosity can be, for example, about 10%-70% (to accommodate ion transport and silicon expansion) when the anode is in a pre-lithiated state; and about 1%-50% when the anode is in a post-lithiated state. It should be noted that pore volume and porosity are different measurements of the same property of a pore structure (i.e., the "empty space" within the pore structure). For example, when silicon is used as the electrochemically active material contained within the pores of a polymer network structure (e.g., a composite material described herein), the pore volume and porosity refer to the "empty" space, i.e., the space not utilized by silicon or carbon.

[0080] In the context of the present disclosure, the term "pore size distribution" refers to the statistical distribution or relative amount of each pore size within a sample volume of a porous material. A narrower pore size distribution means that a relatively large portion of the pores are within a narrow pore size range, thereby optimizing the amount of pores that can surround the electrochemically active material and maximizing the use of the pore volume. In contrast, a wider pore size distribution means that a relatively small portion of the pores are within a narrow pore size range. Therefore, the pore size distribution is typically measured as a function of pore volume and recorded in a pore size distribution graph as a unit size of the full width at half maximum of the main peak.

[0081] In the context of the present disclosure, the term "pore size at the maximum peak from a distribution" refers to the value at a discernible peak on a graph depicting a pore size distribution. The pore size at the maximum peak from a distribution is specifically measured as the pore size at which the maximum percentage of pores are formed. It is typically recorded as the pore size per unit length, e.g., micrometers or nanometers (nm).

[0082] In the context of this disclosure, the term "BET surface area" has its usual meaning and refers to the Brunauer-Emmett-Teller method for determining surface area by N2 adsorption measurement. The BET surface area is expressed in m 2 The term "surface area" is used to represent the total surface area of ​​a porous material per unit mass. Unless otherwise specified, "surface area" refers to the BET surface area. As an alternative to the BET surface area, the geometric surface area of, for example, a polyimide or carbon bead can be calculated based on the diameter of the bead. Generally, such geometric surface area of ​​the beads of the present disclosure is between about 3 and about 700 μm. 2 within the range.

[0083] As used herein, the term "particle size D50" is the cumulative 50% particle size based on volume, which is the particle size at the 50% point on the cumulative curve (i.e., the particle diameter of the 50th percentile (median) of the particle volume) when a cumulative curve is plotted to obtain a volume-based particle size distribution and the entire volume is 100%.

[0084] In the context of this disclosure, the term "density" refers to a measurement of the mass of a material (e.g., a composite material as described herein) per unit volume. The term "density" generally refers to the true or skeletal density of a material, as well as to the bulk density of a material or composition. Density is typically reported as g / cm 3 , g / cc or g / mL.

[0085] Composite properties can be determined using mercury intrusion porosimetry and helium pycnometer experiments. Mercury intrusion porosimetry can be used to determine the porosity, pore size, and pore volume of solid particles. During a typical mercury intrusion porosimetry, a pressurized chamber is used to force mercury into the pores in a porous material. As pressure is applied, mercury first fills the larger pores. As pressure increases, mercury can enter smaller pores. Mercury pycnometer can reach and measure pores larger than about 3nm. Mercury intrusion porosimetry can be used to measure bulk density, skeletal density, and porosity. By varying the test parameters (e.g., pressure range), pores with different sizes can be excluded. If the mercury intrusion porosity is about 3nm, the lower pore size is limited.

[0086] Helium pycnometer determination uses helium to measure the pore volume of solid materials. During the helium pycnometer determination, the sample is sealed in a compartment and helium is added to the compartment. The helium penetrates into the pores of the material. After the system is balanced, the change in pressure can be used to determine the skeletal density of the solid material. The helium pycnometer determination can reach and measure pores greater than about 0.3nm, for example, pores with a size ranging from about 3nm to about 300nm.

[0087] “Hg skeleton density” (g / cm 3 ) is calculated by dividing the mass of the composite particle (g) by the volume of the particle (cm 3 ), where the volume is measured by controlling (e.g., by pressure) the mercury that reaches the pores larger than 3 nm of the particle during the measurement. This volume does not include the volume of the composite's mercury-accessible pores larger than 3 nm. Instead, the volume includes only the volume of the "skeleton" of the composite particle. The volume of pores smaller than 3 nm is considered part of the skeleton and is included in the skeleton density calculation.

[0088] The Hg bulk density is calculated by dividing the mass of the composite particle (g) by the volume of the particle (cm 3), where the volume is measured by controlling (e.g., by pressure) the mercury that does not reach the pores of the particles during the measurement. This volume includes the volume of the pores of the composite material, including pores larger than 3 nm and pores smaller than 3 nm.

[0089] The He skeletal density is calculated by dividing the mass of the composite particle (g) by the volume of the particle (cm 3 ), where the volume is measured by controlling (e.g., by pressure) the helium that reaches the pores larger than 0.3 nm of the particle during the measurement. This volume does not include the volume of the composite's helium accessible pores larger than 0.3 nm. Instead, the volume includes only the volume of the "skeleton" of the composite particle. The volume of pores smaller than 0.3 nm is considered part of the skeleton and is included in the skeleton density calculation.

[0090] Composite materials may also include pores that are inaccessible to both helium and mercury during helium pycnometer or mercury pycnometer testing. For example, some pores formed by removing sacrificial particles may be enclosed in a three-dimensional network structure and are therefore inaccessible to both helium pycnometer and mercury pycnometer. The amount of these inaccessible pores in the composite materials of the present disclosure is generally very small. The inaccessible pores act as part of the skeleton volume without introducing significant changes.

[0091] Various physical properties can be calculated according to the following equations using the mercury (Hg) skeletal density measured by mercury pycnometry (Hg skeletal density), the mercury intrusion bulk density measured by mercury pycnometry (Hg bulk density), and the helium (He) skeletal density tested by helium pycnometry (He skeletal density).

[0092]

[0093] Micropore volume percentage (%, relative to total pore volume) = micropore volume / total pore volume (4) Mesopore volume percentage (%, relative to total pore volume) can be obtained by mercury intrusion by excluding all pores > 50 nm

[0094] Macropore volume percentage (%, relative to total pore volume)

[0095] =1-micropore volume percentage-mesopore volume percentage (5)

[0096] "Total bead porosity level" (%) refers to the ratio of the pore volume in the composite particle to the volume of the composite particle. The total bead porosity level is calculated by equation (1). The total bead porosity level includes pores larger than 0.3 nm that are accessible to helium and mercury.

[0097] “Total pore volume” (cm 3The total pore volume (g) refers to the total pore volume per unit weight of the composite material particles. The total pore volume is calculated by equation (2). The total pore volume includes pores larger than 0.3 nm that are accessible to helium and mercury.

[0098] “Micropore volume” (cm 3 / g) refers to the micropore volume per unit weight of composite material particles. The micropore volume of the composite material (cm 3 / g) is the skeletal density of mercury according to equation (3) (g / cm 3 ) (cm 3 / g) and helium skeleton density (g / cm 3 ) (cm 3 The micropore volume includes pores larger than 0.3 nm but smaller than 3 nm. Micropores are accessible to helium but inaccessible to mercury.

[0099] "Micropore volume percentage" (%) refers to the volume ratio between the volume of micropores and the total pore volume. The micropore volume percentage is calculated by equation (4).

[0100] "Mesopore volume percentage" (%) refers to the volume ratio between the volume of mesopores and the total pore volume. Mesopores refer to pores between about 3 nm and about 50 nm that are accessible to mercury. Pores below 3 nm are inaccessible to mercury. The mesopore volume percentage can be measured directly using a mercury pycnometer by excluding pores greater than 50 nm. The mesopore volume percentage can also be obtained by subtracting the micropore volume percentage (calculated using equation (4)) and the macropore volume percentage (measured by mercury pycnometer) from the total pore volume percentage (100%).

[0101] "Macropore volume percentage" (%) refers to the volume ratio between the volume of macropores and the total pore volume. Macropores are larger than about 50 nm and are accessible to mercury. The macropore volume percentage can be measured directly using mercury pycnometry by excluding pores smaller than 50 nm. The macropore volume percentage can also be obtained by subtracting the micropore volume percentage (calculated by equation (4)) and the mesopore volume percentage (measured by mercury pycnometry) from the total pore volume percentage (100%).

[0102] Composite material properties

[0103] Total porosity

[0104] The composite materials described herein generally include micropores (<3nm), mesopores (3nm-50nm) and macropores (>50nm). The composite materials described herein include a three-dimensional carbon network structure with a substantial amount of macropores. In some aspects, the total porosity level (total bead porosity level) of the three-dimensional carbon network structure is greater than 10%, greater than 20%, greater than 30%, greater than 40%, greater than 50%, greater than 60%, or greater than 70%. In some aspects, the total porosity level of the three-dimensional carbon network structure is 25% to 35%, 30% to 40%, 35% to 45%, 40% to 50%, 55% to 65%, or 60% to 70%.

[0105] Total pore volume

[0106] In some aspects, the aerogel materials or compositions of the present disclosure (without incorporating an electrochemically active material, e.g., silicon) have a relatively large total pore volume of about 1 cc / g or more, 1.5 cc / g or more, 2 cc / g or more, 2.5 cc / g or more, 3 cc / g or more, 3.5 cc / g or more, 4 cc / g or more, or in a range between any two of these values. In other embodiments, the aerogel materials or compositions of the present disclosure (with incorporating an electrochemically active material, e.g., silicon) have a total pore volume of about 0.3 cc / g or more, 0.6 cc / g or more, 0.9 cc / g or more, 1.2 cc / g or more, 1.5 cc / g or more, 1.8 cc / g or more, 2.1 cc / g or more, 2.4 cc / g or more, 2.7 cc / g or more, 3.0 cc / g or more, 3.3 cc / g or more, 3.6 cc / g or more, or in a range between any two of these values. In other aspects, the total pore volume of the composite material is about 0.1 cm 3 / g to about 1.5cm 3 / g, about 0.1cm 3 / g to about 1.0cm 3 / g, about 0.1cm 3 / g to about 0.5cm 3 / g, about 0.1cm 3 / g to about 0.4cm 3 / g, about 0.4cm 3 / g to about 1.0cm 3 / g, or about 0.9cm 3 / g to about 1.4cm 3 / g.

[0107] Pore ​​size distribution

[0108] In certain aspects, the aerogel materials or compositions of the present disclosure have a relatively narrow pore size distribution (full width at half maximum) of about 150 nm or less, 100 nm or less, 50 nm or less, 45 nm or less, 40 nm or less, 35 nm or less, 30 nm or less, 25 nm or less, 20 nm or less, 15 nm or less, 10 nm or less, 5 nm or less, or in a range between any two of these values.

[0109] Macropores, mesopores and micropores

[0110] In some aspects, macropores constitute a volume fraction greater than about 5%, greater than about 10%, greater than about 20%, greater than about 30%, greater than about 40%, greater than about 50%, greater than about 60%, greater than about 70%, or greater than about 80% of the total pore volume of the three-dimensional carbon network structure. In some aspects, macropores constitute a volume fraction of 45% to 55%, 55% to 65%, 65% to 75%, or 70% to 80% of the total pore volume of the three-dimensional carbon network structure. The composite materials described herein generally have a low mesopore volume fraction. In some aspects, mesopores constitute a volume fraction of less than 20%, less than 10%, less than 5%, less than 2%, or less than 1% of the total pore volume of the three-dimensional carbon network structure. In some aspects, mesopores constitute a volume fraction of 10% to 20%, 5% to 10%, or 1% to 5% of the total pore volume of the three-dimensional carbon network structure.

[0111] The composite material described herein includes a higher percentage of micropores compared to mesopores. In some aspects, the micropores constitute a volume fraction of less than 80%, less than 70%, less than 65%, less than 55%, less than 50%, less than 45%, less than 40%, less than 35%, less than 30%, less than 25%, less than 20%, less than 15%, or less than 10% of the total pore volume of the three-dimensional carbon network structure. In some aspects, the micropores constitute about 10% to about 50%, about 10% to about 45%, about 10% to about 40%, about 10% to about 35% of the total pore volume of the three-dimensional carbon network structure; about 10% to about 30%, about 10% to about 25%, about 10% to about 20%, about 10% to about 15%, about 15% to about 25%, about 25% to about 35%, about 35% to about 45%, or about 45% to about 55%.

[0112] Skeletal density

[0113] In some aspects, composite material has the skeletal density of about 1.0g / mL to about 2.5g / mL, about 1.5g / mL to about 2.5g / mL, about 1.0g / mL to about 2.0g / mL or 1.0g / mL to about 1.5g / mL using helium pycnometer determination method measurement. In some aspects, composite material has the skeletal density of about 0.5g / mL to about 2.5g / mL, about 1.5g / mL to about 2.5g / mL, about 1.5g / mL to about 2.0g / mL, about 0.5g / mL to about 2.0g / mL, about 0.5g / mL to about 1.5g / mL or about 0.5g / mL to about 1.0g / mL using mercury intrusion measurement. In some aspects, the composite material has a bulk density measured using mercury intrusion pycnometry of 0.5 g / mL to about 2.5 g / mL, 0.5 g / mL to about 2.0 g / mL, about 0.5 g / mL to about 1.5 g / mL, or about 0.5 g / mL to about 1.0 g / mL.

[0114] In some embodiments, the composite materials of the present disclosure include low bulk density materials, such as carbon aerogels. In some embodiments, the low bulk density material includes a skeleton framework comprising nanofibers, which forms a pore structure comprising an array of interconnected pores. In some embodiments, such materials may have a fibrous morphology. In some embodiments, the composite material is a carbon aerogel, a carbon xerogel, a carbon crystal gel, or a carbon double gel, or a combination thereof. In some embodiments, the composite material is an aerogel. In contrast to aerogels, xerogels such as silica xerogels generally include a compacted structure. Xerogels undergo a substantial volume reduction during ambient pressure drying and may have a lower surface area than aerogels, such as 0 to 100 m 2 / g or about 0 to about 20 m 2 / g, as measured by nitrogen adsorption analysis. In addition, compared with aerogels, xerogels have a more densely packed fibrous morphology. In the context of the present disclosure, the term "fibrous morphology" refers to the structural morphology of nanoporous materials (e.g., carbon aerosols), including pillars, rods, fibers or filaments. Structurally, some embodiments of the carbon network structure have a fibrous morphology, with pillar sizes that produce the aforementioned narrow pore size distribution, porosity and enhanced interconnectivity and other properties. In any embodiment, the fibrous morphology of the carbon network structure may include an average pillar width of about 2-10nm, or even more specifically about 2-5nm.

[0115] In the context of the present disclosure, the term "pillar width" refers to the average diameter of nanopillars, nanorods, nanofibers, or nanofilaments that form a material with a fibrous morphology. It is typically reported as any unit length (e.g., micrometers or nm). Pillar width can be determined by methods known in the art, such as, but not limited to, scanning electron microscope image analysis. In the context of the present disclosure, unless otherwise specified, pillar width measurements are obtained according to this method. In certain embodiments, the material or composition of the present disclosure has a pillar width of about 10nm or less, 9nm or less, 8nm or less, 7nm or less, 6nm or less, 5nm or less, 4nm or less, 3nm or less, 2nm or less, or in a range between any two of these values. An exemplary range of pillar width is about 2-5nm. Smaller pillar widths, such as these, allow a larger number of pillars to be present in the network structure and thus contact the electrochemically active material, which in turn allows more electrochemically active materials to be present in the composite material. This increases conductivity and mechanical strength.

[0116] Method for preparing composite material

[0117] refer to Figure 2, method 200 depicts the manufacture of a composite material, including five steps (210, 220, 230, 240, 250). First, as shown in step 210, silicon particles are provided. Generally speaking, the silicon particles should be homogeneous. In other words, the silicon particles are generally provided by the same source and have a known desired particle size, shape, porosity and other substantially similar material properties. After obtaining the silicon particles, method 200 includes oxidizing the surface of the particles to obtain hydroxyl functional groups on the surface (i.e., step 220). Oxidation of the surface of the silicon particles is necessary for further functionalization of the surface of certain sources of Si particles. Oxidizing the surface of the silicon particles can lead to complete or partial oxidation of the surface Si-H groups. In other words, after the oxidation process, all or a certain percentage of the Si-H groups on the surface of the silicon particles are converted into Si-O or Si-OH groups. The silicon particles can be oxidized in a single or multiple steps. Oxidation can be thermal oxidation (e.g., at elevated temperatures in air), chemical oxidation (e.g., acid and / or oxidant), electrochemical oxidation, or a combination thereof. As shown in step 230, the third step is to form a sacrificial layer on at least a portion of the surface of the silicon particles. The formation of the sacrificial layer on the surface of the silicon particles is carried out before the silicon particles are introduced into the sol-gel solution of the precursor containing the porous three-dimensional network structure. The properties (e.g., thickness, material type) of the sacrificial layer formed in the third step may affect the dispersion of the silicon particles in the sol-gel solution, which is introduced in the fourth step 240. The sacrificial layer can be formed by polymers, metals, natural and synthetic organics, salts, ceramic compounds or combinations thereof. After the sacrificial layer is formed, as shown in step 240, a sol-gel solution containing a polar solvent and a precursor of the porous network structure is provided. The silicon particles are dispersed in the sol-gel solution homogeneously or unevenly (preferably uniformly). The precursor of the porous network structure can be a precursor of an aerogel. After the sol-gel solution is provided to the silicon particles having the sacrificial layer, the silicon particles having the sacrificial layer are treated in the presence of the sol-gel to obtain precursor beads containing silicon particles dispersed in the precursor beads, as shown in 250. The treatment may include gelling the sol-gel solution to form precursor beads. The method 200 further includes a subcritical or supercritical drying step after treating the silicon particles in the presence of the sol-gel solution. For example, the drying step may result in the formation of an aerogel material, such as an aerogel, a xerogel, a bigel, or a combination thereof. In a final step 260, the precursor beads containing silicon particles dispersed throughout the precursor beads are pyrolyzed to obtain a composite material 100 including pore spaces. After pyrolysis, a three-dimensional carbon network structure is formed from the porous network structure.

[0118] In one embodiment, the amount of sacrificial layer removed depends on the duration of the heat treatment (eg, pyrolysis) applied to the precursor beads including silicon particles.

[0119] In some embodiments, the sacrificial layer is formed of a material selected from the group consisting of polymethyl methacrylate (PMMA), polyvinyl pyrrolidone (PVP), polyvinyl acetate (PVAc), polyvinyl alcohol (PVA), polyacrylonitrile (PAN), polyethylene oxide (PEO), polypropylene oxide (PPO), polyethylene oxide copolymers, polypropylene oxide copolymers, polycarbonate (PC), polyvinyl chloride (PVC), polycaprolactone, polyvinylidene fluoride, polystyrene, or a combination thereof. In some embodiments, the sacrificial layer has a thickness less than or equal to about 100 nm, or a thickness between about 100 nm and about 60 nm, or a thickness of about 60 nm to 0.3 nm. In some embodiments, the sacrificial layer has a thickness in the range of about 20% to about 0.01% of the diameter of the silicon particles.

[0120] In some embodiments, the sacrificial layer has a carbonization yield of less than about 20 wt%. In some embodiments, the chemical decomposition temperature of the sacrificial material layer is in a range of about 130°C to about 850°C.

[0121] In the context of the present disclosure, the term "pyrolysis" or "carbonization" refers to the decomposition or conversion of an organic compound or composition into pure or substantially pure carbon by heating. In an embodiment, the term "carbonization yield" refers to the percentage ratio of the weight of the resulting carbon to the weight of the organic compound or composition from which the carbon is produced.

[0122] In some embodiments, the sacrificial layer is uniform over at least a portion of the surface of the silicon particles. In some embodiments, the sacrificial layer is continuous over at least a portion of the surface of the silicon particles. In some embodiments, at least a portion of the surface of the silicon particles is at least 70% of the surface of the silicon particles, at least 90% of the surface of the silicon particles, or at least 95% of the surface of the silicon particles.

[0123] refer to Figure 3, method 300 depicts the manufacture of a composite material, including six steps (310, 320, 330, 340, 350, 360). In this method 300, a sacrificial layer is formed during or after providing a sol-gel solution. First, as shown in step 310, silicon particles are provided. Generally speaking, the silicon particles should be homogeneous. In other words, the silicon particles are generally provided by the same source and have a known desired particle size, shape, porosity and other substantially similar material properties. After obtaining the silicon particles, the method 300 includes oxidizing the surface of the particles to obtain hydroxyl functional groups on the surface (i.e., step 320). Oxidizing the surface of the silicon particles can result in complete or partial oxidation of the surface Si-H groups. In other words, after the oxidation process, all or a certain percentage of the Si-H groups on the surface of the silicon particles are converted into Si-O or Si-OH groups. The silicon particles can be oxidized in a single or multiple steps. Oxidation can be thermal oxidation (e.g., at elevated temperatures in air), chemical oxidation (e.g., acid and / or oxidant), electrochemical oxidation, or a combination thereof. The third step 330 requires silicon particles with hydroxyl functional groups on their surfaces to covalently react with at least one functional silane group. Attaching silane groups to the surface can pave the way for further modification of the silicon particle surface. In addition, the silane groups present on the silicon particle surface may contribute to the dispersion of silicon particles, which is crucial for subsequent steps. After at least one functional silane group is attached to the silicon particle surface, as shown in step 340, a sol-gel solution containing a polar solvent and a precursor of a porous three-dimensional network structure is provided. Silicon particles are dispersed in the sol-gel solution homogeneously or unevenly (preferably uniformly). The precursor of the porous three-dimensional network structure can be a precursor of an aerogel. As shown in step 350, the fifth step is to form a sacrificial layer on at least a portion of the silicon particle surface. Forming a sacrificial layer on the silicon particle surface is carried out in a sol-gel solution containing a precursor of a porous three-dimensional network structure. The properties (e.g., thickness, material type) of the sacrificial layer formed in step 350 may affect the dispersion of silicon particles in the composite material, which is formed in the last step 360. The sacrificial layer can be formed of a polymer, a metal, a natural and synthetic organic compound, a salt, a ceramic compound, or a combination thereof. After forming the sacrificial layer, the silicon particles having the sacrificial layer are treated in the presence of a sol-gel solution to obtain a composite material, as shown in step 360. The treatment can include gelling the sol-gel solution to form a porous three-dimensional network structure. The method 300 further includes a subcritical or supercritical drying step after treating the silicon particles in the presence of the sol-gel solution. For example, the drying step can result in the formation of an aerogel.

[0124] In the method 300 , step 350 of forming a sacrificial layer includes: i. grafting a polymer initiator onto the surface of silicon particles to react with the monomer; and ii. polymerizing the monomer on the surface of the silicon particles to form a sacrificial layer.

[0125] Figure 4A and Figure 4B An exemplary approach for preparing silicon particles with a sacrificial layer is shown. The process for forming a sacrificial layer mainly includes three steps (410, 420, 430). In the first step 410, a silicon particle 401 having a hydroxyl functional group on its surface is covalently reacted with a functional silane group. In this embodiment, 3-aminopropyltriethoxysilane (APTES) 402 is used as a functional silane group. The hydroxyl group reacts with the silane group in a polar solvent (e.g., ethanol 403), as shown in step 410. The reaction occurs at an elevated temperature (e.g., a temperature above 25°C). After APTES is covalently attached to the surface of the silicon particle to form a silicon particle 404 including a -NH2 group on the surface, a polymer initiator (e.g., azobis(4-cyanovaleric acid) (ACPA) 405) is grafted on the surface of the silicon particle for further reaction with the monomer. The step 420 of grafting the polymer initiator on the surface of the silicon particle occurs in a polar solvent (e.g., ethanol 403). The polar solvent selected should be suitable for dissolving the components, for example, the polymer initiator of the reaction. The third step 430 results in the formation of silicon particles 110 with a sacrificial layer. In step 430, the monomer initiator 406 on the surface of the silicon particles undergoes a polymerization reaction with a monomer (e.g., methyl methacrylate 407). The monomer selected for the polymerization reaction depends on the type of sacrificial layer desired to be located on the surface. As shown in step 430, the polymerization reaction can occur in a polar solvent (e.g., water 404). The polymerization reaction occurs at a temperature above 25°C.

[0126] like Figure 4A and 4B The exemplary method for preparing silicon particles with a sacrificial layer shown in can also be applied to method 300. In method 300, a first step 410 in which silicon particles 401 having hydroxyl functional groups on their surfaces are covalently reacted with functional silane groups (e.g., aminopropyltriethoxysilane (APTES) 402) occurs before providing the sol-gel solution. The second step 420 and the third step 430 occur within the sol-gel solution during or after step 340 of providing the sol-gel solution. In other words, steps 420 and 430 are performed within a sol-gel solution containing a precursor of a three-dimensional network structure.

[0127] In some embodiments, the polymer initiator includes azobis(4-cyanovaleric acid) (ACPA), 2,2'-azobis(2-amidinopropane) hydrochloride (V50), ammonium persulfate, 2,2'-azobis(N,N'-dimethyleneisobutylamidine) dihydrochloride (VA044), and ammonium persulfate / sodium metabisulfite. In some embodiments, the polymer initiator includes azobis(4-cyanovaleric acid) (ACPA).

[0128] The step of covalently reacting the hydroxyl groups on the surface of the silicon particles includes using at least one functional group selected from the following: 3-aminopropyltriethoxysilane (APTES), 3-aminopropyltrimethoxysilane (APTMS), N-(2-aminoethyl)-3-aminopropyltriethoxysilane (AEAPTES), and N-(2-aminoethyl)-3-aminopropyltrimethoxysilane (AEAPTMS), and N-(6-aminohexyl)aminomethyltriethoxysilane (AHAMTES), or a combination thereof.

[0129] In some embodiments, the method of preparing a composite material further includes the step of dispersing silicon particles in a sol-gel solution before the step of forming a sacrificial layer. In some embodiments, the method of preparing a composite material further includes the step of dispersing silicon particles in a sol-gel solution after the step of forming a sacrificial layer. In some embodiments, the method of preparing a composite material further includes the step of dispersing silicon particles in a sol-gel solution before and after the step of forming a sacrificial layer.

[0130] In some embodiments, the method of preparing the composite material further comprises treating the composite material to substantially remove the sacrificial layer, for example, pyrolyzing the precursor beads. In one embodiment, treating the composite material to substantially remove the sacrificial layer comprises heating the composite material to a chemical decomposition temperature of the sacrificial layer. In some embodiments, the chemical decomposition temperature of the sacrificial layer is in the range of about 130° C. to about 850° C. In certain embodiments, treating the composite material to partially or completely remove the sacrificial layer provides void space surrounding the silicon particles.

[0131] In some embodiments, the method of preparing a composite material further comprises a subcritical or supercritical drying step after treating the silicon particles in the presence of the sol-gel solution. In some embodiments, a subcritical or supercritical drying step after treating the silicon particles in the presence of the sol-gel solution. In some embodiments, the subcritical or supercritical drying step results in the formation of an aerogel material, e.g., a xerogel, an aerogel, etc.

[0132] Oxidation of the surface of multiple silicon particles may include an acid treatment step. In some embodiments, the acid treatment step includes the use of thiochromic acid or H2O2 (hydrogen peroxide). In some embodiments, the acid treatment step includes the step of ultrasonically treating multiple silicon particles for a period of time (e.g., at least 5 minutes, at least 10 minutes, at least 20 minutes, at least 30 minutes, or at least 60 minutes). Oxidation of the surface of multiple silicon particles may include the step of pyrolysis at a temperature of about 300, about 400, or about 500 to about 600, about 650, about 700, about 800, about 850, or about 900°C. In some embodiments, the temperature is about 650°C. As used herein, the term "pyrolysis" refers to an organic compound or composition that is decomposed or converted into pure or substantially pure carbon by heating. Oxidation of the surface of multiple silicon particles may result in a reduction in the number of Si-H bonds on the surface of the silicon particles.

[0133] In some embodiments, the method for preparing a composite material disclosed herein further includes (before or after the pyrolysis step) a subcritical or supercritical solvent removal (e.g., drying) step after treating a plurality of silicon particles in the presence of a sol-gel solution. The solvent removal method includes, but is not limited to, supercritical drying (or using a supercritical fluid to dry so that the low surface tension of the supercritical fluid is exchanged with the instantaneous solvent in the gel), exchanging the solvent with the supercritical fluid, exchanging the solvent with the fluid subsequently converted to a supercritical state, subcritical or near-critical fluid drying, and sublimating the frozen solvent in a freeze-drying process. See, for example, PCT Patent Application Publication No. WO2016127084A1.

[0134] Composite materials can be in a variety of physical forms. In some embodiments, composite materials can take the form of a monolith. As used herein, the term "monolithic" refers to a material in which the low-density skeleton included in the composite material is mostly (by weight) in the form of a uniform, continuous, self-supporting object. With reference to aerogel materials, monolithic aerogel materials include aerogel materials that are initially formed to have a well-defined shape, but which can subsequently be broken, ruptured or fragmented into non-self-repeating objects. For example, irregular large blocks can be considered monolithic. Monolithic aerogels can take the form of independent structures, or take the form of materials reinforced with fibers or interpenetrating foams.

[0135] In other embodiments, the composite material can be in particulate form, for example as beads or particles obtained by breaking up a monolithic material. As used herein, the term "bead" is meant to include discrete small units or fragments that generally have a spherical shape. In some embodiments, the composite material beads are substantially spherical.

[0136] The composite material in particle form can have various particle diameters. In the case of spherical particles (e.g., beads), the particle diameter is the diameter of the particle. In the case of irregular particles, the term particle diameter refers to the maximum dimension (e.g., length, width or height). The particle diameter can vary according to the physical form, preparation method and any subsequent physical steps performed. In some embodiments, the composite material in particle form can have a particle diameter of about 1 micron to about 1 millimeter. For example, the particle size of the composite material in particle form can be about 1 micron, about 2 microns, about 3 microns, about 4 microns, about 5 microns, about 6 microns, about 7 microns, about 8 microns, about 9 microns, about 10 microns, about 15 microns, about 20 microns, about 25 microns, about 30 microns, about 35 microns, about 40 microns, about 45 microns, about 50 microns, about 60 microns, about 70 microns, about 80 microns, about 90 microns, about 100 microns, about 200 microns, about 300 microns, about 400 microns, about 500 microns, about 600 microns, about 700 microns, about 800 microns, about 90 microns, about 100 microns, about 200 microns, about 300 microns, about 400 microns, about 500 microns, about 600 microns, about 700 microns, about 800 microns, about 900 microns, about 1 mm, or in a range between any two of these values.

[0137] In some embodiments, the composite material has a particle size D90 value less than or equal to 40 microns. In some embodiments, the composite material has a particle size D10 value of at least 1 micron. In some embodiments, the composite material has a particle size D50 in the range of about 5 microns to about 20 microns.

[0138] The density of the composite material can vary. In some embodiments, the composite material has a density of about 0.15 g / cm 3 To about 1.2g / cm 3 The tap density is within the range.

[0139] The surface area of ​​the composite material can vary. For example, the surface area can be up to about 100 m 2 / g, or can be greater than 100m 2 / g. In some embodiments, the composite material has a 2 / g to about 400m 2 The surface area may be in the range of about 1, about 10, or about 50 to about 100, about 200, about 300, or about 400 m / g. 2 / g.

[0140] In some embodiments, the composite material comprises between about 20% and about 85% silicon by weight, such as about 20%, about 25%, about 30%, about 35%, about 40%, about 45%, or about 50 to about 55%, about 60%, about 65%, about 70%, about 75%, about 80%, or about 85% silicon, based on the total weight of the composite material.

[0141] Composite materials can be in a variety of physical forms. In some embodiments, composite materials can take the form of a monolith. As used herein, the term "monolithic" refers to a material in which the low-density skeleton included in the composite material is mostly (by weight) in the form of a uniform, continuous, self-supporting object. With reference to aerogel materials, monolithic aerogel materials include aerogel materials that are initially formed to have a well-defined shape, but which can subsequently be broken, ruptured or fragmented into non-self-repeating objects. For example, irregular large blocks can be considered monolithic. Monolithic aerogels can take the form of independent structures, or take the form of materials reinforced with fibers or interpenetrating foams.

[0142] In other embodiments, the composite material may be in particulate form, for example as beads or particles obtained by breaking up a monolithic material. As used herein, the term "bead" is meant to include discrete small units or fragments that generally have a spherical shape. In some embodiments, the carbon-silicon composite beads are substantially spherical.

[0143] The capacity of the composite material is variable. In some embodiments, the composite material has a specific capacity of at least about 400 mAh / g. In some embodiments, the composite material has a specific capacity of about 400, about 500, about 600, about 700, about 800, about 900, about 1000, or about 1100 mAh / g. In some embodiments, the composite material has a specific capacity of 1200 mAh / g or more, 1400 mAh / g or more, 1600 mAh / g or more, 1800 mAh / g or more, 2000 mAh / g or more, 2400 mAh / g or more, 2800 mAh / g or more, 3200 mAh / g or more, or in any range between two of these values.

[0144] The conductivity of the anode material can vary. In the context of the present disclosure, the term "conductivity" refers to a material's ability to conduct an electric current or other measurement of the ability to allow electrons to flow through or within it. Conductivity is specifically measured as conductance / susceptance / admittance per unit size of the material. It is typically recorded as S / m (Siemens / meter) or S / cm (Siemens / centimeter). The conductivity or resistivity of a material can be determined by methods known in the art, such as, but not limited to: in-line four-point resistivity (using the dual configuration test method of ASTM F84-99). In the context of the present disclosure, unless otherwise specified, measurements of conductivity are obtained according to ASTM F84 (i.e., resistivity (R) measurements are obtained by measuring voltage (V) divided by current (I)). In certain embodiments, the anode materials of the present disclosure have a conductivity of about 10 S / cm or greater, 20 S / cm or greater, 30 S / cm or greater, 40 S / cm or greater, 50 S / cm or greater, 60 S / cm or greater, 70 S / cm or greater, 80 S / cm or greater, or in a range between any two of these values.

[0145] Three-dimensional carbon network structure

[0146] The three-dimensional carbon network structure of the present disclosure includes a carbon-based network structure selected from carbon aerogel, carbon xerogel, carbon bigel, carbon aerogel-xerogel hybrid material, carbon aerogel-bigel hybrid material, carbon aerogel-bigel-xerogel hybrid material, or a combination thereof.

[0147] The aerogels used in the present disclosure can be carbonized to obtain a three-dimensional carbon network structure, for example, the carbon-based aerogels of the present technology. Carbonization can be performed by pyrolysis at elevated temperatures in an inert atmosphere. The carbonized form of the aerogels used in the present disclosure can have a nitrogen content between 0 and 20%. Typical pyrolysis temperature ranges are between 500° C. and 2000° C. The temperature can be increased to reduce the nitrogen content in the resulting carbon aerogel. Pyrolysis is typically performed in an inert atmosphere (i.e., nitrogen, helium, neon, argon, or a combination thereof).

[0148] In some embodiments, the three-dimensional carbon network structure includes a carbon aerogel derived from polyimide. In some embodiments, the dried polyimide aerogel is subjected to a treatment temperature of 400°C or more, 600°C or more, 800°C or more, 1000°C or more, 1200°C or more, 1400°C or more, 1600°C or more, 1800°C or more, 2000°C or more, 2200°C or more, 2400°C or more, 2600°C or more, 2800°C or more, or in a range between any two of these values ​​to perform carbonization of the polyimide aerogel to obtain a carbon aerogel derived from polyimide.

[0149] The present disclosure relates to the formation of three-dimensional carbon network structures (such as carbon aerogels) and their use as electrode materials in energy storage devices, such as as the main anode material in LIBs. For example, the pores of the porous network structure are designed, organized and structured to accommodate particles of silicon or other metalloids or metals, and the expansion of such particles upon lithiation in LIBs. Alternatively, the pores of the porous network structure can be filled with sulfides, hydrides, any suitable polymers, or other additives, wherein contacting the additives with the conductive material is beneficial for providing a more efficient electrode.

[0150] To further expand the exemplary applications within LIBs, when carbon-based aerogel materials are used as the primary electrode material, such as the anode material in the embodiments of the present disclosure, the carbon aerogel porous core has a narrow pore size distribution and provides high electrical conductivity, high mechanical strength, morphology, and sufficient pore volume (at final density) to accommodate a high weight percentage of silicon particles and their expansion.

[0151] In some embodiments, the surface of the three-dimensional carbon network structure may be modified via chemical, physical, or mechanical methods to enhance performance using electrochemically active species contained within the pores of the porous network structure.

[0152] In addition, it is contemplated herein that the three-dimensional carbon network structure (specifically, carbon aerogel) may take the form of a monolithic structure. When used as a monolithic material, the carbon aerogel does not require any binder; in other words, the anode may be binder-free. As used herein, the term "monolithic" refers to an aerogel material in which the main portion (by weight) of the aerogel included in the aerogel material or composition is in the form of a uniform, continuous, interconnected aerogel nanostructure. Monolithic carbon aerogel materials include aerogel materials that are initially formed as gels or aerogel nanostructures with consistent interconnections, but which may subsequently be broken, ruptured or fragmented into inconsistent aerogel nanostructures. The monolithic aerogel may take the form of an independent structure, or take the form of a (fiber or foam) reinforced material. In contrast, using silicon lithiation as an example, the silicon incorporated into the monolithic aerogel can be more efficiently utilized relative to theoretical capacity than the same amount of silicon incorporated into the slurry using conventional processes.

[0153] Monolithic aerogel materials, e.g., monolithic carbon aerogels are differentiated from granular aerogel materials. The term "granular aerogel material" refers to an aerogel material in which a majority (by weight) of the aerogel included in the aerogel material is in the form of granules, particles, microparticles, beads or powders, which can be combined together (i.e., via an adhesive, such as a polymer adhesive) or pressed together, but which lacks the interconnected aerogel nanostructures between individual particles. In general, aerogels in this form will be referred to as having a powder or granular form (as opposed to a monolithic form). It should be noted that although individual particles of the powder have a single structure, individual particles are not considered monolithic herein. Aerogel powders are integrated into electrochemical cells, typically by preparing a paste or slurry from the powder, pouring it onto a substrate and drying it, and optionally including calendering.

[0154] Granular aerogel materials (e.g., carbon aerogel beads) provide certain advantages. For example, in LIB anodes and anode manufacturing processes, granular materials can be used as a direct substitute for other materials such as graphite. Due to the shorter diffusion paths within the granular materials, granular materials can also provide improved lithium ion diffusion rates. Granular materials can also enable electrodes to have enhanced packing density, for example, by adjusting the particle size and packaging configuration. Granular materials can also provide improved silicon proximity due to inter-particle and intra-particle porosity.

[0155] Carbon aerogel can be formed by inorganic materials, organic materials or mixtures thereof. Carbon aerogel can be formed by inorganic aerogel, organic aerogel or mixtures thereof. Inorganic aerogel, organic aerogel or mixtures thereof can be carbonized to obtain a three-dimensional carbon network structure, for example, a porous carbon aerogel of the present disclosure. Aerogel can be formed by inorganic materials, organic materials or mixtures thereof. When formed by organic materials such as phenols, resorcinol-formaldehyde (RF), phloroglucinol-furfural (PF), polyacrylonitrile (PAN), polyimide (PI), polyurethane (PU), polyurea (PUA), polyamine (PA), polybutadiene, polydicyclopentadiene and precursors or polymer derivatives thereof, the organic aerogel can be carbonized (for example, by pyrolysis) to form a carbon aerogel, which can have different or overlapping properties (for example, pore volume, pore size distribution, morphology, etc.) depending on the precursor material and method used.

[0156] Inorganic Aerogel

[0157] Inorganic aerogels can generally be formed from metal oxide or metal alkoxide materials. The metal oxide or metal alkoxide material can be based on the oxide or alkoxide of any metal that can form an oxide. Such metals include, but are not limited to, silicon, aluminum, titanium, zirconium, hafnium, yttrium, vanadium, cerium, etc. Inorganic silica aerogels are traditionally prepared via hydrolysis and condensation of silica-based alkoxides (such as tetraethoxysilane) or via gelation of silicic acid or water glass. Other relevant inorganic precursor materials for the synthesis of silica-based aerogels include, but are not limited to, metal silicates such as sodium silicate or potassium silicate, alkoxysilanes, partially hydrolyzed alkoxysilanes, tetraethoxysilane (TEOS), partially hydrolyzed TEOS, condensation polymers of TEOS, tetramethoxysilane (TMOS), partially hydrolyzed TMOS, condensation polymers of TMOS, tetra-n-propoxysilane, partially hydrolyzed tetra-n-propoxysilane and / or condensation polymers of tetra-n-propoxysilane, polyethyl silicate, partially hydrolyzed polyethyl silicate, monomeric alkylalkoxysilanes, bis-trialkoxyalkyl or aryl silanes, polyhedral silsesquioxanes, or combinations thereof.

[0158] In certain embodiments of the present disclosure, pre-hydrolyzed TEOS such as H-5 (SBH5, Evonik Corp) hydrolyzed with a water / silica ratio of about 1.9-2 can be used as commercially available; or it can be further hydrolyzed before incorporation into the gelation process. Partially hydrolyzed TEOS or TMOS such as polyethyl silicate ( 40) or polymethyl silicate may also be used as commercially available, or may be further hydrolyzed prior to incorporation into the gelling process.

[0159] Inorganic aerogels may also include gel precursors containing at least one hydrophobic group, such as alkyl metal alkoxides, cycloalkyl metal alkoxides, and aryl metal alkoxides, which may impart or improve certain properties in the gel, such as stability and hydrophobicity. Inorganic silica aerogels may specifically include hydrophobic precursors such as alkyl silanes or aryl silanes. Hydrophobic gel precursors may be used as the primary precursor material to form the framework of the gel material. However, in the formation of amalgam aerogels, hydrophobic gel precursors are more often used as co-precursors in combination with simple metal alkoxides. Hydrophobic inorganic precursor materials for the synthesis of silica-based aerogels include, but are not limited to, trimethylmethoxysilane (TMS), dimethyldimethoxysilane (DMS), methyltrimethoxysilane (MTMS), trimethylethoxysilane, dimethyldiethoxysilane (DMDS), methyltriethoxysilane (MTES), ethyltriethoxysilane (ETES), diethyldiethoxysilane, dimethyldiethoxysilane (DMDES), ethyltriethoxysilane, propyltrimethoxysilane, propyltriethoxysilane, phenyltrimethoxysilane, phenyltriethoxysilane (PhTES), hexamethyldisilazane, and hexaethyldisilazane, etc. Derivatives of any of the aforementioned precursors may be used, and in particular certain polymers of other chemical groups may be added or cross-linked to one or more of the aforementioned precursors.

[0160] Organic aerogel

[0161] Organic aerogels are generally formed from carbon-based polymeric precursors. Such polymeric materials include, but are not limited to, resorcinol formaldehyde (RF), polyimide, polyacrylate, polymethyl methacrylate, acrylate oligomers, polyoxyalkylene, polyurethane, polyphenol, polybutadiene, trialkoxysilyl-terminated polydimethylsiloxane, polystyrene, polyacrylonitrile, polyfurfural, melamine formaldehyde, cresol formaldehyde, phenol-furfural, polyether, polyol, polyisocyanate, polyhydroxybenzene, polyvinyl alcohol dialdehyde, polycyanurate, polyacrylamide, various epoxy resins, agar, agarose, chitosan, and combinations thereof. As an example, organic RF aerogels are typically prepared from sol-gel polymerization of resorcinol or melamine with formaldehyde under alkaline conditions.

[0162] In certain embodiments, the aerogel of the present disclosure includes polyamic acid, polyimide, a combination thereof, or a carbon aerogel obtained (i.e., derived) from polyamic acid or polyimide by carbonization. In a specific embodiment, the aerogel includes polyamic acid, polyimide, or a combination thereof, or is obtained by pyrolysis of polyamic acid, polyimide, or a combination thereof. In some embodiments, polyamic acid or polyimide is prepared in an aqueous solution (i.e., via an aqueous sol-gel process). The expression herein about an aqueous solution or an aqueous sol-gel process means that the solution or aqueous sol-gel process is substantially free of any organic solvent. As used herein, in the context of an organic solvent, the term "substantially free of" means that an organic solvent is not intentionally added and there is no organic solvent exceeding a trace amount. For example, in certain embodiments, the aqueous solution may be characterized in that it has less than 1% by volume of an organic solvent, or less than 0.1%, or less than 0.01%, or even 0% by volume of an organic solvent.

[0163] The use of an aqueous sol-gel process is advantageous in providing rapid gelation, making the process easily configurable as a continuous process, e.g., for preparing polyimide beads. Aqueous sol-gel processes for preparing polyamic acid and polyimide gel materials are economically preferred over conventional methods for such materials (e.g., expensive organic solvents are avoided and disposal costs are minimized) and are "green" (i.e., beneficial from an environmental perspective because potentially toxic organic solvents are avoided and the generation of toxic byproducts is minimized or eliminated), and in potentially reducing the total number of operations that must be performed to provide carbon or polyamic acid / polyimide gel materials. As disclosed in International Patent Application Publication No. WO2022 / 125835 and International Patent Application PCT / US2023 / 016821, each of which is incorporated herein by reference in its entirety, polyamic acid and polyimide gels in monolithic or bead form can be prepared in water, which can be converted into aerogels having a nanostructure and having properties similar to those of aerogels prepared by traditional organic solvent-based processes, and the aerogels are optionally pyrolyzed to form corresponding carbon aerogels.

[0164] In some embodiments, the aerogel of the present disclosure is a polyamic acid aerogel in the form of a monolith or beads, wherein the polyamic acid is prepared by acidifying a polyamic acid aqueous solution. In some embodiments, the polyamic acid is dissolved in water in the presence of a base (e.g., an alkali metal hydroxide or a non-nucleophilic amine base). In other embodiments, polyamic acid is prepared in situ under aqueous conditions to directly form a polyamic acid salt solution. In some embodiments, polyamic acid is any commercially available polyamic acid. In other embodiments, polyamic acid ("preformed") has been previously formed and separated, for example, by reacting diamines with tetracarboxylic dianhydride in an organic solvent according to a conventional synthesis method. In some embodiments, the aqueous solution of polyamic acid salt is prepared by the following in situ, for example, reacting diamines with tetracarboxylic dianhydride in the presence of a non-nucleophilic amine, thereby providing an aqueous solution of polyamic acid ammonium salt. Suitable methods for preparing polyamic acid aerogels under such aqueous conditions are disclosed in WO2022 / 125835 and PCT / US2023 / 016821, previously incorporated by reference.

[0165] In some embodiments, the aerogel of the present disclosure is a polyimide aerogel in the form of a monolith or beads, wherein the polyimide is prepared by thermal or chemical imidization of polyamic acid in aqueous solution. Suitable methods for forming monolithic materials or beads under such aqueous conditions (e.g., using droplet or emulsion-based processes) are disclosed in WO2022 / 125835 and PCT / US2023 / 016821, previously incorporated by reference.

[0166] Organic / inorganic hybrid aerogel

[0167] Organic / inorganic hybrid aerogels are primarily composed of organically modified silica ("ormosil") aerogels. These ormosil materials include an organic component covalently bonded to a silica network. Ormosil is typically formed by hydrolysis and condensation of an organically modified silane R--Si(OX)3 with a traditional alkoxide precursor Y(OX)4. In these formulas, X may represent, for example, CH3, C2H5, C3H7, C4H9; Y may represent, for example, Si, Ti, Zr, or Al; and R may be any organic fragment such as methyl, ethyl, propyl, butyl, isopropyl, methacrylate, acrylate, vinyl, epoxide, etc. The organic component in the ormosil aerogel may also be dispersed throughout the silica network or chemically bonded to the silica network.

[0168] In certain embodiments, the aerogels of the present disclosure are inorganic silica aerogels formed primarily from prepolymerized silica precursors (preferably as oligomers), or hydrolyzed silicates formed from silicon alkoxides in alcohol solvents. In certain embodiments, such prepolymerized silica precursors or hydrolyzed silicates may be formed in situ from other precursors or silicates such as alkoxysilanes or water glass. However, the present disclosure as a whole may be practiced with any other aerogel composition known to those skilled in the art and is not limited to any one precursor material or amalgam mixture of precursor materials.

[0169] Silicon particles

[0170] Silicon is generally present in composite materials as silicon particles. In the context of the present disclosure, the term "silicon particles" refers to silicon or silicon-based materials with a certain range of particle diameters. The particle diameter of silicon in the composite material can be variable. The silicon particles of the present disclosure can be nanoparticles, for example, particles with two or three dimensions in the range of about 1nm to about 150nm. The silicon particles of the present disclosure can be fine particles, for example, micron-sized particles with a maximum dimension (for example, diameter for substantially spherical particles) in the range of about 150nm to about 10 microns or more. For example, the silicon particles of the present disclosure can have a maximum dimension (for example, diameter for substantially spherical particles) in the range of about 10nm, 50nm, 60nm, 80nm, 100nm, 120nm, 130nm, 140nm, 150nm, 180nm, 200nm, 500nm, 1 micron, 1.5 microns, 2 microns, 3 microns, 5 microns, 10 microns, 20 microns, 40 microns, 50 microns, 100 microns, or any two of these values.

[0171] In some embodiments, the silicon particles can be monodisperse or substantially monodisperse. In other embodiments, the silicon particles can have a particle size distribution. In the context of the present disclosure, the dimension of the silicon particles is provided based on the median (i.e., D50) of the particle size distribution. In some embodiments, the silicon in the composite material has an average particle size of about 1 μm or less.

[0172] The silicon particles of the present disclosure may be silicon wires, crystalline silicon, amorphous silicon, silicon alloys, silicon oxides (SiOx), and any combination thereof. For the embodiments disclosed herein, the particles (e.g., particles of electroactive materials, such as silicon particles) may have various shapes. In some embodiments, the silicon particles disclosed herein may be substantially spherical. In other embodiments, the particles of electroactive materials may be substantially planar, cubic, ovoid, elliptical, disc-shaped, or annular.

[0173] In one embodiment, before forming the sacrificial layer, the surface of the silicon particles (e.g., silicon nanoparticles) may be modified with functional groups that can assist in dispersing the silicon particles in the precursor beads. In another embodiment, the formation of the sacrificial layer may further assist in dispersing the silicon particles in the precursor beads. In one embodiment, the precursor beads may be sol-gel, aerogel, xerogel, foam structure, etc. In some embodiments, the precursor beads are carbonized according to the various embodiments disclosed herein to obtain the three-dimensional carbon network structure of the present disclosure.

[0174] For example, functional groups can be grafted onto the silicon particle surface by covalent bonds. Before functionalization, the surface of the silicon particle includes silane groups, such as silicon hydride and / or silicon oxide groups. In some embodiments, at least a portion of those silane and silicon oxide groups can exist in the form of a combination of bonded functional groups after the silicon particle surface is functionalized, for example, the silicon particle surface can include silane groups and covalently attached functional groups, silicon oxide groups and covalently attached functional groups or silane and silicon oxide groups and covalently attached functional groups. The presence of functional groups on the silicon particle surface can be detected by various techniques, for example, by infrared spectroscopy.

[0175] The surface of the silicon particles can be functionalized with hydrophilic groups to assist in improving dispersion in the porous network structure. Without being bound by theory, functionalization with hydroxide groups establishes increased covalent bonding between the surface groups on the silicon particles and the porous network structure. Therefore, the functionalized silicon particles can be uniformly dispersed in the porous network structure. For example, hydrophilic hydroxide groups can be grafted to the particle surface by unsaturated diols to increase the hydrophilicity of the silicon particle surface. Increasing the hydrophilicity of the silicon particles allows the particles to become and remain more uniformly dispersed in the network structure, and remain uniformly dispersed in the network structure in any additional treatment (e.g., pyrolysis). In one embodiment, functionalization via diols can improve the dispersion of silicon particles in polyimide sol-gels and / or aerogels or carbon aerogels. Any suitable ethylene glycol can be used, including but not limited to ethylene glycol methyl ether methacrylate, polyethylene glycol methyl ether methacrylate, etc.

[0176] In some embodiments, individual silicon particles are not uniformly dispersed throughout the three-dimensional carbon network structure. In some embodiments, individual silicon particles are homogeneously dispersed throughout the three-dimensional carbon network structure. The expression "homogeneously dispersed" means that the Si particles are dispersed throughout the three-dimensional carbon network structure without large variations in local concentration across the accessible network structure.

[0177] In some embodiments, about 30 wt% to 70 wt%, about 20 wt% to about 50 wt% of the dispersed individual silicon particles within the plurality of silicon particles are in an aggregated state. In some embodiments, less than about 30 wt%, less than about 20 wt%, less than about 10 wt% of the dispersed individual silicon particles within the plurality of silicon particles are in an aggregated state. In some embodiments, homogeneously dispersed Si particles may refer to a distribution of a plurality of Si particles throughout a porous polymer network structure, wherein less than about 30 wt%, less than about 20 wt%, less than about 10 wt% of the dispersed individual silicon particles within the plurality of silicon particles are in an aggregated state.

[0178] Sacrificial layer

[0179] In an exemplary embodiment, the composite material may include a sacrificial material or multiple layers of sacrificial material. In the context of the present disclosure, the term "sacrificial material" or "sacrificial layer" refers to a material or layer that is intended to be sacrificed or at least partially removed in response to the mechanical, thermal, chemical and / or electromagnetic conditions experienced by the layer. For example, the sacrificial material or sacrificial layer may decompose when exposed to high temperature or high and / or continuous stress. In some embodiments, the sacrificial material layer may be disposed on an outer surface, for example, on the outer surface of the core portion of the multilayer material; or disposed on an outer surface, for example, on the outer surface of the multilayer material.

[0180] The sacrificial layer can be selected from the group consisting of: silicones, polyolefins, polyurethanes, phenolic resins, melamines, cellulose acetates, and polystyrenes. In some cases, the material layer is in the form of a foam. In some embodiments, the sacrificial material can be worn away due to exposure to mechanical (such as cyclic) loads. In some embodiments, the sacrificial layer decomposes after exposure to a single mechanical, chemical, and / or thermal event.

[0181] In some embodiments, the chemical decomposition onset temperature of the sacrificial material layer is in the range of about 100°C to about 700°C, about 100°C to about 500°C, about 200°C to about 400°C.

[0182] The polymer used in the sacrificial layer can be selected from a variety of thermoplastic resins, blends of thermoplastic resins, or thermosetting resins. Examples of thermoplastic resins that can be used include polyacetals, polyacrylics, styrene acrylonitrile, polyolefins, acrylonitrile-butadiene-styrene, polycarbonates, polystyrenes, polyethylene terephthalate, polybutylene terephthalate, polyamides (such as but not limited to nylon 6, nylon 6,6, nylon 6,10, nylon 6,12, nylon 11 or nylon 12), polyamide-imides, polyacrylates, polyurethanes, ethylene-propylene rubber (EPR), polyaryl sulfones, polyether sulfones, polyphenylene sulfide, polyvinyl chloride, polysulfones, polyetherimides, polytetrafluoroethylene, ethylene propylene fluoride, polychlorotrifluoroethylene, polyvinylidene fluoride, polyvinyl fluoride, polyether ketones, polyether ether ketones, polyether ketone ketones, or the like, or a combination comprising at least one of the foregoing thermoplastic resins.

[0183] Examples of blends of thermoplastic resins that can be used in the sacrificial layer include acrylonitrile-butadiene-styrene / nylon, polycarbonate / acrylonitrile-butadiene-styrene, acrylonitrile-butadiene styrene / polyvinyl chloride, polyphenylene oxide / polystyrene, polyphenylene oxide / nylon, polysulfone / acrylonitrile-butadiene-styrene, polycarbonate / thermoplastic urethane, polycarbonate / polyethylene terephthalate, polycarbonate / polybutylene terephthalate, thermoplastic elastomer alloy, polyethylene terephthalate / polybutylene terephthalate, styrene-maleic anhydride / acrylonitrile-butadiene-styrene, polyetheretherketone / polyethersulfone, styrene-butadiene rubber, polyethylene / nylon, polyethylene / polyacetal, ethylene-propylene rubber (EPR), etc., or a combination comprising at least one of the foregoing blends.

[0184] Examples of polymer thermosetting resins that can be used in the sacrificial layer include polyurethanes, epoxy resins, phenolic resins, polyesters, polyamides, silicones, etc., or a combination comprising at least one of the foregoing thermosetting resins. Blends of thermosetting resins and blends of thermoplastic resins with thermosetting resins can be used.

[0185] Lithium-ion battery

[0186] A basic embodiment of a lithium-ion battery includes: a cathode; an anode in electrical communication with the cathode; an electrolyte disposed between the anode and the cathode; and a separator also disposed between the anode and the cathode.

[0187] Electrolytes are ion-conducting materials and may include solvents, ionic liquids, metal salts, ions such as metal ions or inorganic ions, polymers, ceramics, and other components. Electrolytes may be organic or inorganic solids or liquids, such as solvents containing dissolved salts (e.g., non-aqueous solvents). Non-aqueous electrolytes include organic solvents such as cyclic carbonates, linear carbonates, fluorinated carbonates, benzonitrile, acetonitrile, tetrahydrofuran, 2-methyltetrahydrofuran, γ-butyrolactone, dioxolane, 4-methyldioxolane, N,N-dimethylformamide, N,N-dimethylacetamide, dimethyl sulfoxide, dioxane, 1,2-dimethoxyethane, sulfolane, dichloroethane, chlorobenzene, nitrobenzene, diethylene glycol, dimethyl ether, and mixtures thereof. Examples of salts that may be included in the electrolyte include lithium salts such as LiPF6, LiBF4, LiSbF6, LiAsF6, LiClO4, LiCF3SO3, Li(CF3SO2)2N, Li(FSO2)2N, LiC4F9SO3, LiAlO2, LiAlCl4, LiN(C x F 2x+1 SO2)(C y F 2y-1 SO2) (wherein x and y are natural numbers), LiCl, LiI, and mixtures thereof. In some embodiments, the liquid molecules include an electrolyte solvent (electrolyte). The electrolyte solvent of the present disclosure may be selected from any one of the above-mentioned suitable electrolytes. In particular, the electrolyte is selected from ethylene carbonate (EC), diethyl carbonate (DEC), dimethyl carbonate (DMC), fluoroethylene carbonate (FEC), fluorinated ether (F-EPE), 1,3-dioxolane (DOL), dimethoxyethane (DME), or a combination thereof.

[0188] The separator is typically a thin, porous or semi-permeable separator with high ion permeability. The separator may be composed of a copolymer, such as an olefin-based polymer (e.g., polyethylene, polypropylene and / or polyvinylidene fluoride). If a solid polymer electrolyte is used as the electrolyte, the solid polymer electrolyte may also be used as a separator.

[0189] The anode is composed of an active anode material that participates in the electrochemical reaction during battery operation. Exemplary anode active materials include elemental materials, such as lithium; alloys, including alloys of Si and Sn, or other lithium compounds; and intercalation host materials, such as graphite. By way of example only, the anode active material may include metals and / or metalloids that can form alloys with lithium, their alloys, or their oxides. Metals and metalloids that can form alloys with lithium include Si, Sn, Al, Ge, Pb, Bi, and Sb. For example, the oxide of the metal / metalloid that can form an alloy with lithium can be lithium titanate, vanadium oxide, lithium vanadium oxide, SnO2, or SiO x (0 <x<2)。

[0190] The cathode is composed of an active cathode material that participates in the electrochemical reaction during battery operation. The active cathode material can be a lithium composite oxide and includes layered materials such as LiCoO2; olivine materials such as LiFePO4; spinel materials such as LiMn2O4; and similar materials. Spinel-type materials include those having a structure similar to natural spinel LiMn2O4, which includes a small amount of nickel cations in addition to lithium cations, and which optionally also includes anions other than manganate. By way of example, such materials include those having the formula LiNi (0.5-x) Mn 1.5 M x Those of O4, wherein 0≤x≤0.2, and M is Mg, Zn, Co, Cu, Fe, Ti, Zr, Ru or Cr.

[0191] In the context of the present disclosure, the term "cycle life" refers to the number of complete charge and discharge cycles that an anode or battery (e.g., LIB) can support before its capacity drops to less than about 80% of its initial nominal capacity. The cycle life is affected by a variety of factors, such as the mechanical strength of the base material (e.g., carbon aerogel) and the maintenance of the interconnectivity of the aerogel. Notably, these factors actually remain relatively unchanged over time, which is a surprising aspect of certain embodiments of the present disclosure. The cycle life can be determined by methods known in the art, such as, but not limited to, cycle testing, in which a battery cell is subjected to repeated charge and discharge cycles at a predetermined current rate and operating voltage. In the context of the present disclosure, unless otherwise specified, the cycle life measurement is obtained according to this method. The energy storage device (such as a battery or its electrode) may have a cycle life of about 25 cycles or more, 50 cycles or more, 75 cycles or more, 100 cycles or more, 200 cycles or more, 300 cycles or more, 500 cycles or more, 1000 cycles or more, or a range between any two of these values.

[0192] The present disclosure includes an electrical energy storage device having at least one anode comprising a composite material of the present technology as described herein, at least one cathode, and an electrolyte having lithium ions. The electrical energy storage device may have a first cycle efficiency (i.e., the coulombic efficiency of the battery cell for the first charge and discharge) of at least 10%, 20%, 30%, 40%, 50%, 60%, 70%, any intermediate value (e.g., 65%), or a range between any two of these values ​​(e.g., a range of about 30% to about 50%). As previously described herein, the reversible capacity may be at least 150 mAh / g. The at least one cathode may be selected from the group consisting of: conversion cathodes, such as lithium sulfide and lithium air; and intercalation cathodes, such as phosphates and transition metal oxides.

[0193] According to different embodiments, the composite material of the present disclosure can be applied to the positive electrode and negative electrode of the electrochemical energy storage device, or applied to the electrode (positive electrode or negative electrode) alone. In various embodiments, the cathode, anode, or solid electrolyte material is coated with the composite material of the present technology.

[0194] Example

[0195] The following examples are included to demonstrate preferred embodiments of the technology. However, those of skill in the art should, based on the present disclosure, appreciate that many changes can be made in the specific embodiments disclosed and still obtain a like or similar result without departing from the spirit and scope of the technology.

[0196] 1.1 Oxidation of silicon particles

[0197] Commercially available silicon particles may or may not include oxidized (partially or completely) silicon particles. Thus, the oxidation step provided herein is optional, depending on the surface functionality of the silicon particles provided by the supplier.

[0198] Silicon particles (available from Evonik; 10-100 g of 100-3000 nm) are heated in a temperature range of 400-800° C. under humidity for 1-5 hours or dispersed in 10-1000 mL of 0.1-5 M thiochromic acid or 10-1000 mL of 1-10 M H2O2 (hydrogen peroxide). For Si dispersion, it is heated to 50-120° C. under constant stirring for 1-10 hours in order to obtain hydroxyl functional groups (or silanol groups) on the surface of the silicon particles. In theory, other oxidants can also be used for this purpose. After stirring the solution for 1-10 hours, the solution is cooled to room temperature and centrifuged to obtain oxidized silicon particles. The obtained silicon particles are washed 3-5 times with 100-3000 mL volumes of water to remove any residual acid and dried at ambient conditions for 3-10 hours. The oxidized silicon particles are characterized by IR spectroscopy ( Figure 5 ) confirmed the surface oxidation, as evidenced by the presence of -1 The intensity of the band at 1052 cm -1 Oxidation by heating the dry powder can also be confirmed by an increase in mass after treatment.

[0199] 1.2 Synthesis of Si particles coated with sacrificial layer

[0200] Oxidized silicon particles (10 grams) were dispersed in 50 mL of ethanol. The dispersion was ultrasonically treated for 30 minutes to prevent aggregation of silicon particles. Then, 1 gram of AEAPTMS was added to the dispersion and stirred on a hot plate for 240 minutes, wherein the dispersion temperature was controlled at 70 ° C. After the dispersion was cooled to room temperature, 0.5 grams of initiator 4,4'-azobis (4-cyanovaleric acid) was added to the dispersion, which was stirred for another 240 minutes. The dispersion was then left to stand overnight to allow the silicon particles to precipitate, after which the top clear solvent was poured out, and the remaining silicon slurry was dispersed in 67 mL of water by stirring at 600 RPM for 5 minutes. The monomer methyl methacrylate (25.3 grams) was added to the dispersion and stirred at 500 RPM on a hot plate, wherein the dispersion temperature was controlled at 80 ° C for 60 minutes. The stirring speed was then reduced to 300 RPM for 60 minutes, after which it was raised to 500 RPM. The dispersion was stirred for another 180 minutes, after which 2.6 grams of polymer modifier (hydroxyethyl) methacrylate was added to the dispersion. The dispersion temperature was changed to 70°C and stirred overnight. The synthesis of silicon particles with sacrificial polymer coating was carried out the next morning. The PPMA-coated silicon particles were analyzed by IR, as shown in FIG. Figure 5 and found in 1950 with 2200cm -1 The characteristic peak of the Si-H bond between the silicon and the PMMA layer disappears, indicating that the silicon surface is well covered by the PMMA layer.

[0201] 1.3 Synthesis of composite Si / C materials containing void spaces

[0202] In a typical synthesis, 12.7 g of p-phenylenediamine (PDA) was added to 313 g of water in a beaker and stirred for 30 minutes until all PDA was dissolved. Then 28.5 g of triethylamine was added to the solution and stirred for 10 minutes. Afterwards, 25.5 g of benzene-1,2,4,5-tetracarboxylic anhydride was added to the above solution and stirred for 4 hours. Then, 1.5 to 25 g of PMMA-modified Si particles were added to the above solution and stirred for 10 minutes. Then acetic anhydride (51.4 g) was poured into the above suspension and stirred for 50 seconds, after which the suspension was poured into 1200 mL of mineral oil containing a surfactant under mixing at 3600 rpm. Then the obtained emulsion was aged overnight, and then filtered. After the filtration was completed, the obtained material was rinsed with ethanol several times and dried in an oven at 700 ° C. While the present disclosure has been partially shown and described with reference to exemplary embodiments thereof, it will be understood by those skilled in the art that various changes in form and details may be made therein without departing from the technical scope encompassed by the appended claims.

[0203] While the present disclosure has been partially shown and described with reference to exemplary embodiments thereof, it will be understood by those skilled in the art that various changes in form and details may be made therein without departing from the technical scope encompassed by the appended claims.

Claims

1. A composite material comprising void spaces, the composite material further comprising: a. Silicon particles having a diameter less than about 1000 nm; and b. A three-dimensional carbon network structure, wherein the pore space is between the outer surface of the silicon particle and the three-dimensional carbon network structure. 2 . The composite material according to claim 1 , wherein the volume of the pore space is 3% to 250% of the volume of the silicon particles. 3 . The composite material according to claim 1 , wherein the three-dimensional carbon network structure comprises a carbon aerogel derived from polyimide.

4. The composite material according to claim 1, wherein the three-dimensional carbon network structure comprises carbon aerogel, carbon xerogel, carbon bigel, carbon aerogel-xerogel hybrid material, carbon aerogel-bigel hybrid material, carbon aerogel-bigel-xerogel hybrid material, or a combination thereof. The composite material according to claim 1 , wherein the three-dimensional carbon network structure is in the form of beads.

6. The composite material of claim 5, wherein the beads are substantially spherical, having a diameter of about 100 nm to about 4 mm, or about 5 μm to about 4 mm. The composite material according to claim 1 , wherein the silicon particles are dispersed within the three-dimensional carbon network structure.

8. The composite material of claim 7, wherein the silicon particles are non-uniformly dispersed throughout the three-dimensional carbon network structure.

9. The composite material of claim 7, wherein about 20 wt% to about 50 wt% of the dispersed silicon particles are in an aggregated state.

10. The composite material of claim 7, wherein less than about 20 wt% of the dispersed silicon particles are in an aggregated state. 11 . The composite material according to claim 1 , wherein the carbon network structure is a porous carbon network structure. 12 . The composite material according to claim 11 , wherein the pore structure of the three-dimensional carbon network structure comprises a pore diameter having a maximum peak of distribution at about 150 nm or less.

13. The composite material of claim 11, wherein the three-dimensional carbon network structure has a pore volume of at least 0.3 cc / g.

14. The composite material of claim 11, wherein the three-dimensional carbon network structure has a porosity of less than about 90% of the three-dimensional carbon network structure.

15. The composite material of claim 1, wherein the composite material has a capacity between about 500 mAh / g and about 3000 mAh / g.

16. The composite material of claim 1, wherein the three-dimensional carbon network structure has an electrical conductivity of at least about 1 S / cm.

17. An energy storage system comprising the composite material according to any one of claims 1 to 16. The composite material according to claim 17 , wherein the energy storage system is a battery.

19. The composite material of claim 18, wherein the battery is a rechargeable battery.

20. The composite material of claim 19, wherein the rechargeable battery is a lithium-ion battery.

21. A rechargeable battery comprising the composite material according to any one of claims 1 to 16.

22. A method for preparing a composite material, the method comprising: a. Providing silicon particles with a diameter of less than 1000nm; b. oxidizing the surface of the silicon particles to obtain hydroxyl groups on the surface; c. forming a sacrificial layer on at least a portion of the surface of the silicon particles; d. providing a sol-gel solution comprising a polar solvent and a precursor of a precursor bead; e. treating the silicon particles in the presence of the sol-gel solution to obtain precursor beads, the precursor beads comprising the silicon particles dispersed within the precursor beads; as well as f. pyrolyzing the precursor beads to obtain the porous network structure composite material, wherein the porous network structure composite material includes pore spaces.

23. The method of claim 22, further comprising a step of subcritical or supercritical drying after treating the silicon particles in the presence of the sol-gel solution and before pyrolyzing the precursor beads comprising the silicon particles.

24. The method of claim 22, further comprising the step of drying at ambient pressure.

25. The method of claim 22, wherein the porous network structure comprises an aerogel, a xerogel, a bicgel, an aerogel-xerogel hybrid material, an aerogel-bicgel hybrid material, an aerogel-bicgel-xerogel hybrid material, or a combination thereof.

26. The method of claim 22, wherein the porous network structure comprises or is derived from polyimide.

27. The method of claim 22, wherein the porous network structure is in the form of beads.

28. The method of claim 22, wherein the porous network structure has a carbonization yield greater than about 30 wt%.

29. The method of claim 22, wherein pyrolyzing the porous network structure carbonizes the sacrificial layer.

30. The method of claim 22, wherein the sacrificial layer has a carbonization yield of less than about 20 wt%.

31. A method for preparing a composite material, the method comprising: a. Providing silicon particles; b. forming a sacrificial layer on at least a portion of the surface of the silicon particles; d. incorporating the silicon particles into a three-dimensional network structure; and e. processing the three-dimensional network structure to obtain a composite material comprising void spaces surrounding the silicon particles.

32. The method of claim 31, wherein at least a portion of the surface of the silicon particle is at least 70% of the surface of the silicon particle, at least 90% of the surface of the silicon particle, or at least 95% of the surface of the silicon particle.

33. The method of claim 31, wherein the three-dimensional network structure comprises an organic material.

34. The method of claim 31, wherein the step of treating the three-dimensional network structure comprises heating the three-dimensional network structure to a carbonization temperature of the sacrificial layer.

35. The method of claim 31, wherein the step of treating the three-dimensional network structure comprises pyrolyzing the three-dimensional network structure.

36. The method of claim 31, wherein the three-dimensional network structure has a carbonization yield greater than about 30 wt%.

37. The method of claim 31, wherein pyrolyzing the three-dimensional network structure carbonizes the sacrificial layer.

38. The method of claim 31, wherein the sacrificial layer has a carbonization yield of less than about 20 wt%.

39. A composite material comprising void spaces surrounding silicon particles, said composite material being obtainable according to any one of claims 22 to 37.