Alloy material
By adjusting the total content of specific elements and reducing the density of nitrogen-containing precipitates, the chemical composition of the alloy material is optimized, and the problem of insufficient grain boundary corrosion resistance of the welding heat-affected part after welding is solved, and high corrosion resistance of the welding heat-affected part is achieved .
Patent Information
- Application Number
- CN202380030192.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-03-31
- Filing Date
- 2023-03-30
- Publication Date
- 2024-11-12
AI Technical Summary
The grain boundary corrosion resistance of the existing alloy materials at the heat-influenced portion of the welding after welding is insufficient, making it difficult to effectively improve.
By adjusting the total content of Ti, Nb, V, Zr, Hf, and Ta and reducing the number of fine nitrogen-containing precipitates at the grain boundary, the chemical composition of the alloy material is optimized to improve the grain boundary corrosion resistance of the welding heat-influenced part.
Even after welding, the alloy material can obtain excellent grain boundary corrosion resistance in the welding heat-influenced portion, which significantly improves the resistance to the corrosion environment.
Smart Images

Figure CN118946680A_ABST
Abstract
Description
Technical Field
[0001] The present disclosure relates to alloy materials. Background Art
[0002] Alloy materials are used in chemical plant equipment such as petroleum refining plants and petrochemical plants. The various devices of chemical plant equipment are, for example, vacuum distillation devices, direct desulfurization devices, contact modification devices, etc. These devices include heating furnace tubes, reaction towers, tanks, heat exchangers, pipes, etc. These devices are welded structures formed by welding materials.
[0003] These chemical plant equipments are in contact with process fluids containing sulfides and / or chlorides. Therefore, the materials used in these equipments are exposed to corrosive environments containing sulfides and / or chlorides. Therefore, the materials used in these equipments require excellent corrosion resistance. For example, alloy materials with high Ni and Cr contents are used in these equipments.
[0004] As mentioned above, alloy materials used in chemical plant equipment are welded to form a part of a welded structure. When such welding is performed, a weld heat affected zone (HAZ) is formed in the alloy material. In the weld heat affected zone, intergranular corrosion is easily caused due to sensitization. Therefore, excellent intergranular corrosion resistance is required for alloy materials used in chemical plant equipment.
[0005] International Publication No. 2017 / 168904 (Patent Document 1) proposes an alloy material having excellent intergranular corrosion resistance.
[0006] The alloy material disclosed in Patent Document 1 has the following chemical composition: in terms of mass%, it contains C: 0.005-0.015%, Si: 0.05-0.50%, Mn: 0.05-1.5%, P: 0.030% or less, S: 0.020% or less, Cu: 1.0-5.0%, Ni: 30.0-45.0%, Cr: 18.0-30.0%, Mo: 2.0-4.5%, Ti: 0.5-2.0%, N: 0.001-0.015%, and Al: 0-0.50%, and the balance is Fe and impurities. The average grain size d (μm) satisfies the formula (1).
[0007] d<4.386 / (C rel +0.15) (1)
[0008] Among them, C in formula (1) rel Defined by formula (2).
[0009] C rel =C-0.125Ti+0.8571N (2)
[0010] In addition, the content (mass %) of the corresponding element is substituted for each element symbol in formula (1) and formula (2).
[0011] In the alloy material disclosed in Patent Document 1, the relative amount of solid solution C (C rel ) and the average grain size d satisfy the formula (1). Therefore, Patent Document 1 states that the generation of Cr-poor regions can be suppressed and the intergranular corrosion resistance can be improved.
[0012] Prior art literature
[0013] Patent Literature
[0014] Patent Document 1: International Publication No. 2017 / 168904 Summary of the invention
[0015] Problem that the invention aims to solve
[0016] The intergranular corrosion resistance at the weld heat affected zone can be improved in the alloy material of Patent Document 1. However, the intergranular corrosion resistance at the weld heat affected zone can be improved by a method different from the method of Patent Document 1.
[0017] An object of the present disclosure is to provide an alloy material capable of obtaining excellent intergranular corrosion resistance in a weld heat affected zone even when welding is performed.
[0018] Solutions for solving problems
[0019] The alloy material disclosed in the present invention has the following configuration.
[0020] An alloy material, whose chemical composition is expressed in mass %
[0021] C: 0.005~0.020%,
[0022] Si: 0.05-0.50%,
[0023] Mn: 0.05-1.00%,
[0024] P: 0.030% or less,
[0025] S: 0.0100% or less,
[0026] Cu: 1.5-3.0%,
[0027] Ni: 35.0~50.0%,
[0028] Cr: 20.0~30.0%,
[0029] Mo: 2.5-4.0%,
[0030] Co: 0.01~0.80%,
[0031] W: 0.01~0.30%,
[0032] Ca: 0.0050% or less,
[0033] N: 0.001~0.015%,
[0034] Al: 0.20% or less,
[0035] B: 0.0030% or less,
[0036] Sn: 0.050% or less,
[0037] Ti: 0.40~0.90%,
[0038] Nb: 0~0.150%,
[0039] V: 0~0.150%,
[0040] Zr: 0~0.150%,
[0041] Hf: 0~0.150%,
[0042] Ta: 0 to 0.150%, and
[0043] The balance is Fe and impurities.
[0044] The total content of Ti, Nb, V, Zr, Hf and Ta is 0.420-1.000%.
[0045] The number density of nitrogen-containing precipitates having a major axis of 10 to 100 nm at the grain boundaries of the alloy material is 20 pieces / μm or less.
[0046] Effects of the Invention
[0047] In the alloy material of the present disclosure, even when welding is performed, excellent intergranular corrosion resistance can be obtained in the weld heat affected zone. BRIEF DESCRIPTION OF THE DRAWINGS
[0048] Figure 1 It shows the total content (%) of Ti, Nb, V, Zr, Hf and Ta and the corrosion rate (g / m 2 hr).
[0049] Figure 2It is the relationship between the number density of fine nitrogen-containing precipitates at the grain boundaries (pieces / μm) and the corrosion rate (g / m) obtained in the intergranular corrosion test based on the AST MA262 C method, which is an indicator of intergranular corrosion resistance. 2 hr).
[0050] Figure 3 The figures show a TEM image of an alloy material satisfying the chemical composition of the present embodiment and a diffraction pattern obtained by performing selected area electron diffraction (Selected Area Electron Diffraction) on fine precipitates indicated by arrows in the TEM image. DETAILED DESCRIPTION
[0051] The present inventors have studied an alloy material capable of obtaining excellent intergranular corrosion resistance in a weld heat affected zone even when welding is performed. As a result, the present inventors have obtained the following findings.
[0052] First, the inventors studied alloy materials having excellent intergranular corrosion resistance also in the weld heat affected zone from the viewpoint of chemical composition. As a result, the inventors believed that if an alloy material having the following chemical composition is used, it is possible to obtain excellent intergranular corrosion resistance also in the weld heat affected zone when welding is performed: C: 0.005-0.020%, Si: 0.05-0.50%, Mn: 0.05-1.00%, P: 0.030% or less, S: 0.0100% or less, Cu: 1.5-3.0%, Ni: 35.0-50.0%, Cr: 20.0-30.0%, Mo: 2. 5~4.0%, Co: 0.01~0.80%, W: 0.01~0.30%, Ca: less than 0.0050%, N: 0.001~0.015%, Al: less than 0.20%, B: less than 0.0030%, Sn: less than 0.050%, Ti: 0.40~0.90%, Nb: 0~0.150%, V: 0~0.150%, Zr: 0~0.150%, Hf: 0~0.150%, Ta: 0~0.150%, and the balance is Fe and impurities.
[0053] Therefore, the inventors of the present invention prepared a test piece simulating the heat affected zone of welding based on the alloy material of the above-mentioned chemical composition. Specifically, a test piece was collected from the alloy material of the above-mentioned chemical composition. A heat treatment simulating welding was applied to the test piece. A test piece simulating the heat affected zone of welding was prepared using the above method. Then, the intergranular corrosion resistance of the test piece was investigated. As a result, there is a situation where excellent intergranular corrosion resistance cannot be obtained in the alloy material satisfying the above-mentioned chemical composition.
[0054] Therefore, the present inventors conducted further studies and obtained the following findings.
[0055] In the heat affected zone of the alloy material, during the heat treatment simulating welding, the solid solution C combines with Cr to form Cr carbides. Therefore, the solid solution Cr at the grain boundary is deficient, and a Cr-poor region is formed at the grain boundary. Due to this Cr-poor region, intergranular corrosion occurs in the heat affected zone of the alloy material.
[0056] Among the elements in the above chemical composition, Ti, Nb, V, Zr, Hf and Ta have high affinity with solid solution C. Therefore, these elements generate carbides. Due to the generation of carbides, the solid solution C in the alloy material decreases. Therefore, it is difficult for Cr to generate Cr carbides, and the formation of Cr-poor regions is suppressed at the grain boundaries.
[0057] Based on the above findings, the present inventors believed that intergranular corrosion resistance could be improved by adjusting the total content of Ti, Nb, V, Zr, Hf and Ta. Therefore, the relationship between the total content Tx (%) of Ti, Nb, V, Zr, Hf and Ta and intergranular corrosion resistance was further investigated.
[0058] Figure 1 The total content Tx (%) of Ti, Nb, V, Zr, Hf and Ta in the alloy material having the above chemical composition and the corrosion rate (g / m) obtained in the intergranular corrosion test based on the AST MA262 C method, which is an indicator of intergranular corrosion resistance 2 hr). Figure 1 The data were prepared based on the data obtained by the experiments described in the examples described later.
[0059] Reference Figure 1 When the total content Tx is 0.420-1.000%, even if the total content Tx increases, the corrosion rate is 0.20g / m 2 hr or less, and extremely excellent intergranular corrosion resistance is obtained.
[0060] On the other hand, when the total content Tx is less than 0.420%, the corrosion rate increases significantly as the total content Tx decreases. Figure 1 In the figure, there is an inflection point near the total content Tx = 0.420%. Moreover, when the total content Tx is greater than 1.000%, the corrosion rate increases significantly with the increase of the total content Tx. Figure 1 There is an inflection point near the total content Tx=1.000%.
[0061] Based on the above findings, it was found that when the total content Tx of Ti, Nb, V, Zr, Hf, and Ta is 0.420 to 1.000%, the intergranular corrosion resistance is improved.
[0062] However, even if the above chemical composition is satisfied and the total content Tx of Ti, Nb, V, Zr, Hf and Ta is set to 0.420-1.000%, there is still a case where the intergranular corrosion resistance is low. Therefore, the present inventors studied a method for improving the intergranular corrosion resistance from the perspective of microstructure rather than the chemical composition. As a result, the present inventors obtained the following findings.
[0063] In the above chemical composition, N is contained in order to improve the strength. Among Ti, Nb, V, Zr, Hf and Ta, which have high affinity with C, Ti and Nb in particular also have high affinity with N. Therefore, Ti and Nb generate nitrides or carbonitrides of nanometer size at the grain boundaries. Hereinafter, in this specification, nitrides and carbonitrides are also referred to as "nitrogen-containing precipitates".
[0064] Such fine nitrogen-containing precipitates dissolve in a highly oxidizing corrosive environment. Therefore, even when there is no Cr-poor region at the grain boundary, if there are many fine nitrogen-containing precipitates at the grain boundary, intergranular corrosion occurs due to the dissolution of the nitrogen-containing precipitates, and the intergranular corrosion resistance decreases.
[0065] Therefore, the present inventors believed that in an alloy material having the above chemical composition and a total content Tx of Ti, Nb, V, Zr, Hf and Ta of 0.420 to 1.000%, if the number density of fine nitrogen-containing precipitates at the grain boundaries can be reduced, excellent intergranular corrosion resistance can be obtained also in the weld heat affected zone. Therefore, the relationship between the number density of fine nitrogen-containing precipitates at the grain boundaries and the intergranular corrosion resistance was further investigated.
[0066] Figure 2 The number density (pieces / μm) of fine nitrogen-containing precipitates at the grain boundaries in an alloy material having the above chemical composition and a total content of Ti, Nb, V, Zr, Hf and Ta of 0.420 to 1.000% and the corrosion rate (g / m) obtained in a grain boundary corrosion test according to the ASTM A262C method, which is an indicator of grain boundary corrosion resistance, are shown. 2 hr). Figure 2 It is prepared based on data obtained from experiments described in the examples described later.
[0067] Reference Figure 2When the number density of fine nitrogen-containing precipitates at the grain boundary is less than 20 / μm, the corrosion rate is 0.20 g / m even if the number density increases. 2 hr or less, an extremely excellent intergranular corrosion resistance is obtained. On the other hand, if the number density of fine nitrogen-containing precipitates at the grain boundaries is greater than 20 / μm, the corrosion rate increases significantly as the number density increases. Figure 2 There is an inflection point near the number density = 20 pieces / μm.
[0068] Based on the above findings, the present inventors have discovered the following findings: in an alloy material having the above-mentioned chemical composition and a total content Tx of Ti, Nb, V, Zr, Hf and Ta of 0.420 to 1.000%, if the number density of fine nitrogen-containing precipitates at the grain boundaries is set to 20 pieces / μm or less, excellent intergranular corrosion resistance can be obtained in the weld heat affected zone even when welding is performed.
[0069] The alloy material of the present embodiment completed based on the above findings has the following structure.
[0070] [1] An alloy material having a chemical composition in mass % as follows:
[0071] C: 0.005~0.020%,
[0072] Si: 0.05-0.50%,
[0073] Mn: 0.05-1.00%,
[0074] P: 0.030% or less,
[0075] S: 0.0100% or less,
[0076] Cu: 1.5-3.0%,
[0077] Ni: 35.0-50.0%,
[0078] Cr: 20.0~30.0%,
[0079] Mo: 2.5-4.0%,
[0080] Co: 0.01~0.80%,
[0081] W: 0.01~0.30%,
[0082] Ca: 0.0050% or less,
[0083] N: 0.001~0.015%,
[0084] Al: 0.20% or less,
[0085] B: 0.0030% or less,
[0086] Sn: 0.050% or less,
[0087] Ti: 0.40~0.90%,
[0088] Nb: 0~0.150%,
[0089] V: 0~0.150%,
[0090] Zr: 0~0.150%,
[0091] Hf: 0~0.150%,
[0092] Ta: 0 to 0.150%, and
[0093] The balance is Fe and impurities.
[0094] The total content of Ti, Nb, V, Zr, Hf and Ta is 0.420-1.000%.
[0095] The number density of nitrogen-containing precipitates having a major axis of 10 to 100 nm at the grain boundaries of the alloy material is 20 pieces / μm or less.
[0096] [2] The alloy material according to [1], wherein
[0097] The chemical composition contains a
[0098] Nb: 0.001~0.150%,
[0099] V: 0.001~0.150%,
[0100] Zr: 0.001~0.150%,
[0101] Hf: 0.001~0.150%, and
[0102] Ta: One or more elements of the group consisting of 0.001 to 0.150%.
[0103] [3] The alloy material according to [1] or [2], wherein
[0104] The alloy material is an alloy tube.
[0105] The alloy material of the present embodiment will be described in detail below. In addition, "%" related to an element means mass % unless otherwise specified.
[0106] [Characteristics of the alloy material of this embodiment]
[0107] The alloy material of the present embodiment satisfies the following features 1 to 3.
[0108] (Feature 1)
[0109] The chemical composition is as follows in mass %: C: 0.005-0.020%, Si: 0.05-0.50%, Mn: 0.05-1.00%, P: 0.030% or less, S: 0.0100% or less, Cu: 1.5-3.0%, Ni: 35.0-50.0%, Cr: 20.0-30.0%, Mo: 2.5-4.0%, Co: 0.01-0.80%, W: 0.01-0. 30%, Ca: less than 0.0050%, N: 0.001~0.015%, Al: less than 0.20%, B: less than 0.0030%, Sn: less than 0.050%, Ti: 0.40~0.90%, Nb: 0~0.150%, V: 0~0.150%, Zr: 0~0.150%, Hf: 0~0.150%, Ta: 0~0.150%, and the balance is Fe and impurities.
[0110] (Feature 2)
[0111] The total content of Ti, Nb, V, Zr, Hf and Ta is 0.420-1.000%.
[0112] (Feature 3)
[0113] The number density of nitrogen-containing precipitates having a major axis of 10 to 100 nm at the grain boundaries of the alloy material is 20 pieces / μm or less.
[0114] Hereinafter, features 1 to 3 will be described.
[0115] [For (Feature 1) Chemical composition]
[0116] The chemical composition of the alloy material of the present embodiment contains the following elements.
[0117] C: 0.005~0.020%
[0118] Carbon (C) improves the strength of the alloy material. If the C content is less than 0.005%, the above-mentioned effects cannot be fully obtained even if the contents of other elements are within the ranges of the present embodiment.
[0119] On the other hand, if the C content exceeds 0.020%, M 23 C6 type Cr carbide. In this case, a Cr-poor region is formed at the grain boundary. Therefore, even if the content of other elements is within the range of this embodiment, the intergranular corrosion resistance of the alloy material is reduced.
[0120] Therefore, the C content is 0.005 to 0.020%.
[0121] The lower limit of the C content is preferably 0.006%, more preferably 0.007%, and further preferably 0.008%.
[0122] The upper limit of the C content is preferably 0.019%, more preferably 0.017%, further preferably 0.015%, further preferably 0.013%.
[0123] Si: 0.05-0.50%
[0124] Silicon (Si) deoxidizes the alloy in the steelmaking process. If the Si content is less than 0.05%, the above-mentioned effects cannot be fully obtained.
[0125] On the other hand, if the Si content exceeds 0.50%, even if the contents of other elements are within the ranges of the present embodiment, inclusions are excessively generated, and the corrosion resistance of the alloy material is reduced.
[0126] Therefore, the Si content is 0.05 to 0.50%.
[0127] The lower limit of the Si content is preferably 0.08%, more preferably 0.12%, and further preferably 0.15%.
[0128] The upper limit of the Si content is preferably 0.45%, more preferably 0.40%, further preferably 0.38%, further preferably 0.35%.
[0129] Mn: 0.05~1.00%
[0130] Manganese (Mn) deoxidizes the alloy. Mn is also an austenite-forming element, stabilizing the austenite in the alloy material. If the Mn content is too low, even if the contents of other elements are within the range of the present embodiment, the above effects cannot be fully obtained.
[0131] On the other hand, if the Mn content exceeds 1.00%, even if the contents of other elements are within the ranges of the present embodiment, inclusions are excessively generated, and the corrosion resistance of the alloy material is reduced.
[0132] Therefore, the Mn content is 0.05 to 1.00%.
[0133] The lower limit of the Mn content is preferably 0.10%, more preferably 0.20%, further preferably 0.30%, further preferably 0.40%.
[0134] The upper limit of the Mn content is preferably 0.90%, more preferably 0.85%, further preferably 0.80%, further preferably 0.70%.
[0135] P: 0.030% or less
[0136] Phosphorus (P) is an impurity that is inevitably contained. That is, the P content is greater than 0%. P segregates at the grain boundaries. Therefore, if the P content is too high, the intergranular corrosion resistance of the alloy material is reduced even if the contents of other elements are within the range of this embodiment.
[0137] Therefore, the P content is set to 0.030% or less.
[0138] The P content is preferably as low as possible. However, excessive reduction of the P content will significantly increase the manufacturing cost. Therefore, in consideration of industrial production, the preferred lower limit of the P content is 0.001%, more preferably 0.002%, and even more preferably 0.003%.
[0139] The upper limit of the P content is preferably 0.028%, more preferably 0.025%, further preferably 0.023%, further preferably 0.020%.
[0140] S: 0.0100% or less
[0141] Sulfur (S) is an impurity that is inevitably contained. That is, the S content is greater than 0%. S segregates at the grain boundaries. Therefore, if the S content is too high, the intergranular corrosion resistance of the alloy material is reduced even if the contents of other elements are within the range of this embodiment.
[0142] Therefore, the S content is 0.0100% or less.
[0143] The S content is preferably as low as possible. However, excessive reduction of the S content will significantly increase the manufacturing cost. Therefore, in consideration of industrial production, the preferred lower limit of the S content is 0.0001%, and more preferably 0.0002%.
[0144] The upper limit of the S content is preferably 0.0050%, more preferably 0.0040%, more preferably 0.0030%, more preferably 0.0020%, and still more preferably 0.0010%.
[0145] Cu: 1.5-3.0%
[0146] Copper (Cu) improves the corrosion resistance of the alloy material in an environment containing non-oxidizing acids and chlorides. If the Cu content is less than 1.5%, the above effect cannot be fully obtained.
[0147] On the other hand, if the Cu content exceeds 3.0%, the hot workability of the alloy material decreases even if the contents of other elements are within the ranges of the present embodiment.
[0148] Therefore, the Cu content is 1.5 to 3.0%.
[0149] The preferred lower limit of the Cu content is 1.6%, more preferably 1.7%.
[0150] The upper limit of the Cu content is preferably 2.5%, more preferably 2.3%, more preferably 2.1%, and further preferably 2.0%.
[0151] Ni: 35.0~50.0%
[0152] Nickel (Ni) is an austenite-forming element and stabilizes austenite in the alloy material. Ni also improves the intergranular corrosion resistance of the alloy material. If the Ni content is less than 35.0%, the above-mentioned effects cannot be fully obtained even if the contents of other elements are within the range of the present embodiment.
[0153] On the other hand, if the Ni content exceeds 50.0%, the intergranular corrosion resistance of the alloy material decreases even if the contents of other elements are within the ranges of the present embodiment. If the Ni content exceeds 50.0%, the manufacturing cost further increases significantly.
[0154] Therefore, the Ni content is 35.0 to 50.0%.
[0155] The lower limit of the Ni content is preferably 36.0%, more preferably 37.0%, and further preferably 38.0%.
[0156] The upper limit of the Ni content is preferably 48.0%, more preferably 46.0%, and further preferably 44.0%.
[0157] Cr: 20.0~30.0%
[0158] Chromium (Cr) improves the intergranular corrosion resistance of the alloy material. If the Cr content is less than 20.0%, the above-mentioned effects cannot be fully obtained even if the contents of other elements are within the ranges of the present embodiment.
[0159] On the other hand, if the Cr content exceeds 30.0%, even if the contents of other elements are within the ranges of the present embodiment, intermetallic compounds represented by σ phases are generated. In this case, the intergranular corrosion resistance of the alloy material decreases.
[0160] Therefore, the Cr content is 20.0 to 30.0%.
[0161] The lower limit of the Cr content is preferably 20.3%, more preferably 20.5%, further preferably 20.8%, further preferably 21.0%.
[0162] The upper limit of the Cr content is preferably 29.0%, more preferably 28.5%, further preferably 28.0%, further preferably 27.5%.
[0163] Mo: 2.5~4.0%
[0164] Molybdenum (Mo) improves the corrosion resistance of the alloy material. If the Mo content is less than 2.5%, the above-mentioned effects cannot be fully obtained even if the contents of other elements are within the ranges of the present embodiment.
[0165] On the other hand, if the Mo content exceeds 4.0%, even if the contents of other elements are within the ranges of the present embodiment, intermetallic compounds represented by σ phases are generated. In this case, the intergranular corrosion resistance of the alloy material decreases.
[0166] Therefore, the Mo content is 2.5 to 4.0%.
[0167] The lower limit of the Mo content is preferably 2.6%, more preferably 2.7%, and further preferably 2.8%.
[0168] The upper limit of the Mo content is preferably 3.9%, more preferably 3.8%, and further preferably 3.7%.
[0169] Co: 0.01~0.80%
[0170] Cobalt (Co) improves the corrosion resistance of the alloy material. If the Co content is less than 0.01%, the above-mentioned effects cannot be fully obtained even if the contents of other elements are within the ranges of the present embodiment.
[0171] On the other hand, if the Co content exceeds 0.80%, the manufacturing cost becomes high even if the contents of other elements are within the ranges of the present embodiment.
[0172] Therefore, the Co content is 0.01 to 0.80%.
[0173] The lower limit of the Co content is preferably 0.03%, more preferably 0.05%, further preferably 0.10%, further preferably 0.20%.
[0174] The upper limit of the Co content is preferably 0.75%, more preferably 0.70%, and further preferably 0.65%.
[0175] W: 0.01~0.30%
[0176] Tungsten (W) improves the corrosion resistance of the alloy material. If the W content is less than 0.01%, the above-mentioned effects cannot be fully obtained even if the contents of other elements are within the ranges of the present embodiment.
[0177] On the other hand, if the W content exceeds 0.30%, the hot workability of the alloy material decreases even if the contents of other elements are within the ranges of the present embodiment.
[0178] Therefore, the W content is 0.01 to 0.30%.
[0179] The lower limit of the W content is preferably 0.02%, more preferably 0.03%.
[0180] The upper limit of the W content is preferably 0.25%, more preferably 0.20%, further preferably 0.15%, further preferably 0.12%.
[0181] Ca: 0.0050% or less
[0182] Calcium (Ca) is inevitably contained. That is, the Ca content is greater than 0%. Ca fixes the S in the alloy material into sulfide and renders it harmless. As a result, the hot workability and weldability of the alloy material are improved. As long as a small amount of Ca is contained, the above effects can be obtained to a certain extent.
[0183] However, if the Ca content exceeds 0.0050%, even if the contents of other elements are within the ranges of the present embodiment, coarse oxides are generated in the alloy material. In this case, the hot workability of the alloy material is reduced.
[0184] Therefore, the Ca content is 0.0050% or less.
[0185] The lower limit of the Ca content is preferably 0.0001%, more preferably 0.0005%, further preferably 0.0010%, further preferably 0.0015%.
[0186] The upper limit of the Ca content is preferably 0.0045%, more preferably 0.0040%, further preferably 0.0035%, further preferably 0.0030%.
[0187] N: 0.001~0.015%
[0188] Nitrogen (N) dissolves in the alloy material to improve the strength of the alloy material. If the N content is less than 0.001%, the above-mentioned effects cannot be fully obtained even if the contents of other elements are within the ranges of the present embodiment.
[0189] On the other hand, when the N content exceeds 0.015%, nitrides are excessively generated at the grain boundaries. In this case, the intergranular corrosion resistance of the alloy material is reduced.
[0190] Therefore, the N content is 0.001 to 0.015%.
[0191] The lower limit of the N content is preferably 0.002%, more preferably 0.003%.
[0192] The upper limit of the N content is preferably 0.012%, more preferably 0.010%, and further preferably 0.009%.
[0193] Al: 0.20% or less
[0194] Aluminum (Al) is inevitably contained. That is, the Al content is greater than 0%. Al deoxidizes the alloy. As long as a small amount of Al is contained, the above-mentioned effect can be obtained to a certain extent.
[0195] However, if the Al content exceeds 0.20%, even if the contents of other elements are within the ranges of the present embodiment, oxide inclusions are excessively generated, and in this case, the corrosion resistance of the alloy material is reduced.
[0196] Therefore, the Al content is 0.20% or less.
[0197] The lower limit of the Al content is preferably 0.01%, more preferably 0.02%, and further preferably 0.03%.
[0198] The upper limit of the Al content is preferably 0.18%, more preferably 0.16%, further preferably 0.14%, further preferably 0.12%.
[0199] B: 0.0030% or less
[0200] Boron (B) is inevitably contained. That is, the B content is greater than 0%. B segregates at the grain boundaries to strengthen the grain boundaries and improve the hot workability of the alloy material. As long as a small amount of B is contained, the above effect can be achieved to a certain extent.
[0201] However, if the B content exceeds 0.0030%, B will excessively segregate at the grain boundaries even if the contents of other elements are within the ranges of the present embodiment. In this case, the hot workability of the alloy material will decrease.
[0202] Therefore, the B content is 0.0030% or less.
[0203] The lower limit of the B content is preferably 0.0001%, more preferably 0.0002%.
[0204] The upper limit of the B content is preferably 0.0025%, more preferably 0.0020%, further preferably 0.0018%, further preferably 0.0016%.
[0205] Sn: 0.050% or less
[0206] The tin (Sn) content is greater than 0%. Sn improves the corrosion resistance of the alloy material. The above effect can be achieved to a certain extent as long as a small amount of Sn is contained.
[0207] However, if the Sn content exceeds 0.050%, the hot workability of the alloy material decreases even if the contents of other elements are within the ranges of the present embodiment.
[0208] Therefore, the Sn content is 0.050% or less.
[0209] The lower limit of the Sn content is preferably 0.001%, more preferably 0.002%.
[0210] The upper limit of the Sn content is preferably 0.040%, more preferably 0.030%, further preferably 0.020%, further preferably 0.015%.
[0211] Ti: 0.40~0.90%
[0212] Titanium (Ti) combines with C to form Ti carbide, which fixes C. Thus, Ti inhibits solid solution C from combining with Cr to form Cr carbide. Therefore, Cr-poor regions are difficult to form at grain boundaries. As a result, the intergranular corrosion resistance of the alloy material is improved. Ti also combines with C and / or N to form Ti carbide, Ti nitride, or Ti carbonitride, which improves the strength of the alloy material. If the Ti content is less than 0.40%, even if the content of other elements is within the range of this embodiment, the above-mentioned effects cannot be fully obtained.
[0213] On the other hand, if the Ti content exceeds 0.90%, even if the contents of other elements are within the ranges of the present embodiment, excessive amounts of Ti nitrides and / or Ti carbonitrides are generated at the grain boundaries. In this case, the intergranular corrosion resistance of the alloy material decreases.
[0214] Therefore, the Ti content is 0.40 to 0.90%.
[0215] The lower limit of the Ti content is preferably 0.41%, more preferably 0.43%, and further preferably 0.45%.
[0216] The upper limit of the Ti content is preferably 0.85%, more preferably 0.80%, further preferably 0.75%, further preferably 0.70%.
[0217] The balance of the chemical composition of the alloy material of the present embodiment is Fe and impurities. Among them, impurities refer to elements mixed from ores, waste materials, or manufacturing environments as raw materials during industrial manufacturing of alloy materials, which are not intentionally contained elements, but are allowed within the range that does not bring significant adverse effects to the effects of the alloy material of the present embodiment.
[0218] [For any element]
[0219] The chemical composition of the alloy of the present embodiment may further contain the following elements.
[0220] Freedom to choose
[0221] Nb: 0~0.150%,
[0222] V: 0~0.150%,
[0223] Zr: 0~0.150%,
[0224] Hf: 0~0.150%, and
[0225] Ta: one or more elements of the group consisting of 0 to 0.150%,
[0226] These elements are all arbitrary elements. These elements all form carbides that are bonded to solid solution C, thereby improving the intergranular corrosion resistance of the alloy material.
[0227] Each element is described below.
[0228] Nb: 0~0.150%
[0229] Niobium (Nb) is an arbitrary element and may not be contained. That is, the Nb content may also be 0%. When contained, Nb combines with C to form Nb carbide, fixing C. Thus, the formation of Cr-poor regions at grain boundaries can be suppressed, and the intergranular corrosion resistance of the alloy material is improved. Nb also combines with C and / or N to form Nb carbide, Nb nitride, or Nb carbonitride, improving the strength of the alloy material. As long as a small amount of Nb is contained, the above-mentioned effect can be obtained to a certain extent.
[0230] However, if the Nb content exceeds 0.150%, even if the contents of other elements are within the ranges of the present embodiment, excessive amounts of Nb nitrides and / or Nb carbonitrides are generated at the grain boundaries. In this case, the intergranular corrosion resistance of the alloy material decreases.
[0231] Therefore, the Nb content is 0 to 0.150%.
[0232] The lower limit of the Nb content is preferably 0.001%, more preferably 0.002%, and further preferably 0.005%.
[0233] The upper limit of the Nb content is preferably 0.140%, more preferably 0.130%, more preferably 0.100%, more preferably 0.070%, more preferably 0.050%, and still more preferably 0.040%.
[0234] V: 0~0.150%
[0235] Vanadium (V) is an arbitrary element and may not be contained. That is, the V content may also be 0%. When contained, V combines with C to form V carbides, which fix C. Thus, the formation of Cr-poor regions at grain boundaries can be suppressed, and the intergranular corrosion resistance of the alloy material is improved. V also combines with C and / or N to form V carbides, V nitrides, or V carbonitrides, which improve the strength of the alloy material. As long as a small amount of V is contained, the above-mentioned effects can be obtained to a certain extent.
[0236] However, if the V content is greater than 0.150%, the strength of the alloy material becomes excessively high even if the contents of other elements are within the range of the present embodiment. In this case, the hot workability of the alloy material is reduced. If the V content is greater than 0.150%, V carbides and / or V carbonitrides are further excessively generated at the grain boundaries. In this case, the intergranular corrosion resistance of the alloy material is reduced.
[0237] Therefore, the V content is 0 to 0.150%.
[0238] The lower limit of the V content is preferably 0.001%, more preferably 0.002%, and further preferably 0.005%.
[0239] The upper limit of the V content is preferably 0.140%, more preferably 0.130%, more preferably 0.100%, more preferably 0.070%, more preferably 0.050%, and still more preferably 0.040%.
[0240] Zr: 0~0.150%
[0241] Zirconium (Zr) is an arbitrary element and may not be contained. That is, the Zr content may also be 0%. When contained, Zr combines with C to form Zr carbide, which fixes C. As a result, the formation of Cr-poor regions at grain boundaries can be suppressed, and the intergranular corrosion resistance of the alloy material is improved. Zr also combines with C and / or N to form Zr carbide, Zr nitride, or Zr carbonitride, which improves the strength of the alloy material. As long as a small amount of Zr is contained, the above-mentioned effect can be obtained to a certain extent.
[0242] However, if the Zr content exceeds 0.150%, the strength of the alloy material becomes excessively high even if the contents of other elements are within the ranges of the present embodiment. In this case, the hot workability of the alloy material decreases.
[0243] Therefore, the Zr content is 0 to 0.150%.
[0244] The lower limit of the Zr content is preferably 0.001%, more preferably 0.002%, further preferably 0.005%, further preferably 0.010%.
[0245] The upper limit of the Zr content is preferably 0.140%, more preferably 0.130%, and further preferably 0.120%.
[0246] Hf: 0~0.150%
[0247] Hafnium (Hf) is an arbitrary element and may not be contained. That is, the Hf content may also be 0%. When contained, Hf combines with C to form Hf carbide, fixing C. Thus, the formation of Cr-poor regions at grain boundaries can be suppressed, and the intergranular corrosion resistance of the alloy material is improved. Hf also combines with C and / or N to form Hf carbide, Hf nitride, or Hf carbonitride, improving the strength of the alloy material. As long as a small amount of Hf is contained, the above-mentioned effect can be obtained to a certain extent.
[0248] However, if the Hf content exceeds 0.150%, the strength of the alloy material becomes excessively high even if the contents of other elements are within the ranges of the present embodiment. In this case, the hot workability of the alloy material decreases.
[0249] Therefore, the Hf content is 0 to 0.150%.
[0250] The lower limit of the Hf content is preferably 0.001%, more preferably 0.002%, further preferably 0.005%, further preferably 0.010%.
[0251] The upper limit of the Hf content is preferably 0.140%, more preferably 0.130%, and further preferably 0.120%.
[0252] Ta: 0~0.150%
[0253] Tantalum (Ta) is an arbitrary element and may not be contained. That is, the Ta content may also be 0%. When contained, Ta combines with C to form Ta carbide, which fixes C. As a result, the formation of Cr-poor regions at grain boundaries can be suppressed, and the intergranular corrosion resistance of the alloy material is improved. Ta also combines with C and / or N to form Ta carbide, Ta nitride or Ta carbonitride, which improves the strength of the alloy material. As long as a small amount of Ta is contained, the above-mentioned effect can be obtained to a certain extent.
[0254] However, if the Ta content exceeds 0.150%, the strength of the alloy material becomes excessively high even if the contents of other elements are within the ranges of the present embodiment. In this case, the hot workability of the alloy material decreases.
[0255] Therefore, the Ta content is 0 to 0.150%.
[0256] The lower limit of the Ta content is preferably 0.001%, more preferably 0.002%, further preferably 0.005%, further preferably 0.010%.
[0257] The upper limit of the Ta content is preferably 0.140%, more preferably 0.130%, and further preferably 0.120%.
[0258] [For (Feature 2) Total Content Tx of Ti, Nb, V, Zr, Hf, and Ta]
[0259] In the alloy material of the present embodiment, the total content Tx of Ti, Nb, V, Zr, Hf, and Ta is 0.420 to 1.000%.
[0260] As described above, Ti, Nb, V, Zr, Hf, and Ta all combine with C to form carbides, thereby fixing C. As a result, these elements inhibit the solid solution C from combining with Cr to form Cr carbides. Therefore, Cr-poor regions are difficult to form at grain boundaries. As a result, the intergranular corrosion resistance of the alloy material is improved.
[0261] like Figure 1 As shown, even if the alloy material satisfies feature 1, if the total content Tx of one or more elements selected from the group consisting of Ti, Nb, V, Zr, Hf and Ta is less than 0.420%, excellent intergranular corrosion resistance cannot be obtained even if the contents of other elements are within the range of the present embodiment. On the other hand, if the total content Tx is greater than 1.000%, nitrides and / or carbonitrides will be excessively generated at the grain boundaries even if the contents of other elements are within the range of the present embodiment. In this case, Figure 1 As shown in this way, the intergranular corrosion resistance of the alloy material decreases.
[0262] If the total content Tx of one or more elements selected from the group consisting of Ti, Nb, V, Zr, Hf and Ta is 0.420 to 1.000%, then Figure 1 As shown in this way, the intergranular corrosion resistance of the alloy material is significantly improved.
[0263] The lower limit of the total content Tx is preferably 0.425%, more preferably 0.440%, more preferably 0.460%, more preferably 0.480%, and further preferably 0.500%.
[0264] The upper limit of the total content Tx is preferably 0.950%, more preferably 0.920%, more preferably 0.900%, more preferably 0.880%, more preferably 0.850%, more preferably 0.830%, and more preferably 0.800%.
[0265] [For (Feature 3) Number density of fine nitrogen-containing precipitates at grain boundaries (pieces / μm)]
[0266] In the alloy material of the present embodiment, the number density of nitrogen-containing precipitates having a major axis of 10 to 100 nm at the grain boundaries is also 20 pieces / μm or less.
[0267] Here, nitrogen-containing precipitates refer to precipitates containing N. That is, nitrogen-containing precipitates are nitrides and / or carbonitrides. In addition, nitrogen-containing precipitates having a major diameter of 10 to 100 nm are referred to as "fine nitrogen-containing precipitates".
[0268] When the alloy material is used in a highly oxidizing corrosive environment, there is a case where the fine nitrogen-containing precipitates present at the grain boundaries dissolve. If the fine nitrogen-containing precipitates dissolve, the intergranular corrosion resistance of the alloy material decreases. Therefore, the number density of fine nitrogen-containing precipitates at the grain boundaries is preferably low.
[0269] The number of fine nitrogen-containing precipitates per 1 μm of grain boundary is defined as the number density of fine nitrogen-containing precipitates (pieces / μm). If the number density of fine nitrogen-containing precipitates is greater than 20 pieces / μm, even if the alloy material satisfies characteristics 1 and 2, sufficient intergranular corrosion resistance cannot be obtained. If the number density of fine nitrogen-containing precipitates is 20 pieces / μm or less, it can be Figure 2 This shows that excellent intergranular corrosion resistance is achieved.
[0270] [Method for determining the number density of fine nitrogen-containing precipitates]
[0271] The number density of fine nitrogen-containing precipitates at the grain boundaries can be determined as follows.
[0272] First, a test piece is collected from the alloy material.
[0273] When the alloy material is an alloy plate, a micro test piece is collected from the t / 4 portion as the observation object area. Wherein, the t / 4 portion refers to the portion at a depth of t / 4 from the surface of the alloy plate when the plate thickness is set to t (mm). When the alloy material is an alloy tube, a micro test piece is collected from the central portion of the wall thickness as the observation object area. When the alloy material is an alloy rod, a micro test piece is collected from the R / 2 portion as the observation object area. Wherein, the R / 2 portion refers to the central portion of the radius R in the cross section perpendicular to the rolling direction of the alloy rod. The size of the micro test piece is not particularly limited.
[0274] After the surface of the micro test piece was mirror-polished, the micro test piece was immersed in a 3% nitric acid etchant for 10 minutes to etch the surface. The etched surface was covered with a carbon vapor-deposited film. The micro test piece with the surface covered with the vapor-deposited film was immersed in a 5% nitric acid etchant for 20 minutes. The vapor-deposited film was peeled off from the immersed micro test piece. After the vapor-deposited film was washed with ethanol, it was scooped out with a mesh sheet and dried.
[0275] The deposited film (replica film) was observed using a transmission electron microscope (TEM). Specifically, an arbitrary position of the deposited film was observed at a magnification of 50,000 times and an acceleration voltage of 200 kV. The size of the observation field is not particularly limited, and is, for example, 2.0 μm×2.0 μm.
[0276] In the bright field image of the observation field, the grain boundaries of the alloy material can be easily confirmed according to the contrast. In addition, the precipitates existing on the grain boundaries can also be easily specified according to the contrast. Therefore, the precipitates existing on the grain boundaries are specified. The long diameter of the specified precipitates is measured. Among them, the long diameter refers to the maximum length (nm) of the line segment connecting the two points of the interface between the precipitate and the parent phase. Among the precipitates on the grain boundaries, the precipitates with a long diameter of 10 to 100 nm are specified. Hereinafter, the precipitates with a long diameter of 10 to 100 nm are referred to as "fine precipitates". In addition, the long diameter of the precipitates can be obtained by performing image analysis on the observation image during TEM observation.
[0277] Figure 3 FIG. 1 is a diagram showing a TEM image of an alloy material satisfying characteristics 1 and 2 and a diffraction pattern obtained by performing selected area electron diffraction (Selected Area Electron Diffraction) on fine precipitates indicated by arrows in the TEM image. When selected area electron diffraction is performed on specified fine precipitates in an alloy material satisfying characteristics 1 and 2, most diffraction patterns are as shown in FIG. Figure 3 As shown in FIG. 1 , the precipitate is determined to be MX type (nitride or carbonitride). That is, the precipitate other than the fine nitrogen-containing precipitate among the specified fine precipitates is hardly contained. Therefore, the specified fine precipitate is regarded as the fine nitrogen-containing precipitate.
[0278] The number of fine nitrogen-containing precipitates existing on the grain boundaries within the observation field is counted. Furthermore, the total length (μm) of the grain boundaries within the observation field is measured. Based on the obtained number of fine nitrogen-containing precipitates and the total length of the grain boundaries, the number density (pieces / μm) of fine nitrogen-containing precipitates at the grain boundaries is calculated. In this embodiment, the number density of fine nitrogen-containing precipitates is calculated by rounding off the first decimal place of the obtained value.
[0279] [Effects of the Alloy Material of the Present Embodiment]
[0280] As described above, the alloy material of the present embodiment satisfies characteristics 1 to 3. Therefore, the alloy material of the present embodiment can obtain excellent intergranular corrosion resistance in a strongly oxidizing corrosive environment. The intergranular corrosion resistance was evaluated by the following method.
[0281] [Evaluation method for intergranular corrosion resistance]
[0282] A test piece with a thickness of 5 mm, a width of 10 mm, and a length of 50 mm was collected from the alloy material. The length direction of the test piece was set to be parallel to the rolling direction of the alloy material. In order to set it as a test piece simulating the heat affected zone of welding, a sensitization treatment was performed on the test piece. Specifically, the test piece was kept at 700°C for 60 minutes. The test piece after keeping was allowed to cool naturally. The above sensitization treatment was performed to make a test piece simulating the heat affected zone of welding.
[0283] The surface of the prepared test piece was finished using wet corundum grinding No. 600, degreased and dried using acetone. The intergranular corrosion test was performed on the test piece according to ASTM A262 C method. Specifically, a test bath of boiling 65% nitric acid was prepared. The test piece was immersed in the test bath for 48 hours. The test piece was taken out from the test bath after 48 hours. The corrosion rate (g / m 2 This operation was repeated 5 times, and the corrosion rate (g / m 2 ·hr). The arithmetic mean of the five corrosion rates obtained was 0.20 g / m 2 When ·hr or less, it is judged that the intergranular corrosion resistance is excellent.
[0284] [Microstructure of the Alloy Material of the Present Embodiment]
[0285] The microstructure of the alloy material of the present embodiment is composed of austenite, except for precipitates and inclusions.
[0286] [Shape of alloy material]
[0287] The shape of the alloy material of the present embodiment is not particularly limited. The alloy material may be an alloy plate, an alloy tube, or an alloy rod. When the alloy material is an alloy tube, the alloy material is preferably a seamless alloy tube.
[0288] [Application of alloy materials]
[0289] The use of the alloy material of the present embodiment is not particularly limited. The alloy material of the present embodiment is particularly suitable for use in a corrosive environment, for example. The alloy material of the present embodiment can be used in equipment related to the petroleum industry, gas industry, petrochemical industry, and chemical industry, for example. The alloy material of the present embodiment is particularly suitable for use in equipment such as primary processing equipment for oil and gas, chemical plants, etc.
[0290] [Method for producing alloy material]
[0291] A method for producing the alloy material according to the present embodiment that satisfies Features 1 to 3 will be described.
[0292] The manufacturing method described below is an example of the manufacturing method of the alloy material of the present embodiment. Therefore, the alloy material satisfying characteristics 1 to 3 can also be manufactured by other manufacturing methods other than the manufacturing method described below. However, the manufacturing method described below is a preferred example of the manufacturing method of the alloy material of the present embodiment.
[0293] The method for producing the alloy material of the present embodiment includes the following steps. However, the cold working step of step 3 is an arbitrary step. In other words, the cold working step of step 3 may not be performed.
[0294] (Process 1) Preparation process
[0295] (Process 2) Hot working process
[0296] (Process 3) Cold working process
[0297] (Step 4) Heat treatment step
[0298] Hereinafter, each step will be described.
[0299] [(Process 1) Preparation process]
[0300] In the preparation step, a billet having the chemical composition of the above-mentioned feature 1 is prepared. The billet may be supplied from a third party or may be manufactured. The billet may be an ingot, a slab, a bloom, or a billet.
[0301] When manufacturing a billet, the billet is manufactured using the following method. A liquid alloy (melt) having the above-mentioned chemical composition is manufactured. A steel ingot is manufactured using the manufactured melt by an ingot casting method. A slab, a bloom, or a billet can also be manufactured using the manufactured melt by a continuous casting method. The manufactured ingot, slab, or billet can also be subjected to hot working to manufacture a billet. For example, a cylindrical billet can also be manufactured by hot forging or initial rolling of an ingot or billet, and the billet can be used as a billet. In this case, the temperature of the billet immediately before hot forging is not particularly limited, and is, for example, 1000 to 1300°C. The method for cooling the billet after hot forging is not particularly limited.
[0302] [(Process 2) Hot working process]
[0303] In the hot working step, the blank prepared in the preparation step is hot worked to produce an intermediate alloy material. The intermediate alloy material may be, for example, an alloy tube, an alloy plate, or an alloy rod.
[0304] When the intermediate alloy material is an alloy tube, the following processing is performed in the hot working process. First, a cylindrical billet is prepared. A through hole is formed along the central axis of the cylindrical billet by mechanical processing. The cylindrical billet with the through hole is heated. The heated cylindrical billet is subjected to hot extrusion represented by a glass lubricant high-speed extrusion method to manufacture the intermediate alloy material (alloy tube). A hot stamping tube method can also be implemented to replace the hot extrusion method.
[0305] In addition, the alloy tube can be manufactured by piercing and rolling by the Mannesmann method instead of the hot extrusion method. In this case, the cylindrical billet is heated. The heated cylindrical billet is subjected to piercing and rolling by a piercer. In the case of piercing and rolling, the piercing ratio is not particularly limited, and is, for example, 1.0 to 4.0. The pierced and rolled cylindrical billet is further hot-rolled by a continuous tube mill, a reducing mill, a sizing mill, etc. to form a hollow tube billet (alloy tube). The heating temperature of the billet in the hot working process is, for example, 1000 to 1300°C. The cumulative cross-sectional reduction rate in the hot working process is not particularly limited, and is, for example, 20 to 80%. In the case of manufacturing the alloy tube by hot working, the temperature of the hollow tube billet just after the hot working (finishing temperature) is preferably above 800°C.
[0306] When the intermediate alloy material is an alloy plate, the hot working process uses, for example, one or more rolling mills equipped with a pair of work rolls. A billet such as a slab is heated. The heated billet is hot worked to produce an alloy plate. Hot working is, for example, hot forging or hot rolling. The heating temperature of the billet before hot working is, for example, 1000 to 1300°C.
[0307] When the intermediate alloy material is an alloy rod, a tandem rolling mill having a plurality of rolling mill stands arranged in a row is used in the hot working process. Each rolling mill stand has a pair of rolls with a pass formed therein. The heated cylindrical billet is hot-rolled using the tandem rolling mill to produce the alloy rod. The heating temperature of the cylindrical billet before hot rolling is, for example, 1000 to 1300°C.
[0308] [(Process 3) Cold working process]
[0309] The cold working process is implemented as needed. In other words, the cold working process may not be implemented. In the case of implementation, the cold working is implemented after the intermediate alloy material is pickled. In the case where the intermediate alloy material is an alloy tube or an alloy rod, the cold working is, for example, cold drawing. In the case where the intermediate alloy material is an alloy plate, the cold working is, for example, cold rolling. The cold working process can be implemented to achieve the manifestation of recrystallization and graining. The cross-sectional reduction rate in the cold working process is not particularly limited, for example, 10 to 90%.
[0310] [(Step 4) Heat treatment step]
[0311] In the heat treatment process, the intermediate alloy material after the hot working process or the cold working process is heat treated. The heat treatment temperature T (°C) is 900 to 1150°C. The holding time t (minutes) of the heat treatment temperature T is 3 to 30 minutes. After the holding time t has passed, the intermediate alloy material is rapidly cooled.
[0312] In the heat treatment step of step 4, the following condition 1 is also satisfied.
[0313] (Condition 1)
[0314] 75 / (4Z)≤ΣA≤32260Z (1)
[0315] Here, ΣA in equation (1) is defined by equation (2), and Z is defined by equation (3).
[0316] ΣA=(t / 60)×(exp(40000 / (T+273))) / 10 10 (2)
[0317] Z=60C / (1.6Ti+5Nb+100N) (3)
[0318] In the formula (2), the heat treatment temperature (° C.) is substituted for T, and the holding time (minutes) at the heat treatment temperature T is substituted for t.
[0319] In the formula (3), the content of the corresponding element in the chemical composition of the alloy material in terms of mass % is substituted for each element symbol.
[0320] Formula (1) is a condition for reducing the number density of fine nitrogen-containing precipitates at the grain boundaries of the alloy material after manufacture. ΣA defined by formula (2) is an index of the amount of fine nitrogen-containing precipitates within the above-mentioned range of heat treatment temperature T and holding time t. Z defined by formula (3) is an index related to the generation of fine nitrogen-containing precipitates in the chemical composition.
[0321] On the premise that the heat treatment temperature T (°C) is in the range of 900 to 1150°C and the holding time t (minutes) is in the range of 3 to 30 minutes, if the chemical composition (C, Ti, Nb and N content) of the intermediate alloy material to be heat treated, the heat treatment temperature T and the holding time t satisfy the formula (1), then in the alloy material after the heat treatment process, the number density of fine nitrogen-containing precipitates at the grain boundaries is reduced to 20 pieces / μm or less. Therefore, in the heat treatment process, the heat treatment temperature T (°C) and the holding time t (minutes) are adjusted to satisfy the formula (1).
[0322] The alloy material of the present embodiment can be manufactured by the above process. The above manufacturing method is an example of the manufacturing method of the alloy material of the present embodiment. Therefore, the manufacturing method of the alloy material of the present embodiment is not limited to the above manufacturing method. As long as features 1 to 3 are satisfied, the manufacturing method of the alloy material is not limited to the above manufacturing method.
[0323] Example
[0324] The effects of the alloy material of the present embodiment will be further specifically described using examples. The conditions in the following examples are an example of conditions used to confirm the feasibility and effects of the alloy material of the present embodiment. Therefore, the alloy material of the present embodiment is not limited to this example of conditions.
[0325] [Manufacturing of alloy materials]
[0326] Steel ingots having the chemical compositions shown in Table 1-1 and Table 1-2 were produced. The shape of the steel ingot was a cylinder with an outer diameter of 120 mm, and the mass of the steel ingot was 30 kg.
[0327] [Table 1-1]
[0328] Table 1-1
[0329]
[0330] [Table 1-2]
[0331] Table 1-2
[0332]
[0333] The blank portion in Table 1-2 means that the content of the corresponding element is 0% in the significant figures (the value up to the minimum digit) specified in the embodiment. In other words, it means that the corresponding element content is 0% when the mantissa of the significant figures (the value up to the minimum digit) specified in the above embodiment is rounded off.
[0334] For example, the Zr content specified in the present embodiment is specified as a numerical value to the third decimal place. Therefore, for test number 1 in Table 1-2, it means that the measured Zr content is 0% when rounded to the fourth decimal place.
[0335] In addition, rounding means that if the digit next to the specified minimum digit (the fraction) is less than 5, it is discarded, and if it is greater than 5, it is rounded up.
[0336] The produced steel ingot was subjected to hot forging to produce a billet (alloy plate) having a thickness of 30 mm. The heating temperature of the steel ingot during hot forging was 1000 to 1300° C. The produced billet was subjected to hot rolling to produce an intermediate alloy material (alloy plate) having a thickness of 10 mm.
[0337] [Table 2]
[0338] Table 2
[0339]
[0340] The intermediate alloy material was subjected to a heat treatment process. The heat treatment temperature T (°C), the holding time t (minutes) of the heat treatment temperature T, ΣA defined by equation (2), and Z defined by equation (3) in the heat treatment process are shown in Table 2. After the holding time t, the intermediate alloy material was water-cooled to room temperature. Alloy materials (alloy plates) of each test number were manufactured using the above process.
[0341] [Evaluation test]
[0342] The following evaluation tests were carried out using the produced alloy materials.
[0343] (Test 1) Test for measuring the number density of fine nitrogen-containing precipitates at grain boundaries
[0344] (Test 2) Intergranular corrosion resistance evaluation test
[0345] Hereinafter, each evaluation test will be described.
[0346] [(Test 1) Test for measuring the number density of fine nitrogen-containing precipitates at grain boundaries]
[0347] The number density (pieces / μm) of fine nitrogen-containing precipitates at the grain boundaries of the alloy material of each test number was obtained by the method described in the above-mentioned [Method for obtaining the number density of fine nitrogen-containing precipitates]. The obtained number density (pieces / μm) of fine nitrogen-containing precipitates is shown in the "Number density (pieces / μm)" column of Table 2.
[0348] [(Test 2) Intergranular corrosion resistance evaluation test]
[0349] The corrosion rate (g / m 2 The obtained corrosion rate is shown in the "Corrosion rate (g / m 2 hr)” column. The corrosion rate is 0.20 g / m 2 When the viscosity is 0.1 hr or less, it is judged that excellent intergranular corrosion resistance is obtained.
[0350] [Evaluation results]
[0351] Table 2 shows the test results.
[0352] The alloy materials of test numbers 1 to 14 satisfy characteristics 1 to 3. Therefore, the corrosion rate is 0.20 g / m 2 hr or less, excellent intergranular corrosion resistance can be obtained in a strongly oxidizing corrosive environment.
[0353] On the other hand, in test number 15, the C content was too high. Therefore, the corrosion rate was greater than 0.20 g / m 2 ·hr, sufficient intergranular corrosion resistance cannot be obtained.
[0354] In test number 16, the Ni content was too low. Therefore, the corrosion rate was greater than 0.20 g / m 2 ·hr, sufficient intergranular corrosion resistance cannot be obtained.
[0355] In test number 17, the Ni content was too high. Therefore, the corrosion rate was greater than 0.20 g / m 2 ·hr, sufficient intergranular corrosion resistance cannot be obtained.
[0356] In test number 18, the Cr content was too low. Therefore, the corrosion rate was greater than 0.20 g / m 2 ·hr, sufficient intergranular corrosion resistance cannot be obtained.
[0357] In test number 19, the Cr content was too high. Therefore, the corrosion rate was greater than 0.20 g / m 2 ·hr, sufficient intergranular corrosion resistance cannot be obtained.
[0358] In test number 20, the Mo content was too high. Therefore, the corrosion rate was greater than 0.20 g / m 2 ·hr, sufficient intergranular corrosion resistance cannot be obtained.
[0359] In test number 21, the V content was too high. Therefore, the corrosion rate was greater than 0.20 g / m 2 ·hr, sufficient intergranular corrosion resistance cannot be obtained.
[0360] In test number 22, the Ti content was too high. Therefore, the corrosion rate was greater than 0.20 g / m 2 ·hr, sufficient intergranular corrosion resistance cannot be obtained.
[0361] In test numbers 23 and 24, although feature 1 is satisfied, the total content Tx of Ti, Nb, V, Zr, Hf, and Ta is greater than 1.000%. Therefore, the corrosion rate is greater than 0.20 g / m 2 ·hr, sufficient intergranular corrosion resistance cannot be obtained.
[0362] In test numbers 25 and 26, although characteristic 1 is satisfied, the total content Tx of Ti, Nb, V, Zr, Hf, and Ta is less than 0.420%. Therefore, the corrosion rate is greater than 0.20 g / m 2 ·hr, sufficient intergranular corrosion resistance cannot be obtained.
[0363] In test number 27, the C content is too low, the W content is too high, and the N content is too high. Therefore, the corrosion rate is greater than 0.20 g / m 2 ·hr, sufficient intergranular corrosion resistance cannot be obtained.
[0364] In test numbers 28 and 29, although characteristics 1 and 2 are satisfied, ΣA is less than 75 / (4Z) in the heat treatment process. Therefore, characteristic 3 is not satisfied. Therefore, the corrosion rate is greater than 0.20 g / m 2 ·hr, sufficient intergranular corrosion resistance cannot be obtained.
[0365] In test numbers 30 and 31, although characteristics 1 and 2 were satisfied, ΣA was greater than 32260Z in the heat treatment process. Therefore, characteristic 3 was not satisfied. Therefore, the corrosion rate was greater than 0.20 g / m 2 ·hr, sufficient intergranular corrosion resistance cannot be obtained.
[0366] The embodiments of the present disclosure have been described above. However, the above embodiments are merely examples for implementing the present disclosure. Therefore, the present disclosure is not limited to the above embodiments, and the above embodiments can be appropriately modified and implemented within the scope of the present disclosure.
Claims
1. An alloy material, the chemical composition of which is C: 0.005-0.020% by mass, Si: 0.05-0.50%, Mn: 0.05-1.00%, P: 0.030% or less, S: 0.0100% or less, Cu: 1.5-3.0%, Ni: 35.0-50.0%, Cr:20.0~30.0%、 Mo: 2.5-4.0%, Co: 0.01~0.80%, W:0.01~0.30%、 Ca: 0.0050% or less, N:0.001~0.015%、 Al: 0.20% or less, B: 0.0030% or less, Sn: 0.050% or less, Ti: 0.40~0.90%, Nb: 0~0.150%, V:0~0.150%、 Zr:0~0.150%、 Hf: 0~0.150%, Ta: 0 to 0.150%, and The balance is Fe and impurities. The total content of Ti, Nb, V, Zr, Hf and Ta is 0.420-1.000%. The number density of nitrogen-containing precipitates having a major axis of 10 to 100 nm at the grain boundaries of the alloy material is 20 pieces / μm or less.
2. The alloy material according to claim 1, wherein: The chemical composition contains Nb: 0.001-0.150%, V:0.001~0.150%、 Zr:0.001~0.150%、 One or more elements of the group consisting of Hf: 0.001 to 0.150% and Ta: 0.001 to 0.150%.
3. The alloy material according to claim 1 or 2, wherein: The alloy material is an alloy tube.