Negative pole piece, sodium ion battery, power utilization device and application

CN118946985AActive Publication Date: 2024-11-12CONTEMPORARY AMPEREX TECHNOLOGY CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202280094242.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2022-09-14
Publication Date
2024-11-12
Estimated Expiration
2042-09-14

AI Technical Summary

Technical Problem

Existing sodium ion batteries are difficult to meet the needs of high safety and high power at the same time, and traditional methods often lead to power losses when improving safety.

Method used

By using hard carbon as the active material in the negative electrode sheet, its particle size and specific surface area are controlled within a specific range, combining soft carbon, graphite and alloyed negative electrode materials, the thermal stability and reactive activity of the battery are optimized to achieve both Comprehensive performance with high safety and high power.

Benefits of technology

It achieves a balance between high safety and high power performance of sodium ion batteries, improves the battery's high temperature resistance and charge and discharge cycle performance, and ensures both the battery's safety and power performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118946985A_ABST
    Figure CN118946985A_ABST
Patent Text Reader

Abstract

The invention relates to a negative pole piece, a sodium ion battery, a power utilization device and application, the negative pole piece comprises a negative active material, the negative active material comprises hard carbon, and 0.6 mu g / m < = (Dv99 + Dv50) / (2 * B) < = 5 mu g / m; dv99 and Dv50 respectively represent the corresponding particle sizes when the cumulative volume distribution percentage of the negative electrode active material reaches 99% and 50%; b represents the specific surface area of the negative pole piece.
Need to check novelty before this filing date? Find Prior Art

Description

Negative electrode sheet, sodium ion battery, power consumption device and application Technical Field

[0001] The present application relates to the technical field of sodium ion batteries, and further to a negative electrode plate, a sodium ion battery, an electrical device and applications. Background Art

[0002] The statements herein merely provide background information related to the present application and do not necessarily constitute prior art.

[0003] As the new energy industry chain grows and develops, expectations for new energy batteries are increasing. Safety, in particular, is increasingly being considered a primary design consideration. The traditional focus on energy range is gradually shifting towards a focus on high safety. Generally, the most important indicator for evaluating a battery's safety is its high-temperature resistance. The higher the temperature a battery can withstand, the less likely it is to spread to surrounding batteries if it catches fire, significantly improving the safety of the battery pack.

[0004] Sodium-ion batteries (SIBs) utilize the intercalation and deintercalation of sodium ions between the positive and negative electrodes to achieve charge and discharge. Compared to the lithium in lithium-ion batteries, sodium resources are more widely distributed, more abundant, and significantly less expensive. Therefore, SIBs are considered a next-generation electrochemical system with the potential to replace lithium-ion batteries. The safety of SIBs is a current research priority, but improving safety often results in a loss of power.

[0005] Therefore, it is urgent to develop sodium-ion batteries that meet both high safety and high power requirements.

[0006] Summary of the Invention

[0007] In view of the above problems, the present application provides a negative electrode plate that can meet the comprehensive requirements of high safety and high power, and is suitable for use in sodium ion batteries. Also provided are a sodium ion battery including the negative electrode plate, an electrical device, and the use of the negative electrode plate in the preparation of a sodium ion battery.

[0008] In a first aspect, the present application provides a negative electrode plate, the negative electrode plate comprising a negative electrode active material, the negative electrode active material comprising hard carbon;

[0009] The negative electrode sheet also meets the following conditions: 0.6 μg / m ≤ (D v 99+D v 50) / (2×B)≤5μg / m; where D v 99 represents the particle size corresponding to when the cumulative volume distribution percentage of the negative electrode active material reaches 99%, in μm; D v50 represents the particle size corresponding to when the cumulative volume distribution percentage of the negative electrode active material reaches 50%, in μm; B represents the specific surface area of ​​the negative electrode sheet, in m 2 / g.

[0010] It is generally believed that the main factors affecting battery safety include the negative electrode, positive electrode, electrolyte, etc. The inventors of the present application have found through a large number of experimental studies that the particle size of the negative electrode active material will affect the safety of the battery. In particular, they have found that the large-size particles have a very significant impact on battery safety. The inventors of the present application have found through a large number of exploratory studies that the larger the particle size of the negative electrode active material, the higher the temperature at which its thermal decomposition reaction begins, and the higher the temperature it can withstand. Moreover, the larger the particle size, the smaller the specific surface area of ​​the negative electrode active material, the slower the reaction rate, and the safer the battery, but it will result in battery power loss. By controlling the particle size of the negative electrode active material and the specific surface area of ​​the negative electrode sheet within a certain range, the battery can have a higher starting reaction temperature while avoiding adverse effects on the reaction activity rate as much as possible.

[0011] In the present application, the negative electrode active material includes hard carbon, which has a higher pyrolysis carbonization temperature, which is conducive to better improving the heat resistance temperature and reducing the heat generation. In addition, the internal interlayer spacing of the hard carbon structure is large, the porosity is high, more active ions can be embedded, and the structure has significantly low expansion, which is conducive to improving the battery's charge and discharge cycle performance and battery life. On this basis, by comprehensively controlling the large particle size in the negative electrode active material and the specific surface area of ​​the negative electrode sheet, the comprehensive advantages of both high safety and high power are achieved. Furthermore, (D v 99+D v 50) / 2 can characterize the large particle size. This feature and the specific surface area B of the negative electrode are used to define the thermal stability coefficient (D v 99+D v 50) / (2×B), by adjusting the thermal stability coefficient of the negative electrode sheet within a suitable range, the battery can be endowed with the characteristics of high safety and high power, and bring excellent high temperature resistance.

[0012] In some embodiments of the present application, the negative electrode active material satisfies the following conditions: 5 μm ≤ (D v 99+D v 50) / 2≤18μm;

[0013] Optionally, the negative electrode active material meets the following conditions: 6 μm ≤ (D v 99+D v 50) / 2≤15μm;

[0014] Optionally, the negative electrode active material meets the following conditions: 7 μm ≤ (D v99+D v 50) / 2≤12μm;

[0015] Optionally, the negative electrode active material meets the following conditions: 8 μm ≤ (D v 99+D v 50) / 2≤10μm.

[0016] By rationally controlling the large particles in the negative electrode active material within a more appropriate range, it is more convenient to combine the fine control of the specific surface area of ​​the negative electrode active material to better achieve the advantages of high battery safety and high power.

[0017] In some embodiments of the present application, the negative electrode sheet satisfies the following conditions: 0.7 μg / m ≤ (D v 99+D v 50) / (2×B)≤5μg / m;

[0018] Optionally, the negative electrode sheet meets the following conditions: 0.8 μg / m ≤ (D v 99+D v 50) / (2×B)≤4.2μg / m.

[0019] By further controlling the thermal stability coefficient of the electrode within the above range, it is beneficial to better balance the impact of large particle size on battery safety and the impact of the specific surface area of ​​the negative electrode active material on battery power, thereby better balancing high battery safety and high power.

[0020] In some embodiments of the present application, the negative electrode active material further satisfies the following conditions: (x·D v 10)≤D v 50≤(y·D v 99); wherein x=2.6 and y=0.4;

[0021] Optionally, x=4, and y=0.3.

[0022] By rationally controlling the D v 50 relative to D v 10. D v The ratio x, y of 99 can better ensure that the small particles and large particles in the negative electrode active material have appropriate particle sizes and contents, better avoid the battery power loss caused by large particles, and maintain a higher power as much as possible while improving battery safety.

[0023] In some embodiments of the present application, the negative electrode plate meets the following conditions: 30 mAh·m -2 ≤C / B≤140mAh·m -2 ; Wherein, C is the gram capacity of the negative electrode;

[0024] Optionally, 40mAh·m -2 ≤C / B≤125mAh·m -2 .

[0025] The inventors of this application have discovered that the C / B value of the negative electrode sheet can, to a certain extent, reflect the reactivity of the negative electrode active material in the negative electrode sheet. By synergistically controlling the gram capacity and specific surface area of ​​the negative electrode sheet, it is beneficial to better control the reaction rate during battery thermal runaway, which helps further improve battery safety. Controlling the negative electrode sheet to have an appropriate gram capacity, thereby controlling the amount of active sodium ion embedded, so that the reaction rate is moderate, and controlling the specific surface area of ​​the negative electrode sheet within a relatively suitable range, so that the ion deintercalation path and polarization of the battery active material are moderate, ensuring the battery's power performance.

[0026] In some embodiments of the present application, the gram capacity C of the negative electrode sheet satisfies the following conditions: 300 mAh / g≤C≤350 mAh / g,

[0027] Optionally, the gram capacity C of the negative electrode plate satisfies the following condition: 310 mAh / g≤C≤340 mAh / g.

[0028] By controlling the negative electrode to have a more appropriate gram capacity, the amount of active sodium ions embedded can be controlled appropriately, so that the reaction rate during thermal runaway of the battery is moderate and the battery safety is improved.

[0029] In some embodiments of the present application, the B is selected from 2.5m 2 / g~10m 2 / g;

[0030] Optionally, the B is selected from 3m 2 / g~7m 2 / g.

[0031] By controlling the specific surface area of ​​the negative electrode within a more appropriate range, the ion deintercalation path and polarization of the battery active material are moderate, which is more conducive to the battery power performance.

[0032] In some embodiments of the present application, the first exothermic reaction peak position T of the differential scanning calorimetry analysis of the negative electrode sheet satisfies 150° C. ≤ T ≤ 180° C.; wherein the test conditions of the differential scanning calorimetry analysis include: nitrogen atmosphere, heating rate of 10° C. / min;

[0033] Optionally, 170°C ≤ T ≤ 180°C.

[0034] By controlling the first exothermic reaction peak position T of the differential scanning calorimetry (DSC) analysis of the negative electrode sheet within a more appropriate range, it is more conducive to further improving battery safety.

[0035] In some embodiments of the present application, the negative electrode active material further comprises one or more of soft carbon, graphite and alloyed negative electrode;

[0036] Optionally, the mass proportion of hard carbon in the negative electrode active material is ≥50%;

[0037] Optionally, the mass proportion of hard carbon in the negative electrode active material is ≥90%.

[0038] Introducing one or more other active materials, such as soft carbon, graphite, and alloyed negative electrodes, based on the active materials of the negative electrode, can leverage the advantages of these materials to provide the battery with better overall performance. For example, soft carbon has a low and stable charge and discharge potential platform, large charge and discharge capacity, high efficiency, and good cycle performance. Graphite, for example, has advantages such as good conductivity, high initial efficiency, and wide availability. For example, alloyed negative electrodes offer advantages such as good power performance and high energy density.

[0039] In a second aspect, the present application provides a sodium ion battery, which includes a positive electrode sheet, the negative electrode sheet described in the first aspect of the present application, a separator and an electrolyte, wherein the separator is arranged between the positive electrode sheet and the negative electrode sheet.

[0040] The sodium ion battery prepared using the negative electrode sheet of the first aspect of the present application has the comprehensive advantages of high safety and high power.

[0041] In some embodiments of the present application, the electrolyte comprises an electrolyte sodium salt, and the electrolyte sodium salt includes one or more sodium salts of sodium hexafluorophosphate, sodium perchlorate, sodium tetrafluoroborate, sodium trifluoromethanesulfonate, sodium bis(trifluoromethanesulfonyl)imide, sodium bis(trifluoromethanesulfonyl)imide, sodium trifluoromethanesulfonate, and sodium difluorophosphate;

[0042] Optionally, the electrolyte sodium salt includes one or more sodium salts of sodium hexafluorophosphate, sodium perchlorate, sodium tetrafluoroborate and sodium trifluoromethanesulfonate.

[0043] In some embodiments of the present application, the electrolyte further comprises an organic solvent, and the organic solvent comprises one or more of ethylene carbonate (EC), dimethyl carbonate (DMC), diethyl carbonate (DEC), ethyl methyl carbonate (EMC), propylene carbonate (PC), ethers such as ethylene glycol dimethyl ether (DME), tetrahydrofuran (THF), 2-methyltetrahydrofuran (2-MTHF), methyl acetate, ethyl propionate, fluoroethylene carbonate, ethyl ether, diethylene glycol dimethyl ether, triethylene glycol dimethyl ether, tetraethylene glycol dimethyl ether and methyl tert-butyl ether;

[0044] Optionally, the organic solvent includes one or more of ethylene carbonate, dimethyl carbonate, diethyl carbonate, ethyl methyl carbonate, propylene carbonate, ethylene glycol dimethyl ether, tetrahydrofuran, and 2-methyltetrahydrofuran. The sodium salt has a high degree of solvation in the solvent and high electrical conductivity, which is conducive to film formation and improves battery power.

[0045] In some embodiments of the present application, the electrolyte further includes an additive, and the additive includes one or more of fluoroethylene carbonate (FEC), vinylene carbonate (VC), vinyl sulfate (DTD), 1,3-propane sultone (PS), 1,3-propenyl-sultone (PST), succinic anhydride (SA), lithium difluorooxalatoborate (LiDFOB), lithium difluorobis(oxalatophosphate) (LiDFOP), tris(trimethylsilyl) phosphate (TMSP), tris(trimethylsilyl) borate (TMSB), ethylene carbonate, propylene carbonate, ethyl methyl carbonate, diethyl carbonate, dimethyl carbonate, dipropyl carbonate, methylpropyl carbonate, ethylpropyl carbonate, butylene carbonate, methyl formate, methyl acetate, ethyl acetate, propyl acetate, methyl propionate, ethyl propionate, propyl propionate, methyl butyrate, ethyl butyrate, 1,4-butyrolactone, cyclopentane, dimethyl sulfone, methyl ethyl sulfone and diethyl sulfone;

[0046] Optionally, the additives include one or more of fluoroethylene carbonate, vinylene carbonate, vinyl sulfate, 1,3-propane sultone, 1,3-propenyl sultone, succinic anhydride, lithium difluorooxalatoborate, lithium difluorobisoxalatophosphate, tris(trimethylsilyl)phosphate, and tris(trimethylsilyl)borate. Selecting the right additives can help the battery quickly form a solid electrolyte interface (SEI) film, increase the thickness and stability of the SEI film, and improve battery safety.

[0047] In some embodiments of the present application, the negative electrode sheet satisfies the following conditions: 0.5°C ≤ T×M ≤ 6°C; wherein T and M are the first exothermic reaction peak position and the first stage weight loss rate of the negative electrode sheet in differential scanning calorimetry (DSC) analysis, respectively. The test conditions of the differential scanning calorimetry analysis include: nitrogen atmosphere, heating rate of 10°C / min;

[0048] Optionally, 0.65°C ≤ T×M ≤ 5.2°C;

[0049] Optionally, 0.75°C≤T×M≤4.5°C.

[0050] The inventors of this application speculate that T×M can, to a certain extent, reflect the tolerance of the negative electrode plate at high temperatures. The particle size of the negative electrode active material affects the starting temperature of the reaction exotherm. The larger the particles, the higher the temperature at which the reaction starts, and the safer the corresponding battery system. However, when the particles are larger, it is not good for battery power. Therefore, how to balance safety and power is crucial for the preparation of batteries with high comprehensive performance. By shifting the position (T) of the first exothermic reaction peak of the differential scanning calorimetry (DSC) analysis of the negative electrode plate to a high temperature, the decomposition reaction temperature (corresponding to M) of the solid electrolyte interface (SEI) film can be increased, which is beneficial to increase the thickness of the SEI film, thereby achieving the effect of further improving safety.

[0051] In some embodiments of the present application, the first-stage weight loss rate M of the differential scanning calorimetry analysis of the negative electrode sheet satisfies the following conditions: 0.25%≤M≤3.5%; wherein the test conditions of the differential scanning calorimetry analysis include: nitrogen atmosphere, heating rate of 10°C / min;

[0052] Optionally, 0.5%≤M≤2.5%;

[0053] Optionally, 0.65%≤M≤2.0%.

[0054] By controlling the first-stage weight loss rate M of the differential scanning calorimetry analysis of the negative electrode sheet within a more appropriate range, the SEI interface stability can be improved, which is beneficial to improving battery safety and achieving better ion transport and charge and discharge performance.

[0055] In some embodiments of the present application, the positive electrode plate includes a positive electrode active material, the positive electrode active material includes a positive electrode active material containing sodium ions, and the positive electrode active material containing sodium ions includes one or more of Prussian blue compounds, sodium transition metal oxides and polyanion compounds.

[0056] The appropriate positive electrode active material can be flexibly selected, making sodium-ion batteries more selective and applicable.

[0057] In a third aspect, the present application provides an electrical device comprising the sodium ion battery described in the second aspect of the present application.

[0058] The electrical device prepared using the sodium ion battery provided in the second aspect of the present application not only has high safety, but also has high power, and can meet the comprehensive needs of consumers for high safety and high performance.

[0059] The details of one or more embodiments of the present application are set forth in the following drawings and description. Other features, objects, and advantages of the present application will become apparent from the description, drawings, and claims. BRIEF DESCRIPTION OF THE DRAWINGS

[0060] In order to better describe and illustrate the embodiments or examples of the applications disclosed herein, reference may be made to one or more of the accompanying drawings. The additional details or examples used to describe the accompanying drawings should not be considered to limit the scope of the disclosed applications, the embodiments or examples currently described, and any of the best modes currently understood for these applications. Moreover, the same reference numerals are used throughout the drawings to represent the same components. In the drawings:

[0061] FIG1 is a graph showing an exothermic curve and a thermogravimetric curve of a differential scanning calorimetry (DSC) test of a negative electrode sheet in one embodiment of the present application, wherein Mass (%) represents the weight loss rate and DTG (% / min) represents the heat release rate;

[0062] FIG2 is a schematic diagram of a sodium ion battery according to an embodiment of the present application;

[0063] FIG3 is an exploded view of the sodium ion battery according to an embodiment of the present application shown in FIG2 ;

[0064] FIG4 is a schematic diagram of an electrical device using a sodium ion battery as a power source according to an embodiment of the present application.

[0065] Description of reference numerals:

[0066] 5. Sodium-ion battery; 51. Shell; 52. Electrode assembly; 53. Cover plate; 6. Electrical device. DETAILED DESCRIPTION

[0067] Below, the embodiments of the negative electrode sheet, sodium ion battery, electrical device and application of the present application are described in detail with appropriate reference to the accompanying drawings. However, there may be cases where unnecessary detailed descriptions are omitted. For example, there are cases where detailed descriptions of well-known matters and repeated descriptions of actually the same structure are omitted. This is to avoid the following description from becoming unnecessarily lengthy and to facilitate the understanding of those skilled in the art. In addition, the drawings and the following description are provided for those skilled in the art to fully understand the present application and are not intended to limit the subject matter described in the claims.

[0068] " range " disclosed in the present application is limited in the form of lower limit and upper limit, and given range is limited by selecting a lower limit and an upper limit, and the selected lower limit and upper limit define the boundary of special range. The scope limited in this way can be to include end value or not include end value, and can be arbitrarily combined, that is, any lower limit can form a range with any upper limit combination. For example, if the scope of 60-120 and 80-110 is listed for specific parameters, it is understood that the scope of 60-110 and 80-120 is also expected. In addition, if the minimum range value 1 and 2 are listed, and if the maximum range value 3,4 and 5 are listed, then the following range can all be expected: 1-3, 1-4, 1-5, 2-3, 2-4 and 2-5. In this application, unless otherwise specified, the numerical range " ab " represents the abbreviation of any real number combination between a and b, wherein a and b are all real numbers. For example, a numerical range of "0-5" indicates that all real numbers between "0-5" are listed herein, and "0-5" is simply an abbreviation for these numerical combinations. Furthermore, when a parameter is expressed as an integer ≥ 2, this is equivalent to disclosing that the parameter is, for example, an integer of 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, etc.

[0069] Unless otherwise specified, all embodiments and optional embodiments of the present application can be combined with each other to form a new technical solution.

[0070] Unless otherwise specified, all steps of the present application may be performed sequentially or randomly, preferably sequentially. For example, the method includes steps (a) and (b), which means that the method may include steps (a) and (b) performed sequentially, or may include steps (b) and (a) performed sequentially. For example, the method may further include step (c), which means that step (c) may be added to the method in any order, for example, the method may include steps (a), (b) and (c), or may include steps (a), (c) and (b), or may include steps (c), (a) and (b), etc.

[0071] Unless otherwise specified, the terms "include" and "comprising" used in this application may be open-ended or closed-ended. For example, "include" and "comprising" may mean that other components not listed may also be included or that only the listed components are included.

[0072] Unless otherwise specified, the term "or" is inclusive in this application. For example, the phrase "A or B" means "A, B, or both A and B." Furthermore, the condition "A or B" is satisfied by any of the following conditions: A is true (or exists) and B is false (or does not exist); A is false (or does not exist) and B is true (or exists); or both A and B are true (or exist).

[0073] In this application, the technical features described in an open manner include closed technical solutions composed of the listed features, and also include open technical solutions containing the listed features.

[0074] In this application, "multiple", "multiple", "several", "multiple times", etc., unless otherwise specified, refer to a quantity greater than or equal to 2. For example, "one or more" means one or more than or equal to two.

[0075] As used herein, "combination thereof", "any combination thereof", "any combination thereof" and the like include all suitable combinations of any two or more of the listed items.

[0076] Herein, the “suitable” mentioned in “suitable combination”, “suitable method”, “any suitable method”, etc. shall be based on the technical solution that can implement the present application.

[0077] Herein, the terms "preferred," "better," "more preferred," and "suitable" are used solely to describe preferred implementations or examples and should not be construed as limiting the scope of protection of this application. If multiple "preferred" terms appear in a technical solution, each "preferred" term is considered independent unless otherwise specified and there are no contradictions or mutual constraints.

[0078] In this application, "further", "further", "particularly" and the like are used for descriptive purposes to indicate differences in content, but should not be understood as limiting the scope of protection of this application.

[0079] In this application, the terms "first," "second," "third," "fourth," etc. in "the first aspect," "the second aspect," "the third aspect," "the fourth aspect," etc. are used for descriptive purposes only and should not be understood as indicating or implying relative importance or quantity, nor should they be understood as implicitly indicating the importance or quantity of the indicated technical features. Furthermore, "first," "second," "third," "fourth," etc. serve only as non-exhaustive enumeration and description, and should be understood not to constitute a closed-ended limitation on quantity.

[0080] In this application, the term "room temperature" generally refers to 4°C to 35°C, preferably 20°C ± 5°C. In some embodiments of this application, room temperature refers to 20°C to 30°C.

[0081] In this application, when referring to a data range, if the unit is only after the right endpoint, it means that the units of the left and right endpoints are the same. For example, 3~5h or 3-5h both mean that the units of the left endpoint "3" and the right endpoint "5" are both hours.

[0082] The weights of the relevant components mentioned in the examples of this application may not only refer to the content of each component, but also represent the weight ratio between the components. Therefore, as long as the content of the relevant components is proportionally enlarged or reduced according to the examples of this application, it is within the scope disclosed in the examples of this application. Furthermore, the weights mentioned in the examples of this application may be units commonly known in the chemical industry, such as μg, mg, g, and kg.

[0083] It is generally believed that the main factors affecting battery safety include the negative electrode, positive electrode, electrolyte, etc. After a large number of experimental studies, the inventors of the present application found that the particle size of the negative electrode active material will affect the safety of the battery. In particular, they found that the large-size particles have a very significant impact on battery safety. After a large number of exploratory studies, the inventors of the present application found that the larger the particle size of the negative electrode active material, the higher the temperature at which its thermal decomposition reaction begins and the higher the temperature it can withstand. Moreover, the larger the particle size, the smaller the specific surface area of ​​the negative electrode active material, the slower the reaction rate, and the safer the battery, but it will result in battery power loss. Therefore, how to balance the safety requirements and power requirements of the battery is crucial for preparing batteries with excellent comprehensive performance.

[0084] For different types of batteries, the parameters of the negative electrode materials, such as particle size and specific surface area, vary greatly. This leads to the fact that when designing the particle size, specific surface area and related parameters of different types of batteries, the parameters between different types of batteries often vary greatly, and special design is required for each battery type. For example, the materials or parameters suitable for lithium-ion batteries may not be suitable for sodium-ion batteries. For example, the negative active material of sodium-ion batteries in traditional technology usually uses hard carbon. v 50 is relatively small, about a few microns (such as 5-6 μm), and the corresponding specific surface area is relatively large; while lithium-ion batteries are more commonly used in traditional technologies. Graphite negative electrode, D v 50 is usually between a dozen and several dozen microns, and its specific surface area is relatively small.

[0085] In response to the above-mentioned common technical problems, in a first aspect, the present application provides a negative electrode plate, wherein the negative electrode plate includes a negative electrode active material, and the negative electrode active material includes hard carbon;

[0086] The negative electrode sheet also meets the following conditions: 0.6 μg / m ≤ (D v 99+D v 50) / (2×B)≤5μg / m; where D v 99 represents the particle size corresponding to when the cumulative volume distribution percentage of the negative electrode active material reaches 99%, in μm; D v50 represents the particle size corresponding to when the cumulative volume distribution percentage of the negative electrode active material reaches 50%, in μm; B represents the specific surface area of ​​the negative electrode sheet, in m 2 / g.

[0087] In the context of this application, the volume cumulative distribution particle size D can be used v N (where N represents any value selected from 0 to 100) is used to characterize the particle size of the material, which refers to the particle size corresponding to when the cumulative volume distribution percentage of the material reaches N%. The particle size is less than or equal to D v The volume percentage of N is N%. v N can be obtained from the volume cumulative distribution curve of the material particle size. If there is no other explanation, the volume cumulative distribution curve starts from zero from the small particle size side. v 99.D v 90.D v 50. D v 10 as an example, D v 99 refers to the particle size corresponding to when the cumulative volume distribution percentage of the material reaches 99%; D v 90 refers to the particle size corresponding to when the cumulative volume distribution percentage of the material reaches 90%; D v 50 refers to the particle size corresponding to when the cumulative volume distribution percentage of the material reaches 50%; D v 10 refers to the particle size corresponding to the cumulative volume distribution percentage of the material reaching 10%. v For example, 50 means that the particle size of 50% of the material volume is less than or equal to D v 50, and the particle size of 50% of the material volume is larger than D v 50. D v For example, 90% of the particles in the material volume have a particle size less than or equal to D v 90, and the particle size of 10% of the material volume is larger than D v 90. D v For example, 10 means that the particle size of 10% of the material volume is less than or equal to D v 10, and the particle size of 90% of the material volume is larger than D v 10. Those skilled in the art will understand that v 99.D v 90.D v 50. D v The particle size distribution of the particle size is 10, and can be measured using instruments and methods known in the art. For example, it can be conveniently measured using a laser particle size analyzer, such as the Mastersizer 2000E laser particle size analyzer or the LS-909 laser particle size analyzer (Omega), manufactured by Malvern Instruments Ltd., UK.

[0088] In the context of this application, (D v 99+D v 50) / 2 can be used to characterize the large particle size in the material and can be recorded as the "average particle size of large particles". v 99 and D v The average value of 50 reflects the particle size of the large particles in the material. A larger value indicates a larger particle size of the large particles in the material. According to the inventors' research, larger particle sizes in the negative electrode active material are associated with higher battery thermal runaway onset temperatures and improved battery safety.

[0089] The negative electrode sheet of the first aspect of the present application includes a negative electrode current collector and a negative electrode film layer provided on at least one surface of the negative electrode current collector, wherein the negative electrode film layer includes a negative electrode active material.

[0090] In the context of this application, unless otherwise specified, the specific surface area B of the negative electrode sheet refers to the specific surface area of ​​the negative electrode film layer (i.e., not considering the contribution of the negative electrode current collector). Further, the specific surface area B of the negative electrode sheet refers to the ratio of the sum of the external surface area of ​​the negative electrode film layer and the internal surface area of ​​the internal pores to the weight of the negative electrode film layer, and the unit can be m 2 / g. The definition of the specific surface area B of the negative electrode sheet can refer to the standard "GB / T 19587-2004".

[0091] In the present application, the specific surface area B of the negative electrode plate can be measured using instruments and methods known in the art. For example, it can be tested using a nitrogen adsorption specific surface area analysis test method and calculated using the BET (Brunauer Emmett Teller) method. The nitrogen adsorption specific surface area analysis test can be performed using a Tri Star II specific surface and pore analyzer from Micromeritics, USA. The test steps can refer to GB / T19587-2004. In some embodiments, the specific surface area of ​​the negative electrode sheet can be tested as follows: a sample to be tested is selected, which can be a directly prepared negative electrode sheet or a negative electrode sheet disassembled from a battery (in this case, it needs to be cleaned with anhydrous ethanol to remove the electrolyte and dried in a vacuum drying oven at 60°C for 1-2 hours); then, nitrogen or argon is used as the adsorption gas, and an adsorption-desorption curve with a relative pressure P / P0 of 0-0.99 is plotted using a surface and porosity analyzer. The specific surface area of ​​the negative electrode sheet is calculated using the BET method, where P represents the equilibrium adsorption pressure and P0 represents the saturated vapor pressure. When the test sample is a negative electrode active material, the negative electrode active material powder can be prepared as follows: The specific surface area of ​​the active material can be tested as follows: the negative electrode active material is dried in a vacuum drying oven at 200°C for 2 hours; then the specific surface area of ​​the negative electrode active material is tested using the above-mentioned gas adsorption test method. In this application, the larger the specific surface area of ​​the negative electrode sheet, the slower the battery thermal runaway reaction rate and the better the battery safety.

[0092] In some embodiments, the particle size and specific surface area of ​​the negative electrode active material can be obtained by the following control or screening methods (but not limited to these methods): Method 1, by selecting different negative electrode material precursors such as wheat straw, coconut shell and asphalt to prepare materials with different specific surface areas; Method 2, by setting different crushing times and rotation speeds and filter screens during the synthesis of the negative electrode material to obtain negative electrode materials with different particle sizes.

[0093] In the context of this application, (D v 99+D v 50) / (2×B) is defined as the electrode thermal stability coefficient, denoted as S. This parameter can reflect the thermal stability of the electrode. When the value is controlled within a reasonable range (0.6μg / m2~5μg / m2), the electrode can withstand high temperatures and the thermal runaway of the electrode is less severe.

[0094] By controlling the particle size of the negative electrode active material and the specific surface area of ​​the negative electrode sheet within a certain range, the battery can have a higher starting reaction temperature while minimizing the adverse effect on the reaction activity rate. In this application, by comprehensively controlling the large particle size of the negative electrode active material and the specific surface area of ​​the negative electrode sheet, the comprehensive advantages of high safety and high power are achieved. Further, (Dv 99+D v 50) / 2 characterizes the large particle size, and this feature is used together with the specific surface area B of the negative electrode to define the thermal stability coefficient (D v 99+D v 50) / (2×B), by adjusting the thermal stability coefficient of the electrode within a suitable range, the battery can be given high safety and high power characteristics, bringing excellent high temperature resistance.

[0095] Furthermore, the negative electrode active material includes hard carbon. Hard carbon has a high pyrolysis carbonization temperature, which helps improve heat resistance and reduce heat generation. Furthermore, hard carbon has a large interlayer spacing and high porosity, allowing for the embedding of a large number of metal ions. This significantly reduces structural expansion, which helps improve the battery's charge-discharge cycle performance and battery life.

[0096] In this application, the larger the particle size of the negative electrode active material, the higher the battery thermal runaway starting temperature and the better the battery safety; the larger the specific surface area of ​​the negative electrode sheet, the slower the battery thermal runaway reaction rate and the better the battery safety. However, if (D v 99+D v 50) / 2 is too large, which will result in lower battery power and energy density. v 99+D v When (D 50) / (2×B) is less than 0.6μg / m, the particle size is too small to increase the reaction temperature of the material or the specific surface area is too large to cause the thermal runaway rate to be too fast; when (D v 99+D v When 50) / (2×B) is greater than 5 μg / m, the particle size of the large particles is too large, resulting in too few normal active sites in the battery, which will deteriorate the charge and discharge performance of the battery.

[0097] In some embodiments, the negative electrode active material satisfies the following conditions: 5 μm ≤ (D v 99+D v 50) / 2≤18μm.

[0098] In some embodiments, the negative electrode active material satisfies the following conditions: 6 μm ≤ (D v 99+D v 50) / 2≤15μm.

[0099] In some embodiments, the negative electrode active material satisfies the following conditions: 7 μm ≤ (D v 99+D v 50) / 2≤12μm.

[0100] In some embodiments, the negative electrode active material satisfies the following conditions: 8 μm ≤ (Dv 99+D v 50) / 2≤10μm.

[0101] In some embodiments, the negative electrode active material (D v 99+D v 50) / 2 can also be selected from any one of the following sizes or any two of the following intervals: 5μm, 5.2μm, 5.4μm, 5.5μm, 5.6μm, 5.8μm, 6μm, 6.2μm, 6.4μm, 6.5μm, 6.6μm, 6.8μm, 7μm, 7.2μm, 7.4μm, 7.5μm, 7.6μm, 7.8μm, 8μm, 8 .2μm, .4μm, 8.5μm, 8.6μm, .8μm, 9μm, 9.5μm, 10μm, 10.5μm, 11μm, 11.5μm, 12μm, 1 2.5μm, 13μm, 13.5μm, 14μm, 15μm, 15.5μm, 16μm, 16.5μm, 17μm, 17.5μm, 17.7μm, etc.

[0102] By rationally controlling the large particles in the negative electrode active material within a more appropriate range, it is more convenient to combine the fine control of the specific surface area of ​​the negative electrode active material to better achieve the advantages of high battery safety and high power.

[0103] In some embodiments, the negative electrode sheet satisfies the following conditions: 0.7 μg / m ≤ (D v 99+D v 50) / (2×B)≤5μg / m.

[0104] In some embodiments, the negative electrode sheet satisfies the following conditions: 0.8 μg / m ≤ (D v 99+D v 50) / (2×B)≤4.2μg / m.

[0105] In some embodiments, the negative electrode sheet (D v 99+D v 50) / (2×B) can also be selected from the intervals consisting of any one or any two of the following: 0.6μg / m, 0.7μg / m, 0.8μg / m, 0.9μg / m, 1μg / m, 1.2μg / m, 1.4μg / m, 1.5μg / m, 1.6μg / m, 1.8μg / m, 2μg / m, 2.2μg / m, 2.5μg / m, 2.6μg / m, 2.8μg / m, 3μg / m, 3.5μg / m, 4μg / m, 4.5μg / m, 5μg / m, 5.5μg / m, 6μg / m, etc.

[0106] By further controlling the thermal stability coefficient of the pole piece (Dv 99+D v 50) / (2×B) is within a more appropriate range, which is conducive to better balancing the impact of large particle size on battery safety and the impact of the specific surface area of ​​the negative electrode sheet on battery power, thereby better taking into account both high battery safety and high power.

[0107] In some embodiments of the present application, the negative electrode active material further satisfies the following conditions: (x·D v 10)≤D v 50≤(y·D v 99); wherein x=2.6 and y=0.4;

[0108] Optionally, x=3, and y=0.3.

[0109] By rationally controlling the D v 50 relative to D v 10. D v The ratio x and y of 99 can better ensure that the small and large particles in the negative electrode active material have appropriate particle sizes and contents, better avoid the energy density loss caused by large particles, and maintain as high energy density as possible while improving battery safety. When x is large, the small particle size is small and the specific surface area is large, which may reduce the temperature tolerance of the material; when x is small, the small particle size is close to the average particle size, which may lead to insufficient filling of the pores between the particles and low electrode energy density. When y is large, the large particles are small and may not play the role of particles filling the pores, and the electrode energy density is low; when y is small, the large particles are too large and the ion shuttle path is long, which may cause the battery power to decrease.

[0110] In some embodiments of the present application, the negative electrode plate meets the following conditions: 30 mAh·m -2 ≤C / B≤140mAh·m -2 ; Wherein, C is the gram capacity of the negative electrode plate.

[0111] In some embodiments, 40 mAh·m -2 ≤C / B≤125mAh·m -2 .

[0112] In some embodiments, the C / B of the negative electrode sheet can also be selected from any one or two of the following intervals: 30 mAh·m -2 、35mAh·m -2 、40mAh·m -2 、45mAh·m -2 、50mAh·m -2 、55mAh·m - 2、60mAh·m -2 、65mAh·m -2 、70mAh·m -2 、75mAh·m -2 、80mAh·m -2 、85mAh·m -2 、90mAh·m -2 、95mAh·m -2 、100mAh·m -2 、105mAh·m -2 、110mAh·m -2 、115mAh·m - 2 、120mAh·m -2 、125mAh·m -2 、130mAh·m -2 、135mAh·m -2 、140mAh·m -2 wait.

[0113] The inventors of this application have discovered that the C / B value of the negative electrode sheet can, to a certain extent, reflect the reactivity of the negative electrode sheet. By synergistically controlling the gram capacity and specific surface area of ​​the negative electrode sheet, it is beneficial to better control the reaction rate during thermal runaway of the battery, which helps to further improve battery safety. Controlling the negative electrode sheet to have an appropriate gram capacity, thereby controlling the amount of active sodium ion embedded, so that the reaction rate is moderate, and controlling the specific surface area of ​​the negative electrode sheet within a relatively suitable range, so that the ion deintercalation path and polarization of the battery active material are moderate, ensuring the battery's power performance.

[0114] When C / B is low (e.g. less than 30mAh·m -2 When C / B is too large (e.g. greater than 140mAh·m -2 When the negative electrode active material has a high gram capacity, the amount of active ion embedding is too large. Once it gets out of control, the intensity is too large, or the electrode surface area is very small, the material particles are large, the de-embedding path of the battery active material ions is too long, the polarization is too large, and the battery power performance is relatively poor.

[0115] In some embodiments of the present application, the gram capacity C of the negative electrode sheet satisfies 300 mAh / g≤C≤350 mAh / g.

[0116] In some embodiments, the gram capacity C of the negative electrode sheet satisfies 310 mAh / g≤C≤340 mAh / g.

[0117] In some embodiments, the gram capacity C of the negative electrode plate can also be selected from any one or two of the following intervals: 300mAh / g, 305mAh / g, 310mAh / g, 315mAh / g, 320mAh / g, 325mAh / g, 330mAh / g, 335mAh / g, 340mAh / g, 345mAh / g, 350mAh / g, etc.

[0118] In this application, the gram capacity of the negative electrode plate can be measured with reference to the WI-ATC-2014 gram capacity test details. Plate processing before testing: It can be a directly prepared negative electrode plate, or it can be a negative electrode plate disassembled from the battery (in this case, it is necessary to use anhydrous ethanol to clean and remove the electrolyte, and then dry it in a vacuum drying oven at 60°C for 2 hours). Then use a sheet punching machine to punch out multiple small discs, weigh the weight of each small disc and take the average value W1, then clean and dry the active material on the small disc, weigh the weight of the small disc substrate and take the average value W2, the weight of the active material (W1-W2), when the negative electrode slurry is coated on both sides, the weight of the negative electrode active material on one side of the substrate of each small disc is (W1-W2) / 2. According to the capacity C0 of the small disc, the gram capacity is calculated as C0 / (W1-W2), unit mAh / g. In some embodiments, C0 can be measured using the following method: A small disc produced by a punching machine is used. The active material layer on one side of the substrate is wiped clean with alcohol. An electrolyte is then injected to form a button cell. The cell is then charged and discharged between 0V and 2V using a 0.1C current. The capacity after a full charge to 2V and a full discharge to 0V is the C0 (in mAh).

[0119] By controlling the negative electrode to have an appropriate gram capacity, the amount of active sodium ions embedded can be controlled appropriately, so that the reaction rate during thermal runaway of the battery is moderate and the battery safety is improved.

[0120] In some embodiments of the present application, the specific surface area B of the negative electrode sheet is selected from 2.5m 2 / g~10m 2 / g.

[0121] In some embodiments, the specific surface area B of the negative electrode sheet is selected from 3m 2 / g~7m 2 / g.

[0122] In some embodiments, the specific surface area B of the negative electrode sheet can also be selected from any one or two of the following intervals: 2.5m 2 / g、3m 2 / g, 3.5m 2 / g、4m 2 / g, 4.5m 2 / g、5m 2 / g, 5.5m 2 / g、6m 2 / g, 6.5m 2 / g、7m 2 / g, 7.5m 2 / g、8m 2 / g、8.5m 2 / g、9m 2 / g, 9.5m 2 / g、10m 2 / g, etc.

[0123] By controlling the specific surface area of ​​the negative electrode sheet and the particle size of the negative electrode active material within a more appropriate range, the ion deintercalation path and polarization of the battery active material are moderate, which is more conducive to the battery power performance.

[0124] In some embodiments of the present application, the first exothermic reaction peak position T of the differential scanning calorimetry analysis of the negative electrode plate satisfies 150°C≤T≤180°C; further, the test conditions of the differential scanning calorimetry analysis include: nitrogen atmosphere, a heating rate of 5°C / min to 10°C / min.

[0125] In this application, when differential scanning calorimetry analysis is performed, unless otherwise specified, the test conditions may include: a nitrogen atmosphere and a heating rate of 5°C / min to 10°C / min. Non-limiting examples of the heating rate include 5°C / min, 7.5°C / min, and 10°C / min.

[0126] In some embodiments, the T satisfies 170°C≤T≤180°C.

[0127] In some embodiments, the T can also be selected from any one or any two of the following: 150°C, 155°C, 160°C, 165°C, 170°C, 175°C, 180°C, etc.

[0128] Controlling the position of the first exothermic reaction peak, T, in differential scanning calorimetry (DSC) analysis of the negative electrode sheet within a suitable range can further improve battery safety. If T is too low, it will not improve battery safety. However, a higher T is technically difficult to implement, requiring the replacement of the organic polymer binder in the traditional electrode powder with a more heat-resistant material and raising the thermal decomposition temperature of the negative electrode active material.

[0129] The negative electrode active material of the negative electrode plate provided in the first aspect of the present application includes at least hard carbon.

[0130] In some embodiments, the mass proportion of hard carbon in the negative electrode active material is ≥50%.

[0131] In some embodiments, the hard carbon accounts for ≥90% by mass of the negative electrode active material.

[0132] In some embodiments, the mass proportion of hard carbon in the negative electrode active material can also be selected from any one of the following percentages or any two of the following intervals: 50%, 55%, 60%, 65%, 70%, 75%, 80%, 85%, 90%, 95%, 96%, 97%, 98%, 99%, 100%, etc.

[0133] Hard carbon has a high pyrolysis carbonization temperature. A higher hard carbon content improves heat resistance and reduces heat generation. Furthermore, hard carbon's structure has a large interlayer spacing and high porosity, allowing for the embedding of a large number of metal ions. This significantly reduces structural expansion, which improves the battery's charge-discharge cycle performance and lifespan.

[0134] In some embodiments of the present application, the negative electrode active material further includes one or more of soft carbon, graphite, and alloyed negative electrode.

[0135] Introducing one or more other active materials, such as soft carbon, graphite, and alloyed negative electrodes, in addition to hard carbon as a negative electrode active material, can leverage the advantages of these materials to provide the battery with better overall performance. For example, soft carbon has a low and stable charge and discharge potential platform, resulting in large charge and discharge capacity, high efficiency, and excellent cycle performance. Graphite, for example, offers advantages such as good conductivity, high initial efficiency, and wide availability. Alloyed negative electrodes, for example, offer advantages such as high power and high energy density.

[0136] Negative electrode

[0137] The negative electrode sheet of the first aspect of the present application comprises a negative electrode current collector and a negative electrode film layer disposed on at least one surface of the negative electrode current collector, wherein the negative electrode film layer comprises a negative electrode active material, as defined above.

[0138] As a non-limiting example, the negative electrode current collector has two surfaces opposite to each other in its thickness direction, and the negative electrode film layer is disposed on either or both of the two opposite surfaces of the negative electrode current collector.

[0139] In some embodiments, the negative electrode current collector may be a metal foil or a composite current collector. For example, as the metal foil, copper foil, aluminum foil, iron foil, or nickel foil may be used. The composite current collector may include a polymer base layer and a metal layer formed on at least one surface of the polymer base layer. The composite current collector may be formed by forming a metal material (copper, copper alloy, nickel, nickel alloy, titanium, titanium alloy, silver, silver alloy, aluminum, aluminum alloy) on a polymer base layer (such as a base material of polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), polyethylene (PE), etc.).

[0140] In some embodiments, the negative electrode film layer may further include a binder. The binder may be selected from at least one of styrene-butadiene rubber (SBR), polyacrylic acid (PAA), sodium polyacrylate (PAAS), polyacrylamide (PAM), polyvinyl alcohol (PVA), sodium alginate (SA), polymethacrylic acid (PMAA), and carboxymethyl chitosan (CMCS).

[0141] In some embodiments, the negative electrode film layer may further include a conductive agent, which may be selected from at least one of superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers.

[0142] In some embodiments, the negative electrode film layer may optionally include other additives, such as a thickener (eg, sodium carboxymethyl cellulose (CMC-Na)).

[0143] In some embodiments, the negative electrode sheet can be prepared by the following method: the components for preparing the negative electrode sheet, such as the negative electrode active material, the conductive agent, the binder and any other components, are dispersed in a solvent (such as deionized water) to form a negative electrode slurry; the negative electrode slurry is coated on the negative electrode current collector, and after drying, cold pressing and other processes, the negative electrode sheet can be obtained.

[0144] In a second aspect, the present application provides a sodium ion battery, which includes a positive electrode plate, the negative electrode plate described in the first aspect of the present application, a separator and an electrolyte, wherein the separator is arranged between the positive electrode plate and the negative electrode plate.

[0145] The sodium ion battery prepared by using the negative electrode sheet of the first aspect of the present application has the comprehensive advantages of high safety and high power. Generally, a sodium ion battery includes a positive electrode sheet, a negative electrode sheet, an electrolyte and a separator. During the charge and discharge process of the battery, the active ions (Na + ) moves back and forth between the positive and negative electrodes. The electrolyte conducts ions between the positive and negative electrodes. The separator, located between the positive and negative electrodes, primarily prevents short circuits between the positive and negative electrodes while allowing ions to pass through.

[0146] It should be understood that, unless otherwise specified, the sodium ion battery of the second aspect is a secondary battery.

[0147] electrolytes

[0148] The electrolyte conducts ions between the positive and negative electrodes. This application does not specifically limit the type of electrolyte; it can be selected based on needs. For example, the electrolyte can be liquid, gel, or solid.

[0149] In some embodiments, the electrolyte is an electrolyte solution comprising an electrolyte sodium salt and a solvent.

[0150] In some embodiments, the electrolyte sodium salt can be selected from one or more of sodium hexafluorophosphate (NaPF6), sodium perchlorate (NaClO4), sodium tetrafluoroborate (NaBF4), sodium bis(fluorosulfonyl)imide, sodium bis(trifluoromethanesulfonyl)imide, sodium trifluoromethanesulfonate, sodium difluorophosphate, and the like.

[0151] In some embodiments, the electrolyte sodium salt includes one or more sodium salts of sodium hexafluorophosphate, sodium perchlorate, sodium tetrafluoroborate, and sodium trifluoromethanesulfonate.

[0152] In some embodiments of the present application, the electrolyte further comprises an organic solvent.

[0153] In some embodiments of the present application, the organic solvent may include one or more of ethylene carbonate, dimethyl carbonate, diethyl carbonate, ethyl methyl carbonate, propylene carbonate, ethylene glycol dimethyl ether, tetrahydrofuran, 2-methyltetrahydrofuran, methyl acetate, ethyl propionate, fluoroethylene carbonate, ethyl ether, diethylene glycol dimethyl ether, triethylene glycol dimethyl ether, tetraethylene glycol dimethyl ether, methyl tert-butyl ether, etc.

[0154] In some embodiments of the present application, the organic solvent may include one or more of ethylene carbonate (EC), dimethyl carbonate (DMC), diethyl carbonate (DEC), ethyl methyl carbonate (EMC), propylene carbonate (PC), ether solvents (such as ethylene glycol dimethyl ether (DME)), tetrahydrofuran (THF) and 2-methyltetrahydrofuran (2-MTHF).

[0155] In some embodiments of the present application, the organic solvent may include one or more of ethylene carbonate, propylene carbonate, diethyl carbonate, dimethyl carbonate, ethyl methyl carbonate, methyl acetate, ethyl propionate, fluoroethylene carbonate, ethyl ether, diethylene glycol dimethyl ether, triethylene glycol dimethyl ether, tetraethylene glycol dimethyl ether, methyl tert-butyl ether, etc.

[0156] Sodium salt has a high degree of solvation in the solvent and high electrical conductivity, which is conducive to film formation and improving battery power.

[0157] In some embodiments of the present application, the electrolyte further comprises an additive.

[0158] In some embodiments of the present application, the additive includes fluoroethylene carbonate (FEC), vinylene carbonate (VC), vinyl sulfate (DTD), 1,3-propane sultone (PS), 1,3-propene sultone (PST), succinic anhydride (SA), lithium difluorooxalatoborate (LiDFOB), lithium difluorobis(oxalatophosphate) (LiDFOP), tris(trimethylsilyl) phosphate (TMSP), tris(trimethylsilyl) borate (TMSB), ethylene carbonate, propylene carbonate, ethyl methyl carbonate, diethyl carbonate, dimethyl carbonate, dipropyl carbonate, methylpropyl carbonate, ethylpropyl carbonate, butylene carbonate, methyl formate, methyl acetate, ethyl acetate, propyl acetate, methyl propionate, ethyl propionate, propyl propionate, methyl butyrate, ethyl butyrate, 1,4-butyrolactone, cyclopentane, dimethyl sulfone, methyl ethyl sulfone and diethyl sulfone. One or more.

[0159] In some embodiments of the present application, the additive includes one or more of fluoroethylene carbonate (FEC), vinylene carbonate (VC), vinyl sulfate (DTD), 1,3-propane sultone (PS), 1,3-propenyl-sultone (PST), succinic anhydride (SA), lithium difluorooxalatoborate (LiDFOB), lithium difluorobis(oxalatophosphate) (LiDFOP), tris(trimethylsilyl) phosphate (TMSP), tris(trimethylsilyl) borate (TMSB), etc.

[0160] By selecting suitable additives, the battery can quickly form a solid electrolyte interface (SEI) film, increase the thickness and stability of the SEI film, and improve battery safety.

[0161] In some embodiments, the battery formation current can be reduced, for example, at 0.05°C or 0.1°C. Furthermore, the formation temperature can be set at 25°C, thereby obtaining a thicker SEI film. In some embodiments, the negative electrode sheet satisfies the following conditions: 0.5°C ≤ T×M ≤ 6°C; where T and M are the first exothermic reaction peak position and first-stage weight loss rate, respectively, as determined by differential scanning calorimetry (DSC) analysis of the negative electrode sheet. Furthermore, the temperature is increased at a rate of 5°C / min to 10°C / min under a nitrogen atmosphere.

[0162] In some embodiments, the negative electrode sheet satisfies the following condition: 0.65°C≤T×M≤5.2°C.

[0163] In some embodiments, the negative electrode sheet satisfies the following condition: 0.75°C≤T×M≤4.5°C.

[0164] In some embodiments, the T×M of the negative electrode plate can also be selected from any one or any two of the following intervals: 0.5°C, 0.52°C, 0.54°C, 0.55°C, 0.56°C, 0.58°C, 0.60°C, 0.65°C, 0.70°C, 0.75°C, 0.80°C, 0.85°C, 0.90°C, 0.95°C, 1°C, 1.5°C, 2°C, 2.5°C, 3°C, 3.5°C, 4°C, 4.5°C, 5°C, 5.5°C, 6°C, etc.

[0165] In the present application, the first exothermic reaction S position (T) and the first weight loss rate (M) of the differential scanning calorimetry (DSC) analysis of the negative electrode sheet can be obtained from the DSC spectrum of the negative electrode sheet. M can reflect the decomposition amount of the solid electrolyte interface (SEI). The DSC test of the negative electrode sheet can refer to the "JYT014-1996" general rules for thermal analysis methods. Unless otherwise specified, the following test method can be used: dry the electrode in a vacuum drying oven at 60°C for 6 hours, take a sample with a weight of W3, raise the temperature to 600°C under a nitrogen atmosphere, and measure the weight loss rate and DCS exothermic peak of the sample.

[0166] In some embodiments, the gas atmosphere is nitrogen, argon, or a combination thereof.

[0167] In some embodiments, the heating rate may be 5°C / min to 10°C / min, with non-limiting examples such as 5°C / min, 10°C / min, etc.

[0168] As previously mentioned, in this application, when differential scanning calorimetry analysis is performed, unless otherwise specified, the test conditions may include: a nitrogen atmosphere and a heating rate of 5°C / min to 10°C / min. Non-limiting examples of heating rates include 5°C / min, 7.5°C / min, and 10°C / min.

[0169] The inventors of this application speculate that T×M can, to a certain extent, reflect the tolerance of the negative electrode plate at high temperatures. The particle size of the negative electrode active material affects the starting temperature of the reaction exotherm. The larger the particles, the higher the temperature at which the reaction starts, and the safer the corresponding battery system. However, when the particles are larger, it will be detrimental to the battery power. Therefore, how to balance safety and battery power is crucial for the preparation of batteries with high comprehensive performance. By shifting the position (T) of the first exothermic reaction peak of the differential scanning calorimetry (DSC) analysis of the negative electrode plate to a high temperature, the decomposition reaction temperature (corresponding to M) of the solid electrolyte interface (SEI) film can be increased, which is beneficial to increase the thickness of the SEI film, thereby achieving the effect of further improving safety.

[0170] In some embodiments of the present application, the first-stage weight loss rate M of the differential scanning calorimetry analysis of the negative electrode sheet satisfies the following conditions: 0.25% ≤ M ≤ 3.5%; further, the test conditions of the differential scanning calorimetry analysis include: nitrogen atmosphere, and a heating step of 5°C / min to 10°C / min (such as 10°C / min).

[0171] In some embodiments, 0.5%≤M≤2.5%.

[0172] In some embodiments, 0.65%≤M≤2%.

[0173] In some embodiments, the M can also be selected from any one of the following percentages or an interval consisting of any two of them: 0.28%, 0.3%, 0.4%, 0.5%, 0.6%, 0.7%, 0.8%, 0.9%, 1.0%, 1.1%, 1.2%, 1.4%, 1.5%, 1.6%, 1.8%, 2.0%, 2.1%, 2.2%, 2.3%, 2.4%, 2.5%, 2.6%, 2.8%, 3%, 3.2%, 3.3%, etc.

[0174] By controlling the first-stage weight loss rate (M) of the negative electrode sheet during differential scanning calorimetry analysis within a suitable range, the SEI interface stability can be improved, which is beneficial for enhancing battery safety and achieving better ion transport and charge-discharge performance. A lower M indicates a thinner SEI, which is less conducive to battery interface stability and poorer battery safety. However, a higher M indicates a thicker SEI, which is detrimental to ion transport and deteriorates charge-discharge performance.

[0175] Positive electrode

[0176] The positive electrode sheet includes a positive electrode current collector and a positive electrode film layer provided on at least one surface of the positive electrode current collector, wherein the positive electrode film layer includes a positive electrode active material.

[0177] In some embodiments, the positive electrode plate includes a positive electrode active material containing sodium ions. In some of these embodiments, the positive electrode active material containing sodium ions includes one or more of a Prussian blue compound, a sodium transition oxide, and a polyanion compound. Flexible selection of suitable positive electrode active materials allows for greater selectivity and wider applicability of sodium-ion batteries.

[0178] The positive electrode active material may include, but is not limited to, one or more of sodium transition metal oxides, polyanion compounds, and Prussian blue compounds. However, the present application is not limited to the aforementioned materials, and other known materials that can be used as positive electrode active materials for sodium ion batteries may also be used.

[0179] In some embodiments, the transition metal in the sodium transition metal oxide may be one or more of Mn, Fe, Ni, Co, Cr, Cu, Ti, Zn, V, Zr, and Ce. Non-limiting examples of sodium transition metal oxides may be Na x ZO2, wherein Z can be one or more of Ti, V, Mn, Co, Ni, Fe, Cr and Cu, <x≤1。

[0180] In some embodiments, the sodium transition metal oxide may be Na 1-x Cu h Fe k Mn l M 1 m O 2-y , where M 1 It can be one or more of Li, Be, B, Mg, Al, K, Ca, Ti, Co, Ni, Zn, Ga, Sr, Y, Nb, Mo, In, Sn and Ba. <x≤0.33,0<h≤0.24,0≤k≤0.32,0<l≤0.68,0≤m<0.1,h+k+l+m=1,0≤y<0.2。

[0181] In some embodiments, the sodium transition metal oxide may be Na 0.67 Mn 0.7 Ni q M 2 0.3-z O2, where M 2 It can be one or more of Li, Mg, Al, Ca, Ti, Fe, Cu, Zn and Ba. <q≤0.1。

[0182] In some embodiments, the sodium transition metal oxide may be Na a Li b Ni c Mn d Fe e O2, of which 0.67 <a≤1,0<b<0.2,0<c<0.3,0.67<d+e<0.8,b+c+d+e=1。

[0183] In some embodiments, the polyanion compound may be a compound having sodium ions, transition metal ions and tetrahedral (YO4) n- A class of compounds with anionic units. The transition metal here can be one or more of Mn, Fe, Ni, Co, Cr, Cu, Ti, Zn, V, Zr and Ce; Y can be one or more of P, S and Si; n represents (YO4) n- valence.

[0184] In some embodiments, the polyanion compound can also be a compound having sodium ions, transition metal ions, tetrahedral (YO4 )n- A class of compounds containing anion units and halogen anions. The transition metal here can be one or more of Mn, Fe, Ni, Co, Cr, Cu, Ti, Zn, V, Zr and Ce; Y can be one or more of P, S and Si, and n represents (YO4) n- valence state; the halogen may be one or more of F, Cl and Br.

[0185] In some embodiments, the polyanion compound can also be a compound having sodium ions, tetrahedral (YO4) n- Anion unit, polyhedron unit (ZO y ) m+ and an optional halogen anion. Y can be one or more of P, S and Si, n represents the valence of (YO4)n-; Z represents a transition metal, which can be one or more of Mn, Fe, Ni, Co, Cr, Cu, Ti, Zn, V, Zr and Ce, m represents (ZO y ) m+ valence state; the halogen may be one or more of F, Cl and Br.

[0186] In some embodiments, the polyanion compound may be NaFePO4, Na3V2(PO4)3, NaM'PO4F, and Na3(VO y )2(PO4)2F 3- 2 y (0≤y≤1) or more; wherein, M' in NaM'PO4F may be one or more of V, Fe, Mn and Ni.

[0187] In some embodiments, the Prussian blue compound may be a compound having sodium ions, transition metal ions and cyanide ions (CN — The transition metal may be one or more of Mn, Fe, Ni, Co, Cr, Cu, Ti, Zn, V, Zr and Ce. Non-limiting examples of Prussian blue compounds include Na a Me b Me' c (CN)6, wherein Me and Me' can each independently be one or more of Ni, Cu, Fe, Mn, Co and Zn, 0 <a≤2,0<b<1,0<c<1。

[0188] In some embodiments, the positive electrode active material layer may further include a conductive agent to improve the conductivity of the positive electrode. The present application does not impose any particular restrictions on the type of conductive agent, and the conductive agent may be selected based on actual needs. For example, the conductive agent may be one or more of superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphite, graphene, and carbon nanofibers.

[0189] In some embodiments, the positive electrode film layer may further optionally include a binder. As a non-limiting example, the positive electrode active material and the optional conductive agent are firmly bonded to the positive electrode current collector. The present application does not particularly limit the type of binder and can be selected according to actual needs. As a non-limiting example, the binder may be polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), vinylidene fluoride-tetrafluoroethylene-propylene terpolymer, vinylidene fluoride-hexafluoropropylene-tetrafluoroethylene terpolymer, tetrafluoroethylene-hexafluoropropylene copolymer, fluorine-containing acrylate resin, polyacrylic acid (PAA), polyvinyl alcohol (PVA), ethylene-vinyl acetate copolymer (EVA), styrene-butadiene rubber (SBR), carboxymethyl cellulose (CMC), sodium alginate (SA), polymethacrylic acid (PMA) and one or more of carboxymethyl chitosan (CMCS).

[0190] In some embodiments, the positive electrode film layer may further include a conductive agent. For example, the conductive agent may include one or more of superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers.

[0191] As an example, the positive electrode current collector has two surfaces opposite to each other in its thickness direction, and the positive electrode film layer is disposed on either or both of the two opposite surfaces of the positive electrode current collector.

[0192] In some embodiments, the positive electrode current collector may be a conductive carbon sheet, metal foil, carbon-coated metal foil, porous metal plate, or a composite current collector. The conductive carbon material of the conductive carbon sheet may be one or more of superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphite, graphene, and carbon nanofibers. The metal material of the metal foil, carbon-coated metal foil, and porous metal plate may each independently be selected from one or more of copper, aluminum, nickel, and stainless steel. The composite current collector may be a composite of a metal foil and a polymer-based film.

[0193] In some embodiments, the positive electrode current collector may be a metal foil or a composite current collector. For example, aluminum foil may be used as the metal foil. The composite current collector may include a polymer material base and a metal layer formed on at least one surface of the polymer material base. The composite current collector may be formed by forming a metal material (aluminum, aluminum alloy, nickel, nickel alloy, titanium, titanium alloy, silver and silver alloy, etc.) on a polymer material substrate (such as a substrate of polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), polyethylene (PE), etc.).

[0194] In some embodiments, the positive electrode sheet can be prepared by the following method: the components for preparing the positive electrode sheet, such as the positive electrode active material, the optional conductive agent, the optional binder and any other components, are dispersed in a solvent (such as N-methylpyrrolidone) to form a positive electrode slurry; the positive electrode slurry is coated on the positive electrode current collector, and after drying, cold pressing and other processes, the positive electrode sheet can be obtained.

[0195] Isolation film

[0196] In some embodiments, the sodium ion battery further includes a separator. The present application has no particular limitation on the type of separator, and any known porous separator with good chemical and mechanical stability can be selected.

[0197] Different battery systems, such as sodium-ion batteries and lithium-ion batteries, have different requirements for the separator structure due to the different diameters of sodium and lithium ions. The larger diameter of sodium ions, unlike the smaller size of lithium ions, places more specific thickness requirements. While achieving the isolation function, it is also necessary to ensure that large-diameter sodium ions can pass through, thereby ensuring good battery rate while maintaining safety.

[0198] In some embodiments, the material of the separator in the sodium-ion battery of the present application can be various materials suitable for separators of electrochemical energy storage devices in the art, including, but not limited to, one or more of glass fiber, non-woven fabric, polyethylene, polypropylene, and polyvinylidene fluoride. The separator can be a single-layer film or a multi-layer composite film, without particular limitation. When the separator is a multi-layer composite film, the materials of each layer can be the same or different, without particular limitation.

[0199] In some embodiments, at least one surface of the isolation membrane includes an insulating material coating. Optionally, the insulating material coating is a ceramic coating.

[0200] In some embodiments, the base material of the separator includes one or more of polyethylene and polypropylene.

[0201] In some embodiments, the thickness of the isolation film is 5 μm to 15 μm. In some embodiments, the thickness of the isolation film is 7 μm to 13 μm. For example, the thickness of the isolation film can be any one or any two of the following ranges: 5 μm, 6 μm, 7 μm, 8 μm, 9 μm, 10 μm, 11 μm, 12 μm, 13 μm, 14 μm, 15 μm, etc.

[0202] In some embodiments, the TD shrinkage of the separator heated at 90° C. for 1 hour is ≤4%. In some embodiments, the TD shrinkage of the separator heated at 90° C. for 1 hour is selected from 0.5% to 3.5%.

[0203] In this application, the TD shrinkage refers to the shrinkage in the width direction, which corresponds to the transverse shrinkage.

[0204] In this application, the shrinkage rate of the separator can be tested using the following method: Cut a 10cm x 10cm piece of separator and place it flat on a smooth glass surface. Then, cut an A4 paper into an area of ​​at least 15cm x 15cm, center the separator over the glass, and tape the four corners of the A4 paper to the glass. The separator is then placed in an oven and heated for 1 hour. After removal, the separator's dimensions are measured.

[0205] The smaller the shrinkage rate, the more stable the isolation membrane is when the battery is baked at high temperature, and the less likely it is to deform and shrink, thereby more effectively avoiding the failure of the positive and negative electrode isolation function and short circuit.

[0206] In some embodiments, the surface density of the isolation film is selected from 2 g / m 2 ~6g / m 2 In some embodiments, the surface density of the isolation film is selected from 3 g / m 2 ~5g / m 2 In some embodiments, the surface density of the isolation film can also be selected from any one or two of the following intervals: 2 g / m 2 , 2.5g / m 2 , 3g / m 2 3.5g / m 2 , 4g / m 2 4.5g / m 2 , 5g / m 2 , 5.5g / m 2 , 6g / m 2 wait.

[0207] In the present application, the surface density of the isolation membrane can be measured using instruments and methods known in the art. For example, the mass of an isolation membrane with a certain area can be weighed using a Sartorius electronic balance, and the surface density of the isolation membrane can be calculated by dividing the mass of the isolation membrane by the area of ​​the isolation membrane.

[0208] The greater the surface density, the less likely it is to puncture the separator, but the weight of the separator will increase; the smaller the surface density, the looser the separator, and the easier it is to be punctured by hard carbon sharp corners and cause a short circuit.

[0209] In some embodiments of the present application, the isolation film satisfies one or more of the following characteristics:

[0210] (tm1): At least one side surface of the isolation membrane includes an insulating material coating, optionally, the insulating material coating is a ceramic coating;

[0211] (tm2) the base material of the isolation membrane comprises one or more of polyethylene and polypropylene;

[0212] (tm3) the thickness of the isolation film is 5 μm to 15 μm, optionally, the thickness of the isolation film is 7 μm to 13 μm;

[0213] (tm4) the shrinkage rate of the separator in the TD direction when heated at 90° C. for 1 hour is ≤4%, and optionally, the shrinkage rate of the separator in the TD direction when heated at 90° C. for 1 hour is selected from 0.5% to 3.5%; and

[0214] (tm5) The surface density of the isolation film is selected from 2g / m 2 ~6g / m 2 Optionally, the surface density of the isolation film is selected from 3g / m 2 ~5g / m 2 .

[0215] Another aspect of the present application also provides the use of the negative electrode sheet described in the first aspect of the present application in the preparation of a sodium ion battery.

[0216] The negative electrode plate of the first aspect of the present application can be used to prepare sodium ion batteries, thereby obtaining the comprehensive advantages of both high safety and high energy density.

[0217] Assembly of sodium-ion batteries

[0218] In some embodiments, the positive electrode sheet, the negative electrode sheet, and the separator can be formed into an electrode assembly through a winding process or a lamination process.

[0219] In some embodiments, the sodium ion battery may include an outer packaging that can be used to encapsulate the electrode assembly and the electrolyte.

[0220] In some embodiments, the outer packaging of the sodium ion battery can be a hard shell, such as a hard plastic shell, an aluminum shell, a steel shell, etc. The outer packaging of the sodium ion battery can also be a soft shell, such as a pouch-type soft shell. The soft shell can be made of plastic, and examples of plastics include polypropylene, polybutylene terephthalate, and polybutylene succinate.

[0221] The present application has no particular limitation on the shape of the sodium ion battery, which may be cylindrical, square, or any other shape. For example, FIG2 shows a sodium ion battery 5 having a square structure as an example.

[0222] In some embodiments, referring to FIG3 , the outer packaging may include a shell 51 and a cover plate 53. The shell 51 may include a bottom plate and a side plate connected to the bottom plate, and the bottom plate and the side plate enclose a receiving cavity. The shell 51 has an opening connected to the receiving cavity, and the cover plate 53 can be covered on the opening to close the receiving cavity. The positive electrode sheet, the negative electrode sheet and the separator can be formed into an electrode assembly 52 through a winding process or a lamination process. The electrode assembly 52 is encapsulated in the receiving cavity. The electrolyte is infiltrated in the electrode assembly 52. ​​The number of electrode assemblies 52 contained in the sodium ion battery 5 can be one or more, and those skilled in the art can select according to actual needs.

[0223] In some embodiments, the above-mentioned positive electrode sheet, separator, and negative electrode sheet are stacked in sequence to obtain a battery cell, and the separator is placed between the positive electrode sheet and the negative electrode sheet to play an isolating role to obtain a battery cell, or the battery cell can be obtained by winding; the battery cell is placed in a packaging shell (which can be a soft pack, a square aluminum shell, a square steel shell, a cylindrical aluminum shell and a cylindrical steel shell), the electrolyte is injected and sealed to obtain a sodium ion battery.

[0224] In a third aspect, the present application provides an electrical device comprising the sodium ion battery described in the second aspect of the present application.

[0225] The electrical device prepared using the sodium ion battery provided in the second aspect of the present application not only has high safety, but also has high energy density, and can meet the comprehensive needs of consumers for high safety and high performance.

[0226] The sodium-ion battery can be used as a power source or energy storage unit for the electrical device. The electrical device may include, but is not limited to, mobile devices, electric vehicles, electric trains, ships, satellites, and energy storage systems. Examples of mobile devices include, but are not limited to, mobile phones and laptops; and examples of electric vehicles include, but are not limited to, pure electric vehicles, hybrid electric vehicles, plug-in hybrid electric vehicles, electric bicycles, electric scooters, electric golf carts, and electric trucks.

[0227] As the power-consuming device, a sodium ion battery can be selected according to its usage requirements.

[0228] FIG4 shows an example of an electric device 6. The electric device is a pure electric vehicle, a hybrid electric vehicle, or a plug-in hybrid electric vehicle. To meet the electric device's requirements for high power and high energy density of sodium-ion batteries, a battery pack or battery module can be used.

[0229] Another example device may be a mobile phone, a tablet computer, a laptop computer, etc. Such a device is generally required to be lightweight and thin, and may use a sodium ion battery as a power source.

[0230] Below, some embodiments of the present application are described. The embodiment described below is exemplary, is only used to explain the present application, and cannot be construed as limiting the present application. The details of the technology or conditions not indicated in the embodiment are carried out according to the description above, or according to the technology or conditions described in the document in this area or according to the product specification. Reagents used or instruments not indicated by the manufacturer are conventional products that can be obtained commercially, or can be synthesized in a conventional manner by commercially available products.

[0231] In the following embodiments, room temperature refers to 20°C to 30°C, and may be 25°C.

[0232] In the following examples, unless otherwise specified, the specifications and models of the following raw materials are:

[0233] The following examples and comparative examples can be prepared with reference to the parameters in Tables 1, 2 and 3.

[0234] 1. Preparation of negative electrode sheet

[0235] Preparation of negative electrode sheet 1

[0236] The negative electrode active material, hard carbon, the conductive agent, Super P, the thickener, sodium carboxymethyl cellulose (CMC), and the binder, styrene-butadiene rubber latex (SBR), were mixed in a mass ratio of 97:0.7:1.8:0.5. The mixture was added to the solvent, deionized water, and stirred evenly in a vacuum mixer to obtain a negative electrode slurry. The solid content of the negative electrode slurry was 56% by weight.

[0237] Among them, the particle size control and screening method of the negative electrode active material is: using phenolic resin generated by the reaction of resorcinol and formaldehyde as a precursor, using polyacrylonitrile (PAN) as a coating carbon source, adjusting the specific surface area and closed pore volume of the material by carbon coating, setting the pyrolysis temperature under nitrogen atmosphere to 1300°C, and obtaining the material of the target size through primary screening and fine screening after pyrolysis.

[0238] The negative electrode slurry prepared above is evenly coated on both sides of the negative electrode collector copper foil by an extrusion coater or a transfer coater, and dried at 85°C. Then, it is cold pressed, trimmed, cut and stripped to obtain a negative electrode sheet with a size of 91mm×5680mm.

[0239] Preparation of negative electrode sheets 2 to 17: The method is basically the same as that of negative electrode sheet 1. The difference between negative electrode sheets 2 to 10, 13, and 14 and negative electrode sheet 1 is that the size of the negative electrode active material is different, and the volume cumulative distribution particle size D shown in Table 1 is used respectively.v 99.D v 50. D v 10. Negative electrode sheets 11-12, 15-17 differ from negative electrode sheet 1 in the type and size of the negative electrode active material. See Table 1.

[0240] 2. Preparation of Sodium Ion Batteries (Examples 1 to 16 and Comparative Examples 1 to 4)

[0241] For each of Examples 1 to 16 and Comparative Examples 1 to 4, the preparation of the negative electrode sheets and the electrolyte solution is as shown in Table 3, and the preparation and assembly methods of the remaining structural components adopt the same parameters, as shown below.

[0242] 2.1. Selection of negative electrode

[0243] The negative electrode sheets of each embodiment and each comparative example were selected according to Table 3.

[0244] 2.2. Preparation of positive electrode sheet

[0245] The positive electrode active material Na2MnFe(CN)6, the conductive agent Super P, and the binder polyvinylidene fluoride (PVDF) were mixed in a mass ratio of 96:2.5:1.5, added to the solvent N-methylpyrrolidone (NMP), and stirred evenly in a vacuum mixer to obtain a slurry for the positive electrode active material layer. The solid content of the slurry was 60% by weight.

[0246] The positive electrode slurry prepared above was evenly coated on the positive electrode current collector aluminum foil, dried at room temperature, and then transferred to a 90°C oven for further drying. It was then cut into discs with a diameter of 88 mm × 5450 mm as positive electrode sheets, which were cold pressed, trimmed, cut and striped to obtain positive electrode sheets with a thickness of 150 μm.

[0247] 2.3. Preparation of isolation membrane

[0248] A 7μm-thick polyethylene (PE) film was used as the separator base. Alumina, sodium carboxymethyl cellulose (CMC), and acrylate were added to deionized water in a weight ratio of 93%:3%:4%. The mixture was stirred evenly in a vacuum mixer to form a slurry. The slurry had a solids content of 55% by weight. The resulting slurry was evenly sprayed onto both sides of the base film at a thickness of 2μm per side to form the separator.

[0249] Preparation of electrolyte

[0250] In an argon atmosphere glove box with a water content of <10 ppm, thoroughly dried sodium salt (NaPF6) was dissolved in the organic solvent ethylene carbonate (EC). Then, the additive vinylene carbonate (VC) was added and mixed thoroughly to obtain an electrolyte. The sodium salt concentration was 1 mol / L. The types and amounts of sodium salt, organic solvent, and additives are shown in Table 3.

[0251] 2.5. Assembly of sodium-ion batteries

[0252] The positive electrode sheet, the separator and the negative electrode sheet are stacked in order so that the separator is between the positive electrode sheet and the negative electrode sheet to play an isolating role. The obtained stack is then wound into a square bare cell, the tabs are welded, the bare cell is placed in a square aluminum shell, and the top cover is laser welded. After vacuum baking at 80°C to remove water, the electrolyte prepared above is injected and sealed. After that, after standing at 45°C, formation (0.02C constant current charging to 3.3V, then 0.1C constant current charging to 3.6V), shaping and capacity testing, a finished hard-shell sodium-ion battery is obtained with a thickness of 28mm, a width of 97.5mm and a length of 148mm.

[0253] 3. Test Method

[0254] 3.1. Negative electrode

[0255] (1) Cumulative volume distribution particle size D of negative electrode active material v N(D v 99.D v 50. D v 10) Testing

[0256] Sample pretreatment: Take a clean beaker, add an appropriate amount of the sample to be tested, add the surfactant sodium lauryl sulfate, and then add deionized water as a dispersant, and perform ultrasonic treatment (frequency 120W, duration 5min) to ensure that the sample is completely dispersed in the dispersant.

[0257] Test: Refer to GB / T 19077-2016 particle size distribution laser diffraction method, use laser particle size analyzer to measure the D v N. Use LS-909 laser particle size analyzer (OMCO) for testing. Pour the sample into the injection tower and circulate it with the solution to the test optical system. The scattered light emitted by the particles under the irradiation of the laser beam is received and its energy distribution is measured. The particle size distribution characteristics (shading brightness: 8% to 12%) can be obtained, and finally the D of the material can be obtained. v N value.

[0258] (2) Test of the specific surface area B of the negative electrode

[0259] The nitrogen adsorption specific surface area analysis test method is used for testing and is calculated using the BET (Brunauer Emmett Teller) method. The nitrogen adsorption specific surface area analysis test can be performed using a Tri Star II surface area and pore analyzer from Micromeritics, USA. The test steps can refer to GB / T 19587-2004.

[0260] The detailed steps are as follows: select the sample to be tested, which can be the negative electrode sheet directly prepared in the above steps, or the negative electrode sheet disassembled from the battery (at this time, it is necessary to use anhydrous ethanol to clean and remove the electrolyte, and then dry it in a vacuum drying oven at 60°C for 2 hours); then use nitrogen as the adsorption gas, and use the specific surface and pore analyzer to map the adsorption and desorption curve with a relative pressure P / P0 of 0 to 0.99 (P is the equilibrium adsorption pressure, P0 is the saturated vapor pressure), and calculate the specific surface area of ​​the negative electrode sheet by the BET method.

[0261] (3) Thermal stability coefficient S of the negative electrode

[0262] Using the formula S=(D v 99+D v 50) / 2B. Among them, (D v 99+D v 50) / 2 is determined using the method in point (1), and B is obtained using the method in point (2).

[0263] (4) Differential scanning calorimetry (DSC) analysis

[0264] Refer to the general principles of thermal analysis methods in JYT014-1996. The following test method can be used: dry the negative electrode in a vacuum drying oven at 60°C for 6 hours, take a sample weighing W3, and program the temperature to 600°C at a heating rate of 10°C / min under a nitrogen atmosphere. Measure the sample's weight loss rate and DCS exothermic peak to obtain the first exothermic reaction peak position T and the first-stage weight loss rate M.

[0265] (5) Reaction rate factor P of the negative electrode

[0266] Calculated using the formula P = C / B, where C is measured according to the method in point (2) of section 1.6.3, and B is obtained using the method in point (2).

[0267] 3.2. Negative electrode and cell performance

[0268] (1) Gram capacity of the negative electrode

[0269] Gram capacity: Refer to the WI-ATC-2014 gram capacity test specifications. The sample to be tested can be the negative electrode directly prepared in the above steps, or the negative electrode disassembled from the battery (in this case, it is necessary to use anhydrous ethanol to clean and remove the electrolyte, and then dry it in a vacuum drying oven at 60°C for 2 hours). Then use a punching machine to punch out 15 small discs with a diameter of 16 mm, and randomly select 12 of them. The weight of each small disc is weighed and the average value is recorded as W1; then the active material on the small disc is cleaned and dried, and the weight of each small disc substrate is weighed and the average value is recorded as W2; on each small disc, the weight of the negative electrode active material on one side of the substrate is (W1-W2) / 2. According to the capacity C0 of the small disc, the gram capacity C=2×C0 / (W1-W2) is calculated, and the unit is mAh / g.

[0270] The C0 test method is as follows: Take the remaining three small discs from the punching process, wipe the active material layer on one side of the substrate with alcohol, use a sodium metal sheet as the counter electrode, inject the electrolyte (refer to 2.4 of Example 2 above), and make a button battery. Then, charge and discharge the battery between 0V and 2V with a current of 0.1C. The capacity after fully charging to 2V and then fully discharging to 0V is C0 (mAh).

[0271] (2) Temperature tolerance

[0272] Use the hot box test method. Refer to the lithium-ion battery heating test method in GB38031-2020.

[0273] At 1.22°C ± 5°C, discharge the battery at 0.33C to 0% SOC, let it rest for 1 hour, and then charge it again at 0.33C constant current and constant voltage to 100% SOC (the upper limit of the battery's specified operating voltage). Place the sample in a high-temperature oven and raise the temperature from room temperature to 0V at a rate of 5°C / min until the battery explodes or the voltage reaches 0V. Observe for 1 hour.

[0274] Among them, SOC represents the state of charge of the battery, which can reflect the remaining capacity of the battery and is numerically defined as the ratio of the remaining capacity to the battery capacity.

[0275] (4) Measurement of 60s pulse discharge power

[0276] The power performance of the battery is determined by measuring the battery's 60s pulse discharge power.

[0277] In more detail, the battery cell was placed in the Nebula battery charge and discharge test system at 25°C, and charged at a constant current and constant voltage rate of 0.5C to a charge cut-off voltage of 3.75V. After standing for 5 minutes, it was discharged at a specific power to ensure that the battery voltage reached 2V at 60s and the discharge stopped. The power at this time was the 60s pulse discharge power.

[0278] 4. Test results and analysis

[0279] Volume cumulative distribution particle size D of the negative electrode sheet v N(D v 99.D v 50. D v 10) The test and analysis results of the electrode specific surface area B, electrode thermal stability coefficient S, DSC analysis, electrode reaction rate factor P, electrode gram capacity C, and electrode reaction rate factor P can be found in Table 1, Table 2, and Figure 1. The DSC analysis and hot box test of the sodium ion batteries prepared in each embodiment and each comparative example show the tolerable temperature.

[0280] Figure 1 shows the exothermic curve and thermogravimetric curve of the negative electrode sheet from a differential scanning calorimetry (DSC) test in Example 3. As can be seen from the figure, the first exothermic peak T of the DSC spectrum is approximately 170°C, and the weight loss rate M in the first stage of the DSC spectrum is approximately 1.2%.

[0281] Negative electrode sheets 1 to 10 and negative electrode sheets 15 to 17 have suitable (D v 99+D v 50) / (2×B) range, are all in the range of 0.6μg / m3 to 5μg / m3, and the sodium ion battery embodiments 1 to 16 prepared using the electrode have a higher hot box test tolerable temperature and a higher 60s pulse discharge power, and have the advantages of both high safety and high power.

[0282] The corresponding (D v 99+D v The value of 50) / (2×B) is outside the range of 0.6 μg / m3 to 5 μg / m3, and the tolerable temperature in the hot box test and the 60s pulse discharge power are inferior to those of the aforementioned embodiments.

[0283] Table 1.

[0284]

[0285] Table 2.

[0286]

[0287] Where S=(D v 99+D v 50) / (2×B).

[0288] It should be noted that the DSC first exothermic reaction peak position T of multiple negative electrode sheets is recorded as 180°C in Table 2, which is the result of rounding off, and there are slight fluctuations between the actual values.

[0289] Table 3.

[0290]

[0291] The technical features of the above-mentioned embodiments can be combined arbitrarily. In order to make the description concise, not all possible combinations of the technical features in the above-mentioned embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.

[0292] It should be noted that the present application is not limited to the above-mentioned embodiments. The above-mentioned embodiments are only examples, and within the scope of the technical solution of the present application, embodiments that have substantially the same structure as the technical idea and exert the same effect are all included in the technical scope of the present application. The above-mentioned embodiments only express several embodiments of the present application, and their descriptions are relatively detailed, but they cannot be understood as limiting the scope of the patent. In addition, without departing from the scope of the subject matter of the present application, various modifications that can be thought of by those skilled in the art to the embodiments and other methods of constructing by combining some of the constituent elements in the embodiments are also included in the scope of the present application. It should be pointed out that for ordinary technicians in this field, without departing from the concept of the present application, several modifications and improvements can be made, which all fall within the scope of protection of the present application. Therefore, the scope of protection of the present application shall be based on the attached claims, and the description and drawings may be used to explain the content of the claims.

Claims

1. A negative electrode sheet comprising a negative electrode active material, wherein the negative electrode active material comprises hard carbon; The negative electrode sheet also meets the following conditions: 0.6 μg / m ≤ (D v 99+D v 50) / (2×B)≤5μg / m, in, D v 99 represents the particle size corresponding to when the cumulative volume distribution percentage of the negative electrode active material reaches 99%, in μm; D v 50 represents the particle size corresponding to when the cumulative volume distribution percentage of the negative electrode active material reaches 50%, in μm; B represents the specific surface area of ​​the negative electrode sheet, in m 2 / g.

2. The negative electrode sheet according to claim 1, wherein: The negative electrode active material satisfies the following conditions: 5 μm≤(D v 99+D v 50) / 2≤18μm; Optionally, the negative electrode active material meets the following conditions: 6 μm ≤ (D v 99+D v 50) / 2≤15μm; Optionally, the negative electrode active material meets the following conditions: 7 μm ≤ (D v 99+D v 50) / 2≤12μm; Optionally, the negative electrode active material meets the following conditions: 8 μm ≤ (D v 99+D v 50) / 2≤10μm.

3. The negative electrode sheet according to claim 1 or 2, wherein: The negative electrode sheet meets the following conditions: 0.7 μg / m ≤ (D v 99+D v 50) / (2×B)≤4.5μg / m; Optionally, the negative electrode sheet meets the following conditions: 0.8 μg / m ≤ (D v 99+D v 50) / (2×B)≤4.2μg / m.

4. The negative electrode sheet according to any one of claims 1 to 3, wherein: The negative electrode active material also meets the following conditions: (x·D v 10)≤D v 50≤(y·D v 99); wherein x=2.6 and y=0.4; Optionally, x=3, and y=0.

3.

5. The negative electrode sheet according to any one of claims 1 to 4, wherein: The negative electrode plate also meets the following conditions: 30mAh·m -2 ≤C / B≤140mAh·m -2 ; Wherein, C is the gram capacity of the negative electrode; Optionally, 40mAh·m -2 ≤C / B≤125mAh·m -2 .

6. The negative electrode sheet according to any one of claims 1 to 5, wherein: The gram capacity C of the negative electrode sheet satisfies the following conditions: 300mAh / g≤C≤350mAh / g, Optionally, the gram capacity C of the negative electrode plate satisfies the following condition: 310 mAh / g≤C≤340 mAh / g.

7. The negative electrode sheet according to any one of claims 1 to 6, wherein: The B is selected from 2.5m 2 / g~10m 2 / g; Optionally, the B is selected from 3m 2 / g~7m 2 / g.

8. The negative electrode sheet according to any one of claims 1 to 7, wherein: The first exothermic reaction peak position T of the differential scanning calorimetry analysis of the negative electrode sheet satisfies the following conditions: 150°C ≤ T ≤ 180°C; wherein the test conditions of the differential scanning calorimetry analysis include: nitrogen atmosphere, heating rate of 10°C / min; Optionally, 170°C ≤ T ≤ 180°C.

9. The negative electrode sheet according to any one of claims 1 to 8, wherein: The negative electrode active material further comprises one or more of soft carbon, graphite and alloyed negative electrode; Optionally, the mass proportion of hard carbon in the negative electrode active material is ≥50%; Optionally, the mass proportion of hard carbon in the negative electrode active material is ≥90%.

10. A sodium ion battery comprising a positive electrode sheet, the negative electrode sheet according to any one of claims 1 to 10, a separator and an electrolyte, wherein the separator is arranged between the positive electrode sheet and the negative electrode sheet.

11. The sodium ion battery according to claim 10, wherein: The electrolyte comprises an electrolyte sodium salt, and the electrolyte sodium salt includes one or more sodium salts of sodium hexafluorophosphate, sodium perchlorate, sodium tetrafluoroborate, sodium trifluoromethanesulfonate, sodium bis(trifluoromethanesulfonyl)imide, sodium bis(trifluoromethanesulfonyl)imide, sodium trifluoromethanesulfonate and sodium difluorophosphate; Optionally, the electrolyte sodium salt includes one or more sodium salts of sodium hexafluorophosphate, sodium perchlorate, sodium tetrafluoroborate and sodium trifluoromethanesulfonate.

12. The sodium ion battery according to claim 11, wherein The electrolyte further comprises an organic solvent, wherein the organic solvent comprises one or more of ethylene carbonate, dimethyl carbonate, diethyl carbonate, ethyl methyl carbonate, propylene carbonate, ethylene glycol dimethyl ether, tetrahydrofuran, 2-methyltetrahydrofuran, methyl acetate, ethyl propionate, fluoroethylene carbonate, ethyl ether, diethylene glycol dimethyl ether, triethylene glycol dimethyl ether, tetraethylene glycol dimethyl ether and methyl tert-butyl ether; Optionally, the organic solvent includes one or more of ethylene carbonate, dimethyl carbonate, diethyl carbonate, ethyl methyl carbonate, propylene carbonate, ethylene glycol dimethyl ether, tetrahydrofuran and 2-methyltetrahydrofuran.

13. The sodium ion battery according to claim 11 or 12, wherein: The electrolyte further comprises an additive, the additive comprising one or more of fluoroethylene carbonate, vinylene carbonate, vinyl sulfate, 1,3-propane sultone, 1,3-propene sultone, succinic anhydride, lithium difluorooxalatoborate, lithium difluorobisoxalatophosphate, tris(trimethylsilyl)phosphate, tris(trimethylsilyl)borate, ethylene carbonate, propylene carbonate, ethyl methyl carbonate, diethyl carbonate, dimethyl carbonate, dipropyl carbonate, methylpropyl carbonate, ethylpropyl carbonate, butylene carbonate, methyl formate, methyl acetate, ethyl acetate, propyl acetate, methyl propionate, ethyl propionate, propyl propionate, methyl butyrate, ethyl butyrate, 1,4-butyrolactone, cyclopentane, dimethyl sulfone, methyl ethyl sulfone and diethyl sulfone; Optionally, the additive includes one or more of fluoroethylene carbonate, vinylene carbonate, vinyl sulfate, 1,3-propane sultone, 1,3-propenyl-sultone, succinic anhydride, lithium difluorooxalatoborate, lithium difluorobisoxalatophosphate, tris(trimethylsilyl)phosphate and tris(trimethylsilyl)borate.

14. The sodium ion battery according to any one of claims 10 to 13, wherein The negative electrode plate meets the following conditions: 0.5°C ≤ T×M ≤ 6°C; in, T and M are the first exothermic reaction peak position and the first stage weight loss rate of the negative electrode sheet, respectively, and the test conditions of the differential scanning calorimetry analysis include: nitrogen atmosphere, heating rate of 10°C / min; Optionally, 0.65°C ≤ T×M ≤ 5.2°C; Optionally, 0.75°C≤T×M≤4.5°C.

15. The sodium ion battery according to any one of claims 10 to 14, wherein The first-stage weight loss rate M of the differential scanning calorimetry analysis of the negative electrode sheet satisfies the following conditions: 0.25%≤M≤3.5%; wherein the test conditions of the differential scanning calorimetry analysis include: nitrogen atmosphere, heating rate of 10°C / min; Optionally, 0.5%≤M≤2.5%; Optionally, 0.6%≤M≤2.1%.

16. The sodium ion battery according to any one of claims 10 to 15, wherein The positive electrode plate includes a positive electrode active material containing sodium ions, and the positive electrode active material containing sodium ions includes one or more of Prussian blue compounds, sodium transition metal oxides and polyanion compounds.

17. An electrical device, wherein: The sodium ion battery comprises the sodium ion battery according to any one of claims 10 to 16.

18. Use of the negative electrode sheet according to any one of claims 1 to 9 in the preparation of sodium ion batteries.

Citation Information

Patent Citations

  • Lithium ion secondary battery

    CN109713237A

  • Sodium ion battery

    CN111525099A

  • Positive pole piece for secondary battery, secondary battery, battery module, battery pack and device

    CN114256443A

  • Positive electrode sheet for secondary battery, secondary battery, battery module, battery pack, and apparatus

    US20210167366A1