Binder for all-solid-state battery, positive electrode for all-solid-state battery, and all-solid-state battery comprising same

By using polymer binder containing hydrogen bond functional groups in all-solid state batteries, self-healing characteristics are formed, and the problem of contact loss between active materials and solid electrolytes is solved, and the electrochemical performance and life of the battery are improved.

CN118946988APending Publication Date: 2024-11-12LG ENERGY SOLUTION LTD +1

Patent Information

Application Number
CN202380031540.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-12-27
Filing Date
2023-12-20
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

During the charging and discharging process, all-solid-state batteries lose contact with the interface of active materials and solid electrolytes, resulting in a decrease in electrochemical performance and life, especially in low-voltage driving environments.

Method used

Using a binder containing the first polymer and the second polymer, both form hydrogen bonds through side link branches on the main chain of the conjugated diene polymer to form self-healing properties, prevent interface losses, improve electrochemical and Mechanical stress suppression ability.

Benefits of technology

In a low voltage drive environment, the initial discharge capacity and Coulomb efficiency of all solid state batteries are improved, and the service life of the battery is extended.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118946988A_ABST
    Figure CN118946988A_ABST
Patent Text Reader

Abstract

The present invention relates to a binder for an all-solid-state battery, the binder containing a first polymer in which a chain containing a first hydrogen-bonding functional group is grafted with a side chain on a conjugated diene-based polymer main chain, and a second polymer in which a chain containing a second hydrogen-bonding functional group is grafted with a side chain on a conjugated diene-based polymer main chain, wherein the first hydrogen bonding functional group of the first polymer and the second hydrogen bonding functional group of the second polymer form a hydrogen bond with each other. The present invention also relates to a positive electrode for an all-solid-state battery comprising a binder for an all-solid-state battery, a conductive material, a positive electrode active material, and a solid electrolyte; and an all-solid-state battery including a positive electrode, a negative electrode, and a solid electrolyte layer provided between the positive electrode and the negative electrode, in which the positive electrode is the positive electrode for the all-solid-state battery.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application claims the benefit of and priority to Korean Patent Application No. 10-2022-0185997, filed on December 27, 2022, the disclosure of which is incorporated herein by reference in its entirety.

[0002] The present invention relates to an adhesive for an all-solid-state battery, a positive electrode for an all-solid-state battery, and an all-solid-state battery comprising the same. Background Art

[0003] Although lithium secondary batteries are mainly used in small devices such as mobile devices and laptops, recent research has expanded to large and medium-sized devices such as energy storage systems (ESS) and electric vehicles (EVs).

[0004] Unlike small batteries, these large and medium-sized lithium secondary batteries have a more severe working environment (such as temperature and shock) and require the use of more cells, so safety needs to be ensured as well as good performance and affordable prices.

[0005] Currently, most commercially available lithium secondary batteries use organic liquid electrolytes containing lithium salts dissolved in flammable organic solvents, which have the potential risk of leakage, fire and explosion. Therefore, the use of solid electrolytes instead of organic liquid electrolytes has been attracting attention as an alternative solution to solve safety issues.

[0006] All-solid-state batteries consist of a positive electrode, a solid electrolyte and a negative electrode. Although both sulfides and oxides can be used as solid electrolytes for all-solid-state batteries, sulfide solid electrolytes are the most promising materials in terms of lithium ion conductivity.

[0007] The driving mechanism of all-solid-state batteries is the transport of lithium ions through the interface between the active material and the solid electrolyte.

[0008] However, due to the volume change of active materials in the all-solid-state battery during continuous charging and discharging, loss of interfacial contact with the solid electrolyte will occur. It is known that the smaller the driving pressure of the all-solid-state battery, the greater this loss, so it is necessary to improve it.

[0009] [Prior art literature]

[0010] [Patent Document]

[0011] (Patent Document 1) Korean Patent No. 10-1970648 (April 15, 2019) Summary of the invention

[0012] [Technical issues]

[0013] The object of the present invention is to provide an adhesive for an all-solid-state battery, the adhesive comprising a first polymer (in which a chain containing a first hydrogen-bonding functional group is grafted with a side chain on the main chain of a conjugated diene polymer) and a second polymer (in which a chain containing a second hydrogen-bonding functional group is grafted with a side chain on the main chain of a conjugated diene polymer), wherein the first hydrogen-bonding functional group of the first polymer and the second hydrogen-bonding functional group of the second polymer form hydrogen bonds with each other, thereby avoiding the loss of interfacial contact with the solid electrolyte due to the volume change of the active material when the all-solid-state battery is repeatedly charged and discharged, thereby exhibiting a property called "self-healing", thereby being able to improve the initial discharge capacity and coulombic efficiency of the all-solid-state battery under a low-voltage driving environment.

[0014] Another object of the present invention is to provide a positive electrode for an all-solid-state battery, which comprises a binder for an all-solid-state battery, a conductive material, a positive electrode active material and a solid electrolyte.

[0015] Another object of the present invention is to provide an all-solid-state battery having improved electrochemical performance and life characteristics by applying the positive electrode active material for the all-solid-state battery to the positive electrode.

[0016] [Technical solution]

[0017] One embodiment of the present invention provides an adhesive for an all-solid-state battery, the adhesive comprising a first polymer (in which a chain containing a first hydrogen-bonding functional group is grafted onto a side chain on the main chain of a conjugated diene polymer) and a second polymer (in which a chain containing a second hydrogen-bonding functional group is grafted onto a side chain on the main chain of a conjugated diene polymer), wherein the first hydrogen-bonding functional group of the first polymer and the second hydrogen-bonding functional group of the second polymer form hydrogen bonds with each other.

[0018] The conjugated diene-based polymer may include repeating units derived from one or more monomers selected from the group consisting of 1,3-butadiene, 2,3-dimethyl-1,3-butadiene, 2-ethyl-1,3-butadiene, 1,3-pentadiene, 2-halo-1,3-butadiene (wherein "halo" refers to a halogen atom), and isoprene.

[0019] The molar ratio of the first hydrogen-bonding functional group or the second hydrogen-bonding functional group to the conjugated diene-based polymer may be 100:1 to 100:30, respectively.

[0020] The first hydrogen-bonding functional group may be at least one selected from the group consisting of a carboxyl group, a hydroxyl group, an amine group, an amide group, a thioether group, a urea group, a thiourea group, an imidazole group, and a sulfonic acid group.

[0021] The second hydrogen-bonding functional group may be at least one selected from the group consisting of an amine group, a carbonyl group, a carboxyl group, a hydroxyl group, an amide group, an ester group, and a glycidyl group.

[0022] The first polymer and the second polymer may be compounds including a mercapto group (—SH) grafted onto a main chain of a conjugated diene-based polymer.

[0023] Another embodiment of the present invention provides a positive electrode for an all-solid-state battery, which includes a binder for an all-solid-state battery, a conductive material, a positive electrode active material, and a solid electrolyte.

[0024] The solid electrolyte may be selected from Li2S-P2S5, Li2S-P2S5-LiX (wherein X is a halogen atom), Li2S-P2S5-Li2O, Li2S-P2S5-Li2O-LiI, Li2S-SiS2, Li2S-SiS2-LiI, Li2S-SiS2-LiBr, Li2S-SiS2-LiCl, Li2S-SiS2-B2S3-LiI, Li2S-SiS2-P2S5-LiI, Li2S-B2S3, Li2S-P2S5-Z m S n (where m and n are positive numbers, Z is any one of Ge, Zn and Ga), Li2S-GeS2, Li2S-SiS2-Li3PO4, Li2S-SiS2-Li p MO q (where p and q are positive numbers, and M is any one of P, Si, Ge, B, Al, Ga, and In), Li 7-x PS 6-x Cl x (where 0≤x≤2), Li 7-x PS 6-x Br x (where 0≤x≤2) and Li 7-x PS 6-x I x At least one of the group consisting of (wherein 0≤x≤2).

[0025] The solid electrolyte may be an argyrodite-type solid electrolyte including one or more selected from the group consisting of Li6PS5Cl, Li6PS5Br, and Li6PS5I.

[0026] Another embodiment of the present invention provides an all-solid-state battery, which includes a positive electrode, a negative electrode, and a solid electrolyte layer arranged between the positive electrode and the negative electrode, wherein the positive electrode includes a positive electrode for an all-solid-state battery.

[0027] [Beneficial Effects]

[0028] According to the present invention, the adhesive for all-solid-state batteries contains a first polymer (in which a chain containing a first hydrogen-bonding functional group is grafted with a side chain on the main chain of a conjugated diene polymer) and a second polymer (in which a chain containing a second hydrogen-bonding functional group is grafted with a side chain on the main chain of a conjugated diene polymer), wherein the first hydrogen-bonding functional group of the first polymer and the second hydrogen-bonding functional group of the second polymer form hydrogen bonds with each other, thereby avoiding the loss of interfacial contact with the solid electrolyte due to the volume change of the active material when the all-solid-state battery is repeatedly charged and discharged, thereby exhibiting a property called "self-healing", which can improve the initial discharge capacity and coulombic efficiency of the all-solid-state battery under a low-voltage driving environment. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] Figure 1 The graph is a graph describing the initial discharge capacity of all-solid-state batteries according to the examples of the present invention and the comparative examples.

[0030] Figure 2 Graphs illustrating the initial coulombic efficiencies of all-solid-state batteries according to embodiments of the present invention and comparative examples.

[0031] Figure 3 This is a diagram showing the results of NMR spectrum measurement that can confirm the presence of hydrogen-bonding functional groups in the binders for all-solid-state batteries of Examples and Comparative Examples of the present invention. DETAILED DESCRIPTION

[0032] The embodiments of the present invention will be described in detail below. It should be noted that the terms and words used in this specification and claims should not be interpreted according to their conventional meanings or dictionary meanings, but should be interpreted in a sense and concept consistent with the technical idea of ​​the present invention based on the principle that the inventor can appropriately define the terminology concept to preferably describe his invention. Therefore, it should be understood that the compositions described in the embodiments listed herein are only the most preferred embodiments of the present invention, not all of the technical ideas of the present invention, and various equivalents and variants that can replace them may exist at the time of application.

[0033] Throughout the specification, when a component “comprising” a component, it may mean further including other components, rather than excluding other components, unless otherwise specified.

[0034] Furthermore, descriptions of limiting or adding components may apply to any invention and are not limited to any particular invention unless otherwise stated.

[0035] Furthermore, in the specification and claims of the present invention, a singular expression includes a plural expression unless otherwise specified.

[0036] In addition, in the description and claims of the present invention, "or" includes "and" unless otherwise specified. Therefore, "comprising A or B" means all three cases: comprising A, comprising B, and comprising A and B.

[0037] Furthermore, all numerical ranges include both ends and all intermediate values ​​unless expressly stated to be excluded.

[0038] <Binder for all-solid-state batteries>

[0039] Hereinafter, a binder for an all-solid-state battery according to one embodiment of the present invention will be described.

[0040] The present invention relates to an adhesive for an all-solid-state battery, which can prevent the active material (especially the positive electrode active material) and the solid electrolyte interface from being separated due to repeated charge and discharge operation of the all-solid-state battery, and improve the initial discharge capacity and coulombic efficiency during low-voltage operation.

[0041] In order to form a stable interface between the positive electrode active material and the solid electrolyte of the all-solid-state battery electrode, coating technology, single crystal active material technology and functional polymer technology for suppressing electrochemical and mechanical stress have been studied. In particular, since functional polymer technology can suppress electrochemical and mechanical stress at the battery level, the research and development of functional polymer technology has attracted much attention as an effective technology.

[0042] The conventional approach is to introduce polar functional groups or form three-dimensional structures to improve the electrochemical and mechanical stress suppression capabilities of non-polar rubber polymers.

[0043] However, there are limitations on suppressing the irreversible interfacial separation that occurs when all-solid-state batteries are subjected to a certain degree of stress.

[0044] Therefore, in order to solve the above problems, the present invention identifies an adhesive for an all-solid-state battery comprising different polymers (wherein chains containing hydrogen-bonding functional groups are grafted onto side chains on the main chain of a conjugated diene polymer), and wherein the hydrogen-bonding functional groups of each polymer form hydrogen bonds with each other, thereby avoiding the loss of interfacial contact with the solid electrolyte due to volume changes in the active material when the all-solid-state battery is repeatedly charged and discharged, thereby exhibiting a property called "self-healing", thereby being able to improve the initial discharge capacity and coulombic efficiency of the all-solid-state battery under a low-voltage driving environment.

[0045] An adhesive for an all-solid-state battery of one embodiment of the present invention may contain a first polymer (in which a chain containing a first hydrogen-bonding functional group is grafted with a side chain on the main chain of a conjugated diene polymer) and a second polymer (in which a chain containing a second hydrogen-bonding functional group is grafted with a side chain on the main chain of a conjugated diene polymer), wherein the first hydrogen-bonding functional group of the first polymer and the second hydrogen-bonding functional group of the second polymer form hydrogen bonds with each other.

[0046] The binder for an all-solid-state battery comprises polymers different from each other, each of which comprises a non-polar conjugated diene polymer as a main chain and a polar functional group capable of forming an internal hydrogen bond is grafted to a side chain, thereby improving the ability of the all-solid-state battery to suppress the electrochemical-mechanical stress generated inside the all-solid-state battery during charging and discharging.

[0047] Specifically, the binder of the present invention can impart a property called "self-healing" through hydrogen bonding between different polymers, thereby preventing the loss of interfacial contact between solid electrolytes due to volume changes of the positive electrode active material during continuous charge and discharge of the all-solid-state battery.

[0048] The conjugated diene polymer may be a copolymer comprising a repeating unit derived from a conjugated diene monomer, and further comprising, for example, a repeating unit derived from a diene monomer having 1 to 10 carbon atoms. The repeating unit derived from a diene monomer having 1 to 10 carbon atoms may be a repeating unit derived from a diene monomer different from the conjugated diene monomer.

[0049] In one embodiment of the present invention, the conjugated diene-based polymer may include repeating units derived from one or more monomers selected from the group consisting of 1,3-butadiene, 2,3-dimethyl-1,3-butadiene, 2-ethyl-1,3-butadiene, 1,3-pentadiene, 2-halo-1,3-butadiene (wherein "halo" refers to a halogen atom) and isoprene.

[0050] Specifically, the non-polar conjugated diene polymer as the main chain of the first polymer or the second polymer can be a homopolymer or copolymer of a conjugated diene monomer. For example, if the conjugated diene polymer contains repeating units derived from 1,3-butadiene, the polymer can be a polymer including repeating units of 1,2-polybutadiene, cis-1,4-polybutadiene and trans-1,4-polybutadiene, or 1,2-polybutadiene and 1,4-polybutadiene, or a polymer including cyclic hydrocarbon repeating units, wherein the repeating units of the conjugated diene polymer and the double bonds in the conjugated diene monomer are connected to each other.

[0051] Preferably, when the conjugated diene polymer contains repeating units derived from 1,3-butadiene, it can be a polymer containing repeating units of 1,2-polybutadiene and 1,4-polybutadiene, as shown in Formula 1 below, wherein the vinyl group contained in the repeating unit of 1,2-polybutadiene can form a graft copolymer with a compound containing a hydrogen bonding functional group.

[0052] [Formula 1]

[0053]

[0054] In one embodiment of the present invention, the first hydrogen-bonding functional group grafted to the side chain of the first polymer contained in the adhesive for all-solid-state batteries can be a "hydrogen bond donor" so that it can hydrogen bond with the second hydrogen-bonding functional group of the second polymer, or it can be any type that can form hydrogen bonds with a hydrogen bond acceptor.

[0055] For example, the first hydrogen-bonding functional group may be at least one selected from the group consisting of a carboxyl group, a hydroxyl group, an amine group, an amide group, a thioether group, a urea group, a thiourea group, an imidazole group, and a sulfonic acid group, and is preferably a carboxyl group.

[0056] In one embodiment of the present invention, the second hydrogen-bonding functional group grafted to the side chain of the second polymer contained in the adhesive for all-solid-state batteries can be a "hydrogen bond acceptor", thereby being able to form a hydrogen bond with the first hydrogen-bonding functional group of the first polymer, or it can be any type that can form a hydrogen bond with a hydrogen bond donor.

[0057] For example, the second hydrogen-bonding functional group may be an amine group, a carbonyl group, a carboxyl group, a hydroxyl group, an amide group, an ester group or a glycidyl group, preferably an amine group.

[0058] When the carboxyl group plays the role of hydrogen bond donor in the first hydrogen-bonding functional group, it can be understood that the hydrogen atom of the hydroxyl part of the carboxyl group (rather than the carbonyl group) plays the role of hydrogen bond donor. Similarly, if the amine group in the first hydrogen-bonding functional group plays the role of "hydrogen bond donor", it can be understood that the two hydrogen atoms of the amine group play the role of hydrogen bond donor.

[0059] In addition, when the carboxyl group in the second hydrogen-bonding functional group plays the role of a "hydrogen bond acceptor", it can be understood that the unshared electron pair of the oxygen atom of the carbonyl group contained in the carboxyl group plays the role of a hydrogen bond acceptor, and when the amine group in the second hydrogen-bonding functional group plays the role of a "hydrogen bond acceptor", it can be understood that the unshared electron pair of the nitrogen atom of the amine group plays the role of a hydrogen bond acceptor.

[0060] In one embodiment of the present invention, the molar ratio of the first hydrogen-bonding functional group to the conjugated diene polymer may be 100:1 to 100:30.

[0061] Furthermore, in one embodiment of the present invention, the molar ratio of the second hydrogen-bonding functional group to the conjugated diene-based polymer may be 100:1 to 100:30.

[0062] For example, the molar ratio of each hydrogen-bonding functional group to the conjugated diene polymer may be 100:1 or more, 100:2 or more, 100:3 or more, 100:4 or more, 100:5 or more, 100:6 or more, 100:7 or more, 100:8 or more, or 100:9 or more, 100:30 or less, 100:29 or less, 100:28 or less, 100:27 or less, 100:26 or less, 100:25 or less, 100:24 or less, 100:23 or less, 100:22 or less, 100:21 or less, 100:20 or less, 100:19 or less, 100:18 or less, 100:17 or less, 100:16 or less, 100:15 or less, 100:14 or less, 100:13 or less, 100:12 or less, or 100:11 or less.

[0063] If the molar ratio of each hydrogen-bonding functional group is less than the above ratio, the first polymer and the second polymer in the adhesive will not be able to form internal hydrogen bonds with each other, thereby failing to fully impart the adhesive with "self-healing properties"; if the ratio exceeds the above ratio, the material containing each hydrogen-bonding functional group may remain in the electrode and produce side reactions with, for example, the sulfide solid electrolyte in the positive electrode, so it should be appropriately adjusted within the above range.

[0064] In one embodiment of the present invention, the first polymer and the second polymer may be compounds including a thiol group (—SH) grafted onto a main chain of a conjugated diene-based polymer.

[0065] In other words, the first polymer and the second polymer contained in the adhesive of the present invention can be formed by graft polymerization of thiol radicals formed by a compound containing a mercapto group and double bonds of a conjugated diene polymer as the main chain of each polymer through a thiol-ene reaction.

[0066] The thiol-ene reaction is a reaction in which a thiol group of a thiol-containing compound and a double bond of a conjugated diene polymer form an alkyl sulfide using free radicals generated by ultraviolet irradiation or heating. The advantage of the thiol-ene reaction is that the polymer can be formed quickly and in high yield under mild conditions.

[0067] For example, in a first polymer, the double bonds of a conjugated diene polymer are mixed with a compound containing a thiol group and a first hydrogen-bonding functional group, and the mixture is irradiated with ultraviolet light, so that the double bonds and the thiol groups of the conjugated diene polymer are grafted through a thiol-ene reaction to form an alkyl sulfide, wherein a portion of the first hydrogen-bonding functional group of the compound containing a thiol group and a first hydrogen-bonding functional group that is not connected to the conjugated diene polymer can remain in a state capable of forming hydrogen bonds with the second hydrogen-bonding functional group of the second polymer.

[0068] The compound containing a thiol group and a first hydrogen-bonding functional group may include 3-mercaptopropionic acid, 3-mercaptopropionic ester, ethylene glycol di-(3-mercaptopropionic ester), trimethylolpropane tris(3-mercaptopropionic ester), pentaerythritol tetra(3-mercaptopropionic ester), dipentaerythritol hexa(3-mercaptopropionic ester), ethoxylated trimethylolpropane tris(3-mercaptopropionic ester), tris[2-(3-mercaptopropionyloxy)ethyl]isocyanurate, polycaprolactone ... (3-mercaptopropionate), pentaerythritol tetrakis (3-mercaptobutyrate), 1,4-bis (3-mercaptobutyryloxy) butane, 1,3,5-tris (3-mercaptobutoxyethyl) -1,3,5-triazine-2,4,6 (1H,3H,5H) -trione, trimethylolpropane tris (3-mercaptobutyrate), etc., but not limited to these, as long as a molecule contains both a thiol group and a hydrogen-bonding functional group, preferably 3-mercaptopropionic acid.

[0069] In the second polymer, the double bonds of the conjugated diene polymer are mixed with a compound containing a thiol group and a second hydrogen-bonding functional group, and the mixture is irradiated with ultraviolet light, so that the double bonds and the thiol groups of the conjugated diene polymer are grafted through a thiol-ene reaction to form an alkyl sulfide, wherein a portion of the second hydrogen-bonding functional groups in the compound containing a thiol group and a second hydrogen-bonding functional group that are not connected to the conjugated diene polymer can maintain a state of being able to form hydrogen bonds with the first hydrogen-bonding functional groups of the first polymer.

[0070] Compounds containing a thiol group and a second hydrogen-bonding functional group may include cysteamine, 4-aminobutane-1-thiol, 5-aminobutane-1-thiol, 1-aminopropane-2-thiol, 2-amino-1-butanethiol, 3-amino-1-butanethiol, 4-amino-2-butanethiol, 6-amino-1-hexanethiol and 7-amino-1-heptanethiol, but are not limited thereto. As long as a thiol group and a hydrogen-bonding functional group are contained in one molecule at the same time, cysteamine is preferred.

[0071] Hereinafter, a method of manufacturing a binder for an all-solid-state battery will be described.

[0072] The binder for an all-solid-state battery may be prepared by preparing a first polymer and a second polymer and mixing them.

[0073] First, a conjugated diene polymer compound as a main chain and a compound containing a first hydrogen-bonding functional group can be added to a solvent together with a photoinitiator to prepare a first polymer solution, which is then irradiated with ultraviolet light to obtain a first polymer through a thiol-ene reaction that forms free radicals.

[0074] The conjugated diene-based polymer as the first polymer main chain and the compound containing the first hydrogen-bonding functional group have been described above, and their detailed description will be omitted below.

[0075] There is no limitation on the solvent as long as it does not react with the sulfide solid electrolyte and can disperse the conjugated diene polymer and the compound containing the first hydrogen-bonding functional group without affecting their properties, for example, one selected from the group consisting of 1,1-dichloro-1-fluoroethane, dichloropropane, cyclohexane, methylcyclohexane, ethylcyclohexane, trichloroethylene, 1,2-dichloroethylene, dichloromethane, trichloroethane, dibromomethane, pentane, 1,2-dichloroethane, heptane, hexane, xylene, toluene, butyl butyrate and n-propyl bromide, or a mixed solvent of two or more.

[0076] There is no limitation on the photoinitiator, as long as it can cause a free radical reaction between the double bond of the conjugated diene polymer and the thiol group of the compound containing the first hydrogen-bonding functional group, such as 2,2-dimethoxy-2-phenylacetophenone (DMPA), benzoyl peroxide, 2,2-diethoxyacetophenone, 3-hydroxyacetophenone, 1-hydroxycyclohexyl phenyl ketone, benzophenone, 2-hydroxy-2-methylpropiophenone, 2,2-diethoxyacetophenone, 2,2-dimethoxy-2-phenylacetophenone or a combination thereof.

[0077] The second polymer can also be prepared by the same method as the first polymer, except that a compound containing a second hydrogen-bonding functional group is used.

[0078] Then, the first polymer solution and the second polymer solution are mixed to prepare a polymer mixture solution, and the solution is dried to prepare a binder for an all-solid-state battery containing the first polymer and the second polymer.

[0079] If necessary, the adhesive for all-solid-state batteries prepared above can be further added together with a photoinitiator to a solvent of the same type as the solvent used to prepare the corresponding polymer solution above to prepare an adhesive solution, and the solution is dried and then irradiated with an ultraviolet light source.

[0080] <Positive electrode for all-solid-state batteries>

[0081] On the other hand, one embodiment of the present invention provides a positive electrode for an all-solid-state battery including a binder for an all-solid-state battery.

[0082] In one embodiment, a positive electrode for an all-solid-state battery may include the above-mentioned binder for an all-solid-state battery, a conductive material, a positive electrode active material, and a solid electrolyte.

[0083] Since the details of the binder for an all-solid-state battery are the same as described above, a detailed description of the binder contained in the positive electrode for an all-solid-state battery of the present invention is omitted below.

[0084] The binder for all-solid-state batteries may be included in an amount of about 0.01 to 10 parts by weight, or 0.01 to 5 parts by weight, or 0.01 to 3 parts by weight, based on a total of 100 parts by weight of the positive electrode for the all-solid-state battery.

[0085] In addition to the adhesive for the all-solid-state battery of the present invention, it may further include an acrylic adhesive, a polyvinylidene fluoride (PVDF) adhesive, a polytetrafluoroethylene (PTFE) adhesive or a butadiene rubber adhesive (such as nitrile rubber (NBR)) in an amount within the above range, and various other polymer adhesives.

[0086] The positive electrode active material contained in the positive electrode for an all-solid-state battery is not particularly limited as long as the material can reversibly absorb and release lithium ions. For example, it may include one or more of a complex of metals selected from cobalt, manganese, nickel, iron, and combinations thereof and lithium.

[0087] As a more specific example, a compound represented by any one of the following chemical formulae may be used as the core of the positive electrode active material: Li a A 1-b R b D2 (where 0.90≤a≤1.8 and 0≤b≤0.5); Li a E 1-b R b O 2-c D c (where 0.90≤a≤1.8, 0≤b≤0.5 and 0≤c≤0.05); LiE 2-b R b O 4-c D c (where 0≤b≤0.5, 0≤c≤0.05); Li a Ni 1-b- c Co b R c D α (where 0.90≤a≤1.8, 0≤b≤0.5, 0≤c≤0.05 and 0<α≤2); Li a Ni 1-b-c Co b R c O 2-α Z α (where 0.90≤a≤1.8, 0≤b≤0.5, 0≤c≤0.05 and 0<α<2); Li a Ni 1-b-c Co b R c O 2-αZ2 (where 0.90≤a≤1.8, 0≤b≤0.5, 0≤c≤0.05 and 0<α<2); Li a Ni 1-b-c Mn b R c D α (where 0.90≤a≤1.8, 0≤b≤0.5, 0≤c≤0.05 and 0<α≤2); Li a Ni 1-b-c Mn b R c O 2-α Z α (where 0.90≤a≤1.8, 0≤b≤0.5, 0≤c≤0.05 and 0<α<2); Li a Ni 1-b-c Mn b R c O 2-α Z2 (where 0.90≤a≤1.8, 0≤b≤0.5, 0≤c≤0.05 and 0<α<2); Li a Ni b E c G d O2 (where 0.90≤a≤1.8, 0≤b≤0.9, 0≤c≤0.5 and 0.001≤d≤0.1); Li a Ni b Co c Mn d G e O2 (where 0.90≤a≤1.8, 0≤b≤0.9, 0≤c≤0.5, 0≤d≤0.5 and 0≤e≤0.1); Li a NeG b O2 (where 0.90≤a≤1.8 and 0.001≤b≤0.1); Li a CoG b O2 (where 0.90≤a≤1.8 and 0.001≤b≤0.1); Li a MnG b O2 (where 0.90≤a≤1.8 and 0.001≤b≤0.1); Li a Mn b O4 (where 0.90≤a≤1.8 and 0.001≤b≤0.1); QO2; QS2; LiQS2; V2O5; LiV2O5; LiTO2; LiNiVO4; Li (3-f) J2(PO4)3(where 0≤f≤2);Li (3-f) Fe2(PO4)3 (where 0≤f≤2); and LiFePO4.

[0088] In the above chemical formula, A is Ni, Co, Mn or a combination thereof; R is Al, Ni, Co, Mn, Cr, Fe, Mg, Sr, V, a rare earth element or a combination thereof; D is O, F, S, P or a combination thereof; E is Co, Mn or a combination thereof; Z is F, S, P or a combination thereof; G is Al, Cr, Mn, Fe, Mg, La, Ce, Sr, V or a combination thereof; Q is Ti, Mo, Mn or a combination thereof; T is Cr, V, Fe, Sc, Y or a combination thereof; J is V, Cr, Mn, Co, Ni, Cu or a combination thereof.

[0089] In one embodiment, the positive active material may have a particle size of about 0.01 μm to 50 μm, and may have a form of secondary particles aggregated by agglomeration of a plurality of particles.

[0090] There is no particular limitation on the conductive material contained in the positive electrode for an all-solid-state battery, as long as it has conductivity and does not cause any chemical changes in the battery, for example, it is selected from one or a mixture of two or more of the following: graphite, such as natural graphite or artificial graphite; carbon black, such as carbon black, acetylene black, Ketjen black, channel black, furnace black, lamp black or summer black; conductive fibers, such as vapor grown carbon fibers (VGCF) or metal fibers; fluorinated carbon powder; metal powder, such as aluminum powder or nickel powder; conductive whiskers, such as zinc oxide or potassium titanate; conductive metal oxides, such as titanium oxide; and conductive materials, such as polyphenyl derivatives.

[0091] According to one embodiment of the present invention, based on 100% by weight of the positive electrode for all-solid-state batteries, the positive electrode for all-solid-state batteries may include 0% to 30% by weight of conductive material. According to a specific embodiment of the present invention, the content of the conductive material may be more than 0.5% by weight, more than 1% by weight, more than 3% by weight, or more than 5% by weight within the above range, or less than 15% by weight, less than 10% by weight, less than 7% by weight, or less than 5% by weight. For example, based on 100% by weight of the positive electrode for all-solid-state batteries, the content of the conductive material may be 0.5% to 5% by weight. When the content of the conductive material exceeds the above upper limit, the energy density is reduced due to the low percentage of active materials, and when the content of the conductive material is lower than the above lower limit, the capacity utilization rate is reduced due to the electronic conductivity being lower than the required level.

[0092] For example, the solid electrolyte contained in the positive electrode for an all-solid-state battery may be a sulfide-based solid electrolyte, wherein the sulfide-based solid electrolyte may be represented by the following formula 2.

[0093] [Formula 2]

[0094] Li k M 2 l S m X 2n ,

[0095] wherein, M 2 is Sn, Mg, Ba, B, Al, Ga, In, Si, Ge, Pb, N, P, As, Sb, Bi, Ti, V, Cr, Mn, Fe, Co, Ni, Cu, Y, Zr, Nb, Mo, Tc, Ru, Rh, Pd, Ag, Hf, Ta, W or La, X 2 is F, Cl, Br, I, Se, Te or O, and 0 < k ≤ 6, 0 < l ≤ 6, 0 < m ≤ 6 and 0 ≤ n ≤ 6.

[0096] For example, in Formula 2, M 2 may be B, Si, Ge, P or N.

[0097] For example, in Formula 2, X 2 may be F, Cl, Br, I or O.

[0098] For example, the sulfide-based solid electrolyte represented by Formula 2 may be one or more selected from the group consisting of: Li2S-P2S5, Li2S-P2S5-LiX (where X is a halogen atom), Li2S-P2S5-Li2O, Li2S-P2S5-Li2O-LiI, Li2S-SiS2, Li2S-SiS2-LiI, Li2S-SiS2-LiBr, Li2S-SiS2-LiCl, Li2S-SiS2-B2S3-LiI, Li2S-SiS2-P2S5-LiI, Li2S-B2S3, Li2S-P2S5-Z m S n (where m and n are integers, and Z is any one selected from Ge, Zn or Ga), Li2S-GeS2, Li2S-SiS2-Li3PO4, Li2S-SiS2-Li p MO q (where p and q are positive numbers, and M is any one selected from P, Si, Ge, B, Al, Ga or In), Li 7-x PS 6-x Cl x (where 0 ≤ x ≤ 2), Li 7-x PS 6-x Br x (where 0 ≤ x ≤ 2) and Li 7-x PS 6-x I x (where 0 ≤ x ≤ 2).

[0099] In addition, the sulfide-based solid electrolyte may preferably be an argyrodite-type solid electrolyte containing one or more selected from the group consisting of Li6PS5Cl, Li6PS5Br and Li6PS5I.

[0100] The positive electrode for an all-solid-state battery according to one embodiment of the present invention may include a current collector and a positive electrode active material layer formed on at least one side of the current collector, wherein the positive electrode active material layer may include the above-mentioned binder, solid electrolyte, conductive material and positive electrode active material.

[0101] The positive electrode can be manufactured according to methods well known in the art, although not limited to a specific manufacturing method, but for example, can be manufactured by mixing a positive electrode active material, a solid electrolyte, a conductive material and a binder in a solvent to produce a slurry-based positive electrode mixture, and then applying the positive electrode mixture to a positive electrode current collector.

[0102] The positive electrode current collector is usually manufactured to a thickness of 3 μm to 500 μm. There is no particular limitation on this type of positive electrode current collector, as long as it has high conductivity without causing chemical changes in the battery, for example, stainless steel, aluminum, nickel, titanium, calcined carbon, or aluminum or stainless steel surface treated with carbon, nickel, titanium, silver. The current collector may also have microscopic irregularities formed on its surface to increase the adhesion of the positive electrode active material, and may be in the form of a film, sheet, foil, mesh, porous material, foam, non-woven material, etc.

[0103] In addition to the above-mentioned positive electrode active material, solid electrolyte, conductive material and binder, the positive electrode may further include additives such as fillers, coating agents, dispersants or ion conductive aids. As fillers, coating agents, dispersants or ion conductive aids, materials known to be commonly used for electrodes for all-solid-state secondary batteries can be used.

[0104] For example, the thickness of the positive electrode may be 70 μm to 150 μm.

[0105] <All-solid-state battery>

[0106] Another embodiment of the present invention provides an all-solid-state battery, which includes a positive electrode, a negative electrode, and a solid electrolyte layer arranged between the positive electrode and the negative electrode, wherein the positive electrode is the above-mentioned positive electrode for the all-solid-state battery.

[0107] Since the positive electrode contained in the all-solid-state battery has been described in detail above, the negative electrode and solid electrolyte contained in the all-solid-state battery will be described in detail below.

[0108] For example, the solid electrolyte layer provided between the positive electrode and the negative electrode may include a sulfide-based solid electrolyte. The sulfide-based solid electrolyte may be the same as or different from the sulfide-based solid electrolyte contained in the positive electrode.

[0109] For specific information on sulfide-based solid electrolytes, see the cathode section above.

[0110] The elastic modulus or Young's modulus of the solid electrolyte may be, for example, 35 GPa or less, 30 GPa or less, 27 GPa or less, 25 GPa or less, or 23 GPa or less. The elastic modulus or Young's modulus of the solid electrolyte is, for example, 10 GPa to 35 GPa, 15 GPa to 35 GPa, 15 GPa to 30 GPa, or 15 GPa to 25 GPa. By making the elastic modulus of the solid electrolyte within this range, it is easier to achieve pressing and / or sintering of the solid electrolyte.

[0111] The solid electrolyte layer also includes, for example, a binder. For example, the binder contained in the solid electrolyte layer may be styrene-butadiene rubber (SBR), polytetrafluoroethylene, polyvinylidene fluoride or polyethylene, or any other binder used in the art. The binder of the solid electrolyte layer may be the same or different from the binder of the positive electrode active material layer and the negative electrode active material layer.

[0112] Then, the negative electrode of the all-solid-state battery may include a negative electrode current collector and a negative electrode active material layer.

[0113] The thickness of the negative electrode active material layer is, for example, less than 50%, less than 40%, less than 30%, less than 20%, less than 10% or less than 5% of the thickness of the positive electrode active material layer. The thickness of the negative electrode active material layer is, for example, 1 μm to 20 μm, 2 μm to 10 μm, or 3 μm to 7 μm. If the thickness of the negative electrode active material layer is too thin, the lithium dendrites formed between the negative electrode active material layer and the negative electrode current collector may cause the negative electrode active material layer to collapse, making it difficult to improve the cycle characteristics of the all-solid-state battery. If the thickness of the negative electrode active material layer is excessively increased, the energy density of the all-solid-state battery is reduced, and the internal resistance of the all-solid-state battery is increased due to the negative electrode active material layer, making it difficult to improve the cycle characteristics of the all-solid-state battery.

[0114] The negative electrode active material layer contains, for example, a negative electrode active material that forms an alloy or a compound with lithium.

[0115] For example, the negative electrode active material contained in the negative electrode active material layer has, for example, a particle shape. The granular negative electrode active material has, for example, an average particle size of less than 4 μm, less than 3 μm, less than 2 μm, less than 1 μm, less than 900 nm. The average particle size of the negative electrode active material is, for example, 10 nm to less than 4 μm, 10 nm to less than 3 μm, 10 nm to less than 2 μm, 10 nm to less than 1 μm, or 10 nm to less than 900 nm. The average particle size of the negative electrode active material may be within this range to promote the reversible absorption and / or desorption of lithium during charging and discharging. For example, the average particle size of the negative electrode active material is the volume equivalent median diameter (D50) measured using a laser particle size distribution instrument.

[0116] The negative electrode active material contained in the negative electrode active material layer includes, for example, one or more selected from carbon-based negative electrode active materials and metal or semi-metal negative electrode active materials.

[0117] The carbon-based negative electrode active material is particularly amorphous carbon. For example, amorphous carbon is carbon black (CB), acetylene black (AB), furnace black (FB), Ketjen black (KB) or graphene, but it is not limited thereto and may be any carbon classified as amorphous carbon in the art. Amorphous carbon is non-crystalline or very low-crystallinity carbon, which is different from crystalline carbon or graphite carbon.

[0118] The metal or semi-metal negative electrode active material includes one or more selected from the group consisting of gold (Au), platinum (Pt), palladium (Pd), silicon (Si), silver (Ag), aluminum (Al), bismuth (Bi), tin (Sn) and zinc (Zn), but is not limited thereto, as long as the metal or semi-metal negative electrode active material can form an alloy or compound with lithium in the art. For example, nickel (Ni) is not a metal negative electrode active material because it cannot form an alloy with lithium.

[0119] The negative electrode active material layer may contain one negative electrode active material, or a mixture of multiple different negative electrode active materials. For example, the negative electrode active material layer may contain only amorphous carbon, or may contain one or more selected from the group consisting of gold (Au), platinum (Pt), palladium (Pd), silicon (Si), silver (Ag), aluminum (Al), bismuth (Bi), tin (Sn) and zinc (Zn). Alternatively, the negative electrode active material layer contains amorphous carbon and a mixture of one or more selected from the group consisting of gold (Au), platinum (Pt), palladium (Pd), silicon (Si), silver (Ag), aluminum (Al), bismuth (Bi), tin (Sn) and zinc (Zn). For example, the mixing ratio of amorphous carbon to silver (Ag) is 10:1 to 1:2, 5:1 to 1:1 or 4:1 to 2:1 by weight, but it is not limited thereto and can be selected according to the characteristics required for the all-solid-state battery. By having a negative electrode active material of this composition, the cycle characteristics of the all-solid-state battery can be further improved.

[0120] The negative electrode active material contained in the negative electrode active material layer includes, for example, a mixture of first particles comprising amorphous carbon and second particles comprising metal or semimetal. The metal or semimetal includes, for example, gold (Au), platinum (Pt), palladium (Pd), silicon (Si), silver (Ag), aluminum (Al), bismuth (Bi), tin (Sn) or zinc (Zn). In addition, the semimetal is a semiconductor. Based on the total weight of the mixture, the content of the second particles is 8% to 60% by weight, 10% to 50% by weight, 15% to 40% by weight, or 20% to 30% by weight. By having the second particles within this content range, the cycle characteristics of, for example, all-solid-state batteries can be further improved.

[0121] The negative electrode active material layer includes, for example, a binder. For example, the binder may be, but need not be limited to, styrene-butadiene rubber (SBR), polytetrafluoroethylene, polyvinylidene fluoride, polyethylene, vinylidene fluoride / hexafluoropropylene copolymer, polyacrylonitrile, polymethyl methacrylate, or any other binder known in the art. The binder may be composed of a single binder or a plurality of different binders.

[0122] By including a binder in the negative electrode active material layer, the negative electrode active material layer can be stabilized on the negative electrode current collector. In addition, although the volume and / or relative position of the negative electrode active material layer changes during the charge and discharge process, the cracking of the negative electrode active material layer can still be suppressed. For example, if the negative electrode active material layer does not include a binder, the negative electrode active material layer is easily separated from the negative electrode current collector. In the case where the negative electrode active material layer is separated from the negative electrode current collector, the negative electrode current collector is exposed to the outside and contacts the solid electrolyte layer, thereby increasing the possibility of a short circuit. For example, the negative electrode active material layer is prepared by applying a slurry of a dispersed material constituting the negative electrode active material layer to the negative electrode current collector and drying it. By including a binder in the negative electrode active layer, a stable dispersion of the negative electrode active material in the slurry can be achieved. For example, when the slurry is applied to the negative electrode current collector by screen printing, clogging of the screen (for example, clogging of agglomerates of the negative electrode active material) can be prevented.

[0123] The negative electrode current collector includes, for example, a material that does not react with lithium (i.e., does not form alloys and compounds). The material constituting the negative electrode current collector may be, for example, copper (Cu), stainless steel, titanium (Ti), iron (Fe), cobalt (Co), nickel (Ni), or any material used as an electrode current collector in the art, but need not be limited thereto. The negative electrode current collector may be composed of one of the above metals or an alloy or cladding material of two or more metals. The negative electrode current collector may be in the form of, for example, a plate or foil.

[0124] The negative electrode active material layer may further include conventional additives used in all-solid-state batteries, such as fillers, dispersants, ion conductors, and the like.

[0125] For example, all-solid-state batteries can be made by fabricating positive electrode, negative electrode, and solid electrolyte layers and then stacking these layers.

[0126] The present invention provides a battery module comprising the above-mentioned all-solid-state battery as a unit cell, a battery pack comprising the battery module, and a device comprising the battery pack as a power source.

[0127] Specific examples of such devices include, but are not limited to, power tools powered by electric motors; electric vehicles, including electric vehicles (EV), hybrid electric vehicles (HEV), plug-in hybrid electric vehicles (PHEV); electric two-wheeled vehicles, including electric bicycles (E-bikes) and electric scooters (E-scooters); electric golf carts; and power storage systems.

[0128] [Example]

[0129] Specific embodiments of the present invention are listed below. However, the following embodiments are only used to specifically illustrate or describe the present invention, and are not intended to limit the present invention. In addition, those skilled in the art are sufficient to infer matters not described, so they are omitted in this article.

[0130] Preparation Example 1: Preparation of Binder for All-Solid State Batteries

[0131] (1) 5.0 g of polybutadiene as a conjugated diene polymer, 0.98 g of 3-mercaptopropionic acid as a compound containing a first hydrogen-bonding functional group, and 0.02 g of 2,2-dimethoxy-2-phenylacetophenone as a photoinitiator were added to 25 ml of dichloromethane as a solvent (the molar ratio of polybutadiene to 3-mercaptopropionic acid was 10:1); the mixed solution was illuminated with a mercury light source with a wavelength of 365 nm (the light source intensity was 85 mW / cm 2 ) and mixed at 300 rpm for 4 hours at room temperature to prepare a solution of a first polymer (PB-COOH) in which a chain side chain containing a carboxyl group is grafted to a polybutadiene side chain.

[0132] (2) 5.0 g of polybutadiene as a conjugated diene polymer, 0.71 g of cysteamine as a compound containing a second hydrogen-bonding functional group, and 0.02 g of 2,2-dimethoxy-2-phenylacetophenone as a photoinitiator were added to a mixed solvent of 25 ml of dichloromethane and 2.5 ml of ethanol (the molar ratio of polybutadiene to cysteamine was 10:1); the mixed solution was illuminated with a mercury light source with a wavelength of 365 nm (the light source intensity was 85 mW / cm 2 ) and mixed at 300 rpm for 4 hours at room temperature to prepare a solution of a second polymer (PB-NH2) in which chain side chains containing amino groups were grafted to polybutadiene side chains.

[0133] (3) The first polymer solution and the second polymer solution prepared above were added to a round-bottom flask, and mixed at 300 rpm for 12 hours at room temperature to prepare a mixed solution of the first polymer and the second polymer. The mixed polymer solution was dried at room temperature to prepare a PB-COOH / PB-NH2 polymer, i.e., a binder for an all-solid-state battery.

[0134] (4) To 10 ml of dichloromethane as a solvent, the PB-COOH / PB-NH2 polymer prepared above, trimethylolpropane tris(3-mercaptopropionic acid) as a crosslinking agent, and 2,2,2-dimethoxy-2-phenylacetophenone as a photoinitiator were added and mixed for 30 minutes to prepare a mixed solution. The mixed solution was dried at room temperature and then irradiated at a wavelength of 365 nm (light intensity of 85 mW / cm 2) The reaction was carried out under irradiation with a mercury light source for 2 hours to prepare a binder for an all-solid-state battery.

[0135] Comparative Preparation Example 1: Preparation of Binder for All-Solid State Batteries

[0136] 5.0 g of polybutadiene as a conjugated diene polymer was added to 25 ml of dichloromethane as a solvent, mixed at 300 rpm at room temperature for 12 hours to prepare a mixed solution, and then the mixed solution was dried at room temperature to prepare a binder for an all-solid-state battery.

[0137] Example 1: Manufacturing of positive electrode for all-solid-state battery

[0138] By using LiNi as the positive electrode active material 0.8 Co 0.1 Mn 0.1 O2, Li6PS5Cl as solid electrolyte, vapor-grown carbon nanofiber (VGCF) as conductive material TM -H, Showa Denko) and the binder prepared in Preparation Example 1 were mixed in a weight ratio of 70:27.5:1:1.5 to prepare a positive electrode slurry, which was applied to one side of an aluminum current collector having a thickness of 15 μm and dried at 60° C. to prepare a positive electrode for an all-solid-state battery.

[0139] Comparative Example 1: Production of positive electrode for all-solid-state battery

[0140] The positive electrode for an all-solid-state battery of Comparative Example 1 was prepared in the same steps as in Example 1, except that the binder prepared in Comparative Preparation Example 1 was used instead of the binder prepared in Preparation Example 1.

[0141] Experimental Example 1: NMR Spectrum Analysis

[0142] The spectra of the adhesives of Preparation Example 1 and Comparative Preparation Example 1 were measured by nuclear magnetic resonance spectroscopy (NMR), and the results were as follows: Figure 3 shown.

[0143] refer to Figure 3 It can be seen that, compared with the adhesive of the comparative preparation example, a hydrogen bonding functional group, a carboxyl group or an amine group is introduced into the conjugated diene polymer of the adhesive of Example 1.

[0144] Experimental Example 2: Evaluation of initial discharge capacity and initial coulombic efficiency of all-solid-state batteries

[0145] The initial discharge capacity and initial coulombic efficiency of the all-solid-state batteries containing the positive electrodes of Example 1 and Comparative Example 1 were evaluated.

[0146] The all-solid-state battery was manufactured by the following method.

[0147] 150 mg of Li6PS5Cl as a fully solid electrolyte was loaded into the molded cell and then granulated at a pressure of 70 MPa. The positive electrodes of Example 1 and Comparative Example 1 prepared by the above process were loaded on one side of the solid electrolyte particles. 0.5 A composite negative electrode in which In and a solid electrolyte were mixed in a weight ratio of 8:2 was loaded on the other side and then pressurized to a pressure of 370 MPa to fabricate an all-solid-state half-cell. In order to analyze the performance of each electrode based on the driving pressure, the tightening strength of the bolts was adjusted so that a driving pressure of 70 MPa or 2 MPa could be applied, respectively. When evaluating the all-solid-state half-cell, the cell was first sealed to prevent gas from penetrating into the interior of the cell, and then the cell was transferred to a constant temperature chamber for electrochemical evaluation.

[0148] For the all-solid-state batteries containing the positive electrodes of Example 1 and Comparative Example 1, the initial discharge capacity can be evaluated by the following test method.

[0149] The battery was charged at a rate of 0.1C (C-rate) until the voltage reached 4.3V (relative to Li), and charging was stopped at 4.3V (relative to Li). The battery was then discharged at a C-rate of 0.1C until the voltage reached 3.0V (relative to Li) during discharge (1st cycle). The results are shown in Tables 1 and Figure 1 shown.

[0150] For the all-solid-state batteries containing the positive electrodes of Example 1 and Comparative Example 1, the initial coulombic efficiency can be measured by the following test method.

[0151] The battery was charged at a rate of 0.1C (C-rate) until the voltage reached 4.3V (relative to Li), and charging was cut off at 4.3V (relative to Li). The battery was then discharged at a C-rate of 0.1C until the voltage reached 3.0V (relative to Li) during discharge (1st cycle). This charge and discharge test was repeated 25 cycles to measure the capacity retention of the discharge capacity, and the results are shown in Tables 1 and 2. Figure 2 shown.

[0152] [Table 1]

[0153] Driving pressure(MPa) Initial discharge capacity (mAh / g) Initial Coulombic efficiency (%) Example 1 2 164.3 78.3 Comparative Example 1 2 154.9 77.5 Example 1 70 163.6 81.5 Comparative Example 1 70 167.1 82.1

[0154] Refer to Table 1 and Figure 1 and Figure 2 It can be seen that the all-solid-state battery containing the positive electrode of Example 1 has excellent initial discharge capacity and initial coulombic efficiency when the driving pressure is low (2MPa) compared with the all-solid-state battery containing the positive electrode of Comparative Example 1. On the other hand, when the driving pressure is high (70MPa), the performance difference between the all-solid-state batteries with the positive electrodes of Example 1 and Comparative Example 1 is not obvious. It can be understood that the "self-healing" adhesive of the present invention can effectively inhibit the interface detachment of the active material and the solid electrolyte that occurs when the driving pressure is low.

[0155] Although the preferred embodiments of the present invention have been described in detail above, the scope of the present invention is not limited thereto, and various modifications and improvements of the basic concept of the present invention defined in the appended claims by those skilled in the art also belong to the scope of the present invention.

Claims

1. An adhesive for an all-solid-state battery, comprising: A first polymer, wherein a chain containing a first hydrogen-bonding functional group is grafted to a side chain on the main chain of the conjugated diene polymer; and A second polymer, wherein the chain containing the second hydrogen-bonding functional group is grafted to the side chain on the main chain of the conjugated diene polymer, in, The first hydrogen-bonding functional group of the first polymer and the second hydrogen-bonding functional group of the second polymer form a hydrogen bond with each other.

2. The binder for all-solid-state batteries according to claim 1, wherein The conjugated diene-based polymer includes repeating units derived from one or more monomers selected from the group consisting of 1,3-butadiene, 2,3-dimethyl-1,3-butadiene, 2-ethyl-1,3-butadiene, 1,3-pentadiene, 2-halogeno-1,3-butadiene and isoprene, wherein halo refers to a halogen atom.

3. The binder for all-solid-state batteries according to claim 1, wherein The molar ratio of the first hydrogen-bonding functional group or the second hydrogen-bonding functional group to the conjugated diene polymer is 100:1 to 100:

30.

4. The binder for all-solid-state batteries according to claim 1, wherein The first hydrogen-bonding functional group is at least one selected from the group consisting of a carboxyl group, a hydroxyl group, an amine group, an amide group, a thioether group, a urea group, a thiourea group, an imidazole group and a sulfonic acid group.

5. The binder for all-solid-state batteries according to claim 1, wherein The second hydrogen-bonding functional group is at least one selected from the group consisting of an amine group, a carbonyl group, a carboxyl group, a hydroxyl group, an amide group, an ester group and a glycidyl group.

6. The binder for all-solid-state batteries according to claim 1, wherein In the first polymer and the second polymer, a compound containing a mercapto group (—SH) is grafted onto the main chain of the conjugated diene-based polymer. 7 . A positive electrode for an all-solid-state battery, comprising the binder according to claim 1 , a conductive material, a positive electrode active material and a solid electrolyte.

8. The positive electrode for an all-solid-state battery according to claim 7, wherein: The solid electrolyte is at least one selected from the group consisting of: Li2S-P2S5; Li2S-P2S5-LiX, wherein X is a halogen atom; Li2S-P2S5-Li2O; Li2S-P2S5-Li2O-LiI; Li2S-SiS2; Li2S-SiS2-LiI; Li2S-SiS2-LiBr; Li2S-SiS2-LiCl; Li2S-SiS2-B2S3-LiI; Li2S-SiS2-P2S5-LiI; Li2S-B2S3; Li2S-P2S5-Z m S n , where m and n are positive numbers, and Z is any one of Ge, Zn and Ga; Li2S-GeS2; Li2S-SiS2-Li3PO4; Li2S-SiS2-Li p MO q , where p and q are positive numbers, M is any one of P, Si, Ge, B, Al, Ga and In; Li 7-x PS 6-x Cl x , where 0≤x≤2; Li 7-x PS 6-x Br x , where 0≤x≤2; and Li 7-x PS 6-x I x , where 0≤x≤2.

9. The positive electrode for an all-solid-state battery according to claim 7, wherein: The solid electrolyte is an argyrodite-type solid electrolyte including one or more selected from the group consisting of Li6PS5Cl, Li6PS5Br and Li6PS5I.

10. An all-solid-state battery, comprising: positive electrode; a negative electrode; and A solid electrolyte layer is provided between the positive electrode and the negative electrode, in, The positive electrode comprises the positive electrode for an all-solid-state battery according to claim 7.

Citation Information

Patent Citations

  • Binder composition for secondary battery, electrode slurry compositon comprising the same, electrode and secondary battery

    KR101970648B1

  • Binder for all-solid-state battery, positive electrode for all-solid-state battery and all-solid-state battery comprising the same

    KR1020240103642A

Cited By

  • Binder for battery and application thereof

    CN119709048A