Electrode assembly including surface-treated separator, secondary battery including same, and method for manufacturing electrode assembly
By performing corona surface treatment on the diaphragm, an alternating structure of adhesive and non-adhesive parts is formed, the problem of easy folding of the diaphragm in the electrode assembly is solved, and the adhesion and electrolyte impregnation performance of the electrode assembly are improved.
Patent Information
- Application Number
- CN202380029164.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-12-02
- Filing Date
- 2023-11-27
- Publication Date
- 2024-11-12
AI Technical Summary
During the manufacturing process, existing electrode assemblies lack adhesion between the diaphragm and the electrode, which makes the diaphragm easy to fold, affecting the electrolyte impregnation and gas release performance.
By treating the corona surface of the diaphragm, an alternating structure of the adhesive part and the non-adhesive part is formed, which enhances the adhesion between the diaphragm and the electrode, while maintaining the impregnation ability of the electrolyte and prevents the diaphragm from folding.
The interface adhesion between the separator and the electrode of the electrode is improved, the impregnation ability of the electrolyte and the stability of the separator are ensured, and the problem of diaphragm folding is avoided.
Smart Images

Figure CN118946997A_ABST
Abstract
Description
Technical Field
[0001] The present application claims the benefit of priority based on Korean Patent Application No. 10-2022-0166693 filed on December 2, 2022, and the entire contents of the Korean Patent Application are incorporated herein by reference.
[0002] The present invention relates to an electrode assembly including a surface-treated separator, a secondary battery including the electrode assembly, and a method of manufacturing the electrode assembly. Background Art
[0003] In recent years, due to the depletion of fossil fuels, the price of energy has continued to rise, environmental pollution is becoming a growing concern, and at the same time, the demand for environmentally friendly alternative energy is becoming an indispensable factor in future life. Therefore, research on various power generation technologies such as nuclear power, solar energy, wind power, and tidal power is being carried out, and power storage devices for more efficient use of generated energy are also attracting great interest.
[0004] In particular, with the development of technology and the increase in demand for mobile devices, the demand for batteries as energy sources is rapidly increasing, and thus, research on batteries that can meet various demands is being conducted.
[0005] In terms of battery shape, there is a high demand for square and pouch-type secondary batteries that can be applied to products such as mobile phones due to their thin thickness, and in terms of materials, there is a high demand for lithium secondary batteries such as lithium-ion batteries and lithium-ion polymer batteries that have advantages such as high energy density, discharge voltage and output stability.
[0006] Generally, a secondary battery is a structure in which an electrode assembly including a positive electrode, a negative electrode and a separator disposed therebetween is embedded in a battery case, and positive and negative electrode tabs are sealed to expose extended positive and negative electrode leads, respectively.
[0007] In addition, the electrode assembly includes a structure in which a positive electrode, a separator, and a negative electrode are sequentially stacked. Figure 1 Schematic diagram illustrating the folding phenomenon of the separator of the electrode assembly. Figure 1 In the electrode assembly 1, the separator 50 is folded due to various process flows occurring during the manufacture of the secondary battery. In particular, the edge region A of the separator 50 is particularly susceptible to folding.
[0008] Figure 2 is a schematic diagram illustrating a front view of a conventional electrode assembly. Figure 2The folded electrode assembly 1 is a structure including a positive electrode 30, a negative electrode 40, and a sheet-like separator sheet 60 formed by winding a plurality of unit cells, and a separator 50 is interposed between the positive electrode 30 and the negative electrode 40. Here, the unit cell includes an A-type dual cell 10 stacked in the order of positive electrode 30 / separator 50 / negative electrode 40 / separator 50 / positive electrode 30, and a C-type dual cell 20 stacked in the order of negative electrode 40 / separator 50 / positive electrode 30 / separator 50 / negative electrode 40.
[0009] Since there is no separate adhesive layer on the separator 50, the conventional electrode assembly 1 has a problem of low adhesion between the electrode and the separator 50. In order to solve this problem, the unit cell having the stacked electrodes and the separator 50 is sometimes laminated, hot-pressed, etc. to achieve excessive dry adhesion. However, in this case, although the adhesion between the electrode of the unit cell and the separator 50 can be greatly improved, processes such as lamination or hot pressing are performed on the front surface of the electrode and the separator 50, which greatly reduces electrolyte impregnation and gas release, and may cause performance degradation of the secondary battery such as Li plating.
[0010] Therefore, it is necessary to develop a method that can improve the adhesion between the separator and the electrode interface while providing good electrolyte impregnation and preventing the separator from folding. Summary of the invention
[0011] Technical issues
[0012] The present invention is directed to solving the above-mentioned problems and provides an electrode assembly capable of preventing a separator from being folded, a secondary battery including the electrode assembly, and a method of manufacturing the electrode assembly.
[0013] Technical Solution
[0014] The present invention provides an electrode assembly suitable for a secondary battery. In one embodiment, the electrode assembly according to the present invention is a structure having n stacked unit cells including a positive electrode, a negative electrode, and a separator interposed between the positive electrode and the negative electrode, wherein n is an integer greater than or equal to 2, and the separator sheet is disposed between the unit cells. For example, n is an integer in the range of 2 to 20. The separator embedded in the unit cell includes a corona surface-treated adhesive portion and a non-corona surface-treated non-adhesive portion, wherein the separator sheet is a structure that has not been corona surface-treated.
[0015] The present invention also provides a secondary battery including the electrode assembly. For example, the secondary battery is a pouch-type secondary battery.
[0016] In addition, the present invention provides a method for manufacturing an electrode assembly for a secondary battery. In one embodiment, the method for manufacturing an electrode assembly according to the present invention includes the following steps: performing corona discharge on one or both sides of the diaphragm for surface treatment; forming a unit cell including a positive electrode, a negative electrode, and a diaphragm sheet inserted between the positive electrode and the negative electrode; and manufacturing the electrode assembly by positioning n unit cells (where n is an integer greater than or equal to 2) on a sheet-like diaphragm sheet and winding the diaphragm sheet in one direction. Here, the diaphragm embedded in the unit cell includes a bonding portion after the corona surface and a non-bonding portion after the non-corona surface. In addition, the diaphragm sheet is a structure that has not been corona surface treated.
[0017] Beneficial Effects
[0018] The present invention increases the interfacial adhesion between electrodes and separators forming an electrode assembly without reducing their impregnation ability with electrolytes. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] Figure 1 is a schematic diagram illustrating a separator folding phenomenon occurring in a conventional electrode assembly.
[0020] Figure 2 is a schematic diagram illustrating a stacked structure of a conventional electrode assembly.
[0021] Figure 3 is a schematic diagram illustrating a stacked structure of an electrode assembly according to one embodiment.
[0022] Figure 4 is a schematic diagram illustrating a process for manufacturing an electrode assembly.
[0023] Figure 5 is a schematic diagram illustrating an electrode stack structure according to one embodiment.
[0024] Figure 6 is a schematic diagram illustrating a bonding pattern of a separator located inside a unit cell according to one embodiment.
[0025] Figure 7 is a schematic diagram illustrating a stacked structure of an electrode assembly according to one embodiment.
[0026] Figure 8 is a schematic diagram illustrating a bonding pattern of a separator according to one embodiment.
[0027] Fig. 9 It is a schematic diagram illustrating a process of corona treating the surface of the separator. DETAILED DESCRIPTION
[0028] The present invention provides an electrode assembly suitable for a secondary battery. In one embodiment, the electrode assembly according to the present invention is a structure having n stacked unit cells including a positive electrode, a negative electrode, and a separator interposed between the positive electrode and the negative electrode, wherein n is an integer greater than or equal to 2, and the separator sheet is disposed between the unit cells. For example, n is an integer in the range of 2 to 20. The separator embedded in the unit cell includes an adhesive portion that has been subjected to a corona surface treatment and a non-adhesive portion that has not been subjected to a corona surface treatment, wherein the separator sheet is a structure that has not been subjected to a corona surface treatment.
[0029] In one embodiment, the separator sheet is wound between the stacked unit cells and wrapped around the unit cells. Therefore, the electrode assembly according to the present invention forms a stacked and folded structure.
[0030] In one example, in an electrode assembly according to the present invention, a unit cell includes an A-type dual cell and a C-type dual cell; a diaphragm sheet of the unit cell includes an adhesive portion that has been corona surface treated and a non-adhesive portion that has not been corona surface treated; and a plurality of A-type dual cells and a plurality of C-type dual cells are alternately arranged up and down with the diaphragm sheet between them.
[0031] In one embodiment, the unit cell includes: a positive electrode terminal extending in a first direction of the positive electrode; and a negative electrode terminal extending in a first direction of the negative electrode. Here, the direction in which the positive electrode terminal is formed and the direction in which the negative electrode terminal is formed may be the same, or may be opposite to each other. In addition, the separator includes: a first adhesive portion in which a corona surface treatment is performed at an edge region where the positive electrode terminal is located; and a second adhesive portion in which a corona surface treatment is performed at an edge region where the negative electrode terminal is located.
[0032] In one embodiment, the surface of the separator is a structure in which adhesive portions and non-adhesive portions are alternately arranged.
[0033] In another embodiment, the adhesive portion is formed on one or both sides of the diaphragm.
[0034] In a specific example, the area in which the bonding portion is formed is in the range of 10% to 70% of the area of the diaphragm.
[0035] In another specific example, the bonding portion forms a pattern. The pattern is at least one of stripes, grids, dots, and polygons.
[0036] In addition, the present invention provides a secondary battery including the electrode assembly described above. For example, the secondary battery is a pouch-type secondary battery.
[0037] The present invention also provides a method for manufacturing an electrode assembly for a secondary battery. In one embodiment, the method for manufacturing an electrode assembly according to the present invention comprises the following steps:
[0038] Surface treatment is performed by applying a corona discharge to one or both sides of the diaphragm;
[0039] forming a unit cell including a positive electrode, a negative electrode, and a separator interposed between the positive electrode and the negative electrode; and
[0040] A method for manufacturing an electrode assembly includes: arranging n unit cells on a sheet-like diaphragm, wherein n is an integer greater than or equal to 2; and winding the diaphragm in one direction.
[0041] Here, the separator embedded in the unit cell includes a bonded portion that has been subjected to corona surface treatment and a non-bonded portion that has not been subjected to corona surface treatment. In addition, the separator sheet is a structure that has not been subjected to corona surface treatment.
[0042] In one embodiment, the surface treatment is performed by electrifying the surface of the diaphragm via a plasma generator.
[0043] In a specific example, in the case of corona discharge, the discharge range is in the range of 1.0 kV to 3.0 kV.
[0044] In another specific example, during corona discharge, the discharge is at 30 W·min / m 2 Up to 300W·min / m 2 within the range. DETAILED DESCRIPTION
[0046] The present invention can have various modifications and various embodiments, and therefore the specific embodiments thereof will be described in detail below. However, it should be understood that the present invention is not limited to the specific embodiments, and includes all modifications, equivalents or alternatives within the spirit and technical scope of the present invention.
[0047] The terms "comprising", "including" and "having" used herein indicate the presence of characteristics, quantities, steps, actions, parts or components or combinations thereof described in the specification, and it should be understood that the possibility of the presence or addition of one or more other characteristics, quantities, steps, actions, parts, components or combinations thereof is not precluded. In addition, in the present invention, when a portion of a layer, film, region, plate, etc. is disposed "on" another portion, this includes not only the case where a portion is "directly disposed on another portion", but also the case where another portion is interposed therebetween. On the contrary, when a portion of a layer, film, region, plate, etc. is disposed "under" another portion, this includes not only the case where a portion is "directly disposed under another portion", but also the case where another portion is interposed therebetween. In addition, in the present application, "on" may include not only the case where it is disposed on the upper portion, but also the case where it is disposed on the lower portion.
[0048] In the present invention, the X-axis direction refers to a direction perpendicular to a direction in which an electrode joint (positive electrode or negative electrode) in an electrode assembly having a stacked structure protrudes, the Y-axis direction refers to a direction in which an electrode joint (positive electrode or negative electrode) protrudes, and the Z-axis direction refers to a direction perpendicular to the X-axis and Y-axis directions.
[0049] The present invention provides an electrode assembly, a lithium secondary battery including the electrode assembly, and a method for manufacturing the electrode assembly.
[0050] A conventional stacked or stacked / folded electrode assembly includes a diaphragm sheet and a plurality of unit cells stacked by the diaphragm sheet. The unit cell has a positive electrode and a negative electrode alternately stacked with a diaphragm interposed therebetween. If a separate adhesive layer is not formed on the diaphragm inside the unit cell of the folded electrode assembly, the diaphragm-electrode interface is peeled off by various flows in the process, resulting in the problem of folding the diaphragm. In addition, in order to improve the adhesion between the diaphragm and the electrode interface, sometimes excessive dry bonding is achieved when processes such as lamination or hot pressing are performed on the entire surface of the diaphragm, which can greatly increase the adhesion between the electrode and the diaphragm of the unit cell, but the impregnation and gas release performance of the electrolyte are greatly reduced, and performance degradation factors of secondary batteries such as Li plating may occur.
[0051] Therefore, the present invention is an electrode assembly having a structure in which a plurality of unit cells including a positive electrode, a negative electrode, and a separator interposed between the positive electrode and the negative electrode are wound into a sheet-like separator sheet, wherein the separator of the unit cell includes a bonding portion that has been corona surface treated, wherein the bonding portion forms a bonding portion in an edge area where an electrode joint is located to improve the adhesion of the edge area of the separator, and allows a viscous solution to be impregnated between non-bonding portions in which no bonding portion is formed to ensure wetting.
[0052] Hereinafter, an electrode assembly according to the present invention and a method for manufacturing a lithium secondary battery and the electrode assembly including the same will be described in detail.
[0053] Figure 3 is a front view of an electrode assembly according to one embodiment of the present invention, and Figure 4 is a perspective view of an electrode assembly manufactured by winding sequentially arranged unit cells on a separator sheet. Figure 3 and Figure 4The electrode assembly 100 of the present invention comprises a positive electrode 130, a negative electrode 140 and a plurality of unit cells with a separator 150 inserted between the positive electrode 130 and the negative electrode 140, wherein the unit cells comprise a plurality of A-type dual cells 110 and a plurality of C-type dual cells 120; the separator (150) of the unit cells comprises an adhesive portion (151) subjected to a corona surface treatment and a non-adhesive portion (152) not subjected to a corona surface treatment; wherein the plurality of A-type dual cells (110) and the plurality of C-type dual cells (120) are alternately arranged up and down with a separator sheet (160) therebetween, but the separator sheet (160) is not subjected to a corona surface treatment.
[0054] Specifically, the electrode assembly 100 is a structure in which a plurality of unit cells are stacked, and the unit cells include an A-type dual cell 110 and a C-type dual cell 120. The A-type dual cell 110 has a structure in which a positive electrode 130, a separator 150, a negative electrode 140, a separator 150, and a positive electrode 130 are sequentially stacked, and the C-type dual cell 120 has a structure in which a negative electrode 140, a separator 150, a positive electrode 130, a separator 150, and a negative electrode 140 are sequentially stacked. The unit cells having such a stacking structure are stacked face to face with the separator sheet 160 interposed therebetween, thereby forming a structure such as Figure 3 The structure shown.
[0055] The electrode assembly 100 of the present invention is applicable to any structure in which unit cells are stacked, but as an example, may be a stacked structure, a stacked / folded structure, or a laminated / stacked structure.
[0056] The separator 150 of the unit cell of the present invention may include a corona surface-treated adhesive portion 151, which may improve the adhesion between the separator 150 and the electrode. In addition, the separator 150 of the unit cell of the present invention may include a non-adhesive portion 152 that is not corona surface-treated, which may impregnate electrolyte between electrodes facing each other above and below the non-adhesive portion 152 that is not corona surface-treated, and the adhesive portion 151 and the non-adhesive portion 152 may form a pattern to prevent electrolyte or bubbles from being trapped.
[0057] In addition, the diaphragm 160 is not subjected to a corona surface treatment. The electrode assembly of the present invention is a structure in which the diaphragm sheet 160 is stacked with a unit cell. The diaphragm sheet 160 facing up and down with the positive electrode 130 or the negative electrode 140 of the unit cell is relatively less likely to fold compared to the diaphragm 150 inside the unit cell due to the reduction in adhesion. On the other hand, in some cases, the electrolyte impregnation between the diaphragm sheet 160 and the electrode may be problematic. Therefore, instead of applying a corona surface treatment to the diaphragm sheet 160 to improve the adhesion between the unit cell and the electrode, the diaphragm sheet 160 is not subjected to a corona surface treatment to improve the electrolyte impregnation capability.
[0058] Figure 5 is a schematic diagram illustrating a side view of an electrode assembly according to one embodiment of the present invention, and Figure 6 is a schematic diagram illustrating a bonding pattern of a separator located inside a unit cell according to one embodiment of the present invention. Figure 5 and Figure 6 , the unit cell of the present invention includes a positive electrode tab 131 extending in one direction of the positive electrode 130 and a negative electrode tab 141 extending in one direction of the negative electrode 140. The separator 150 of the present invention includes a first adhesive portion 151a formed by corona surface treatment on the edge area where the positive electrode tab 131 is located, and a second adhesive portion 151b formed by corona surface treatment on the edge area where the negative electrode tab 141 is located. In the electrode assembly 100 in the stacked form of the present invention, the area where the interface adhesion between the separator 150 of the unit cell and the electrode is weak is the edge area of the separator 150 located in the direction where the electrode tab protrudes. In the process of the electrode assembly, there is a problem that the electrode tab may bend to form a gap between the separator 150 and the electrode, and the gap causes the separator 150 to fold. Therefore, the present invention is characterized in that a corona surface-treated adhesive portion 151 is included on the separator 150 of the unit cell, but the corona surface treatment is performed on the edge area where the electrode tab is located.
[0059] Specifically, the separator 150 may include a first adhesive portion 151a that is subjected to a corona surface treatment on the edge region where the positive electrode tab 131 is located and a second adhesive portion 151b that is subjected to a corona surface treatment on the edge region where the negative electrode tab 141 is located to increase the adhesiveness of the edge region where the positive electrode tab 131 is located, thereby solving the problem of folding of the separator 150 of the unit cell. In addition, a non-corona patterned non-adhesive portion 152 is provided in the region between the first adhesive portion 151a and the second adhesive portion 151b, so that the electrolyte flowing to the non-adhesive portion 152 can be smooth, thereby improving electrolyte impregnation.
[0060] In a specific example, the adhesive portion 151 of the present invention may be formed on one side or both sides of the diaphragm 150. Figures 3 to 5 It is illustrated that the adhesive portion 151 is formed on both sides of the separator 150, but it is obvious that the adhesive portion 151 may be formed only on one side of the separator 150. However, if the adhesive portion 151 is formed only on one side of the separator 150, the impregnation ability of the electrolyte may be increased, but the adhesion between the electrode tab where the adhesive portion 151 is not formed and the other side of the separator 150 may be reduced, so it is preferable to form the adhesive portion 151 on both sides of the separator 150.
[0061] In addition, the separator 150 of the unit cell of the present invention may have the same shape as the coating portion. When assembled in this manner, since the separator 150 used in one unit cell is the same, the process time for manufacturing the electrode assembly 100 may be relatively shortened, thereby improving productivity.
[0062] In addition, the adhesive portion 151 may be in the range of 10% to 70% of the total area of the separator 150, preferably in the range of 20% to 60%, and more preferably in the range of 30% to 50%. If the adhesive portion 151 is less than 10% of the total area of the separator 150, the area required for bonding to the electrode may not be sufficient to ensure sufficient adhesion. In addition, if the adhesive portion 151 is greater than 70% of the total area, the non-adhesive portion 152 may have a smaller area, resulting in less electrolyte flow, which may lead to more frequent capture.
[0063] Furthermore, the bonding part 151 forms a regular pattern on the separator 150, wherein the pattern may be formed in one or more of a stripe pattern, a grid pattern, a dot pattern, and a polygonal pattern. Preferably, in order to improve the productivity and internal flow of the electrolyte, the contact assembly is formed in a stripe pattern.
[0064] In addition, the number of repetitions of the pattern in the separator 150 is preferably 1 to 4. If the number of repetitions of the pattern exceeds 4, the pattern of the coating portion in the separator 150 becomes too detailed and productivity of the electrode assembly 100 decreases.
[0065] In addition, if the separator 150 of the present invention is used as a separator in a lithium secondary battery, the separator 150 of the present invention can be used without any specific restrictions, and it is particularly desirable that the separator 150 has a low resistance to the ion migration of the electrolyte and an excellent ability to wet the electrolyte. Specifically, a porous polymer film made of a polyolefin-based polymer such as an ethylene homopolymer, a propylene homopolymer, an ethylene / butene copolymer, an ethylene / hexene copolymer, and an ethylene / methacrylate copolymer can be used, or a laminated structure of two or more layers thereof can be used. In addition, conventional porous non-woven fabrics can be used, such as non-woven fabrics made of high melting point glass fibers, polyethylene terephthalate fibers, etc. In addition to the above materials, a polymer with high heat resistance can also be used to manufacture the separator 150. In addition, the separator 150 of the present invention can be a composite porous safety enhanced separator (SRS) separator. In a specific example, the SRS separator can be manufactured using inorganic particles and a binder polymer as an active layer component on a polyolefin-based or polyester-based separator substrate. In addition, the separator 150 may be a porous thin film having a pore size of 0.01 μm to 10 μm and a thickness of 5 μm to 300 μm.
[0066] In addition, the separator 160 of the present invention may also include one or more mixtures selected from any of the aforementioned materials.
[0067] In addition, the corona surface treatment source can be air, oxygen (O2) or nitrogen (N2). In the corona surface treatment, the significant improvement of wettability is achieved by the synergistic effect of the physical surface modification of the discharge itself and the chemical surface modification by generating functional groups. This chemical surface modification occurs when high-energy electrons or ions collide and generate free radicals or ions on the diaphragm 150 substrate, and the surrounding air, oxygen, nitrogen, ozone, moisture, etc. react with them, introducing polar functional groups such as carbonyl, carboxyl, hydroxyl, cyano, etc. to cause chemical surface modification.
[0068] In addition, the corona surface treatment source can perform corona treatment using plasma with a polymer, that is, when particles with high energy in a plasma state collide with the surface of the diaphragm 150 substrate, energy is transferred to the colliding surface of the diaphragm 150, and the diaphragm 150 can be chemically or physically activated to improve the adhesion between the layers of the polymer mixture.
[0069] In addition, the binder polymer mixture may include a porous inorganic filler and a binder polymer. By adding an inorganic filler to the binder polymer mixture, the mechanical strength of the separator 150 may be increased, thereby ensuring the safety of the battery by external force, etc. Such a separator 150 may simultaneously improve the electrochemical safety and performance of the battery by connecting and fixing the inorganic filler due to the binder polymer and forming a heat-resistant pore structure due to the interstitial volume between the inorganic fillers.
[0070] The concentration of the inorganic filler may be 60 wt % to 90 wt %, preferably 70 wt % to 80 wt % based on the weight of the polymer mixture layer. If the concentration of the inorganic filler is too low, the required mechanical strength cannot be maintained, and conversely, if the concentration of the inorganic filler is too high, the porosity of the separator 150 cannot be ensured due to the excessive amount of inorganic components, which results in a decrease in ionic conductivity and thus an increase in internal resistance.
[0071] Figure 7 is a perspective view illustrating a side view of an electrode assembly according to another embodiment of the present invention, and Figure 8 is a perspective view illustrating a bonding pattern of a separator located inside a unit cell according to another embodiment of the present invention. Figure 7 and Figure 8The electrode assembly 200 of the present invention is a structure in which a separator sheet 260 is provided between stacked unit cells. Here, the unit cells include an A-type dual cell 210 stacked in the order of positive electrode 230 / separator 250 / negative electrode 240 / separator 250 / positive electrode 230, and a C-type dual cell 220 stacked in the order of negative electrode 240 / separator 250 / positive electrode 230 / separator 250 / negative electrode 240.
[0072] The separator 250 of the present invention has a structure in which the adhesive portion 251 and the non-adhesive portion 252 are alternately arranged with each other, but includes a third adhesive portion located between the first adhesive portion 251a and the second adhesive portion 251b, wherein the third adhesive portion may be n (n is an integer greater than or equal to 1). In other words, the separator 250 may include a third adhesive portion 251c between the first adhesive portion 251a formed by corona surface treatment on the edge region where the positive electrode tab 231 is located and the second adhesive portion 251b formed by corona surface treatment on the edge region where the negative electrode tab 241 is located, wherein the third adhesive portion 251c may be one or more. Figure 7 The electrode assembly 200 having one third adhesive portion 251c formed between the first adhesive portion 251a and the second adhesive portion 251b is illustrated but not limited thereto. By further forming the third adhesive portion 251c on the surface of the separator 250 in this manner, the interfacial adhesion between the central region of the separator 250 and the electrode, and between the edge region of the separator 250 and the electrode can be increased. However, if the area of the third adhesive portion 251c is too large, or if the number of the third adhesive portions 251c is large, the electrolyte impregnation capability may be deteriorated, and therefore it is desirable to appropriately form the third adhesive portion 251c according to the purpose.
[0073] Fig. 9 Schematic diagram of a plasma generator for corona treatment of the surface of a diaphragm according to an embodiment of the present invention. Fig. 9 The diaphragm 150 subjected to corona surface treatment by the plasma generator 170 is the diaphragm 150 inserted into the unit cell, and although Fig. 9 The corona surface treatment on one side of the diaphragm 150 is exemplified, but is not limited thereto, and both sides of the diaphragm 150 may be subjected to the corona surface treatment.
[0074] In a specific example of the present invention, the corona surface treatment uses a plasma generator 170 to electrify the surface of the diaphragm 150. In one example, the apparatus for corona treating the surface of the diaphragm 150 may include a roller portion 171 including a metal member 172 and a plasma generating portion 173, which is spaced apart from the roller portion 171 and generates plasma by interacting with the metal member 172 to irradiate the surface of the diaphragm 150. The plasma generating portion 173 is spaced apart from the diaphragm 150 and generates plasma by interacting with the metal member 172 to irradiate the surface of the diaphragm 150. One type of plasma generated may be plasma generated by corona discharge. Specifically, the plasma generating portion 173 includes a main body 174 spaced apart from the roller portion 171, an electrode member 175 connected to the main body 174 and generating plasma on the surface of the diaphragm 150 at a position facing the metal member 172 to form an adhesive layer on the surface of the diaphragm 150, and a guide member 176 that fixes the electrode member 175 and the main body 174 or moves the position of the electrode member 175 to a direction (TD direction) perpendicular to the conveying direction of the diaphragm 150.
[0075] The body 174 is elongated in a direction (TD direction) perpendicular to the conveying direction of the diaphragm 150, and may have a length corresponding to or longer than the width length of the diaphragm 150. The body 174 may be composed of a non-metal material.
[0076] The electrode member 175 is provided on the outer surface of the body 174 corresponding to the conveying direction (MD direction) of the diaphragm 150, and may have a structure including a plurality of electrode members arranged side by side in a direction (TD direction) perpendicular to the conveying direction of the diaphragm 150. The electrode member 175 may be provided with at least one pair of electrode members 175 for applying corona surface treatment to the edges positioned on both sides of the conveying direction (MD) of the diaphragm 150, and may be provided with additional electrode members 175 as needed for applying corona surface treatment to the areas other than the edges positioned on the both sides. In this way, by having a plurality of electrode members, an adhesive layer is formed only on the surface of the diaphragm 150 located between the electrode member 175 and the metal member 172, and since plasma is not generated on the surface of the diaphragm 150 without the electrode member 175, a non-adhesive layer is formed to form a patterned adhesive layer in the form of stripes.
[0077] As a specific example, the electrode member 175 may be a corona discharge electrode. The corona discharge electrode may stably generate plasma that interacts with the metal member 172 to provide corona surface treatment on the surface of the diaphragm 150.
[0078] The guide member 176 may fix the plurality of electrode members 175 to the body 174, and may move each of the plurality of electrode members 175 in a direction (TD direction) perpendicular to the conveying direction of the diaphragm 150. In a specific example, the guide member 176 may include a guide groove (not shown) extending in a direction (TD direction) perpendicular to the conveying direction of the diaphragm 150 and a fixing member (not shown) engaging and fixing the electrode member 175 in the guide groove. The electrode member 175 is detachable in the guide groove and slidably movable along the guide groove and can be repositioned. Since the electrode member 175 is detachable in the guide groove, the number of electrode members 175 can be adjusted, and since the electrode member 175 can be slidably movable along the guide groove, the position of the electrode member 175 can be adjusted according to the use, thereby adjusting the position of the adhesive layer formed on the surface of the diaphragm 150 and adjusting the pattern width.
[0079] Furthermore, the guide member 176 may include an indicator member (not shown) having scales on its surface in a direction (TD direction) perpendicular to the feeding direction of the diaphragm 150. The indicator member enables accurate confirmation of the position of the electrode member 175, thereby improving the accuracy of the corona surface treatment.
[0080] In a specific example of the present invention, the discharge range of the corona surface treatment may be in the range of 1.0 kV to 3.0 kV, and preferably in the range of 1.5 kV to 2.5 kV. When the discharge range is less than 1.0 kV, it is difficult to perform uniform corona surface treatment on the diaphragm surface, and when the discharge range exceeds 3.0 kV, it may not be easy to operate the corona generating device when performing corona treatment in a fine pattern, so it is preferred to discharge within the above range.
[0081] In addition, in corona surface treatment, the discharge amount can be 30W·min / m 2 Up to 300W·min / m 2 In the range of 100 W·min / m 2 Up to 200W·min / m 2 When the discharge capacity is less than 30W·min / m 2 In the case of 300W·min / m, it may be difficult to achieve the desired effect due to the difficulty in detailed surface treatment of the diaphragm surface, and when the discharge amount is greater than 300W·min / m 2 In the case of , the characteristics of the separator may change, so it is preferred to discharge within the above range.
[0082] In addition, the present invention provides a lithium secondary battery including an electrode assembly as described above. In a specific example, the electrode assembly included in the lithium secondary battery of the present invention is an electrode assembly having a positive electrode, a negative electrode and a plurality of unit cells wound into a sheet-like diaphragm sheet, the unit cells including an A-type dual cell and a C-type dual cell, the diaphragm of the unit cell including an adhesive portion subjected to a corona surface treatment and a non-adhesive portion not subjected to a corona surface treatment, and wherein a plurality of A-type dual cells and a plurality of C-type dual cells are alternately arranged up and down with a diaphragm sheet between them, and the electrode assembly is characterized in that the diaphragm sheet is not subjected to a corona surface treatment.
[0083] The lithium secondary battery of the present invention is a structure in which an electrode assembly is sealed inside a battery housing together with an electrolyte solution. The type of secondary battery is not particularly limited, but as a specific example, it can be a lithium secondary battery such as a lithium ion (Li-ion) secondary battery, a lithium polymer (Li-polymer) secondary battery or a lithium ion polymer (Li-ion polymer) secondary battery, etc., which has advantages such as high energy density, discharge voltage, output stability, etc.
[0084] In the lithium secondary battery of the present invention, the electrode may be a structure in which an electrode active material layer is formed by applying an electrode forming slurry including an electrode active material on an electrode collector. The electrode slurry may be applied to at least one side of a current collector.
[0085] Here, the current collector may be a positive electrode current collector or a negative electrode current collector, and the electrode active material may be a positive electrode active material or a negative electrode active material. In addition, the electrode slurry may further include a conductive material and a binder in addition to the electrode active material.
[0086] In the present invention, the thickness of the positive electrode collector is generally 3 μm to 500 μm. Such a positive electrode collector is not particularly limited as long as it has high conductivity in use without causing chemical changes in the battery core, and for example, stainless steel, aluminum, nickel, titanium, calcined carbon, or surface treatment with carbon, nickel, titanium, silver, etc. on the surface of aluminum or stainless steel can be used. The current collector may also have microscopic irregularities formed on its surface to increase the adhesion of the positive electrode active material, and may be in the form of a film, sheet, foil, net, porous body, foam, non-woven body, etc.
[0087] In the case of a sheet of a negative electrode current collector, it is generally made to have a thickness of 3 μm to 500 μm. Such a negative electrode current collector is not particularly limited as long as it has conductivity during use without causing chemical changes in the battery core, and for example, copper, stainless steel, aluminum, nickel, titanium, calcined carbon, treatment of the surface of copper or stainless steel with carbon, nickel, titanium, silver, etc., aluminum-cadmium alloy, etc. can be used. In addition, as with the positive electrode current collector, fine irregularities can be formed on the surface to strengthen the bonding force of the negative electrode active material, and can be used in various forms such as films, sheets, foils, nets, porous bodies, foams, non-woven bodies, etc.
[0088] The positive electrode active material of the present invention is a material capable of generating an electrochemical reaction, such as a lithium transition metal oxide comprising two or more transition metals, and a layered compound such as lithium cobalt oxide (LiCoO2), lithium nickel oxide (LiNiO2), etc. substituted with one or more transition metals; a lithium manganese oxide substituted with one or more transition metals; a lithium manganese oxide of the formula LiNi 1-y Lithium nickel-based oxides represented by MyO2 (wherein M = Co, Mn, Al, Cu, Fe, Mg, B, Cr, Zn or Ga and including one or more of the above elements, 0.01≤y≤0.7), etc.; Lithium nickel-based oxides represented by the formula Li 1+z Ni b Mn c Co 1-(b+c+d) M d O (2-e) A e Indicated by Li 1+z Ni 1 / 3 Co 1 / 3 Mn 1 / 3 O2、Li 1+z Ni 0.4 Mn 0.4 Co 0.2 Lithium nickel cobalt manganese composite oxides such as O2 (wherein -0.5≤z≤0.5, 0.1≤b≤0.8, 0.1≤c≤0.8, 0≤d≤0.2, 0≤e≤0.2, b+c+d<1, M=Al, Mg, Cr, Ti, Si or Y, and A=F, P or Cl); Lithium nickel cobalt manganese composite oxides such as Li 1+x M 1-y M' y PO 4-z X z (wherein, M=transition metal, preferably Fe, Mn, Co or Ni, M'=Al, Mg or Ti, X=F, S or N, and -0.5≤x≤+0.5, 0≤y≤0.5, 0≤z≤0.1) olivine-based lithium metal phosphate represented by the above is an example, but not limited thereto.
[0089] The negative electrode active material can be, for example, carbon such as anthracite, graphitized carbon, etc.; Li x Fe2O3 (0 ≤ x ≤ 1), Li x WO2 (0 ≤ x ≤ 1), Sn x Me 1-x Me' y O z (Me: Mn, Fe, Pb, Ge; Me’: Al, B, P, Si; elements 1, 2, 3 of the periodic table; halogens; 0 < x ≤ 1; 1 ≤ y ≤ 3; 1 ≤ z ≤ 8) and other metal composite oxides; lithium metal; lithium alloy; silicon-based alloy; tin-based alloy; metal oxides such as SnO, SnO2, PbO, PbO2, Pb2O3, Pb3O4, Sb2O3, Sb2O4, Sb2O5, GeO, GeO2, Bi2O3, Bi2O4, Bi2O5, etc.; conductive polymers such as polyacetylene; lithium-cobalt-nickel-based materials; and so on.
[0090] Based on the total weight of the mixture including the positive electrode active material, the conductive material is usually added in an amount of 1 wt% to 30 wt%. There is no particular limitation on such conductive materials as long as they are conductive in use without causing chemical changes in the battery cell, for example, graphite such as natural graphite or artificial graphite; carbon black such as carbon black, acetylene black, Ketjen black, channel black, furnace black, lamp black, summer black, etc.; conductive fibers such as carbon fiber or metal fiber; metal powders such as carbon fluoride, aluminum, nickel powder; conductive whiskers such as zinc oxide, potassium titanate; conductive metal oxides such as titanium oxide; and conductive materials such as polyphenylene derivatives, etc.
[0091] The binder is a component that helps bind the active material, the conductive material, etc. to the current collector, and is usually added in an amount of 1 wt% to 30 wt% based on the total weight of the mixture including the positive electrode active material. Examples of such binders include: polyvinylidene fluoride, polyvinyl alcohol, carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose, regenerated cellulose, polyvinylpyrrolidone, tetrafluoroethylene, polyethylene, polypropylene, ethylene-propylene-diene terpolymer (EPDM), sulfonated EPDM, styrene-butene rubber, fluorinated rubber, and various copolymers, etc.
[0092] In addition, this electrode slurry can be prepared by dissolving an electrode active material, a conductive material, and a binder, etc. in a solvent. There is no particular restriction on the type of solvent, as long as the electrode active material, etc. can be dispersed, and an aqueous solvent or a non-aqueous solvent can also be used. For example, the solvent can be a commonly used solvent in the art, and can be dimethyl sulfoxide (DMSO), isopropanol, N-methylpyrrolidone (NMP), acetone or water, etc., and one of these solvents can be used alone, or a mixture of two or more of these solvents can be used. Considering the application thickness, manufacturing yield, processability, etc. of the slurry, the amount of the solvent can make the slurry have a suitable viscosity, and there is no particular restriction.
[0093] Furthermore, in a lithium secondary battery, the electrolyte may include, but is not limited to, organic solvents and lithium salts conventionally used in electrolytes.
[0094] Organic solvents can be used without any particular restrictions, as long as they can serve as a medium that allows ions involved in the electrochemical reaction in the battery cell to move. Specifically, organic solvents include ester-based solvents such as methyl acetate, ethyl acetate, γ-butyrolactone, ε-caprolactone, etc.; ether-based solvents such as dibutyl ether or tetrahydrofuran; ketone-based solvents such as cyclohexanone; aromatic hydrocarbon solvents such as benzene and fluorobenzene; carbonate solvents such as dimethyl carbonate (DMC), diethyl carbonate (DEC), methyl ethyl carbonate (MEC), ethyl methyl carbonate (EMC), ethylene carbonate (EC), propylene carbonate (PC), etc.
[0095] Among them, carbonate solvents are preferred, and more preferably a mixture of a cyclic carbonate having high ionic conductivity and high dielectric constant (e.g., ethylene carbonate or propylene carbonate) and a linear carbonate-based compound having low viscosity (e.g., methyl ethyl carbonate, dimethyl carbonate or diethyl carbonate) which can improve the charge and discharge performance of the battery.
[0096] The lithium salt may be any compound capable of providing lithium ions used in a lithium secondary battery, but is not limited thereto. Specifically, the lithium salt may be LiPF6, LiClO4, LiAsF6, LiBF4, LiSbF6, LiAlO4, LiAlCl4, LiCF3SO3, LiC4F9SO3, LiN(C2F5SO3)2, LiN(C2F5SO2)2, LiN(CF3SO2)2. LiCl, LiI or LiB(C2O4)2, etc. may be used. Preferably, the lithium salt is included in the electrolyte at a concentration of about 0.6 mol% to 2 mol%.
[0097] In addition to the above components of the electrolyte, the electrolyte may also contain, for example, pyridine, triethyl phosphite, triethanolamine, cyclic ether, ethylenediamine, N-glyme, caproic acid triamide, nitrobenzene derivatives, sulfur, quinone imine dyes, N-substituted oxazolidinones, N,N-substituted imidazolidines, ethylene glycol dialkyl ethers, ammonium salts, pyrrole, 2-methoxyethanol or aluminum chloride as one or more additives, with the purpose of improving the life characteristics of the battery cell, inhibiting the reduction of the battery cell capacity, increasing the discharge capacity of the battery cell, etc. In this case, the additive may be contained in an amount of 0.1wt% to 5wt% based on the total weight of the electrolyte.
[0098] The lithium secondary battery of the present invention can be manufactured by placing a separator between the positive electrode and the negative electrode to form an electrode assembly, which is placed in a cylindrical battery cell case or a square battery cell case, and then the electrolyte is injected. Alternatively, the electrode assembly can be manufactured by stacking the electrode assembly, impregnating the electrode assembly with the electrolyte, and then placing the obtained product in the battery cell case and sealing it.
[0099] When manufacturing the lithium secondary battery of the present invention, the electrode assembly can be dried to remove one or more organic solvents selected from the group consisting of N-methyl-2-pyrrolidone (NMP), acetone, ethanol, propylene carbonate, ethyl methyl carbonate, ethylene carbonate and dimethyl carbonate used in manufacturing the positive electrode. If an electrolyte having the same component as the organic solvent used in the preparation of the positive electrode is used as the electrolyte, the process of drying the electrode assembly can be omitted.
[0100] In contrast to the above-described lithium secondary battery, lithium secondary batteries according to other embodiments of the present invention may be solid-state batteries.
[0101] The battery case may be any conventionally used in the art, and its shape is not limited depending on the intended use of the battery, for example, it may be cylindrical such as a can, angular, pouch-shaped, or coin-shaped.
[0102] The lithium secondary battery according to the present invention stably exhibits excellent discharge capacity, output characteristics and capacity retention rate, and can therefore be used in portable devices such as mobile phones, notebook computers and digital cameras, and in the field of electric vehicles such as energy storage systems (ESS) and hybrid electric vehicles (HEV).
[0103] The present invention also provides a method for manufacturing an electrode assembly. The foregoing description of the electrode assembly may be redundant with the detailed description of the electrode assembly, the entire contents of which are incorporated herein by reference.
[0104] In one example, according to a method for manufacturing an electrode assembly of the present invention, the method includes the following steps: manufacturing an electrode assembly having a structure in which a plurality of unit cells including a positive electrode, a negative electrode and a separator inserted between the positive electrode and the negative electrode are wound into a sheet-like separator sheet; performing corona surface treatment on one or both sides of a separator substrate; stacking the positive electrode sheet and the negative electrode sheet with the separator inserted thereon and subjected to corona discharge treatment, and cutting them into predetermined sizes to manufacture unit cells including a type A dual cell and a type C dual cell; and manufacturing an electrode assembly having a structure in which a plurality of unit cells are located on a sheet-like separator sheet and the separator sheet is wound in one direction so that the type A dual cell and the type C dual cell are alternately arranged up and down with the separator therebetween; wherein the separator sheet of the unit cell includes a bonding portion that has been subjected to corona surface treatment and a non-bonding portion that has not been subjected to corona surface treatment, and the separator sheet has not been subjected to corona surface treatment.
[0105] In the surface treatment by performing corona discharge on one or both sides of the diaphragm, the diaphragm substrate is conveyed by a roller portion including a metal member, and a plasma generating portion spaced apart from the roller portion generates plasma on the surface of the diaphragm substrate by mutual reaction with the metal member to form an adhesive layer. In a specific example, the plasma generating unit includes an electrode member and generates plasma by interaction between the electrode member and the metal member. Here, the electrode member may be made of a corona discharge electrode. Since the adhesive layer is formed only on the surface of the diaphragm positioned between the electrode member and the metal member, and plasma is not generated on the surface of the diaphragm without the electrode member, a non-adhesive layer may be formed to form a strip-shaped patterned adhesive layer.
[0106] The steps of manufacturing unit cells including type A dual cells and type C dual cells, wherein each of the positive electrode substrate, negative electrode substrate and separator substrate that have been subjected to corona surface treatment and conveyed by rollers is cut and stacked to conform to the type A dual cell structure (a structure in which the positive electrode, separator, negative electrode, separator and positive electrode are stacked in sequence) or the type C dual cell structure (a structure in which the negative electrode, separator, positive electrode, separator and negative electrode are stacked in sequence), and heat-fused using a laminator or a hot press to produce unit cells such as type A dual cells or type C dual cells.
[0107] The step of manufacturing an electrode assembly, wherein a plurality of unit cells are located on a sheet-like diaphragm sheet, and the diaphragm sheet is wound in one direction to manufacture an electrode assembly having a structure in which A-type dual cells and C-type dual cells are alternately arranged up and down on the diaphragm sheet. The electrode assembly can be manufactured by placing the A-type dual cells at the starting point of the winding, arranging them sequentially into a repeating pattern such as C-type dual cells, C-type dual cells, A-type dual cells, A-type dual cells, C-type dual cells, C-type dual cells, and then winding to produce an electrode assembly centered on the A-type dual cells. Alternatively, the C-type dual cells can be placed at the beginning of the winding, sequentially arranged into a repeating pattern with A-type dual cells, A-type dual cells, C-type dual cells, C-type dual cells, A-type dual cells, A-type dual cells, and then winding to produce an electrode assembly centered on the C-type dual cells.
[0108] In addition, the diaphragm sheet is not subjected to corona surface treatment. Since the diaphragm sheet is stacked with the unit cell and the probability of the diaphragm sheet folding due to flow is lower than the probability of the diaphragm sheet folding inside the unit cell, the diaphragm sheet is not subjected to corona surface treatment in order to improve electrolyte impregnation rather than increase the interface adhesion between the diaphragm sheet and the electrode sheet of the unit cell.
[0109] In another example, in a method for manufacturing an electrode assembly according to the present invention, a unit cell includes: a positive electrode connector extending in a first direction of the positive electrode and a negative electrode connector extending in a second direction of the negative electrode, and the separator includes: a first bonding portion formed by corona surface treatment on an edge area where the positive electrode connector is located and a second bonding portion formed by corona surface treatment on an edge area where the negative electrode connector is located.
[0110] In the corona discharge surface treatment of one or both sides of the diaphragm substrate, the edges of the two side portions in the conveying direction (MD direction) of the diaphragm correspond to the positions of the electrode joints facing the inside of the unit cell to be manufactured in the future. Therefore, in the corona surface treatment of the diaphragm substrate, the edges of the two side portions in the conveying direction (MD direction) of the diaphragm can be subjected to the corona surface treatment to improve the bonding portion of the edges of the diaphragm facing the electrode joints of the unit cell to be manufactured in the future.
[0111] In another example, in a method for manufacturing an electrode assembly according to the present invention, the separator may be an electrode assembly having a structure in which a bonding portion and a non-bonding portion are alternately arranged with each other, including a third bonding portion located between the first bonding portion and the second bonding portion, wherein the third bonding portion includes n (n is an integer greater than or equal to 1). One or more third bonding portions may be formed between the first bonding portion and the second bonding portion to improve the adhesion between the separator and the electrode. The number of the third bonding portions is not particularly limited, but may be set to be suitable for the purpose in consideration of the impermeability of the electrolyte.
[0112] [Description of Reference Signs]
[0113] 1, 100, 200: Electrode assembly
[0114] 10, 110, 210: Type A dual-cell
[0115] 20, 120, 220: C-type dual-cell
[0116] 30, 130, 230: positive electrode
[0117] 40, 140, 240: negative electrode
[0118] 50, 150, 250: Diaphragm
[0119] 60, 160, 260: diaphragm
[0120] 131, 231: Positive terminal
[0121] 141, 241: Negative terminal
[0122] 151, 251: bonding part
[0123] 151a, 251a: first bonding portion
[0124] 151b, 251b: Second bonding portion
[0125] 152, 252: Non-bonded part
[0126] 170: Plasma Generator
[0127] 171: Roller part
[0128] 172: Metal components
[0129] 173: Plasma generation part
[0130] 174: Main body
[0131] 175: Electrode components
[0132] 176: Guide component
[0133] 251c: Third bonding part
Claims
1. An electrode assembly, comprising: A structure having n stacked unit cells including a positive electrode, a negative electrode and a separator interposed between the positive electrode and the negative electrode, wherein n is an integer greater than or equal to 2, and a separator sheet is provided between the unit cells, The separator embedded in the unit cell includes a bonding portion that has been subjected to a corona surface treatment and a non-bonding portion that has not been subjected to a corona surface treatment. Wherein, the diaphragm sheet is a structure that has not been subjected to corona surface treatment.
2. The electrode assembly according to claim 1, wherein: The separator sheet is a structure wound between the stacked unit cells and wrapped around the unit cells.
3. The electrode assembly according to claim 1, wherein: The unit cell comprises: a positive electrode connector, the positive electrode connector being formed to extend in a first direction of the positive electrode; and a negative electrode connector, the negative electrode connector being formed to extend in a first direction of the negative electrode; and Wherein, the diaphragm comprises: a first adhesive portion, the first adhesive portion being subjected to a corona surface treatment at an edge region where the positive electrode terminal is located; and The second adhesive portion is subjected to a corona surface treatment at an edge region where the negative electrode terminal is located.
4. The electrode assembly according to claim 1, wherein: The surface of the separator has a structure in which the adhesive portions and the non-adhesive portions are alternately arranged.
5. The electrode assembly according to claim 1, wherein: The adhesive portion is formed on one side of the diaphragm or on both sides of the diaphragm.
6. The electrode assembly according to claim 1, wherein: The area where the bonding portion is formed is in the range of 10% to 70% of the area of the separator.
7. The electrode assembly according to claim 1, wherein: The bonding portion forms a pattern, and The pattern is at least one of stripes, grids, dots and polygons. 8 . A secondary battery comprising the electrode assembly according to claim 1 .
9. The secondary battery according to claim 8, wherein The secondary battery is a pouch type secondary battery.
10. A method for manufacturing an electrode assembly as a method for manufacturing an electrode assembly for a secondary battery, the method comprising the following steps: Surface treatment is performed by performing corona discharge on one side of the diaphragm or on both sides of the diaphragm; forming a unit cell including a positive electrode, a negative electrode, and a separator interposed between the positive electrode and the negative electrode; and Arranging n unit cells on a sheet-like separator, and winding the separator in one direction, wherein n is an integer greater than or equal to 2; The separator embedded in the unit cell includes an adhesive portion that has been subjected to a corona surface treatment and a non-adhesive portion that has not been subjected to a corona surface treatment, The diaphragm sheet is a structure without corona surface treatment.
11. The method for manufacturing an electrode assembly according to claim 10, wherein: The surface treatment is performed by energizing the surface of the diaphragm via a plasma generator.
12. The method for manufacturing an electrode assembly according to claim 10, wherein: In the case of corona discharge, the discharge range is in the range of 1.0 kV to 3.0 kV.
13. The method for manufacturing an electrode assembly according to claim 10, wherein: During corona discharge, the discharge range is 30W·min / m 2 Up to 300W·min / m 2 within the range.