Battery monomer, battery and electric device

CN118947003APending Publication Date: 2024-11-12CONTEMPORARY AMPEREX TECHNOLOGY CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202280094182.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2022-12-29
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The electrode components of the battery cells tend to precipitate metal in the bending area, causing dendrites to grow, causing internal short circuits and affecting the safety of the battery.

Method used

A porous insulating layer is provided in the bending area of ​​the electrode assembly of the battery cell to prevent dendrite contact and conduction, buffer the bending stress, and reduce the risk of active material loss.

Benefits of technology

It effectively delays short circuits caused by dendrites, extends the service life of battery cells, improves safety, and improves charge and discharge performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118947003A_ABST
    Figure CN118947003A_ABST
Patent Text Reader

Abstract

The invention discloses a battery cell, a battery (1) and a power utilization device. The battery cell comprises at least one electrode assembly (10). The electrode assembly (10) comprises a positive pole piece (11), a negative pole piece (12), a diaphragm (13) and a porous insulating layer (14). And the positive pole piece (11), the diaphragm (13) and the negative pole piece (12) are laminated and wound. At least one part of the porous insulating layer (14) is arranged in the bending area (16) of the electrode assembly (10), and the porous insulating layer (14) is arranged between the positive pole piece (11) and the diaphragm (13) or between the negative pole piece (12) and the diaphragm (13). Based on the structure, the service life of the battery monomer can be correspondingly prolonged, and the safety of the battery monomer can be correspondingly improved.
Need to check novelty before this filing date? Find Prior Art

Description

Battery cells, batteries and electrical devices Technical Field

[0001] The present application relates to the field of battery technology, and in particular to a battery cell, a battery, and an electrical device. Background Art

[0002] A battery cell typically contains at least one electrode assembly. This assembly is formed by winding a positive electrode sheet, a negative electrode sheet, and a separator separating the two electrodes into a coiled structure. The electrode assembly comprises a main body and a folded region disposed at the end of the main body. However, during battery cell use, the folded region of the electrode assembly is susceptible to metal deposition. Over time, dendrites can also form in the folded region. These dendrites can easily cause internal short circuits in the battery cell, compromising its safety. Technical issues

[0003] The embodiments of the present application provide a battery cell, a battery, and an electrical device, aiming to solve the problem that the electrode assembly of the existing battery cell is prone to growing dendrites in the bending area, causing internal short circuits in the battery cell and affecting the safety of the battery cell. Technical Solutions

[0004] The technical solution adopted in the embodiment of this application is:

[0005] In a first aspect, a battery cell is provided, wherein the battery cell includes at least one electrode assembly, the electrode assembly including a positive electrode sheet, a negative electrode sheet, a separator, and a porous insulating layer;

[0006] The positive electrode sheet, the separator and the negative electrode sheet are stacked and wound;

[0007] At least a portion of the porous insulating layer is disposed in a bending region of the electrode assembly. The porous insulating layer is disposed between the positive electrode sheet and the separator, or between the negative electrode sheet and the separator.

[0008] The battery cell provided in the embodiment of the present application has a porous insulating layer provided between the bent portion of the positive electrode sheet or the negative electrode sheet of any circle and the diaphragm. Based on this, the active ions can be allowed to freely penetrate through the pores of the porous insulating layer to ensure that the porous insulating layer does not have a significant impact on the charging and discharging process of the battery cell, thereby ensuring the charging and discharging performance of the battery cell. On this basis, the porous insulating layer with insulating properties can also be used to hinder the dendrites, so as to effectively delay the occurrence of the phenomenon of "dendrites directly causing internal short circuits in the battery cell", and effectively delay the occurrence of the phenomenon of "dendrites heating up due to short circuits and melting the diaphragms around the dendrites, causing direct contact and short circuit between the positive electrode sheet and the negative electrode sheet at the place where the diaphragm melts", thereby correspondingly extending the service life of the battery cell and correspondingly improving the safety of the battery cell.

[0009] Furthermore, the battery cell provided in the embodiment of the present application can also provide a buffering effect on the bending stress borne by the bent portion of the electrode sheet through the porous insulating layer provided between the bent portion of the electrode sheet and the diaphragm during the winding and pre-pressing of the electrode assembly and during the use of the battery cell, thereby effectively reducing the risk of tearing defects in the bent portion of the electrode sheet leading to a reduction in active material, effectively reducing the risk of metal precipitation in the bent area of ​​the electrode assembly due to a reduction in active material, and effectively alleviating the growth rate of dendrites, thereby correspondingly extending the service life of the battery cell and correspondingly improving the safety of the battery cell.

[0010] In some embodiments, in the bending region, at least one porous insulating layer is disposed on the inner side of the innermost positive electrode plate.

[0011] By adopting the above scheme, on the one hand, when "metal precipitation occurs at the bent part of the innermost circle of the negative electrode sheet, and dendrites grow from the defects of the bent part of the diaphragm over time", the growing dendrites can be insulated and blocked by a porous insulating layer arranged on the inner side of the bent part of the innermost circle of the positive electrode sheet to prevent the dendrites from directly contacting the conductive positive electrode sheet and the negative electrode sheet. This can effectively delay the occurrence of "dendrites directly causing internal short circuits in the battery cell" between the innermost circle of the positive electrode sheet and the innermost circle of the negative electrode sheet where metal precipitation is easy to occur, and effectively delay the occurrence of "dendrites heating up due to short circuits and melting the diaphragm around the dendrites, causing direct contact and short circuit between the positive electrode sheet and the negative electrode sheet where the diaphragm melts", thereby correspondingly extending the service life of the battery cell and improving the safety of the battery cell.

[0012] On the other hand, during the winding and pre-pressing of the electrode assembly and during the use of the battery cell, the porous insulating layer disposed inside the bent portion of the innermost positive electrode tab can buffer the compressive stress experienced by the bent portion of the innermost positive electrode tab, thereby reducing the risk of tearing defects in the bent portion of the innermost positive electrode tab, which could lead to a reduction in active material. It can even buffer the tensile stress experienced by the bent portion of the innermost negative electrode tab, thereby reducing the risk of tearing defects in the bent portion of the innermost negative electrode tab, which could lead to a reduction in active material. This effectively reduces the risk of metal precipitation exacerbated by the reduction in active material, and effectively mitigates the growth rate of dendrites between the innermost positive and negative electrode tabs, thereby correspondingly extending the service life of the battery cell and improving the safety of the battery cell.

[0013] In some embodiments, in the bending region, at least one porous insulating layer is disposed on the outer side of the innermost positive electrode sheet.

[0014] By adopting the above solution, during the winding and pre-pressing of the electrode assembly and during the use of the battery cell, the porous insulating layer disposed outside the bent portion of the innermost positive electrode tab can buffer the tensile stress experienced by the bent portion of the innermost positive electrode tab, thereby reducing the risk of tearing defects in the bent portion of the innermost positive electrode tab, leading to a reduction in active material. It can even buffer the compressive stress experienced by the bent portion of the second innermost negative electrode tab, thereby reducing the risk of tearing defects in the bent portion of the second innermost negative electrode tab, leading to a reduction in active material. This effectively reduces the risk of metal precipitation exacerbated by the reduction in active material and effectively mitigates the growth rate of dendrites between the innermost positive electrode tab and the second innermost negative electrode tab, thereby correspondingly extending the service life of the battery cell and improving the safety of the battery cell.

[0015] By adopting the above solution, during the use of the battery cell, a porous insulating layer provided on the outside of the bent portion of the innermost positive electrode tab can be used to insulate and block dendrites growing toward it, thereby preventing the dendrites from directly contacting and conducting the innermost positive electrode tab and the next innermost negative electrode tab. This effectively delays the occurrence of dendrites directly causing internal short circuits in the battery cell between the innermost positive electrode tab and the next innermost negative electrode tab, and effectively delays the occurrence of dendrites heating up due to the short circuit and melting the diaphragm surrounding the dendrite, causing direct contact and short circuiting between the positive and negative electrode tabs where the diaphragm melts, thereby correspondingly extending the service life of the battery cell and improving the safety of the battery cell.

[0016] In some embodiments, two porous insulating layers are provided in the bending region, wherein one porous insulating layer is provided on the inner side of the innermost circle of the positive electrode sheet, and the other porous insulating layer is provided on the outer side of the innermost circle of the positive electrode sheet.

[0017] By adopting the above solution, the bending zone can effectively delay the risk of short circuits through two porous insulating layers in the "innermost positive electrode sheet and the innermost negative electrode sheet" and "innermost positive electrode sheet and the second innermost negative electrode sheet" where metal precipitation is prone to occur and the metal precipitation is relatively serious. It can also effectively relieve the compression stress and tensile stress in the bent portion of the innermost positive electrode sheet, which is subject to greater bending stress and prone to tearing defects, thereby reducing the risk of bending and tearing, thereby effectively extending the service life of the battery cell and effectively improving the safety of the battery cell. While maximizing the effectiveness of the porous insulating layer, by adopting the above solution, the number of porous insulating layers set can also be reduced, thereby ensuring and improving the energy density of the electrode assembly and battery cell.

[0018] In some embodiments, the electrode assembly has a main body region and a bending region disposed on an end side of the main body region;

[0019] The porous insulating layer comprises a bending section bent in the bending area, and an extending section connected to the end of the bending section and arranged in the main area.

[0020] By adopting the above scheme, the setting area of ​​the porous insulating layer can be extended accordingly, and the preset position of the porous insulating layer on the continuous positive electrode sheet or the continuous negative electrode sheet has a wider tolerance range, thereby effectively ensuring that when the electrode assembly is wound, the porous insulating layer can retain the bent section clamped between the bent part of the electrode sheet and the diaphragm, and can adapt to the extended section extending to the main area according to the position tolerance, thereby effectively reducing the accuracy requirements for the preset position of the porous insulating layer on the continuous positive electrode sheet or the continuous negative electrode sheet, and effectively ensuring and improving the production yield of the electrode assembly.

[0021] By adopting the above scheme, the porous insulating layer can also reliably stabilize the relative position and relative state of the porous insulating layer through the curved section clamped between the bent part of the pole piece and the diaphragm, and the extended section clamped between the straight part of the pole piece and the diaphragm, thereby effectively reducing the risk of displacement of the porous insulating layer during the use of the battery cell, and effectively ensuring that the porous insulating layer can function stably and reliably for a long time during the use of the battery cell.

[0022] In some embodiments, the porous insulating layer is bonded to the positive electrode sheet or the negative electrode sheet by dissolving the adhesive.

[0023] By adopting the above solution, the porous insulating layer can be bonded to the continuous positive electrode sheet or the continuous negative electrode sheet at a preset position by dissolving the adhesive before winding, so as to stabilize the preset position and preset state relative to the electrode sheet. Based on this, during the winding process of the electrode assembly, the porous insulating layer can be ensured to be wound along with the continuous positive electrode sheet or the continuous negative electrode sheet in a stable position and state relative to the electrode sheet, and wound into the bending area, thereby conveniently and quickly achieving the installation of the porous insulating layer, and effectively ensuring and improving the positional accuracy and effectiveness of the porous insulating layer in the formed electrode assembly, which can effectively ensure and improve the production efficiency and production yield of the electrode assembly.

[0024] In some embodiments, the battery cell includes an electrolyte for soaking the electrode assembly, and the electrolyte contains dissolved glue.

[0025] By adopting the above scheme, when the electrode assembly and the electrolyte are encapsulated inside the battery cell, at least a portion of the dissolving glue bonded between the electrode piece and the porous insulating layer dissolves in the electrolyte, so as to reduce or even eliminate the obstruction of the corresponding areas of the electrode piece and the porous insulating layer, thereby facilitating the active ions to freely and normally penetrate the porous insulating layer, and facilitating the active ions to freely and normally embed into the electrode piece, thereby effectively ensuring that the setting of the porous insulating layer will not have a significant impact on the charging and discharging process of the battery cell, and effectively ensuring the charging and discharging performance of the battery cell.

[0026] In some embodiments, the dissolving adhesive is a modified acrylic pressure-sensitive adhesive, and the electrolyte contains a modified acrylic resin.

[0027] By adopting the above scheme, on the one hand, the dissolving glue can be made to have the liquid viscosity properties of a pressure-sensitive adhesive, so that the dissolving glue can be conveniently, quickly and reliably formed on one side of the porous insulating layer along its thickness direction by coating. On the other hand, the dissolving glue can be made to have the solid elastic properties of a pressure-sensitive adhesive, so that the dissolving glue can be easily and reliably bonded to the electrode sheet with only a small pressure before winding, so that the porous insulating layer can be stably installed to the preset position of the continuous positive electrode sheet or the continuous negative electrode sheet conveniently and quickly. On the other hand, the dissolving glue can be made to have the easily degradable properties of a modified acrylic resin, so that the dissolving glue can be quickly and easily dissolved in the electrolyte when the electrode assembly and the electrolyte are encapsulated into the interior of the battery cell without leaving any residue.

[0028] In some embodiments, an absolute value of a difference between the porosity of the porous insulating layer and the porosity of the separator is less than or equal to 25%.

[0029] By adopting the above scheme, the porosity of the porous insulating layer can be made almost the same as that of the diaphragm. Based on this, active ions can freely and normally penetrate the porous insulating layer and the diaphragm, thereby effectively ensuring that the setting of the porous insulating layer will not have a significant impact on the charging and discharging process of the battery cell, and effectively ensuring the charging and discharging performance of the battery cell.

[0030] In some embodiments, an absolute value of a difference between the porosity of the porous insulating layer and the porosity of the separator is less than or equal to 10%.

[0031] By adopting the above scheme, the porosity of the porous insulating layer can be set to be similar to the porosity of the diaphragm. In this way, active ions can freely and normally penetrate the porous insulating layer and the diaphragm, thereby effectively ensuring that the setting of the porous insulating layer will not have a significant impact on the charging and discharging process of the battery cell, and can effectively ensure and improve the charging and discharging performance of the battery cell.

[0032] In some embodiments, the porous insulating layer is a polyolefin separator.

[0033] By adopting the above scheme, a porous insulating layer can be made by using a polyolefin diaphragm such as a polypropylene diaphragm to ensure that the porosity of the porous insulating layer is similar to or even the same as the porosity of the diaphragm, thereby ensuring that active ions can freely and normally penetrate the porous insulating layer and the diaphragm, effectively ensuring that the setting of the porous insulating layer will not have a significant impact on the charging and discharging process of the battery cell, and effectively ensuring the charging and discharging performance of the battery cell.

[0034] In some embodiments, the porosity of the porous insulating layer is 40% to 50%.

[0035] By adopting the above solution, on the one hand, the air permeability of the porous insulating layer can be ensured to be moderate, and the active ions can be ensured to freely and normally penetrate the porous insulating layer. On the other hand, it can be ensured that when the dissolved glue is applied to the side of the porous insulating layer, a small amount of glue penetrates into the pores of the porous insulating layer, while a large amount of glue remains on the surface of the porous insulating layer, thereby ensuring the adhesion of the dissolved glue and ensuring that the porous insulating layer can be reliably temporarily fixed to the electrode via the dissolved glue. On the other hand, it can be ensured that when the dissolved glue is dissolved in the electrolyte, a small amount of glue remains in the pores of the porous insulating layer, thereby reducing the blocking effect of the dissolved glue on the pores of the porous insulating layer, ensuring that active ions can freely and normally penetrate the porous insulating layer, and ensuring conductivity.

[0036] In some embodiments, the pore diameter of the porous insulating layer is A, the thickness of the porous insulating layer is B, and 24≤B / A≤400.

[0037] By adopting the above solution, the thickness B of the porous insulating layer and the pore diameter A of the porous insulating layer can be made moderate. Based on this, on the one hand, it is difficult for dendrites to pierce or pass through the porous insulating layer, thereby ensuring the porous insulating layer's dendrite barrier effect; on the other hand, it allows active ions to easily shuttle through the porous insulating layer and the shuttle path is short, thereby reducing the risk of active ion precipitation due to shuttle difficulties. This effectively extends the service life of the battery cell and effectively improves the safety of the battery cell.

[0038] In some embodiments, the thickness B of the porous insulating layer is 12 um to 20 um.

[0039] By adopting the above scheme, the thickness B of the porous insulating layer can be ensured to be moderate, so as to reduce the influence of the porous insulating layer on the energy density of the battery cell and the penetration rate of active ions through the porous insulating layer on the basis of ensuring that the porous insulating layer can form a better insulating barrier effect on the dendrites growing toward it, thereby ensuring the electrical conductivity, ensuring the charging and discharging performance of the battery cell, extending the service life of the battery cell accordingly, and improving the safety of the battery cell accordingly.

[0040] In some embodiments, the pores of the porous insulating layer have a pore diameter A of 0.05 micrometers (um) to 0.5 um.

[0041] By adopting the above scheme, on the one hand, the air permeability of the porous insulating layer can be guaranteed to be moderate, and the active ions can be guaranteed to be able to freely and normally penetrate the pores of the porous insulating layer. On the one hand, it can be guaranteed that when the dissolved glue is applied to the side of the porous insulating layer, the amount of glue that penetrates into the pores of the porous insulating layer is small, while the amount of glue left on the surface of the porous insulating layer is large, thereby ensuring the adhesion of the dissolved glue and ensuring that the porous insulating layer can be reliably temporarily fixed to the electrode via the dissolved glue. On the one hand, it can be guaranteed that when the dissolved glue is dissolved in the electrolyte, the amount of glue remaining in the pores of the porous insulating layer is small, thereby reducing the blocking effect of the dissolved glue on the pores of the porous insulating layer, ensuring that the active ions can freely and normally penetrate the pores of the porous insulating layer, and ensuring the electrical conductivity. On the one hand, during the use of the battery cell, the porous insulating layer can be guaranteed to have a blocking effect on dendrites growing from the defects of the diaphragm, and reduce the risk of dendrites growing from the pores of the porous insulating layer, thereby correspondingly extending the service life of the battery cell and correspondingly improving the safety of the battery cell.

[0042] In some embodiments, the tensile strength of the porous insulating layer in the width direction thereof is greater than or equal to 1000 kgf / cm2. 2 ).

[0043] By adopting the above scheme, it can be ensured that the porous insulating layer has sufficient tensile strength in its width direction, which can effectively reduce the risk of fracture and cracking defects of the porous insulating layer under the action of tension, thereby ensuring and improving the insulating barrier effect of the porous insulating layer on dendrites growing from the defects of the diaphragm, and effectively reducing the risk of dendrites continuing to grow along the fracture and cracking defects of the porous insulating layer, thereby correspondingly extending the service life of the battery cell and correspondingly improving the safety of the battery cell.

[0044] In some embodiments, the elongation of the porous insulating layer in a width direction thereof is greater than or equal to 10%.

[0045] By adopting the above solution, it can be ensured that the porous insulating layer has sufficient elongation in its width direction, so as to ensure that the porous insulating layer can adaptively extend and deform with the electrode assembly, thereby ensuring that the effective range of the porous insulating layer can cover the corresponding area of ​​the electrode piece, and ensuring that the porous insulating layer can form a reliable insulation barrier effect on the dendrites grown from the defects of the diaphragm.

[0046] In some embodiments, the shrinkage rate of the porous insulating layer at 105 degrees Celsius (° C.) is 0-3%.

[0047] By adopting the above solution, it can be ensured that the porous insulating layer undergoes less dimensional shrinkage due to the internal temperature of the battery cell during the use of the battery cell, thereby ensuring that the effective range of the porous insulating layer can cover the corresponding area of ​​the electrode, and ensuring that the porous insulating layer can form a reliable insulating barrier effect on dendrites growing from defects in the diaphragm.

[0048] In a second aspect, a battery is provided, wherein the battery includes the battery cell provided in the embodiment of the present application.

[0049] By adopting the above solution, the battery can ensure and extend the battery life and ensure and improve the battery safety by applying the battery cells provided in the embodiments of the present application.

[0050] In a third aspect, an electrical device is provided, wherein the electrical device includes the battery or battery cell provided in an embodiment of the present application.

[0051] By adopting the above solution, the electrical device can ensure and extend the service life of the electrical device and ensure and improve the safety of the electrical device by applying the battery or battery cell provided in the embodiment of the present application. BRIEF DESCRIPTION OF THE DRAWINGS

[0052] In order to clearly illustrate the technical solutions in the embodiments of the present application, the following briefly introduces the drawings required for use in the embodiments of the present application or the exemplary technical description. Obviously, the drawings described below are only some embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work.

[0053] FIG1 is a schematic structural diagram of a vehicle provided in an embodiment of the present application;

[0054] FIG2 is an exploded schematic diagram of a battery provided in an embodiment of the present application;

[0055] FIG3 is an exploded schematic diagram of a battery cell provided in an embodiment of the present application;

[0056] FIG4 is a schematic cross-sectional view of a battery cell provided in an embodiment of the present application;

[0057] FIG5 is a schematic structural diagram of an electrode assembly provided in an embodiment of the present application;

[0058] FIG6 is a partial schematic diagram of the electrode assembly provided in FIG5 ;

[0059] FIG7 is a second partial schematic diagram of the electrode assembly provided in FIG5 ;

[0060] FIG8 is a schematic structural diagram of the positive electrode sheet, dissolved glue and porous insulating layer provided in an embodiment of the present application.

[0061] Among them, the reference numerals in the figures are:

[0062] 1-battery, 2-controller, 3-motor; 100-battery unit, 200-box, 201-first part, 202-second part;

[0063] 10-electrode assembly, 11-positive electrode sheet, 111-positive electrode tab, 112-innermost positive electrode sheet, 12-negative electrode sheet, 121-negative electrode tab, 122-innermost negative electrode sheet, 123-next inner negative electrode sheet, 13-diaphragm, 14-porous insulating layer, 141-bending section, 142-extension section, 15-main body, 16-bending section, 17-dissolving glue; 20-electrolyte; 30-shell, 40-end cover, 50-electrode terminal. Modes for Carrying Out the Invention

[0064] In order to make the technical problems, technical solutions and beneficial effects to be solved by this application clear and understandable, the present application is described in detail below with reference to the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain this application and are not intended to limit this application.

[0065] In the description of this application, it should be understood that the terms "length", "width", "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside", "outside", etc., indicating the orientation or position relationship, are based on the orientation or position relationship shown in the accompanying drawings, and are only for the convenience of describing this application and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as a limitation on this application.

[0066] Furthermore, the terms "first" and "second" are used for descriptive purposes only and should not be construed as indicating or implying relative importance or implicitly specifying the number of technical features being referred to. Thus, a feature defined as "first" or "second" may explicitly or implicitly include one or more of such features. Throughout the description of this application, "plurality" means two or more, unless otherwise specifically defined.

[0067] In this application, unless otherwise expressly specified or limited, terms such as "mounted," "connected," "connect," and "fixed" should be understood in a broad sense. For example, they may refer to fixed connections, detachable connections, or integration; mechanical connections or electrical connections; direct connections or indirect connections through an intermediate medium; and internal connections between two components or interactions between two components. Those skilled in the art will understand the specific meanings of these terms in this application based on specific circumstances.

[0068] A battery cell is the smallest unit for storing and outputting electrical energy. A battery cell typically contains at least one electrode assembly. The electrode assembly is the component within the battery cell where electrochemical reactions occur. The electrode assembly can be formed into a roll structure by winding a positive electrode sheet, a negative electrode sheet, and a separator separating the positive and negative electrode sheets. The rolled electrode assembly has a main body region and a bending region disposed at the end of the main body region. When the battery cell is charging, the positive electrode sheet generates active ions. The active ions provided by the positive electrode sheet can penetrate the pores of the separator and move to the negative electrode sheet and embed into the negative active material of the negative electrode sheet. Conversely, when the battery cell is discharging, the active ions embedded in the negative active material of the negative electrode sheet are released. The active ions released from the negative electrode sheet can penetrate the pores of the separator and move to the positive electrode sheet and embed into the positive active material of the positive electrode sheet.

[0069] However, the applicant found that:

[0070] 1. In the bending zone, since the positive electrode tabs of any circle are located outside the negative electrode tabs of the same circle, the curvature radius of the positive electrode tabs of any circle will be relatively larger than the curvature radius of the negative electrode tabs of the same circle. For example, since the positive electrode tabs of the innermost circle are located outside the negative electrode tabs of the innermost circle, the curvature radius of the positive electrode tabs of the innermost circle will be relatively larger than the curvature radius of the negative electrode tabs of the innermost circle. Based on this, in the bending zone, the area of ​​the positive electrode tabs of any circle will be relatively larger than the area of ​​the negative electrode tabs of the same circle. As a result, during the charging process of the battery cell, the positive electrode tabs with larger areas and relatively more positive active materials will generate more active ions, but the negative electrode tabs with smaller areas and relatively less negative active materials have insufficient space for active ions to embed, resulting in the precipitation of active ions that cannot be embedded in the negative active materials, resulting in metal precipitation.

[0071] 2. During the process of winding the positive electrode sheet, separator, and negative electrode sheet to form a rolled electrode assembly, the bent portions of the positive and negative electrode sheets (i.e., the portions of the electrode sheets corresponding to the bent areas) will bend and bend, and the radius of curvature will decrease as the inner circles become smaller, causing the positive active material in the bent portion of the positive electrode sheet to partially fall off (i.e., powdering). The negative active material in the bent portion of the negative electrode sheet will also experience powdering. Furthermore, since the radius of curvature of the negative electrode sheet in any circle is relatively smaller than the radius of curvature of the positive electrode sheet in the same circle, the powdering of the bent portion of the negative electrode sheet during bending will be relatively severe. The powdering phenomenon will reduce the content of active material on the electrode sheet, resulting in a decrease in the number of sites available for active ions to embed in the negative electrode sheet with reduced negative active material during the charging process of the battery cell, thereby increasing the number of active ions that cannot be embedded in the negative active material and exacerbating the metal precipitation phenomenon.

[0072] 3. During the winding and pre-pressing of the electrode assembly, as well as during the use of the battery cells, the bent portions of the positive and negative electrode sheets are subjected to greater forces due to bending. The smaller the radius of curvature, the greater the forces applied. This can lead to tearing defects in the bent portions of the positive and negative electrode sheets. If tearing defects occur, the active material at the torn portion will fall off. This can also prevent the active material from being embedded during the charge and discharge process of the battery cells, increasing the amount of active ions released and exacerbating metal precipitation.

[0073] Based on this, the applicant discovered that during the use of the battery cell, metal precipitation is prone to occur in the bending area of ​​the electrode assembly. The continuous diaphragm may have defects such as large pore size and damage in local areas, resulting in the precipitation of active ions that easily grow dendrites at the defects of the diaphragm in the bending area as the battery cell is used for a longer time. As the dendrites grow, they easily contact and conduct the positive and negative pole pieces, causing a short circuit inside the battery cell, thereby affecting the safety of the battery cell. During the short circuit, the dendrites will generate heat and melt the diaphragm part on the side of the dendrite, causing the diaphragm defects to expand, resulting in direct contact and short circuit between the positive and negative pole pieces at the place where the diaphragm melts, thereby aggravating the short circuit phenomenon and seriously affecting the safety of the battery cell.

[0074] Therefore, some embodiments of the present application provide a battery cell, which is provided with a porous insulating layer between the bent part of the positive electrode plate or the negative electrode plate of any circle and the diaphragm, so as to ensure that the porous insulating layer does not have a significant impact on the charging and discharging process of the battery cell. The porous insulating layer with insulating properties can hinder the dendrites, thereby effectively delaying the occurrence of the phenomenon of "dendrites directly causing internal short circuits in the battery cell", and effectively delaying the occurrence of the phenomenon of "dendrites heating up due to short circuits and melting the diaphragms on the sides of the dendrites, causing direct contact and short circuit between the positive electrode plate part and the negative electrode plate part at the place where the diaphragm melts", thereby correspondingly extending the service life of the battery cell and correspondingly improving the safety of the battery cell. Moreover, during the winding and pre-pressing of the electrode assembly and during the use of the battery cell, the battery cell can also form a buffering effect on the bending stress borne by the bent portion of the electrode piece through the porous insulating layer, thereby effectively reducing the risk of tearing defects in the bent portion of the electrode piece leading to a reduction in active material, effectively reducing the risk of metal precipitation in the bent area of ​​the electrode assembly due to the reduction in active material, and effectively alleviating the growth rate of dendrites, thereby correspondingly extending the service life of the battery cell and improving the safety of the battery cell.

[0075] The battery cells disclosed in the embodiments of the present application can be used independently or in combination with other battery cells to form modular batteries that can provide higher voltage and capacity, such as battery modules, battery modules or battery packs. The battery cells and batteries disclosed in the embodiments of the present application can be used in electrical devices that use battery cells and batteries as power sources, or in various energy storage systems that use battery cells and batteries as energy storage elements. The electrical devices may be, but are not limited to, vehicles, mobile phones, portable devices, laptops, ships, spacecraft, electric toys and power tools, etc. Vehicles may be fuel vehicles, gas vehicles or new energy vehicles, and new energy vehicles may be pure electric vehicles, hybrid vehicles or extended-range vehicles, etc. Spacecraft include airplanes, rockets, space shuttles and spacecraft, etc. Electric toys include fixed or mobile electric toys, such as game consoles, electric car toys, electric ship toys and electric airplane toys, etc. Power tools include metal cutting power tools, grinding power tools, assembly power tools and railway power tools, such as electric drills, electric grinders, electric wrenches, electric screwdrivers, electric hammers, impact drills, concrete vibrators and electric planers, etc.

[0076] In order to illustrate the technical solution provided by the present application, the following is a detailed description with reference to specific drawings and embodiments, taking "the electrical device being a vehicle" as an example.

[0077] Please refer to Figure 1, which is a schematic structural diagram of a vehicle provided in some embodiments of the present application. The vehicle can be a fuel vehicle, a gas vehicle or a new energy vehicle. The new energy vehicle can be a pure electric vehicle, a hybrid vehicle or an extended-range vehicle, etc. A battery 1 is provided inside the vehicle, and the battery 1 can be provided at the bottom, head or tail of the vehicle. The battery 1 is used to power the vehicle. For example, the battery 1 can be used as an operating power source for the vehicle. The vehicle may also include a controller 2 and a motor 3. The controller 2 is used to control the battery 1 to power the motor 3, for example, for starting, navigating and operating power requirements during driving of the vehicle.

[0078] In some embodiments of the present application, the battery 1 can serve not only as the operating power source of the vehicle, but also as the driving power source of the vehicle, replacing or partially replacing fuel or natural gas to provide driving power for the vehicle.

[0079] Please refer to Figure 2, which is an exploded schematic diagram of a battery 1 provided in some embodiments of the present application. The battery 1 includes a battery cell 100 and a housing 200, with the battery cell 100 housed within the housing 200. The housing 200 is used to provide a storage space for the battery cell 100 and can have various structures. In some embodiments, the housing 200 can include a first portion 201 and a second portion 202, which overlap with each other and together define a storage space for the battery cell 100. The second portion 202 can be a hollow structure with one end open, and the first portion 201 can be a plate-like structure, with the first portion 201 overlapping the open side of the second portion 202, so that the first portion 201 and the second portion 202 jointly define a storage space. Alternatively, the first portion 201 and the second portion 202 can each be a hollow structure with one end open, with the open side of the first portion 201 overlapping the open side of the second portion 202. Of course, the box body 200 formed by the first part 201 and the second part 202 can be in various shapes, such as a cylinder, a cuboid, etc.

[0080] In the battery 1 , there may be multiple battery cells 100 , and the multiple battery cells 100 may be connected in series, in parallel, or in mixed connection. Mixed connection means that the multiple battery cells 100 are connected in both series and in parallel.

[0081] Specifically, the battery unit 100 can be a battery cell. Multiple battery cells can be directly connected in series, in parallel, or in a mixed manner, and then the battery cell structure can be housed in the housing 200. The battery cell can be a lithium-ion secondary battery, a lithium-ion primary battery, a lithium-sulfur battery, a sodium-lithium-ion battery, a sodium-ion battery, or a magnesium-ion battery, etc.; the battery cell can be cylindrical, flat, rectangular, or in other shapes, etc.; the battery cell can be packaged in different ways to form a cylindrical battery cell, a square battery cell, or a soft-pack battery cell, etc.; this application does not impose any restrictions on this.

[0082] Alternatively, the battery unit 100 may be a battery module or battery assembly. Multiple battery cells may be connected in series, parallel, or in series to form a modular structure, i.e., a battery module or battery assembly. Multiple battery modules or battery assembly may then be connected in series, parallel, or in series to form a single unit, which is then housed within the housing 200.

[0083] Of course, the battery 1 may also include other structures. For example, the battery 1 may also include a busbar component (not shown in the figure) for achieving electrical connection between the multiple battery cells 100 .

[0084] Of course, in some embodiments, the battery 1 may not include the box body 200 , but rather a plurality of battery cells may be electrically connected and formed into a whole through necessary fixing structures and then assembled into an electrical device.

[0085] Please refer to Figures 3 and 4, which are schematic diagrams of the battery cell structure provided in some embodiments of the present application. A battery cell is the smallest unit that stores and outputs electrical energy. A battery cell includes components such as an electrode assembly 10, an electrolyte 20, a housing 30, and an end cap 40.

[0086] The end cap 40 is a component that covers the opening of the housing 30 to isolate the internal environment of the battery cell from the external environment. In some embodiments, the shape of the end cap 40 can be adapted to match the shape of the housing 30 to fit the housing 30. In some embodiments, the end cap 40 can be made of a material with a certain degree of hardness and strength. This prevents deformation when subjected to compression or collision, thereby enhancing the structural strength and safety of the battery cell. Of course, this embodiment does not limit the material of the end cap 40; the end cap 40 can be made of copper, iron, aluminum, stainless steel, aluminum alloy, plastic, and other materials. In some embodiments, the end cap 40 may be provided with functional components such as electrode terminals 50. The electrode terminals 50 can be used to electrically connect to the electrode assembly 10 for inputting or outputting electrical energy. In some embodiments, the end cap 40 may also be provided with a pressure relief mechanism (not shown) to release internal pressure when the internal pressure or temperature of the battery cell reaches a threshold. In some embodiments, an insulating member (not shown) may be provided inside the end cap 40 to isolate the electrical connection components within the housing 30 from the end cap 40 to reduce the risk of short circuits. Alternatively, the insulating member may be made of plastic, rubber, or the like.

[0087] The housing 30 is a component that cooperates with the end cap 40 to form the internal environment of the battery cell. The internal environment formed by the housing 30 and the end cap 40 can be used to accommodate components such as the electrode assembly 10 and the electrolyte 20. In some embodiments, the housing 30 and the end cap 40 can be separate components. An opening can be provided in the housing 30, and the end cap 40 is placed over the opening to form the internal environment of the battery cell. In some embodiments, the end cap 40 and the housing 30 can also be integrated. Specifically, the end cap 40 and the housing 30 can form a common connection surface before other components are inserted into the housing. When the interior of the housing 30 needs to be enclosed, the end cap 40 is placed over the housing 30. The housing 30 can be of various shapes and sizes, such as a rectangular parallelepiped, a cylinder, a hexagonal prism, etc. Specifically, the shape of the housing 30 can be determined based on the specific shape and size of the electrode assembly 10. The housing 30 can be made of a variety of materials, such as copper, iron, aluminum, stainless steel, aluminum alloy, plastic, etc., and this embodiment of the present application is not intended to be limiting.

[0088] The electrode assembly 10 is a component in the battery cell where electrochemical reactions occur. The housing 30 may include one or more electrode assemblies 10. Referring to Figure 5, the electrode assembly 10 includes a positive electrode sheet 11, a negative electrode sheet 12, and a separator 13. The separator 13 separates the positive electrode sheet 11 from the negative electrode sheet 12. The positive electrode sheet 11, the negative electrode sheet 12, and the separator 13 separating the positive electrode sheet 11 from the negative electrode sheet 12 can be processed by winding to form a roll structure. The electrode assembly 10 with a roll structure has a main body area 15 and a bending area 16 arranged on the end side of the main body area 15. Among them, the parts of the positive electrode sheet 11 and the negative electrode sheet 12 that do not have active materials each constitute a pole ear. The pole ear is the current transmission end of the electrode assembly 10, which is used to connect to the electrode terminal 50 and transmit current. The tab of the positive electrode sheet 11 is the positive electrode tab 111 , and the tab of the negative electrode sheet 12 is the negative electrode tab 121 . The positive electrode tab 111 and the negative electrode tab 121 can be located together on one side of the main body area 15 or respectively on two opposite sides of the main body area 15 .

[0089] The electrolyte 20 is the liquid that soaks the electrode assembly 10. When the battery cell is charging, the positive electrode plate 11 generates active ions. These active ions can penetrate the pores of the separator 13, travel through the electrolyte 20 to the negative electrode plate 12, and become embedded in the negative active material of the negative electrode plate 12. Conversely, when the battery cell is discharging, the active ions embedded in the negative active material of the negative electrode plate 12 are released. The released active ions can penetrate the pores of the separator 13, travel through the electrolyte 20 to the positive electrode plate 11, and become embedded in the positive active material of the positive electrode plate 11.

[0090] Referring to Figures 4, 5, 6, and 7, some embodiments of the present application provide a battery cell, wherein the battery cell includes at least one electrode assembly 10. The electrode assembly 10 includes a positive electrode sheet 11, a negative electrode sheet 12, a separator 13, and a porous insulating layer 14. The positive electrode sheet 11, the separator 13, and the negative electrode sheet 12 are stacked and wound. At least a portion of the porous insulating layer 14 is provided in a bending region 16 of the electrode assembly 10, and the porous insulating layer 14 is provided between the positive electrode sheet 11 and the separator 13, or between the negative electrode sheet 12 and the separator 13.

[0091] It should be noted that the electrode assembly 10 is a component in a battery cell where electrochemical reactions occur. One or more electrode assemblies 10 may be disposed inside a battery cell.

[0092] In the electrode assembly 10, the positive electrode sheet 11 is a continuous positive electrode sheet 11, the negative electrode sheet 12 is a continuous negative electrode sheet 12, and the separator 13 is a continuous separator 13. Two continuous separators 13 are provided. Before winding, one continuous separator 13 is provided between the continuous positive electrode sheet 11 and the continuous negative electrode sheet 12, and the other continuous separator 13 is provided on the side of the continuous negative electrode sheet 12 away from the continuous positive electrode sheet 11, or on the side of the continuous positive electrode sheet 11 away from the continuous negative electrode sheet 12. Based on this, when the positive electrode sheet 11, the separator 13 and the negative electrode sheet 12 are wound and pre-pressed to form a rolled structure, the two continuous separators 13 can separate the positive electrode sheet 11 and the negative electrode sheet 12 to prevent the positive electrode sheet 11 and the negative electrode sheet 12 from direct contact and causing a short circuit. Among them, the separator 13 has a number of pores that allow active ions to penetrate freely.

[0093] As shown in FIG5 , the electrode assembly 10 in a rolled structure has a main body region 15 and a bending region 16 . The main body region 15 is a relatively straight portion located in the middle of the rolled structure, while the bending region 16 is a bent portion located at the end of the main body region 15 .

[0094] It should also be noted that, in the electrode assembly 10 , the porous insulating layer 14 may be provided in one bending region 16 , or in multiple bending regions 16 .

[0095] One or more porous insulating layers 14 may be provided in the bending region 16 where the porous insulating layer 14 is provided. The porous insulating layer 14 may be provided between any circle of the positive electrode sheet 11 and the separator 13, or between any circle of the negative electrode sheet 12 and the separator 13.

[0096] Specifically, the porous insulating layer 14 can be preset at a preset position of the continuous positive electrode sheet 11 or the continuous negative electrode sheet 12 before winding, so that when the positive electrode sheet 11, the diaphragm 13 and the negative electrode sheet 12 are wound into a roll structure, the porous insulating layer 14 can be clamped between the bent part of the electrode sheet and the diaphragm 13, so that the porous insulating layer 14 can be installed conveniently and quickly, and the porous insulating layer 14 can be tightly clamped between the bent part of the electrode sheet and the diaphragm 13 to achieve a stable position and state of the porous insulating layer 14.

[0097] It should also be noted that the porous insulating layer 14 has electrolyte resistance, so that the porous insulating layer 14 does not dissolve in the electrolyte 20 .

[0098] The porous insulating layer 14 has a number of pores through which active ions can freely penetrate. Therefore, during the charge and discharge process of the battery cell, the active ions can freely pass through the porous insulating layer 14 and the separator 13, and move between the positive electrode plate 11 and the negative electrode plate 12. This effectively ensures that the provision of the porous insulating layer 14 does not significantly affect the charge and discharge process of the battery cell, effectively maintaining the charge and discharge performance of the battery cell.

[0099] The porous insulating layer 14 is made of insulating material and has good insulating properties.

[0100] Based on this, when the porous insulating layer 14 is disposed between the bent portion of the positive electrode tab 11 and the separator 13 in any circle, even during the battery cell charging process, active ions are released from the bent portion of the negative electrode tab 12, and as the battery cell is used for a longer time, dendrites grow from the defects in the bent portion of the separator 13. The porous insulating layer 14 disposed between the positive electrode tab 11 and the separator 13 in any circle can also insulate and block the growing dendrites, preventing the dendrites from directly contacting and conducting the positive and negative electrode tabs 11 and 12, and even effectively slowing the growth rate of the dendrites to a certain extent. This can effectively delay the occurrence of "dendrites directly causing internal short circuits in the battery cell" and the occurrence of "dendrites heating up due to short circuits and melting the separator 13 around the dendrites, causing direct contact and short circuits between the positive and negative electrode tabs 11 and 12 at the melted separator 13." This can correspondingly extend the service life of the battery cell and improve the safety of the battery cell.

[0101] When the porous insulating layer 14 is provided between the bent portion of the negative electrode plate 12 of any circle and the diaphragm 13, even during the charging process of the battery cell, active ions are released from the bent portion of the negative electrode plate 12. The porous insulating layer 14 provided between the negative electrode plate 12 of any circle and the diaphragm 13 can shield and protect the bent portion of the diaphragm 13. This can effectively delay the occurrence of the phenomenon of "the released active ions breaking through the porous insulating layer 14", the phenomenon of "the dendrites directly causing a short circuit inside the battery cell", and the phenomenon of "the dendrites heating up due to the short circuit and melting the diaphragm 13 on the side of the dendrites, causing a direct contact and short circuit between the positive electrode plate 11 and the negative electrode plate 12 where the diaphragm 13 melts", thereby correspondingly extending the service life of the battery cell and improving the safety of the battery cell.

[0102] In summary, the battery cell provided in the embodiment of the present application has a porous insulating layer 14 provided between the bent portion of the positive electrode sheet 11 or the negative electrode sheet 12 of any circle and the diaphragm 13. Based on this, the pores of the porous insulating layer 14 can allow active ions to freely penetrate to ensure that the porous insulating layer 14 does not have a significant impact on the charging and discharging process of the battery cell, thereby ensuring the charging and discharging performance of the battery cell. On this basis, the porous insulating layer 14 with insulating properties can also be used to hinder dendrites, so as to effectively delay the occurrence of the phenomenon of "dendrites directly causing internal short circuits in the battery cell", and effectively delay the occurrence of the phenomenon of "dendrites heating up due to short circuits and melting the diaphragm 13 on the side of the dendrites, causing direct contact and short circuit between the positive electrode sheet 11 and the negative electrode sheet 12 at the place where the diaphragm 13 melts", thereby correspondingly extending the service life of the battery cell and improving the safety of the battery cell.

[0103] Furthermore, the battery cell provided in the embodiment of the present application can also provide a buffering effect on the bending stress borne by the bent portion of the electrode sheet through the porous insulating layer 14 provided between the bent portion of the electrode sheet and the diaphragm 13 during the winding and pre-pressing of the electrode assembly 10 and during the use of the battery cell, thereby effectively reducing the risk of tearing defects in the bent portion of the electrode sheet leading to a reduction in active material, effectively reducing the risk of metal precipitation in the bending area 16 of the electrode assembly 10 due to a reduction in active material, and effectively mitigating the growth rate of dendrites, thereby correspondingly extending the service life of the battery cell and correspondingly improving the safety of the battery cell.

[0104] Please refer to FIG. 5 , FIG. 6 , and FIG. 7 . In some embodiments of the present application, in the bending region 16 , at least one porous insulating layer 14 is disposed on the inner side of the innermost positive electrode plate 112 .

[0105] It should be noted that in the electrode assembly 10, a porous insulating layer 14 may be provided in one bending region 16, or multiple bending regions 16 may be provided with porous insulating layers 14. In the bending regions 16 provided with porous insulating layers 14, at least one porous insulating layer 14 is provided on the inner side of the bent portion of the innermost positive electrode tab 112.

[0106] Because the radius of curvature decreases toward the innermost circle, the bent portion of the innermost positive electrode tab 112 and the bent portion of the innermost negative electrode tab 122 are subject to greater bending stress and are more susceptible to powder loss, resulting in metal deposition between the bent portion of the innermost positive electrode tab 112 and the bent portion of the innermost negative electrode tab 122. Furthermore, because the bent portion of the innermost positive electrode tab 112 is relatively outward of the bent portion of the innermost negative electrode tab 122, metal deposition is likely to occur from the bent portion of the innermost negative electrode tab 122 during battery cell charging.

[0107] Therefore, by adopting the above scheme, on the one hand, when "metal precipitation occurs at the bent portion of the innermost circle negative electrode sheet 122, and dendrites grow from the defects of the bent portion of the diaphragm 13 over time", the growing dendrites can be insulated and blocked by the porous insulating layer 14 arranged on the inner side of the bent portion of the innermost circle positive electrode sheet 112 to prevent the dendrites from directly contacting the conductive positive electrode sheet 11 and the negative electrode sheet 12. This can effectively delay the occurrence of "dendrites directly causing internal short circuits in the battery cell" between the innermost circle positive electrode sheet 112 and the innermost circle negative electrode sheet 122 where metal precipitation is easily generated, and effectively delay the occurrence of "dendrites heating up due to short circuits and melting the diaphragm 13 on the side of the dendrites, causing direct contact and short circuit between the positive electrode sheet 11 and the negative electrode sheet 12 where the diaphragm 13 melts", thereby correspondingly extending the service life of the battery cell and improving the safety of the battery cell.

[0108] On the other hand, during the winding and pre-pressing of the electrode assembly 10 and during the use of the battery cell, the porous insulating layer 14 disposed on the inner side of the bent portion of the innermost positive electrode tab 112 can buffer the compressive stress borne by the bent portion of the innermost positive electrode tab 112, thereby reducing the risk of tearing defects in the bent portion of the innermost positive electrode tab 112, which leads to a reduction in active material. It can even buffer the tensile stress borne by the bent portion of the innermost negative electrode tab 122, thereby reducing the risk of tearing defects in the bent portion of the innermost negative electrode tab 122, which leads to a reduction in active material. This can effectively reduce the risk of metal precipitation caused by the reduction in active material, and can effectively alleviate the growth rate of dendrites between the innermost positive electrode tab 112 and the innermost negative electrode tab 122, thereby correspondingly extending the service life of the battery cell and improving the safety of the battery cell.

[0109] Please refer to FIG. 5 , FIG. 6 , and FIG. 7 . In some embodiments of the present application, in the bending region 16 , at least one porous insulating layer 14 is disposed on the outer side of the innermost positive electrode sheet 112 .

[0110] It should be noted that in the electrode assembly 10, a porous insulating layer 14 may be provided in one bending region 16, or multiple bending regions 16 may be provided with porous insulating layers 14. In the bending regions 16 provided with porous insulating layers 14, at least one porous insulating layer 14 is provided outside the bent portion of the innermost positive electrode tab 112.

[0111] Because the bent portion of the innermost positive electrode tab 112 is subject to significant bending stress, the aforementioned solution allows the porous insulating layer 14 disposed outside the bent portion of the innermost positive electrode tab 112 to buffer the tensile stress experienced by the bent portion of the innermost positive electrode tab 112 during the winding and pre-pressing of the electrode assembly 10 and during the use of the battery cell. This reduces the risk of tearing defects in the bent portion of the innermost positive electrode tab 112, leading to a reduction in active material. Furthermore, the porous insulating layer 14 can buffer the compressive stress experienced by the bent portion of the second innermost negative electrode tab 123, reducing the risk of tearing defects in the bent portion of the second innermost negative electrode tab 123, leading to a reduction in active material. This effectively reduces the risk of metal precipitation exacerbated by the reduction in active material and mitigates the growth rate of dendrites between the innermost positive electrode tab 112 and the second innermost negative electrode tab 123, thereby correspondingly extending the service life and improving the safety of the battery cell.

[0112] The second innermost negative electrode sheet 123 is a circle of negative electrode sheets 12 located outside the innermost positive electrode sheet 112. When the battery cell is charging, the active ions provided by the outer surface of the innermost positive electrode sheet 112 can freely penetrate the porous insulating layer 14 and the separator 13, move to the second innermost negative electrode sheet 123, and embed into the negative active material of the second innermost negative electrode sheet 123.

[0113] Therefore, by adopting the above solution, during the use of the battery cell, the porous insulating layer 14 provided on the outside of the bent portion of the innermost positive electrode tab 112 can be used to insulate and block the dendrites growing toward it, thereby preventing the dendrites from directly contacting and conducting the innermost positive electrode tab 112 and the second innermost negative electrode tab 123. This can effectively delay the occurrence of the phenomenon of "dendrites directly causing internal short circuits in the battery cell" between the innermost positive electrode tab 112 and the second innermost negative electrode tab 123, and effectively delay the occurrence of the phenomenon of "dendrites heating up due to short circuits and melting the diaphragm 13 on the side of the dendrites, causing direct contact and short circuit between the positive electrode tab 11 and the negative electrode tab 12 where the diaphragm 13 melts", thereby correspondingly extending the service life of the battery cell and improving the safety of the battery cell.

[0114] Please refer to Figures 5, 6, and 7. In some embodiments of the present application, the bending area 16 is provided with two porous insulating layers 14, one of which is arranged on the inner side of the innermost positive electrode plate 112, and the other porous insulating layer 14 is arranged on the outer side of the innermost positive electrode plate 112.

[0115] It should be noted that in the electrode assembly 10, a porous insulating layer 14 may be provided in one bending region 16, or multiple bending regions 16 may be provided with porous insulating layers 14. In the bending region 16 provided with a porous insulating layer 14, a porous insulating layer 14 is provided on both the inner side and the outer side of the bent portion of the innermost positive electrode tab 112.

[0116] By adopting the above solution, the bending zone 16 can effectively delay the risk of short circuits through the two porous insulating layers 14 in the "innermost positive electrode sheet 112 and the innermost negative electrode sheet 122" and "innermost positive electrode sheet 112 and the second innermost negative electrode sheet 123" where metal precipitation is likely to occur and the metal precipitation is relatively serious. It can also effectively relieve the compression stress and tensile stress at the bent portion of the innermost positive electrode sheet 112, which is subject to greater bending stress and is prone to tearing defects, thereby reducing the risk of bending and tearing, thereby effectively extending the service life of the battery cell and effectively improving the safety of the battery cell. While maximizing the effectiveness of the porous insulating layer 14, by adopting the above solution, the number of porous insulating layers 14 set can also be reduced, thereby ensuring and improving the energy density of the electrode assembly 10 and the battery cell.

[0117] 5 , 6 , and 7 , in some embodiments of the present application, the electrode assembly 10 includes a main body region 15 and a bending region 16 disposed at an end of the main body region 15 . The porous insulating layer 14 includes a bent section 141 bent in the bending region 16 , and an extension section 142 connected to an end of the bent section 141 and disposed in the main body region 15 .

[0118] It should be noted that, as shown in Figure 5, the electrode assembly 10 with a rolled structure has a main area 15 and a bending area 16. The main area 15 is a relatively straight part of the rolled structure that is relatively located in the middle, while the bending area 16 is a bent part of the rolled structure that is located at the end side of the main area 15.

[0119] The porous insulating layer 14 has a curved section 141, which is disposed in the bend region 16, that is, on the inside or outside of the bent portion of the electrode. The porous insulating layer 14 has one or two extension sections 142. When one extension section 142 is provided, the extension section 142 extends from one end of the curved section 141 and is disposed in the main body region 15. When two extension sections 142 are provided, the two extension sections 142 extend from opposite ends of the curved section 141 and are both disposed in the main body region 15. The extension lengths of the two extension sections 142 can be the same or different.

[0120] Since the porous insulating layer 14 is preset at the preset position of the continuous positive electrode sheet 11 or the continuous negative electrode sheet 12 before winding, by adopting the above scheme, the setting area of ​​the porous insulating layer 14 can be extended accordingly, and the porous insulating layer 14 has a wider fault tolerance range at the preset position on the continuous positive electrode sheet 11 or the continuous negative electrode sheet 12, thereby effectively ensuring that when the electrode assembly 10 is wound, the porous insulating layer 14 can retain the bent section 141 clamped between the bent part of the electrode sheet and the diaphragm 13, and can adapt to the extension section 142 extending to the main area 15 according to the position tolerance, thereby effectively reducing the accuracy requirements for the preset position of the porous insulating layer 14 on the continuous positive electrode sheet 11 or the continuous negative electrode sheet 12, and effectively ensuring and improving the production yield of the electrode assembly 10.

[0121] By adopting the above scheme, the porous insulating layer 14 can also be reliably stabilized by the bent section 141 clamped between the bent part of the electrode and the diaphragm 13, and the extended section 142 clamped between the straight part of the electrode (that is, the part of the electrode corresponding to the main area 15) and the diaphragm 13, thereby effectively reducing the risk of the porous insulating layer 14 shifting during the use of the battery cell, and effectively ensuring that the porous insulating layer 14 can function stably and reliably in a long-lasting manner during the use of the battery cell.

[0122] Please refer to FIG. 4 , FIG. 5 , and FIG. 8 . In some embodiments of the present application, the porous insulating layer 14 is bonded to the positive electrode sheet 11 or the negative electrode sheet 12 by dissolving the adhesive 17 .

[0123] It should be noted that, before winding, a dissolving glue 17 is provided on one side of the porous insulating layer 14 along the thickness direction a thereof.

[0124] The dissolving glue 17 may be coated on the entire area of ​​the side surface of the porous insulating layer 14 , that is, in the thickness direction a of the porous insulating layer 14 , the projected area of ​​the dissolving glue 17 is equal to the projected area of ​​the porous insulating layer 14 .

[0125] The dissolved glue 17 can also be applied to a portion of the side surface of the porous insulating layer 14, that is, the projected area of ​​the dissolved glue 17 is smaller than the projected area of ​​the porous insulating layer 14 in the thickness direction a of the porous insulating layer 14. In this scenario, the dissolved glue 17 can be applied to any area of ​​the side surface of the porous insulating layer 14, for example, on the four edges of the side surface of the porous insulating layer 14, and this embodiment does not impose a limitation on this. In this scenario, the ratio of the projected area of ​​the dissolved glue 17 to the projected area of ​​the porous insulating layer 14 in the thickness direction a of the porous insulating layer 14 can be any value, for example, 50%, and this embodiment does not impose a limitation on this.

[0126] By adopting the above solution, before winding, the porous insulating layer 14 can be bonded to the preset position of the continuous positive electrode sheet 11 or the continuous negative electrode sheet 12 by dissolving the glue 17, so as to stabilize the preset position and preset state relative to the electrode sheet. Based on this, during the winding process of the electrode assembly 10, it can be ensured that the porous insulating layer 14 can be wound along with the continuous positive electrode sheet 11 or the continuous negative electrode sheet 12 in a stable position and state relative to the electrode sheet, and is wound to the bending area 16, so that the porous insulating layer 14 can be installed conveniently and quickly, and the position accuracy and effectiveness of the porous insulating layer 14 in the formed electrode assembly 10 can be effectively guaranteed and improved, which can effectively guarantee and improve the production efficiency and production yield of the electrode assembly 10.

[0127] Please refer to FIG. 4 , FIG. 5 , and FIG. 8 . In some embodiments of the present application, the battery cell includes an electrolyte 20 for soaking the electrode assembly 10 . The electrolyte 20 contains a dissolving glue 17 .

[0128] It should be noted that the dissolving glue 17 is easily soluble in the electrolyte 20 .

[0129] Before winding, the porous insulating layer 14 can be bonded to a preset position of the continuous positive electrode sheet 11 or the continuous negative electrode sheet 12 by dissolving the glue 17 to stabilize the preset position and preset state relative to the electrode sheet, so that the porous insulating layer 14 can be wound with the positive electrode sheet 11, the separator 13 and the negative electrode sheet 12 to form the electrode assembly 10.

[0130] When the electrode assembly 10 and the electrolyte 20 are encapsulated inside the battery cell, at least a portion of the dissolving glue 17 bonded between the electrode and the porous insulating layer 14 can be dissolved in the electrolyte 20 to reduce or even eliminate the obstruction of the corresponding areas of the electrode and the porous insulating layer 14, thereby facilitating the free and normal penetration of active ions through the porous insulating layer 14, and facilitating the free and normal embedding of active ions into the electrode, thereby effectively ensuring that the setting of the porous insulating layer 14 will not have a significant impact on the charging and discharging process of the battery cell, and effectively ensuring the charging and discharging performance of the battery cell.

[0131] After the battery cell is formed, the dissolved glue 17 bonded between the electrode and the porous insulating layer 14 may be completely dissolved in the electrolyte 20, or partially dissolved in the electrolyte 20 with some remaining between the electrode and the porous insulating layer 14. When the dissolved glue 17 partially remains between the electrode and the porous insulating layer 14, although it will slightly block the corresponding areas of the electrode and the porous insulating layer 14, it will not significantly affect the charging and discharging process of the battery cell. Therefore, this embodiment does not exclude the situation where "the dissolved glue 17 partially dissolves in the electrolyte 20 and partially remains between the electrode and the porous insulating layer 14."

[0132] Please refer to FIG. 4 , FIG. 5 , and FIG. 8 . In some embodiments of the present application, the dissolving adhesive 17 is a modified acrylic pressure-sensitive adhesive, and the electrolyte 20 contains a modified acrylic resin.

[0133] It should be noted that the dissolving adhesive 17 is a modified acrylic pressure-sensitive adhesive. This modified acrylic pressure-sensitive adhesive combines the liquid viscosity of pressure-sensitive adhesive and can be easily, quickly, and reliably applied to one side of the porous insulating layer 14 along its thickness direction a in the early stage, thereby facilitating the dissolving adhesive 17 to form an adhesive layer.

[0134] The modified acrylic pressure-sensitive adhesive also combines the solid elastic properties of pressure-sensitive adhesive. Before winding, only a little pressure is required to achieve bonding between the dissolved adhesive 17 and the electrode sheet, thereby facilitating the porous insulating layer 14 to be quickly and reliably bonded to the preset position of the continuous positive electrode sheet 11 or the continuous negative electrode sheet 12 via the dissolved adhesive 17.

[0135] This modified acrylic pressure-sensitive adhesive also incorporates the readily degradable properties of modified acrylic resin. When the electrode assembly 10 and electrolyte 20 are encapsulated within the battery cell, it rapidly dissolves in the electrolyte 20 and leaves little adhesive residue. Because the modified acrylic pressure-sensitive adhesive dissolves in the electrolyte 20, the electrolyte 20 within the battery cell will contain a modified acrylic resin component.

[0136] Therefore, by adopting the above solution, on the one hand, the dissolving glue 17 can be made to have the liquid viscosity properties of a pressure-sensitive adhesive, so that the dissolving glue 17 can be easily, quickly, and reliably formed on one side of the porous insulating layer 14 along its thickness direction a by coating. On the other hand, the dissolving glue 17 can be made to have the solid elastic properties of a pressure-sensitive adhesive, so that the dissolving glue 17 can be easily and reliably bonded to the electrode sheet with only a small pressure before winding, so that the porous insulating layer 14 can be easily and quickly stably installed at the preset position of the continuous positive electrode sheet 11 or the continuous negative electrode sheet 12. On the other hand, the dissolving glue 17 can be made to have the easily degradable properties of a modified acrylic resin, so that the dissolving glue 17 can be quickly and easily dissolved in the electrolyte 20 without leaving any residue when the electrode assembly 10 and the electrolyte 20 are encapsulated inside the battery cell.

[0137] Please refer to FIG. 4 , FIG. 5 , and FIG. 8 . In some embodiments of the present application, the initial thickness of the dissolving glue 17 is 2 um to 8 um.

[0138] It should be noted that the initial thickness of the dissolved glue 17 refers to the dimension of the dissolved glue 17 along the thickness direction a of the porous insulating layer 14 before winding.

[0139] By adopting the above solution, on the one hand, the adhesion between the dissolving glue 17 and the electrode sheet can be guaranteed before winding, thereby ensuring that the porous insulating layer 14 can be reliably temporarily fixed to the electrode sheet via the dissolving glue 17. On the other hand, when the electrode assembly 10 and the electrolyte 20 are encapsulated inside the battery cell, the dissolving glue 17 can be ensured to dissolve quickly in the electrolyte 20, thereby reducing the amount of residual glue on the porous insulating layer 14. This can reduce the blocking effect of the dissolving glue 17 on the pores of the porous insulating layer 14, ensure that active ions can freely and normally penetrate the porous insulating layer 14, and maintain electrical conductivity.

[0140] Referring to FIG. 4 and FIG. 5 , in some embodiments of the present application, the absolute value of the difference between the porosity of the porous insulating layer 14 and the porosity of the diaphragm 13 is less than or equal to 25%.

[0141] It should be noted that, in this embodiment, the porosity can be determined by the gas replacement method. Specifically, it can be determined by referring to GB / T 24586-2009 through the following steps: the porous insulating layer 14 or the diaphragm 13 is immersed in ethyl methyl carbonate (EMC) for cleaning, then filled into a specific device, and measured by the gas replacement method. Among them, the percentage of the pore volume in the porous insulating layer 14 to the total volume of the porous insulating layer 14 is the porosity of the porous insulating layer 14, and the percentage of the pore volume in the diaphragm 13 to the total volume of the diaphragm 13 is the porosity of the diaphragm 13. Specifically, porosity = (V-V0) / V×100%, where V0 is the true volume and V is the apparent volume.

[0142] It should also be noted that the porosity of the porous insulating layer 14 can be greater than the porosity of the diaphragm 13, and the difference between the porosity of the porous insulating layer 14 and the porosity of the diaphragm 13 is less than or equal to 25%. For example, the porosity of the porous insulating layer 14 is 50%, the porosity of the diaphragm 13 is 35%, and the difference between the porosity of the porous insulating layer 14 and the porosity of the diaphragm 13 is 15%. For another example, the porosity of the porous insulating layer 14 is 40%, and the porosity of the diaphragm 13 is 35%, and the difference between the porosity of the porous insulating layer 14 and the porosity of the diaphragm 13 is 5%.

[0143] The porosity of the porous insulating layer 14 may also be smaller than the porosity of the diaphragm 13 , and the difference between the porosity of the diaphragm 13 and the porosity of the porous insulating layer 14 is less than or equal to 25%.

[0144] By adopting the above solution, the porosity of the porous insulating layer 14 can be made not much different from the porosity of the diaphragm 13. Based on this, active ions can freely and normally penetrate the porous insulating layer 14 and the diaphragm 13, thereby effectively ensuring that the setting of the porous insulating layer 14 will not have a significant impact on the charging and discharging process of the battery cell, and effectively ensuring the charging and discharging performance of the battery cell.

[0145] Referring to FIG. 4 and FIG. 5 , in some embodiments of the present application, the absolute value of the difference between the porosity of the porous insulating layer 14 and the porosity of the diaphragm 13 is less than or equal to 10%.

[0146] By adopting the above solution, the porosity of the porous insulating layer 14 can be set to be similar to the porosity of the diaphragm 13. In this way, active ions can freely and normally penetrate the porous insulating layer 14 and the diaphragm 13, thereby effectively ensuring that the setting of the porous insulating layer 14 will not have a significant impact on the charging and discharging process of the battery cell, and effectively ensuring and improving the charging and discharging performance of the battery cell.

[0147] Please refer to FIG. 4 and FIG. 5 . In some embodiments of the present application, the porous insulating layer 14 is a polyolefin membrane, such as a polypropylene (PP) membrane.

[0148] By adopting the above scheme, the porous insulating layer 14 can be made of a polyolefin membrane such as a polypropylene membrane to ensure that the porosity of the porous insulating layer 14 is similar to or even the same as the porosity of the membrane 13, thereby ensuring that active ions can freely and normally penetrate the porous insulating layer 14 and the membrane 13, and effectively ensuring that the setting of the porous insulating layer 14 will not have a significant impact on the charging and discharging process of the battery cell, thereby effectively ensuring the charging and discharging performance of the battery cell.

[0149] Please refer to FIG. 4 , FIG. 5 , and FIG. 8 . In some embodiments of the present application, the porosity of the porous insulating layer 14 is 40% to 50%.

[0150] It should be noted that, in theory, the greater the porosity of the porous insulating layer 14, the better the air permeability. However, as the porosity of the porous insulating layer 14 increases, when the same mass of dissolved glue 17 is applied to the side of the porous insulating layer 14, the amount of glue that penetrates into the pores of the porous insulating layer 14 will increase, and the amount of glue that remains on the surface of the porous insulating layer 14 will decrease, causing the adhesion of the dissolved glue 17 to deteriorate, thereby causing the temporary fixing effect between the porous insulating layer 14 and the electrode sheet to deteriorate. Moreover, when the electrode assembly 10 and the electrolyte 20 are encapsulated into the interior of the battery cell, as the porosity of the porous insulating layer 14 increases, the same mass of dissolved glue 17 that remains in the pores of the porous insulating layer 14 will increase, causing the air permeability of the porous insulating layer 14 and the penetration rate of active ions to deteriorate, thereby causing the electrical conductivity to deteriorate.

[0151] Therefore, by adopting the above solution, on the one hand, the air permeability of the porous insulating layer 14 can be ensured to be moderate, and the active ions can freely and normally penetrate the porous insulating layer 14. On the other hand, it can ensure that when the dissolving glue 17 is applied to the side of the porous insulating layer 14, a small amount of glue penetrates into the pores of the porous insulating layer 14, while a large amount of glue remains on the surface of the porous insulating layer 14, thereby ensuring the adhesion of the dissolving glue 17 and ensuring that the porous insulating layer 14 can be reliably temporarily fixed to the electrode via the dissolving glue 17. On the other hand, it can ensure that when the dissolving glue 17 is dissolved in the electrolyte 20, a small amount of glue remains in the pores of the porous insulating layer 14, thereby reducing the blocking effect of the dissolving glue 17 on the pores of the porous insulating layer 14, ensuring that the active ions can freely and normally penetrate the porous insulating layer 14, and ensuring electrical conductivity.

[0152] Referring to FIG. 4 , FIG. 5 , and FIG. 8 , in some embodiments of the present application, the pore diameter of the porous insulating layer 14 is A, the thickness of the porous insulating layer 14 is B, and 24≤B / A≤400.

[0153] It should be noted that the porous insulating layer 14 has a plurality of pores, and the pore diameter A of the porous insulating layer 14 refers to the radial size of each pore of the porous insulating layer 14 .

[0154] It is understandable that the pore size A of each pore of the porous insulating layer 14 may be exactly the same or different. The pore size may refer to the pore size when the pore size of each pore is the same, or the pore size of any part of the pores when the pore size of each pore is not exactly the same.

[0155] It is understood that the shape of each hole in the porous insulating layer 14 can be circular or other shapes such as rectangular. When the hole is circular, the hole diameter A refers to the hole diameter; when the hole is rectangular or other shapes, the hole diameter A refers to the size of the hole in the radial direction perpendicular to the central axis.

[0156] It should also be noted that the thickness B of the porous insulating layer 14 refers to the dimension of the porous insulating layer 14 along the thickness direction a thereof.

[0157] B / A refers to the ratio of the thickness B of the porous insulating layer 14 to the pore diameter A of the pores of the porous insulating layer 14 in the same unit.

[0158] When B / A is less than 24, the thickness B of the porous insulating layer 14 will be too small, and the pore size A of the porous insulating layer 14 will be too large. At this time, dendrites will more easily pierce the porous insulating layer 14 or pass through the porous insulating layer 14, and the barrier effect will not be achieved.

[0159] When B / A is greater than 400, the thickness B of the porous insulating layer 14 will be too large, and the pore size A of the porous insulating layer 14 will be too small. At this time, the path for the active ions to shuttle in the porous insulating layer 14 will be too long, and because the pore size A of the porous insulating layer 14 is too small, the active ions have difficulty in shuttling, which can easily cause more active ions to precipitate.

[0160] Therefore, by adopting the above solution, the thickness B of the porous insulating layer 14 and the pore diameter A of the porous insulating layer 14 can be made moderate. Based on this, on the one hand, it is difficult for dendrites to pierce or pass through the porous insulating layer 14, thereby ensuring the porous insulating layer 14's dendrite barrier effect; on the other hand, it allows active ions to easily shuttle through the porous insulating layer 14 and the shuttle path is short, thereby reducing the risk of active ion precipitation due to shuttle difficulties. This can effectively extend the service life of the battery cell and effectively improve the safety of the battery cell.

[0161] Please refer to FIG. 4 , FIG. 5 , and FIG. 8 . In some embodiments of the present application, the thickness B of the porous insulating layer 14 is 12 um to 20 um.

[0162] It should be noted that, in theory, the greater the thickness B of the porous insulating layer 14, the better the insulating barrier effect of the porous insulating layer 14 on dendrites. However, as the thickness B of the porous insulating layer 14 increases, the energy density of the battery cell decreases, and the penetration rate of active ions through the porous insulating layer 14 decreases, resulting in poor electrical conductivity and even exacerbated metal precipitation.

[0163] Therefore, by adopting the above-mentioned scheme, the thickness B of the porous insulating layer 14 can be ensured to be moderate, so as to ensure that the porous insulating layer 14 can form a better insulating barrier effect on the dendrites growing toward it, while reducing the influence of the porous insulating layer 14 on the energy density of the battery cell and the penetration rate of active ions through the porous insulating layer 14, thereby ensuring the electrical conductivity, ensuring the charging and discharging performance of the battery cell, extending the service life of the battery cell accordingly, and improving the safety of the battery cell accordingly.

[0164] Please refer to FIG. 4 , FIG. 5 , and FIG. 8 . In some embodiments of the present application, the pore diameter A of the pores of the porous insulating layer 14 is 0.05 um to 0.5 um.

[0165] It should be noted that, in theory, the larger the pore size A of the porous insulating layer 14, the better the air permeability. However, as the pore size A of the porous insulating layer 14 increases, when the same mass of dissolved glue 17 is applied to the side of the porous insulating layer 14, the amount of glue that penetrates into the pores of the porous insulating layer 14 will increase, and the amount of glue remaining on the surface of the porous insulating layer 14 will decrease, causing the adhesion of the dissolved glue 17 to deteriorate, thereby causing the temporary fixing effect of the porous insulating layer 14 to deteriorate. Moreover, when the electrode assembly 10 and the electrolyte 20 are encapsulated into the interior of the battery cell, as the pore size A of the porous insulating layer 14 increases, the same mass of dissolved glue 17 remaining in the pores of the porous insulating layer 14 will increase, causing the air permeability of the porous insulating layer 14 and the penetration rate of active ions to deteriorate, thereby causing the electrical conductivity to deteriorate. Moreover, as the pore diameter A of the porous insulating layer 14 increases, during the use of the battery cell, the porous insulating layer 14 will have a worse barrier effect on dendrites growing from defects in the diaphragm 13 , and there may even be a risk of dendrites growing from the pores of the porous insulating layer 14 .

[0166] Therefore, by adopting the above solution, on the one hand, the air permeability of the porous insulating layer 14 can be ensured to be moderate, and the active ions can freely and normally penetrate the pores of the porous insulating layer 14. On the other hand, it can ensure that when the dissolving glue 17 is applied to the side of the porous insulating layer 14, a small amount of glue penetrates into the pores of the porous insulating layer 14, while a large amount of glue remains on the surface of the porous insulating layer 14, thereby ensuring the adhesion of the dissolving glue 17 and ensuring that the porous insulating layer 14 can be reliably temporarily fixed to the electrode via the dissolving glue 17. On the other hand, it can ensure that when the dissolving glue 17 is dissolved in the electrolyte 20, a small amount of glue remains in the pores of the porous insulating layer 14, thereby reducing the blocking effect of the dissolving glue 17 on the pores of the porous insulating layer 14, ensuring that the active ions can freely and normally penetrate the pores of the porous insulating layer 14, and ensuring electrical conductivity. On the one hand, during the use of the battery cell, the porous insulating layer 14 can ensure the barrier effect of dendrites growing from the defects of the diaphragm 13 and reduce the risk of dendrites growing from the pores of the porous insulating layer 14, thereby correspondingly extending the service life of the battery cell and improving the safety of the battery cell.

[0167] Please refer to FIG4, FIG5, and FIG8. In some embodiments of the present application, the tensile strength of the porous insulating layer 14 in the width direction b is greater than or equal to 1000 kgf / cm 2 .

[0168] It should be noted that the extension direction of the porous insulating layer 14 corresponds to the extension direction of the electrode, which is also the winding direction of the electrode. The width direction b of the porous insulating layer 14 corresponds to the width direction of the electrode. The tensile strength of the porous insulating layer 14 along the width direction b can be measured by applying a tensile force to the porous insulating layer 14 along the width direction b until the porous insulating layer 14 can no longer withstand the tensile force and breaks. The tensile strength of the porous insulating layer 14 along the width direction b reflects the ability of the porous insulating layer 14 to resist damage in the width direction b when subjected to a tensile force.

[0169] Because the porous insulating layer 14 is disposed in the bending region 16, the porous insulating layer 14 is subjected to a certain amount of tension during the winding and pre-pressing of the electrode assembly 10 and during the use of the battery cell. Based on this, by adopting the above solution, it is possible to ensure that the porous insulating layer 14 has sufficient tensile strength in its width direction b, which can effectively reduce the risk of the porous insulating layer 14 breaking or cracking under the action of tension, thereby ensuring and improving the insulating barrier effect of the porous insulating layer 14 on dendrites growing from defects in the diaphragm 13, and effectively reducing the risk of dendrites continuing to grow along the fracture and cracking defects of the porous insulating layer 14, thereby correspondingly extending the service life of the battery cell and correspondingly improving the safety of the battery cell.

[0170] It should be noted that when the porous insulating layer 14 has sufficient tensile strength in its width direction b, the tensile strength of the porous insulating layer 14 in its extension direction can basically meet the requirements. Therefore, this embodiment does not specifically limit the tensile strength of the porous insulating layer 14 in its extension direction.

[0171] Please refer to FIG. 4 , FIG. 5 , and FIG. 8 . In some embodiments of the present application, the elongation of the porous insulating layer 14 in the width direction b thereof is greater than or equal to 10%.

[0172] It should be noted that, by applying a tensile force along the width direction b to the porous insulating layer 14 until the porous insulating layer 14 can no longer withstand the tensile force and is broken, the percentage of the tensile deformation part of the porous insulating layer 14 in its width direction b to the original length is the elongation of the porous insulating layer 14 in its width direction b.

[0173] Because the electrode assembly 10 may expand and deform during battery cell use, the porous insulating layer 14 disposed in the bend region 16 of the electrode assembly 10 must exhibit a certain degree of elongation and deformation. Therefore, the above-described solution ensures that the porous insulating layer 14 has sufficient elongation in its width direction b, ensuring that the porous insulating layer 14 can adaptively extend and deform along with the electrode assembly 10. This ensures that the porous insulating layer 14's effective range covers the corresponding area of ​​the electrode sheet and can reliably provide an insulating barrier against dendrites growing from defects in the separator 13.

[0174] Please refer to FIG. 4 , FIG. 5 , and FIG. 8 . In some embodiments of the present application, the shrinkage rate of the porous insulating layer 14 at 105° C. is 0-3%.

[0175] It should be noted that the shrinkage rate of the porous insulating layer 14 at 105°C can be obtained by comparing the shrinkage of the “dimensions of the porous insulating layer 14 at 105°C” with the “dimensions of the porous insulating layer 14 at room temperature”.

[0176] During the use of a battery cell, as the battery cell's internal temperature gradually increases, the porous insulating layer 14 may shrink and deform. If the shrinkage is too large, the effective range of the porous insulating layer 14 may not cover the corresponding area of ​​the entire electrode. Based on this, by adopting the above solution, the degree of dimensional shrinkage of the porous insulating layer 14 caused by the internal temperature of the battery cell can be guaranteed to be small during the use of the battery cell, thereby ensuring that the effective range of the porous insulating layer 14 can cover the corresponding area of ​​the electrode, and ensuring that the porous insulating layer 14 can form a reliable insulation barrier effect on dendrites growing from defects in the diaphragm 13.

[0177] Please refer to FIG. 2 . Some embodiments of the present application further provide a battery 1 , wherein the battery 1 includes a battery cell provided in an embodiment of the present application.

[0178] By adopting the above solution, the battery 1 can ensure and extend the service life of the battery 1 and ensure and improve the safety of the battery 1 by applying the battery cells provided in the embodiments of the present application.

[0179] Please refer to FIG1 . Some embodiments of the present application further provide an electrical device, wherein the electrical device includes a battery 1 or a battery cell provided in an embodiment of the present application.

[0180] By adopting the above solution, the electrical device can ensure and extend the service life of the electrical device and ensure and improve the safety of the electrical device by applying the battery 1 or battery cell provided in the embodiment of the present application.

[0181] The above are merely optional embodiments of the present application and are not intended to limit the present application. For those skilled in the art, the present application may have various modifications and variations. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present application should be included within the scope of the claims of the present application.

Claims

1. A battery cell, wherein: The battery cell includes at least one electrode assembly, and the electrode assembly includes a positive electrode sheet, a negative electrode sheet, a separator and a porous insulating layer; The positive electrode sheet, the separator and the negative electrode sheet are stacked and wound; At least a portion of the porous insulating layer is disposed in a bending region of the electrode assembly, and the porous insulating layer is disposed between the positive electrode sheet and the separator, or between the negative electrode sheet and the separator.

2. The battery cell according to claim 1, wherein: In the bending region, at least one of the porous insulating layers is arranged on the inner side of the innermost circle of the positive electrode sheet.

3. The battery cell according to claim 1, wherein: In the bending region, at least one of the porous insulating layers is arranged on the outer side of the innermost circle of the positive electrode sheet.

4. The battery cell according to claim 1, wherein: The bending area is provided with two porous insulating layers, one of which is arranged on the inner side of the innermost circle of the positive electrode sheet, and the other porous insulating layer is arranged on the outer side of the innermost circle of the positive electrode sheet.

5. The battery cell according to claim 1, wherein The electrode assembly comprises a main body region and a bending region arranged at an end side of the main body region; The porous insulating layer comprises a bent section bent in the bending region, and an extending section connected to an end of the bent section and arranged in the main region. The battery cell according to claim 1 , wherein: The porous insulating layer is bonded to the positive electrode sheet or the negative electrode sheet by dissolving the adhesive.

7. The battery cell according to claim 6, wherein: The battery cell includes an electrolyte for soaking the electrode assembly, and the electrolyte contains dissolved glue.

8. The battery cell according to claim 6 or 7, wherein: The dissolving adhesive is a modified acrylic pressure-sensitive adhesive, and the electrolyte contains modified acrylic resin.

9. The battery cell according to any one of claims 1 to 8, wherein: An absolute value of a difference between a porosity of the porous insulating layer and a porosity of the separator is less than or equal to 25%.

10. The battery cell according to claim 9, wherein: An absolute value of a difference between a porosity of the porous insulating layer and a porosity of the separator is less than or equal to 10%.

11. The battery cell according to any one of claims 1 to 8, wherein: The porous insulating layer is a polyolefin separator.

12. The battery cell according to any one of claims 1 to 8, wherein: The porosity of the porous insulating layer is 40% to 50%.

13. The battery cell according to any one of claims 1 to 8, wherein: The pore diameter of the porous insulating layer is A, the thickness of the porous insulating layer is B, and 24≤B / A≤400.

14. The battery cell according to claim 13, wherein: The thickness B of the porous insulating layer is 12um-20um.

15. The battery cell according to claim 13, wherein: The pore diameter A of the porous insulating layer is 0.05um-0.5um.

16. The battery cell according to any one of claims 1 to 8, wherein: The tensile strength of the porous insulating layer in its width direction is greater than or equal to 1000 kgf / cm 2 .

17. The battery cell according to any one of claims 1 to 8, wherein: The porous insulating layer has an elongation in a width direction greater than or equal to 10%.

18. The battery cell according to any one of claims 1 to 8, wherein: The shrinkage rate of the porous insulating layer at 105° C. is 0-3%.

19. A battery, wherein: The battery comprises the battery cell according to any one of claims 1 to 18.

20. An electrical device, wherein: The electrical device comprises the battery according to claim 19, or the battery cell according to any one of claims 1 to 18.

Citation Information

Cited By

  • Battery cell, battery and electric device

    CN119944101A