NiCo2O4 nanoparticles and preparation method thereof, perovskite battery and related assembly
By adding crosslinking agent to nickel and cobalt sources and heating under alkaline environment, the problem of uneven size of NiCo2O4 nanoparticles is solved, and smaller and more uniform nanoparticles are achieved, which improves perovskite Performance and stability of solar cells.
Patent Information
- Application Number
- CN202411023700.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-29
- Publication Date
- 2024-11-15
AI Technical Summary
The synthesis of traditional NiCo2O4 nanoparticles is difficult to achieve precise control of size and morphology, resulting in inconsistent performance in practical applications.
By adding a crosslinking agent to the nickel and cobalt sources and heating it in an alkaline environment to form a sol, the growth of nickel and cobalt coprecipitation is controlled, and NiCo2O4 nanoparticles with smaller particle size and uniformity are obtained through calcination.
The size uniformity of NiCo2O4 nanoparticles is improved, the density and flatness of the hole transport layer in perovskite solar cells is enhanced, interface defects and leakage current are reduced, and device performance and stability are improved.
Smart Images

Figure CN118954624A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of solar cells, and more particularly to a NiCo 2 O 4 Nanoparticles and preparation methods thereof, perovskite cells, photovoltaic modules, and photovoltaic systems. Background Art
[0002] Perovskite photovoltaic cells have attracted widespread attention due to their advantages such as long carrier diffusion length, high absorption coefficient, and adjustable band gap. They are considered to be the third generation of photovoltaic cells that are expected to replace traditional crystalline silicon photovoltaic cells. Inverse perovskite solar cells have been favored by the industry due to their relatively excellent stability. Nanoparticles, as an important nanomaterial, have broad application potential in energy conversion, catalysis, biomedicine and other fields. Among them, NiCo 2 O 4 Nanoparticles have attracted much attention due to their excellent electrochemical performance. 2 O 4 Nanoparticle synthesis of NiCo 2 O 4 The poor size consistency of nanoparticles limits their performance in practical applications.
[0003] It should be noted that the above content is not necessarily prior art, nor is it intended to limit the scope of patent protection of this application. Summary of the invention
[0004] The present application embodiment provides a NiCo 2 O 4 Nanoparticles and preparation methods thereof, perovskite cells, photovoltaic modules, and photovoltaic systems are provided to solve or alleviate one or more of the technical problems raised above.
[0005] In a first aspect, an embodiment of the present application provides a NiCo 2 O 4 The method for preparing nanoparticles comprises the following operations:
[0006] Mixing a nickel source, a cobalt source and a cross-linking agent into a first solvent to obtain a mixed solution, and heating the mixed solution to obtain a sol;
[0007] Adjusting the sol to alkalinity to obtain nickel-cobalt coprecipitation;
[0008] Calcine the nickel-cobalt coprecipitate to obtain NiCo 2 O 4 Nanoparticles.
[0009] In the first aspect of the embodiment of the present application, the nickel source and the cobalt source are coprecipitated by relying on an alkaline environment, and the spatial network obtained by cross-linking with a cross-linking agent is used to limit the growth of the nickel-cobalt coprecipitate, so that its particle size is smaller and the uniformity is higher, thereby obtaining a NiCo 2 O 4 Nanoparticles.
[0010] In a second aspect, an embodiment of the present application provides a NiCo 2 O 4 The nanoparticles are prepared according to the preparation method described in the first aspect. 2 O 4 Nanoparticles have smaller particle size and higher uniformity.
[0011] A third aspect of the present application provides a perovskite solar cell, comprising a hole transport layer, wherein the hole transport layer comprises the NiCo 2 O 4 Nanoparticles. As a result, they are more evenly distributed on the substrate (transparent conductive glass film or perovskite photoactive layer), and the resulting hole transport layer is more compact and flat, with fewer interface defects, which weakens the carrier extraction barrier at the interface and reduces leakage current generation, thereby improving device performance.
[0012] A fourth aspect of an embodiment of the present application provides a photovoltaic module, comprising: at least one cell string, wherein the cell string comprises at least two perovskite solar cells as described above.
[0013] A fifth aspect of an embodiment of the present application provides a photovoltaic system, which includes the photovoltaic assembly as described above. BRIEF DESCRIPTION OF THE DRAWINGS
[0014] In the accompanying drawings, unless otherwise specified, the same reference numerals throughout the multiple drawings represent the same or similar parts or elements. These drawings are not necessarily drawn to scale. It should be understood that these drawings only depict some embodiments disclosed in the present application and should not be regarded as limiting the scope of the present application.
[0015] Figure 1 The NiCo 2 O 4 Flowchart of the nanoparticle preparation method.
[0016] Figure 2 It is a schematic diagram of the structure of the perovskite battery provided in the embodiment of the present application.
[0017] Description of reference numerals:
[0018] 1-transparent conductive glass film; 2-hole transport layer; 3-perovskite photoactive layer; 4-passivation layer; 5-electron transport layer; 6-buffer layer; 7-counter electrode. DETAILED DESCRIPTION
[0019] Embodiments of the present application are described in detail below, and examples of the embodiments are shown in the accompanying drawings. In the accompanying drawings, for clarity, the sizes of layers, regions, elements and their relative sizes may be exaggerated. Wherein the same or similar reference numerals throughout represent the same or similar elements or elements with the same or similar functions. The embodiments described below with reference to the accompanying drawings are exemplary and are only used to explain the present application, and cannot be understood as limitations on the present application. It should be noted that, in the absence of conflict, the embodiments in the present application and the features in the embodiments can be combined with each other.
[0020] It should be understood that when an element or layer is referred to as "on ...", "adjacent to ...", "connected to" or "coupled to" other elements or layers, it can be directly on, adjacent to, connected to or coupled to other elements or layers, or there can be intervening elements or layers. On the contrary, when an element is referred to as "directly on ...", "directly adjacent to ...", "directly connected to" or "directly coupled to" other elements or layers, there is no intervening element or layer. It should be understood that although the terms first, second, third, etc. can be used to describe various elements, components, regions, layers and / or parts, these elements, components, regions, layers and / or parts should not be limited by these terms. These terms are only used to distinguish one element, component, region, layer or part from another element, component, region, layer or part. Therefore, without departing from the teachings of the present disclosure, the first element, component, region, layer or part discussed below can be represented as the second element, component, region, layer or part. And when the second element, component, region, layer or part is discussed, it does not mean that the present disclosure necessarily has the first element, component, region, layer or part.
[0021] In this application, unless otherwise clearly specified and limited, the terms "installed", "connected", "connected", "fixed" and the like should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection or an indirect connection through an intermediate medium, it can be the internal connection of two elements or the interaction relationship between two elements, unless otherwise clearly defined. For ordinary technicians in this field, the specific meanings of the above terms in this application can be understood according to specific circumstances.
[0022] It should be noted that the terms "first", "second", etc. in the specification and claims of the present application and the above-mentioned drawings are used to distinguish similar objects, and are not necessarily used to describe a specific order or sequence. It should be understood that the terms used in this way can be interchangeable where appropriate, so that the embodiments of the present application described herein can be implemented in an order other than those illustrated or described herein, for example. In addition, the terms "including" and "having" and any of their variations are intended to cover non-exclusive inclusions, for example, a process, method, system, product or device that includes a series of steps or units is not necessarily limited to those steps or units that are clearly listed, but may include other steps or units that are not clearly listed or inherent to these processes, methods, products or devices.
[0023] Hereinafter, exemplary embodiments according to the present application will be described in more detail with reference to the accompanying drawings. It should be noted that these exemplary embodiments can be implemented in many different forms and should not be construed as being limited to the embodiments described herein.
[0024] Currently, NiCo 2 O 4 The synthesis methods of (spinel nickel cobalt oxide) nanoparticles are often difficult to achieve for NiCo 2 O 4 Precise control of nanoparticle morphology and size can easily lead to uneven morphology and size distribution.
[0025] Accordingly, the first aspect of the embodiment of the present application provides a NiCo 2 O 4 Preparation method of nanoparticles, by adding a cross-linking agent to prevent NiCo 2 O 4 The NiCo nanoparticles were prepared by agglomeration and precipitation. 2 O 4 The nanoparticle size is more uniform; in addition, the NiCo 2 O 4 When nanoparticles are used in fields such as solar cells, they help improve the long-term stability and performance consistency of materials and devices. See below for details.
[0026] like Figure 1 As shown, the embodiment of the present application provides a NiCo 2 O 4 The method for preparing nanoparticles comprises the following operations:
[0027] S1, mixing a nickel source, a cobalt source and a cross-linking agent into a first solvent to obtain a mixed solution, and heating the mixed solution to obtain a sol;
[0028] S2, adjusting the sol to alkalinity to obtain nickel-cobalt coprecipitation;
[0029] S3, calcining the nickel-cobalt coprecipitate to obtain NiCo 2 O 4 Nanoparticles.
[0030] In this embodiment, the cross-linking agent is cross-linked under heating conditions to form a spatial network structure. After the nickel source and the cobalt source are mixed to form a solution, a nickel-cobalt coprecipitate is formed in an alkaline environment. In the process of forming the nickel-cobalt coprecipitate, the spatial network structure plays a role in limiting the excessive growth of the nickel-cobalt coprecipitate, thereby controlling the particle size of the nickel-cobalt coprecipitate, making the particle size of the nickel-cobalt coprecipitate smaller and more uniform, and then after calcination, a NiCo with a smaller and more uniform particle size is obtained. 2 O 4 Nanoparticles.
[0031] In some embodiments, in S1, in the mixed solution, the molar ratio of nickel atoms in the nickel source to cobalt atoms in the cobalt source is 1:(1-4), for example, 1:1, 1:2, 1:3, 1:4, 1:5, etc.; thereby, the cobalt source is present in excess, so that the added nickel source participates in the reaction as much as possible to obtain nanoparticles of the target chemical formula.
[0032] The nickel source can be any substance that can provide nickel ions in water, and the cobalt source can be any substance that can provide cobalt ions in water. This embodiment does not limit the nickel source and the cobalt source. As some examples, the nickel source includes Ni(NO 3 ) 2 6H 2 O、NiCl 2 6H 2 O、NiSO 4 6H 2 O.Ni(CH 3 COO 2 ·4H 2 O. As other examples, the cobalt source includes Co(NO 3 ) 2 6H 2 O、CoCl 2 6H 2 O. CoSO 4 6H 2 At least one of O.
[0033] In some embodiments, in S1, the crosslinking agent includes at least one of N,N'-methylenebisacrylamide and N-isopropylacrylamide. Further, the concentration of the crosslinking agent is 30g / L-120g / L, for example, 30g / L, 40g / L, 50g / L, 60g / L, 70g / L, 80g / L, 90g / L, 100g / L, 110g / L, 120g / L, etc.
[0034] In some embodiments, in S1, the mixed solution is heated to 50°C to 100°C to obtain a sol, for example, 50°C, 60°C, 70°C, 90°C, 100°C, etc. Thus, during the heating process, the cross-linking agent in the mixed solution begins to cross-link to form a three-dimensional network structure, the nickel ions and the cobalt ions are attached to the three-dimensional network structure, and the mixed solution is transformed into a sol state.
[0035] In some embodiments, in S2, the pH of the sol is adjusted to 8-14, for example, the pH is adjusted to 8, 9, 10, 11, 13.4, etc. Therefore, when the pH of the sol is in this range, it is more conducive to the formation of nickel-cobalt coprecipitation. Preferably, the pH is 10-11. It is understood that the means for adjusting the pH of the sol can be to add an alkaline substance to the sol, such as adding KOH, NaOH, NH 3 ·H 2 O, etc., and an alkaline solution may also be added, such as a KOH aqueous solution, a NaOH aqueous solution, an ammonia solution, etc. Further, the alkaline solution may be 0.01mol / L to 10mol / L. For example, 0.01mol / L, 1mol / L, 5mol / L, 10mol / L, etc. Preferably, when the alkali solution is used to adjust the pH, a dropwise addition method is adopted.
[0036] In some embodiments, after obtaining the nickel-cobalt co-precipitate in S2, it also includes washing and drying the nickel-cobalt co-precipitate. Furthermore, at least one of centrifugal washing, suction filtration washing, and filtration washing can be used for washing, and the washing can be performed 1 to 30 times; further, the washing liquid used for washing the nickel-cobalt co-precipitate includes at least one of deionized water, methanol, and ethanol. Thus, substances that do not participate in the reaction are washed away. After washing, it is dried. As some examples, the nickel-cobalt co-precipitate can undergo a crystal transformation to obtain NiCo 2 O 4 Nanoparticles. Further, the drying time is 1h to 96h at 80°C to 100°C.
[0037] In some embodiments, in S3, the calcination includes: calcining at a temperature of 200°C to 300°C in an air atmosphere, for example, 200°C, 250°C, 280°C, 300°C, so that the calcination time is 1h to 48h, for example, 1h, 10h, 20h, 33h, 48h, etc., thereby ensuring that the crystal transformation is complete while saving energy. Optionally, the calcination also includes washing, using an organic solvent to wash the NiCo 2 O 4 Nanoparticles are used to remove organic impurities. Exemplarily, the organic solvent includes at least one of N,N-dimethylformamide (DMF), dimethyl sulfoxide (DMSO), and N-methylpyrrolidone (NMP).
[0038] The second aspect of the embodiment of the present application provides a NiCo prepared in the first aspect. 2 O 4 Nanoparticles. Thus, NiCo 2 O 4 The size uniformity of the nanoparticles is improved. According to relevant tests, the NiCo 2 O 4 The particle size distribution width PDI (Polydispersity index) of the nanoparticles is small, indicating that NiCo 2 O 4 The particle size of nanoparticles is relatively uniform and the particle size distribution is relatively concentrated.
[0039] In a third aspect of the embodiment of the present application, a perovskite solar cell is provided, comprising a hole transport layer, wherein the hole transport layer comprises the NiCo 2 O 4 Nanoparticles. Therefore, due to NiCo 2 O 4 The nanoparticles are small and uniform, which improves the performance and stability of the device and solves the problem of NiCo 2 O 4 The uneven hole transport layer caused by the uneven size of nanoparticles results in leakage current, which in turn affects the performance and stability of the device.
[0040] In some embodiments, the hole transport layer in the perovskite solar cell is prepared by the following method:
[0041] The NiCo 2 O 4 The nanoparticles and the imidazole salts are dispersed in a second solvent to obtain a dispersion; the dispersion is coated on a transparent conductive glass film or a perovskite photoactive layer to obtain a hole transport layer.
[0042] Therefore, imidazolate salts in the dispersion will passivate NiCo 2 O 4 The nanoparticles have surface defects and form a stable double electrical layer on their surface, which stabilizes the colloid and makes it less likely to aggregate.
[0043] Further, the imidazolium salt may include at least one of 1-ethyl-3-methylimidazolium bromide, 1-ethyl-3-methylimidazolium iodide, and 1-ethyl-3-methylimidazolium chloride. Thus, while maintaining the colloidal stability, the electrical performance can also be optimized when used as an additive material for the hole transport layer.
[0044] Optionally, the concentration of the imidazole salt in the dispersion is 0.1 mg / mL to 0.5 mg / mL, for example, 0.1 mg / mL, 0.25 mg / mL, 0.5 mg / mL, etc.
[0045] In some specific embodiments, when preparing the hole transport layer, the second solvent includes at least one of water, isopropanol, ethanol, and chlorobenzene.
[0046] In some specific embodiments, when preparing the hole transport layer, the NiCo in the dispersion 2 O 4 The mass concentration of the nanoparticles is 5 mg / mL to 70 mg / mL, for example, 5 mg / mL, 15 mg / mL, 35 mg / mL, 70 mg / mL, etc. Thus, a high content of NiCo is provided. 2 O 4 Nanoparticles are beneficial for subsequent coating.
[0047] In some specific embodiments, when preparing the hole transport layer, during coating, multiple coating methods may be used, or one coating method may be used for multiple or single coatings. Exemplarily, the coating method includes at least one of slit coating, spin coating, blade coating, and spray coating.
[0048] In some embodiments, the perovskite solar cell is an inverted perovskite solar cell. Figure 2 , the perovskite solar cell also includes a transparent conductive glass film 1, a perovskite photoactive layer 3, a passivation layer 4, an electron transport layer 5, a buffer layer 6 and a counter electrode 7; the hole transport layer 2, the perovskite photoactive layer 3, the passivation layer 4, the electron transport layer 5, the buffer layer 5 and the counter electrode 7 are sequentially stacked on the transparent conductive glass film 1. Thus, it is applied to inverted perovskite solar cells. The materials and sizes of each layer of the perovskite solar cell can be selected by those skilled in the art according to needs. As some examples, the perovskite solar cell meets at least one of the following conditions: (A) the transparent conductive glass film includes indium tin oxide conductive glass (ITO conductive glass), fluorine-doped SnO 2 Conductive glass (FTO conductive glass), indium tin oxide conductive plastic (ITO conductive plastic), fluorine-doped SnO 2 One of the conductive plastics (FTO conductive plastics); (B) the transparent conductive glass film has a square resistance of 5Ω / sq to 25Ω / sq; (C) the hole transport layer has a thickness of 1nm to 70nm; (D) the perovskite material of the perovskite photoactive layer has a chemical formula of FA x Cs 1-x PbI 3, wherein x is 0.85 to 1; (E) the thickness of the perovskite photoactive layer is 1 nm to 800 nm. (F) the passivation layer includes at least one of 1,3-diaminopropane dihydroiodide (PDADI), 2-phenylethylamine hydroiodide (PEAI), phenylethylammonium bromide (PEABr), dihydroiodic acid ethylenediamine (CAS: 5700-49-2), and formamidine hydroiodide (FAI); (G) the thickness of the passivation layer is 5 nm to 50 nm; (H) the electron transport layer includes carbon 60 (C60), carbon 60 derivative (PC61 BM), carbon 70 (PC71 BM); (I) the thickness of the electron transport layer is 1nm to 50nm; (J) the buffer layer includes at least one of polymethyl methacrylate (PMMA), 2,9-dimethyl-4,7-diphenyl-1,10-phenanthroline, and sodium propargyl sulfonate (PS); (K) the thickness of the buffer layer is 1nm to 50nm; (L) the counter electrode includes at least one of Ag, Au, Cu, Al, ITO, FTO, indium zinc oxide (IZO), silver nanowires, and carbon materials; (M) the thickness of the counter electrode is 1nm to 500nm. Thus, the comprehensive performance of the perovskite solar cell is optimized.
[0049] The embodiment of the present application may also provide a photovoltaic module (not shown), including at least one battery string, the battery string includes at least two perovskite solar cells as described above, and adjacent perovskite solar cells can be connected together by series welding.
[0050] The embodiment of the present application can provide a photovoltaic system, including the photovoltaic components in any of the above embodiments. The advantages of the above photovoltaic components are also possessed by the photovoltaic system, which will not be repeated here. The above photovoltaic system has a wide range of applications, not only limited to photovoltaic power stations, such as ground power stations, rooftop power stations and water power stations, but also includes various equipment and devices that use solar energy to generate electricity, such as user solar power supplies, solar street lights, solar cars and solar buildings. Of course, it can be understood that the application scenarios of the photovoltaic system are not limited to this, that is to say, the photovoltaic system can be used in all fields where solar energy is required for power generation. Taking the photovoltaic power generation system network as an example, the photovoltaic system may include a photovoltaic array, a junction box and an inverter. The photovoltaic array may be an array combination of multiple photovoltaic components. For example, multiple photovoltaic components may form multiple photovoltaic arrays. The photovoltaic array is connected to a junction box. The junction box can converge the current generated by the photovoltaic array. The converged current flows through the inverter and is converted into the alternating current required by the mains power grid, and then connected to the mains network to realize solar power supply.
[0051] The following will conduct performance tests on the method for manufacturing the perovskite solar cell provided in the embodiments of the present application and related comparative examples.
[0052] Example 1
[0053] S0, by weight, 1.803 parts of Ni(NO 3 ) 2 6H 2 O. 3.609 parts Co(NO 3 ) 2 6H 2 O and 2.5 parts of N,N'-methylenebisacrylamide were mixed into 50 parts of water, heated to 80°C to obtain a sol, KOH aqueous solution was added dropwise until the pH of the sol was 10, stirred for 1 hour to react, filtered to obtain a nickel-cobalt coprecipitate, then centrifuged, washed and dried; after drying, calcined at 240°C for 2 hours, the nickel-cobalt coprecipitate was converted into NiCo 2 O 4 Nanoparticles; the reaction product is washed with DMF to remove unreacted organic matter, and then dried.
[0054] NiCo 2 O 4 Nanoparticles and 1-ethyl-3-methylimidazolium bromide were dispersed in deionized water and ultrasonically prepared into a dispersion. 2 O 4 The concentration of the nanoparticles was 20 mg / mL, and the concentration of 1-ethyl-3-methylimidazolium bromide was 0.25 mg / mL.
[0055] S1, using NiCo 2 O 4 The nanoparticle dispersion was spin-coated on ITO transparent conductive glass to prepare 30nm thick NiCo 2 O 4 Layer, namely, hole transport layer;
[0056] S2. Prepare 550 nm thick FA on the hole transport layer using the anti-solvent-free method 0.90 Cs 0.10 PbI 3 layer, which is the perovskite photoactive layer;
[0057] S3, preparing a 5 nm thick PDADI passivation layer on the perovskite photoactive layer by spin coating;
[0058] S4, depositing a 30 nm thick C60 electron transport layer and a 6 nm thick 2,9-dimethyl-4,7-diphenyl-1,10-phenanthroline buffer layer on the passivation layer in sequence by thermal evaporation;
[0059] S5. Depositing a 120 nm thick Ag electrode 7 on the buffer layer by thermal evaporation to obtain a perovskite solar cell.
[0060] Example 2
[0061] The rest is the same as Example 1, except that:
[0062] The calcination temperature in S0 is 200°C and the calcination time is 24h.
[0063] Example 3
[0064] The rest is the same as Example 1, except that:
[0065] The calcination temperature in S0 is 300°C and the calcination time is 4 h.
[0066] Example 4
[0067] The other parts are the same as those in Example 1, except that the pH in S0 is 11.
[0068] Example 5
[0069] The other parts are the same as those in Example 1, except that the pH in S0 is 8.
[0070] Example 6
[0071] The other parts are the same as those in Example 1, except that the pH in S0 is 14.
[0072] Comparative Example 1
[0073] The other parts are the same as those in Example 1, except that: no cross-linking agent N,N'-methylenebisacrylamide is added to S0.
[0074] Comparative Example 2
[0075] The other aspects are the same as those of Example 1, except that no alkali solution is added to SO. The sol state is observed to have not changed during the stirring process, and no precipitation occurs, indicating that in a non-alkaline environment, without the participation of a precipitant, nickel-cobalt coprecipitation does not occur. 2 O 4 Nanoparticles, so S1 to S5 were not performed.
[0076] The perovskite solar cells of Examples 1 to 6 and Comparative Example 1 were subjected to IV tests. The IV tests were conducted under standard test conditions (STC), i.e., the light intensity was 1000 W / m 2 , the solar panel temperature is 25°C, the air mass is AM1.5, and the data obtained after analyzing the IV curve are shown in Table 1. The perovskite solar cells of Examples 1 to 6 and Comparative Example 1 are subjected to 1000 W / m 2 The maximum power point output stability test was carried out under the conditions of 25℃ and AM 1.5G. The test results are as follows: 80 See Table 1.
[0077] Table 1
[0078]
[0079] Note: 80 The lifetime at which the efficiency drops to 80% of the initial value.
[0080] It can be seen from Table 1 that the performance of the devices in Examples 1 to 6 is better than that in Comparative Example 1. This is because after using the cross-linking agent, the cross-linked three-dimensional network will limit the growth of the nickel-cobalt coprecipitate, and thus the NiCo 2 O 4 Nanoparticles are smaller and more uniform than unrestricted particle sizes. Thanks to this, NiCo 2 O 4 The dispersion of nanoparticles is more evenly distributed on the ITO transparent conductive glass, and the resulting hole transport layer is more dense and smooth, with fewer interface defects, which weakens the carrier extraction barrier at the interface and reduces the leakage current, thereby improving the device performance. 2 O 4 The nanoparticles are larger and non-uniform, thus, leakage current and interface defects may occur when used as hole transport layers in perovskite solar cells. Furthermore, the device performance of Examples 5 to 6 is inferior to that of Examples 1 to 4. The particle size of the precipitate formed in Example 5 is too small due to its low pH, and the NiCo 2 O 4 The particle size of the nanoparticles is too small to form a stable colloid and settle locally. The surface of the prepared film is uneven, which will cause leakage current and poor interface contact. In Example 6, due to the high pH, the precipitation growth in the spatial network structure formed by the local cross-linking agent is too large, resulting in the NiCo 2 O 4 The nanoparticles have uneven particle sizes, which will cause leakage current and interface defects in perovskite solar cells as hole transport layers, which is not conducive to the transport and extraction of carriers, and thus damages the device performance.
[0081] It should also be noted that "one embodiment", "another embodiment", "embodiment", etc. mentioned in this application refer to the specific features, structures or characteristics described in conjunction with the embodiment included in at least one embodiment generally described in this application. The same expression appearing in multiple places in the specification does not necessarily refer to the same embodiment. Further, when a specific feature, structure or characteristic is described in conjunction with any embodiment, it is claimed that the realization of such feature, structure or characteristic in conjunction with other embodiments also falls within the scope of this application.
[0082] In the above embodiments, the description of each embodiment has its own emphasis. For parts that are not described in detail in a certain embodiment, reference can be made to the relevant descriptions of other embodiments.
[0083] It should also be noted that the above are only preferred embodiments of the present application, and the patent protection scope of the present application is not limited thereto. Any equivalent structure or equivalent process transformation made using the contents of the present application specification and drawings, or directly or indirectly used in other related technical fields, are also included in the patent protection scope of the present application.
Claims
1. A method for preparing NiCo2O4 nanoparticles, characterized in that: The following operations are included: Mixing a nickel source, a cobalt source and a cross-linking agent into a first solvent to obtain a mixed solution, and heating the mixed solution to obtain a sol; Adjusting the sol to alkalinity to obtain nickel-cobalt coprecipitation; The nickel-cobalt coprecipitate is calcined to obtain NiCo2O4 nanoparticles.
2. The method for preparing NiCo2O4 nanoparticles according to claim 1, characterized in that: The mixed solution satisfies at least one of the following characteristics: (a) the molar ratio of nickel atoms in the nickel source to cobalt atoms in the cobalt source is 1:(1-4); (b) the concentration of the cross-linking agent is 30 g / L-120 g / L; (c) the cross-linking agent comprises at least one of N,N'-methylenebisacrylamide and N-isopropylacrylamide; (d) The first solvent comprises water.
3. The method for preparing NiCo2O4 nanoparticles according to claim 1, characterized in that: Heating the mixed solution to obtain a sol comprises: The mixed solution is heated to 50° C. to 100° C. to obtain a sol.
4. The method for preparing NiCo2O4 nanoparticles according to claim 1, characterized in that: The step of adjusting the sol to be alkaline includes adjusting the pH of the sol to 10-11.
5. The method for preparing NiCo2O4 nanoparticles according to claim 1, characterized in that: The calcination comprises: The calcination is performed at a temperature of 200°C to 300°C in an air atmosphere.
6. A NiCo2O4 nanoparticle, characterized in that: Prepared according to the preparation method according to any one of claims 1 to 5.
7. A perovskite solar cell, characterized in that: It comprises a hole transport layer, wherein the hole transport layer comprises the NiCo2O4 nanoparticles according to claim 6.
8. The perovskite solar cell according to claim 7, characterized in that The hole transport layer is prepared by the following method: Dispersing the NiCo2O4 nanoparticles and imidazole salts according to claim 6 in a second solvent to obtain a dispersion; The dispersion is coated on a transparent conductive glass film or a perovskite photoactive layer to obtain the hole transport layer.
9. The perovskite solar cell according to claim 8, characterized in that The imidazolium salts include at least one of 1-ethyl-3-methylimidazolium bromide, 1-ethyl-3-methylimidazolium iodide and 1-ethyl-3-methylimidazolium chloride.
10. The perovskite solar cell according to claim 8, characterized in that: The second solvent includes at least one of water, isopropanol, ethanol, and chlorobenzene; The mass concentration of the NiCo2O4 nanoparticles in the dispersion is 5 mg / mL to 70 mg / mL; The coating includes at least one of slit coating, spin coating, blade coating, and spray coating.
11. The perovskite solar cell according to claim 8, characterized in that: It also includes a transparent conductive glass film, a perovskite photoactive layer, a passivation layer, an electron transport layer, a buffer layer and a counter electrode; Wherein, the transparent conductive glass film, the hole transport layer, the perovskite photoactive layer, the passivation layer, the electron transport layer, the buffer layer and the counter electrode are stacked in sequence.
12. The perovskite solar cell according to claim 11, characterized in that: Meet at least one of the following conditions: (A) the transparent conductive glass film comprises one of indium tin oxide conductive glass, fluorine-doped SnO2 conductive glass, indium tin oxide conductive plastic, and fluorine-doped SnO2 conductive plastic; (B) the sheet resistance of the transparent conductive glass film is 5Ω / sq to 25Ω / sq; (C) the hole transport layer has a thickness of 1 nm to 70 nm; (D) The chemical formula of the perovskite material in the perovskite photoactive layer is FA x Cs 1-x PbI3, where x is 0.85 to 1; (E) the thickness of the perovskite photoactive layer is 1 nm to 800 nm; (F) the passivation layer comprises at least one of 1,3-diaminopropane dihydroiodide, 2-phenylethylamine hydroiodide, phenylethylamine bromide, ethylenediamine dihydroiodide, and formamidine hydroiodide; (G) the thickness of the passivation layer is 5nm to 50nm; (H) the electron transport layer comprises at least one of carbon 60, a carbon 60 derivative, and carbon 70; (I) the thickness of the electron transport layer is 1 nm to 50 nm; (J) the buffer layer comprises at least one of polymethyl methacrylate, 2,9-dimethyl-4,7-diphenyl-1,10-phenanthroline, and sodium propargyl sulfonate; (K) the buffer layer has a thickness of 1 nm to 50 nm; (L) the counter electrode comprises at least one of Ag, Au, Cu, Al, indium tin oxide conductive glass, fluorine-doped SnO2 conductive glass, indium zinc oxide conductive film, silver nanowires, and carbon materials; (M) The thickness of the counter electrode is 1 nm to 500 nm.
13. A photovoltaic module, characterized in that: include: At least one cell string, the cell string comprising at least two perovskite solar cells according to any one of claims 7 to 12.
14. A photovoltaic system, characterized in that: The photovoltaic system comprises the photovoltaic assembly according to claim 13.