High-temperature antioxidant ceramic aerogel and preparation method thereof
By coating silicon carbide and zirconium carbide precursor coatings on the nanostructure of silicon nitride ceramic aerogel to form an antioxidant coating, the silicon nitride ceramic aerogel is easily oxidized and failed in high-temperature aerobic environment. The problem is that low-cost, efficient large-scale preparation and excellent antioxidant properties are achieved, and are suitable for the field of high-temperature thermal insulation.
Patent Information
- Application Number
- CN202411024549.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-29
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2044-07-29
AI Technical Summary
The existing silicon nitride ceramic aerogels are prone to oxidation failure in high-temperature aerobic environments, and are costly to produce at high cost, which limits their application in the field of high-temperature thermal insulation.
The combined structure of one-dimensional silicon nitride nanowires and two-dimensional silicon nitride nanoribbons is adopted, and the silicon carbide and zirconium carbide precursor coatings are coated in sequence inside and outside the surface, and the antioxidant coating is formed by in-situ ceramic to form. The eutectic liquid film of silica and zirconium dioxide is used to block oxygen and improve oxidation resistance.
It significantly improves the high-temperature oxidation resistance and elastic plasticity of silicon nitride aerogel, achieves stable use in an aerobic environment of 1500℃, reduces preparation costs, and is suitable for aerospace, high-temperature kilns and fire-fighting equipment and other fields.
Smart Images

Figure CN118955165A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of ceramic aerogels, and in particular relates to a high-temperature anti-oxidation ceramic aerogel and a preparation method thereof. Background Art
[0002] Ceramic aerogel is a new type of material with extremely low density, high porosity, low thermal conductivity and high temperature resistance. It is widely regarded as a potential innovative material in the field of thermal insulation in the future. At present, ceramic aerogels can be mainly divided into two categories according to their chemical composition: oxide ceramic aerogels and non-oxide ceramic aerogels. Oxide ceramic aerogels are prone to crystal embrittlement and structural collapse under high temperature conditions, so their use temperature is greatly limited and it is difficult to exceed 1000°C. In contrast, non-oxide ceramic aerogels have better high-temperature stability, among which silicon nitride aerogels are particularly prominent, showing excellent mechanical flexibility and high temperature resistance. However, the current silicon nitride aerogel preparation technology is costly, difficult to mass produce, and prone to oxidation failure in an aerobic environment above 1100°C, making it difficult to use stably for a long time. For example, the journal Materials Research Express (2019, 1250c4) reported the research results of Yang et al., pointing out that silicon nitride nanowires will quickly oxidize and fail in an aerobic environment above 1100°C, and will be completely converted into silicon dioxide when reaching 1500°C. Solving the problems of preparation cost and thermal stability in high-temperature aerobic environments will help achieve large-scale preparation of silicon nitride ceramic aerogels with higher temperature resistance, thereby promoting the application of this material in the field of high-temperature thermal insulation.
[0003] At present, there are few reports on patents and papers that simultaneously achieve low-cost large-scale preparation of silicon nitride aerogels and improved antioxidant properties. For example, the Chinese invention patent with publication number CN 114956858 A - a layered elastic-plastic silicon nitride ceramic aerogel and its preparation method, using siloxane as a raw material, first prepares a silicon nitride nanowire film on graphite paper, and then tears the film off the graphite paper, and then stacks it with silicon nitride ceramic hard sheets to form silicon nitride aerogel. This method is not suitable for large-scale preparation of aerogels. And the Chinese invention patent with publication number CN 113929470A - a silicon nitride nanobelt aerogel and its preparation method, short carbon fibers and polysiloxane are mixed and cured, and heated in nitrogen to prepare silicon nitride nanofiber aerogel. This method is a large-scale preparation of silicon nitride aerogel, but the prepared aerogel will fail due to oxidation in an aerobic environment at 1100°C. The Chinese invention patent with publication number CN 110028048 A - a method for preparing a high-temperature resistant and lightweight silicon nitride aerogel material, using the sol-gel method to obtain a precursor wet gel, and then obtaining a block silicon nitride aerogel through supercritical drying and high-temperature heat treatment. Although this method can achieve large-scale preparation of aerogels, the supercritical drying process consumes a lot of energy, the preparation cost is high, and the use temperature of the prepared aerogel in an aerobic environment does not exceed 1100°C. The Chinese invention patent with publication number CN 112047742 A - a low-cost preparation method for large-size silicon nitride nanobelt aerogel, using low-cost silicon powder and nitrogen as raw materials to directly synthesize silicon nitride, although it can achieve low-cost preparation, the oxidation resistance temperature of the prepared aerogel is only 1000°C. For example, the Chinese invention patent with publication number CN 111205106 A - a silicon nitride@carbon absorbing foam and its preparation method and application and the journal "ACS Nano" (2024, 4c03816) reported the method of coating pyrolytic carbon on the surface of silicon nitride aerogel by hydrothermal method and chemical vapor deposition method. Although the two methods have improved the heat resistance temperature of silicon nitride aerogel in an inert atmosphere to a certain extent, the pyrolytic carbon coating layer will be rapidly oxidized in an aerobic environment above 400°C. The Chinese invention patent with publication number CN 113999015A - a lightweight and high-strength elastic ceramic and its preparation method, the silicon nitride aerogel is subjected to high-temperature pre-oxidation treatment to form an oxide film on the surface of the silicon nitride nanowires. Although this method can improve the elasticity and plasticity of the aerogel, it cannot be used for a long time in an aerobic environment at 1100°C.
[0004] In summary, the current research on low-cost and large-scale preparation of silicon nitride ceramic aerogels that can serve stably in high-temperature aerobic environments is still in a technical gap. Summary of the invention
[0005] In order to overcome the shortcomings of the above-mentioned prior art, the purpose of the present invention is to provide a high-temperature anti-oxidation ceramic aerogel and a preparation method thereof, so as to solve the defects of traditional ceramic aerogels that are easily oxidized and fail at ultra-high temperatures and are difficult to prepare on a large scale at low cost, which makes it difficult for traditional ceramic aerogels to be used in thermal insulation fields such as aerospace, high-temperature kilns and fire-fighting equipment.
[0006] In order to achieve the above object, the present invention adopts the following technical solutions:
[0007] The present invention provides a high-temperature anti-oxidation ceramic aerogel, wherein the main body of the high-temperature anti-oxidation ceramic aerogel is silicon nitride aerogel, and the nanostructure of the silicon nitride aerogel is one of a one-dimensional silicon nitride nanowire and a two-dimensional silicon nitride nanobelt, or a combination of the two nanostructures;
[0008] The nanostructure of the silicon nitride aerogel is sequentially coated with a silicon carbide precursor coating and a zirconium carbide precursor coating from the inside to the outside.
[0009] In one embodiment, the element composition of the high temperature oxidation resistant ceramic aerogel is nitrogen, silicon, carbon, and zirconium.
[0010] In one embodiment, in an oxygen environment, the silicon carbide precursor coating and the zirconium carbide precursor coating undergo in-situ ceramicization and oxidation as the temperature rises; the silicon carbide precursor coating and the zirconium carbide precursor coating are transformed into silicon dioxide coating and zirconium dioxide coating.
[0011] In one embodiment, after the melting temperature of silicon dioxide is reached, the silicon dioxide coating forms a flowing silicon dioxide molten liquid, and the zirconium dioxide nanoparticles in the zirconium dioxide coating dissolve in the silicon dioxide molten liquid to form a binary eutectic liquid film.
[0012] The present invention also provides a method for preparing high-temperature oxidation-resistant ceramic aerogel, comprising the following steps:
[0013] S1: adding a metal catalyst to a polysiloxane sol, stirring evenly to obtain a mixed sol, impregnating a polymer foam skeleton into the mixed sol, drying to form a mixed xerogel foam, and then performing a high temperature heat treatment to obtain a silicon nitride aerogel;
[0014] S2: preparing polycarbosilane sol, immersing silicon nitride aerogel in the polycarbosilane sol, taking it out and performing the first curing treatment to obtain silicon carbide precursor / silicon nitride composite ceramic aerogel;
[0015] S3: preparing polyzirconium carbide sol, impregnating silicon carbide precursor / silicon nitride composite ceramic aerogel into the polyzirconium carbide sol, taking it out and performing a second curing treatment to obtain zirconium carbide precursor / silicon carbide precursor / silicon nitride composite ceramic aerogel.
[0016] In one embodiment, in S1, the mass ratio of the polysiloxane sol, the metal catalyst, and the polymer foam skeleton is (1-30): (1-5): (1-30).
[0017] In one embodiment, in S1, the metal catalyst is a composite of one or more of a platinum catalyst, a palladium catalyst, a copper catalyst, and a nickel catalyst; the polymer foam skeleton is a composite of one or more of a polyurethane foam, a polystyrene foam, a polypropylene foam, a polyethylene foam, a polystyrene copolymer foam, a polymethyl methacrylate foam, a polyphenylene sulfide foam, and a melamine foam.
[0018] In one embodiment, in S2, the polycarbosilane sol is prepared by uniformly mixing a carbon source, a silicon source, an organic solvent and water;
[0019] The mass ratio of the carbon source, the silicon source, the organic solvent and the water is (1-50): (1-50): (1-200): (1-200).
[0020] In one embodiment, in S3, the polyzirconium carbene sol is prepared by uniformly mixing a carbon source, a zirconium source, an organic solvent and water;
[0021] The mass ratio of the carbon source, the zirconium source, the organic solvent and water is (1-50): (1-50): (1-200): (1-200).
[0022] In one embodiment, in S1, the drying temperature is 30-150° C.; the high temperature heat treatment temperature is 1350-1650° C., and the high temperature heat treatment is performed in a nitrogen-containing atmosphere;
[0023] In S2 and S3, the temperature of the first curing treatment and the second curing treatment is 150-300° C., and the first curing treatment and the second curing treatment are performed under an inert atmosphere.
[0024] Compared with the prior art, the present invention has the following beneficial effects:
[0025] The present invention provides a high-temperature oxidation-resistant ceramic aerogel. The structural components of silicon nitride aerogel are one-dimensional silicon nitride nanowires and two-dimensional silicon nitride nanobelts. Compared with granular and nanosheet structural components, these large aspect ratio nanowires and nanobelts have higher mechanical deformation capacity, giving silicon nitride aerogel excellent compression rebound and anti-bending capabilities. A dual-component antioxidant coating of silicon carbide precursor and zirconium carbide precursor is coated on the nanostructure surface of silicon nitride aerogel. The antioxidant coating formed by nanoparticles undergoes in-situ ceramicization during the heating process. This process absorbs a large amount of heat energy, plays a role in active thermal protection, and effectively reduces the direct damage of high temperature to the aerogel structure.
[0026] Furthermore, in a high-temperature aerobic environment, due to the presence of oxygen, the formed silicon carbide and zirconium carbide ceramics will be oxidized and transformed into silicon dioxide and zirconium dioxide, and the nano zirconium dioxide particles will dissolve in the molten silicon dioxide to form a dense binary eutectic liquid film, which can effectively block the contact between oxygen and silicon nitride, prevent it from being oxidized and causing the performance to decline, and significantly improve the high-temperature oxidation resistance of the aerogel. At the same time, the nano zirconium oxide particles can increase the viscosity of the molten silicon dioxide liquid, play a stronger nail column effect, thereby improving its ability to resist high-temperature airflow or high-temperature flame impact. In addition, the molten liquid film can weld silicon nitride nano-components, limit the positional displacement after compression, thereby effectively improving the elasticity and plasticity of the aerogel. Therefore, the antioxidant composite ceramic aerogel prepared by the present invention has higher temperature resistance, oxidation resistance, and elasticity and plasticity, and can be widely used in aerospace, high-temperature kilns, fire-fighting equipment and other thermal insulation fields.
[0027] The present invention provides a method for preparing high-temperature antioxidant ceramic aerogels, which uses an easily available polymer foam skeleton as a carbon source and template for synthesizing silicon nitride aerogels, and forms silicon nitride aerogels in one step by a carbon thermal reduction reaction, thereby realizing efficient preparation of aerogels. In addition, due to the high porosity of the prepared aerogels themselves, the aerogels have a good adsorption effect on the precursor sol of the coating, which is conducive to efficiently coating the nanostructured surface of the silicon nitride aerogel with a dual antioxidant coating of a silicon carbide precursor and a zirconium carbide precursor, so the above-mentioned preparation method has the advantages of low cost and being conducive to large-scale production. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] Figure 1 This is an optical photograph of the high-temperature oxidation-resistant ceramic aerogel prepared in Example 1 of the present invention;
[0029] Figure 2 This is an EDS spectrum analysis diagram of the high temperature oxidation resistant ceramic aerogel prepared in Example 1 of the present invention;
[0030] Figure 3 The infrared thermal imaging photographs of the high-temperature oxidation-resistant ceramic aerogel prepared in Example 1 of the present invention under the scouring of a butane spray gun (about 1300° C.); wherein, Figures a, b, c, and d represent the infrared thermal imaging images at 5, 10, 15, and 30 minutes, respectively;
[0031] Figure 4 This is a SEM comparison of the high-temperature oxidation-resistant ceramic aerogel prepared in Example 1 of the present invention before and after oxidation treatment at 1500°C for 1 hour; wherein Figure a is a schematic diagram before heat treatment, and Figure b is a schematic diagram after heat treatment. DETAILED DESCRIPTION
[0032] In order to enable those skilled in the art to understand the characteristics and effects of the present invention, the following is a general description and definition of the terms and expressions mentioned in the specification and claims. Unless otherwise specified, all technical and scientific terms used in the text are the common meanings understood by those skilled in the art for the present invention. In the event of a conflict, the definition in this specification shall prevail.
[0033] The theories or mechanisms described and disclosed herein, whether correct or incorrect, should not limit the scope of the present invention in any way, that is, the present invention can be implemented without being limited by any specific theory or mechanism.
[0034] Herein, all features such as values, quantities, contents and concentrations defined in the form of numerical ranges or percentage ranges are for simplicity and convenience only. Accordingly, the description of numerical ranges or percentage ranges should be considered to have included and specifically disclosed all possible secondary ranges and individual values within the range (including integers and fractions).
[0035] In this document, unless otherwise specified, “includes,” “including,” “contains,” “has,” or similar terms cover the meanings of “consisting of” and “mainly consisting of,” for example, “A includes a” covers the meanings of “A includes a and other” and “A only includes a.”
[0036] In this document, in order to make the description concise, not all possible combinations of various technical features in various embodiments or examples are described. Therefore, as long as there is no contradiction in the combination of these technical features, the various technical features in various embodiments or examples can be combined arbitrarily, and all possible combinations should be considered to be within the scope of this specification.
[0037] The invention provides a high-temperature oxidation-resistant ceramic aerogel and a preparation method thereof.
[0038] On one hand, the present invention provides a high-temperature antioxidant ceramic aerogel, wherein the main body of the high-temperature antioxidant ceramic aerogel is silicon nitride aerogel, and the nanostructure of the silicon nitride aerogel is one of a one-dimensional silicon nitride nanowire and a two-dimensional silicon nitride nanobelt, or a combination of two nanostructures; the nanostructure of the silicon nitride aerogel is sequentially coated with a silicon carbide precursor coating and a zirconium carbide precursor coating from the inside to the outside.
[0039] More importantly, in an oxygen environment, the silicon carbide precursor coating and the zirconium carbide precursor coating undergo in-situ ceramicization and oxidation as the temperature rises; the silicon carbide precursor coating and the zirconium carbide precursor coating form silicon carbide and zirconium carbide ceramics that are further oxidized and transformed into silicon dioxide coatings and zirconium dioxide coatings.
[0040] On the basis of the above, after the melting temperature of silicon dioxide is reached, the silicon dioxide coating forms a flowing silicon dioxide molten liquid, and the zirconium dioxide nanoparticles in the zirconium dioxide coating dissolve in the silicon dioxide molten liquid to form a binary eutectic liquid film.
[0041] like Figure 1 As shown, the high temperature oxidation resistant ceramic aerogel provided in one embodiment is a light yellow three-dimensional block with a density of 20 to 80 mg / cm 3 The main component of the high temperature oxidation resistant ceramic aerogel is silicon nitride, and the structural elements of the silicon nitride aerogel are one-dimensional silicon nitride nanowires and two-dimensional silicon nitride nanobelts.
[0042] In the high-temperature oxidation-resistant ceramic aerogel, a dual-component oxidation-resistant coating of a silicon carbide precursor and a zirconium carbide precursor is uniformly coated on the surface of the silicon nitride nanostructure; the main elements of the high-temperature oxidation-resistant ceramic aerogel are nitrogen, silicon, carbon and zirconium.
[0043] The high temperature oxidation resistant ceramic aerogel has an extremely low thermal conductivity of 0.032-0.058 W / mk; the high temperature oxidation resistant ceramic aerogel has excellent oxidation resistance, and its microscopic morphology does not change significantly after being treated in an aerobic environment at 1500° C. for 1 hour.
[0044] On the other hand, the present invention provides a method for preparing a high-temperature antioxidant ceramic aerogel, which comprises the following steps: preparing a polysiloxane sol and adding a metal catalyst, stirring evenly to obtain a mixed sol, immersing a polymer foam skeleton in the sol, drying to form a mixed dry gel foam, and then subjecting the mixed dry gel foam to high-temperature heat treatment in a nitrogen-containing atmosphere to obtain a silicon nitride aerogel; immersing the prepared silicon nitride aerogel in a polycarbosilane sol, taking it out after adsorption saturation, and subjecting it to curing treatment to obtain a silicon carbide precursor / silicon nitride composite ceramic aerogel, wherein the curing treatment process is carried out in an oven and can also be understood as heating to achieve curing; immersing the silicon carbide precursor / silicon carbide composite ceramic aerogel in a polyzirconium carbane sol, taking it out after adsorption saturation, and subjecting it to curing treatment to obtain a zirconium carbide precursor / silicon carbide precursor / silicon nitride composite ceramic aerogel, i.e., a high-temperature antioxidant ceramic aerogel. The curing treatment process is also carried out in an oven and can also be understood as heating to achieve curing.
[0045] The specific steps of the above preparation method are as follows:
[0046] Step 1) prepare polysiloxane sol and add metal catalyst, stir evenly to obtain mixed sol, immerse the polymer foam skeleton in the sol for 30 to 120 minutes, dry at 30 to 150° C. to form mixed dry gel foam, and then heat treat at high temperature in a nitrogen atmosphere to obtain silicon nitride aerogel.
[0047] Step 2) prepare polycarbosilane sol, immerse the silicon nitride aerogel prepared in S1 in the sol, take it out after adsorption saturation, and cure it at 150-300° C. in an inert atmosphere to obtain a silicon carbide precursor / silicon nitride composite ceramic aerogel.
[0048] Step 3) prepare polyzirconium carbide sol, immerse the silicon carbide precursor / silicon nitride composite ceramic aerogel prepared in S2 in the sol, take it out after adsorption saturation, and cure it at 150-300°C in an inert atmosphere to obtain a zirconium carbide precursor / silicon carbide precursor / silicon nitride composite ceramic aerogel, i.e., a high-temperature antioxidant ceramic aerogel.
[0049] The specific dosage and process conditions are as follows:
[0050] In step 1), the process of preparing the polysiloxane sol is as follows: silicone resin, ethanol and water are uniformly mixed in a mass ratio of 3:10:8 to obtain the polysiloxane sol.
[0051] In step 1), the mass ratio of the polysiloxane sol, the metal catalyst and the polymer foam skeleton is (1-30): (1-5): (1-30); the metal catalyst can be: a platinum catalyst, a palladium catalyst, a copper catalyst, a nickel catalyst or a composite of one or more thereof; the polymer foam skeleton can be: a polyurethane foam, a polystyrene foam, a polypropylene foam, a polyethylene foam, a polystyrene copolymer foam, a polymethyl methacrylate foam, a polyphenylene sulfide foam and a melamine foam or a composite of one or more thereof; the nitrogen-containing atmosphere can be: a composite of one or two of nitrogen and ammonia; the temperature of the high-temperature heat treatment is 1350-1650°C.
[0052] In step 2), the polycarbosilane is prepared by mixing a carbon source, a silicon source, an organic solvent and water in a mass ratio of (1-50): (1-50): (1-200): (1-200), stirring the mixture evenly to obtain a polycarbosilane sol.
[0053] In step 3), the polyzirconium carbene is prepared by mixing a carbon source, a zirconium source, an organic solvent and water in a mass ratio of (1-50): (1-50): (1-200): (1-200), stirring the mixture evenly to obtain a polyzirconium carbene sol.
[0054] The above-mentioned organic solvents include but are not limited to ethanol, ethylene glycol, acetone, xylene, tert-butanol and other solvents.
[0055] The present invention will be further described below in conjunction with specific embodiments. It should be understood that these embodiments are only used to illustrate the present invention and are not intended to limit the scope of the present invention. In addition, it should be understood that after reading the content taught by the present invention, those skilled in the art can make various changes or modifications to the present invention, and these equivalent forms fall within the scope limited by the appended claims of the application equally.
[0056] The following examples use conventional instruments and equipment in the art. The experimental methods in the following examples where specific conditions are not specified are usually carried out under conventional conditions or under conditions recommended by the manufacturer. The various raw materials used in the following examples are conventional commercial products unless otherwise specified, and their specifications are conventional specifications in the art. In the specification of the present invention and the following examples, unless otherwise specified, "%" means weight percentage, "part" means weight part, and ratio means weight ratio.
[0057] Embodiment 1:
[0058] Step 1) prepare polysiloxane sol and add platinum catalyst, stir evenly to obtain mixed sol, immerse melamine foam skeleton in the sol for 60 minutes, dry at 100° C. to form mixed dry gel foam, and then heat treat at 1500° C. in a nitrogen atmosphere to obtain silicon nitride aerogel.
[0059] Step 2) Weigh 1 g of furfuryl alcohol, 5 g of ethyl orthosilicate, 10 g of acetone, and 20 g of water, mix them, and stir them evenly to obtain a polycarbosilane sol. The silicon nitride aerogel prepared in step 1 is immersed in the sol, taken out after adsorption saturation, and cured at 200° C. in an inert atmosphere to obtain a silicon carbide precursor / silicon nitride composite ceramic aerogel.
[0060] Step 3) Weigh 1 g of furfuryl alcohol, 5 g of zirconyl nitrate, 10 g of ethanol, and 20 g of water, mix them, and stir them evenly to obtain a polyzirconium carbene sol. The silicon carbide precursor / silicon nitride composite ceramic aerogel prepared in step 2 is immersed in the sol, taken out after adsorption saturation, and cured at 180° C. in an inert atmosphere to obtain a zirconium carbide precursor / silicon carbide precursor / silicon nitride composite ceramic aerogel, i.e., a high-temperature antioxidant ceramic aerogel.
[0061] The density of the prepared high-temperature oxidation-resistant ceramic aerogel is 40 mg / cm3, and the thermal conductivity at room temperature is 0.042 W / mk. Figure 1 It can be seen that the high temperature oxidation resistant ceramic aerogel is light yellow three-dimensional block. Figure 2 It can be seen that the main elements of the antioxidant composite ceramic aerogel are nitrogen, silicon, carbon and zirconium. Figure 3 It can be seen that the high-temperature oxidation-resistant ceramic aerogel still maintains excellent thermal insulation performance under the 1300°C butane flame erosion. After 30 minutes of erosion, the back temperature of the aerogel is stabilized at 95°C. Figure 4It can be seen that the microstructure of the antioxidant composite ceramic aerogel does not change substantially after being treated in an aerobic environment at 1500°C for 1 h, which proves that the aerogel has excellent high-temperature antioxidant properties.
[0062] Embodiment 2:
[0063] Step 1) prepare polysiloxane sol and add copper catalyst, stir evenly to obtain mixed sol, immerse polymethyl methacrylate foam skeleton in the sol for 80 minutes, dry at 60° C. to form mixed dry gel foam, and then heat treat at 1450° C. in a nitrogen atmosphere to obtain silicon nitride aerogel.
[0064] Step 2) Weigh 2 g of furfuryl alcohol, 5 g of ethyl orthosilicate, 20 g of acetone, and 40 g of water, mix them, and stir them evenly to obtain a polycarbosilane sol. The silicon nitride aerogel prepared in step 1 is immersed in the sol, taken out after adsorption saturation, and cured at 260° C. in an inert atmosphere to obtain a silicon carbide precursor / silicon nitride composite ceramic aerogel.
[0065] Step 3) Weigh 2 g of furfuryl alcohol, 5 g of zirconyl nitrate, 20 g of ethanol, and 40 g of water, mix them, and stir them evenly to obtain a polyzirconium carbene sol. The silicon carbide precursor / silicon nitride composite ceramic aerogel prepared in step 2 is immersed in the sol, taken out after adsorption saturation, and cured at 180° C. in an inert atmosphere to obtain a zirconium carbide precursor / silicon carbide precursor / silicon nitride composite ceramic aerogel, i.e., a high-temperature antioxidant ceramic aerogel.
[0066] Embodiment 3:
[0067] Step 1) Prepare a polysiloxane sol and add a platinum catalyst, stir evenly to obtain a mixed sol, immerse the polyurethane foam skeleton in the sol for 120 minutes, dry at 60°C to form a mixed dry gel foam, and then heat treat at 1400°C in a nitrogen atmosphere to obtain a silicon nitride aerogel.
[0068] Step 2) Weigh 2 g of furfuryl alcohol, 10 g of ethyl orthosilicate, 30 g of acetone, and 20 g of water, mix them, and stir them evenly to obtain a polycarbosilane sol. The silicon nitride aerogel prepared in step 1 is immersed in the sol, taken out after adsorption saturation, and cured at 300° C. in an inert atmosphere to obtain a silicon carbide precursor / silicon nitride composite ceramic aerogel.
[0069] Step 3) Weigh 1 g of furfuryl alcohol, 10 g of zirconyl nitrate, 20 g of ethanol, and 30 g of water, mix them, and stir them evenly to obtain a polyzirconium carbene sol. The silicon carbide precursor / silicon nitride composite ceramic aerogel prepared in step 2 is immersed in the sol, taken out after adsorption saturation, and cured at 150° C. in an inert atmosphere to obtain a zirconium carbide precursor / silicon carbide precursor / silicon nitride composite ceramic aerogel, i.e., a high-temperature antioxidant ceramic aerogel.
[0070] Embodiment 4:
[0071] Step 1) Prepare polysiloxane sol and add nickel catalyst, stir evenly to obtain mixed sol, immerse polyethylene foam skeleton in the sol for 80 minutes, dry at 150° C. to form mixed dry gel foam, and then heat treat at 1600° C. in a nitrogen atmosphere to obtain silicon nitride aerogel.
[0072] Step 2) Weigh 4 g of furfuryl alcohol, 8 g of ethyl orthosilicate, 30 g of acetone, and 40 g of water, mix them, and stir them evenly to obtain a polycarbosilane sol. The silicon nitride aerogel prepared in step 1 is immersed in the sol, taken out after adsorption saturation, and cured at 180° C. in an inert atmosphere to obtain a silicon carbide precursor / silicon nitride composite ceramic aerogel.
[0073] Step 3) Weigh 4 g of furfuryl alcohol, 7 g of zirconyl nitrate, 20 g of ethanol, and 30 g of water, mix them, and stir them evenly to obtain a polyzirconium carbene sol. The silicon carbide precursor / silicon nitride composite ceramic aerogel prepared in step 2 is immersed in the sol, taken out after adsorption saturation, and cured at 200° C. in an inert atmosphere to obtain a zirconium carbide precursor / silicon carbide precursor / silicon nitride composite ceramic aerogel, i.e., a high-temperature antioxidant ceramic aerogel.
[0074] Embodiment 5:
[0075] Step 1) prepare polysiloxane sol and add palladium catalyst, stir evenly to obtain mixed sol, immerse polypropylene foam skeleton in the sol for 80 minutes, dry at 30°C to form mixed dry gel foam, and then heat treat at 1650°C in a nitrogen atmosphere to obtain silicon nitride aerogel.
[0076] Step 2) Weigh 1 g of furfuryl alcohol, 1 g of ethyl orthosilicate, 1 g of acetone, and 1 g of water, mix them, and stir them evenly to obtain a polycarbosilane sol. The silicon nitride aerogel prepared in step 1 is immersed in the sol, taken out after adsorption saturation, and cured at 300° C. in an inert atmosphere to obtain a silicon carbide precursor / silicon nitride composite ceramic aerogel.
[0077] Step 3) Weigh 1 g of furfuryl alcohol, 1 g of zirconyl nitrate, 1 g of ethanol, and 1 g of water, mix them, and stir them evenly to obtain a polyzirconium carbene sol. The silicon carbide precursor / silicon nitride composite ceramic aerogel prepared in step 2 is immersed in the sol, taken out after adsorption saturation, and cured at 150° C. in an inert atmosphere to obtain a zirconium carbide precursor / silicon carbide precursor / silicon nitride composite ceramic aerogel, i.e., a high-temperature antioxidant ceramic aerogel.
[0078] Embodiment 6:
[0079] Step 1) prepare polysiloxane sol and add palladium catalyst, stir evenly to obtain mixed sol, immerse the polystyrene copolymer foam skeleton in the sol for 80 minutes, dry at 150° C. to form a mixed dry gel foam, and then heat treat at 1350° C. in a nitrogen atmosphere to obtain silicon nitride aerogel.
[0080] Step 2) Weigh 50 g of furfuryl alcohol, 50 g of ethyl orthosilicate, 200 g of acetone, and 200 g of water, mix them, and stir them evenly to obtain a polycarbosilane sol. The silicon nitride aerogel prepared in step 1 is immersed in the sol, taken out after adsorption saturation, and cured at 150° C. in an inert atmosphere to obtain a silicon carbide precursor / silicon nitride composite ceramic aerogel.
[0081] Step 3) Weigh 2 g of furfuryl alcohol, 5 g of zirconyl nitrate, 20 g of ethanol, and 40 g of water, mix them, and stir them evenly to obtain a polyzirconium carbene sol. The silicon carbide precursor / silicon nitride composite ceramic aerogel prepared in step 2 is immersed in the sol, taken out after adsorption saturation, and cured at 300 ° C in an inert atmosphere to obtain a zirconium carbide precursor / silicon carbide precursor / silicon nitride composite ceramic aerogel, that is, a high-temperature antioxidant ceramic aerogel.
[0082] Embodiment 7:
[0083] Step 1) prepare polysiloxane sol and add palladium catalyst, stir evenly to obtain mixed sol, immerse polystyrene foam skeleton in the sol for 80 minutes, dry at 150° C. to form mixed dry gel foam, and then heat treat at 1350° C. in a nitrogen atmosphere to obtain silicon nitride aerogel.
[0084] Step 2) Weigh 2 g of furfuryl alcohol, 5 g of ethyl orthosilicate, 20 g of acetone, and 40 g of water, mix them, and stir them evenly to obtain a polycarbosilane sol. The silicon nitride aerogel prepared in step 1 is immersed in the sol, taken out after adsorption saturation, and cured at 150° C. in an inert atmosphere to obtain a silicon carbide precursor / silicon nitride composite ceramic aerogel.
[0085] Step 3) Weigh 50 g of furfuryl alcohol, 50 g of zirconyl nitrate, 200 g of ethanol, and 400 g of water, mix them, and stir them evenly to obtain a polyzirconium carbene sol. The silicon carbide precursor / silicon nitride composite ceramic aerogel prepared in step 2 is immersed in the sol, taken out after adsorption saturation, and cured at 300 ° C in an inert atmosphere to obtain a zirconium carbide precursor / silicon carbide precursor / silicon nitride composite ceramic aerogel, that is, a high-temperature antioxidant ceramic aerogel.
[0086] Embodiment 8:
[0087] Step 1) prepare polysiloxane sol and add palladium catalyst, stir evenly to obtain mixed sol, immerse polyphenylene sulfide foam skeleton in the sol for 80 minutes, dry at 150° C. to form mixed dry gel foam, and then heat treat at 1350° C. in a nitrogen atmosphere to obtain silicon nitride aerogel.
[0088] Step 2) Weigh 2 g of furfuryl alcohol, 5 g of ethyl orthosilicate, 20 g of acetone, and 40 g of water, mix them, and stir them evenly to obtain a polycarbosilane sol. The silicon nitride aerogel prepared in step 1 is immersed in the sol, taken out after adsorption saturation, and cured at 150° C. in an inert atmosphere to obtain a silicon carbide precursor / silicon nitride composite ceramic aerogel.
[0089] Step 3) Weigh 2 g of furfuryl alcohol, 5 g of zirconyl nitrate, 20 g of ethanol, and 40 g of water, mix them, and stir them evenly to obtain a polyzirconium carbene sol. The silicon carbide precursor / silicon nitride composite ceramic aerogel prepared in step 2 is immersed in the sol, taken out after adsorption saturation, and cured at 300 ° C in an inert atmosphere to obtain a zirconium carbide precursor / silicon carbide precursor / silicon nitride composite ceramic aerogel, that is, a high-temperature antioxidant ceramic aerogel.
[0090] In summary, the high-temperature antioxidant ceramic aerogel prepared by the present invention has excellent flexibility, thermal insulation and antioxidant properties, and can be prepared at low cost and on a large scale. It has great application potential in thermal insulation fields such as aerospace, high-temperature kilns and fire protection engineering.
[0091] The above contents are only for explaining the technical idea of the present invention and cannot be used to limit the protection scope of the present invention. Any changes made on the basis of the technical solution in accordance with the technical idea proposed by the present invention shall fall within the protection scope of the claims of the present invention.
Claims
1. A high temperature oxidation resistant ceramic aerogel, characterized in that: The main body of the high-temperature oxidation-resistant ceramic aerogel is silicon nitride aerogel, and the nanostructure of the silicon nitride aerogel is one of one-dimensional silicon nitride nanowires and two-dimensional silicon nitride nanobelts, or a combination of the two nanostructures; The nanostructure of the silicon nitride aerogel is sequentially coated with a silicon carbide precursor coating and a zirconium carbide precursor coating from the inside to the outside.
2. The high temperature oxidation resistant ceramic aerogel according to claim 1, characterized in that: The elements of the high temperature oxidation resistant ceramic aerogel are nitrogen, silicon, carbon and zirconium.
3. The high temperature oxidation resistant ceramic aerogel according to claim 1, characterized in that: In an oxygen environment, the silicon carbide precursor coating and the zirconium carbide precursor coating undergo in-situ ceramicization and oxidation as the temperature rises; the silicon carbide precursor coating and the zirconium carbide precursor coating are transformed into silicon dioxide coating and zirconium dioxide coating.
4. The high temperature oxidation resistant ceramic aerogel according to claim 3, characterized in that: After reaching the melting temperature of silicon dioxide, the silicon dioxide coating forms a flowing silicon dioxide molten liquid, and the zirconium dioxide nanoparticles in the zirconium dioxide coating dissolve in the silicon dioxide molten liquid to form a binary eutectic liquid film.
5. A method for preparing high temperature oxidation resistant ceramic aerogel according to any one of claims 1 to 4, characterized in that: The following steps are involved: S1: adding a metal catalyst to a polysiloxane sol, stirring evenly to obtain a mixed sol, impregnating a polymer foam skeleton into the mixed sol, drying to form a mixed xerogel foam, and then performing a high temperature heat treatment to obtain a silicon nitride aerogel; S2: preparing polycarbosilane sol, immersing silicon nitride aerogel in the polycarbosilane sol, taking it out and performing the first curing treatment to obtain silicon carbide precursor / silicon nitride composite ceramic aerogel; S3: preparing polyzirconium carbide sol, impregnating silicon carbide precursor / silicon nitride composite ceramic aerogel into the polyzirconium carbide sol, taking it out and performing a second curing treatment to obtain zirconium carbide precursor / silicon carbide precursor / silicon nitride composite ceramic aerogel.
6. The method for preparing high temperature oxidation resistant ceramic aerogel according to claim 5, characterized in that: In S1, the mass ratio of the polysiloxane sol, the metal catalyst and the polymer foam skeleton is (1-30): (1-5): (1-30).
7. The method for preparing high temperature oxidation resistant ceramic aerogel according to claim 5, characterized in that: In S1, the metal catalyst is a composite of one or more of a platinum catalyst, a palladium catalyst, a copper catalyst, and a nickel catalyst; the polymer foam skeleton is a composite of one or more of a polyurethane foam, a polystyrene foam, a polypropylene foam, a polyethylene foam, a polystyrene copolymer foam, a polymethyl methacrylate foam, a polyphenylene sulfide foam, and a melamine foam.
8. The method for preparing high temperature oxidation resistant ceramic aerogel according to claim 5, characterized in that: In S2, the polycarbosilane sol is prepared by uniformly mixing a carbon source, a silicon source, an organic solvent and water; The mass ratio of the carbon source, the silicon source, the organic solvent and the water is (1-50): (1-50): (1-200): (1-200).
9. The method for preparing high temperature oxidation resistant ceramic aerogel according to claim 5, characterized in that: In S3, the polyzirconium carbene sol is prepared by uniformly mixing a carbon source, a zirconium source, an organic solvent and water; The mass ratio of the carbon source, the zirconium source, the organic solvent and water is (1-50): (1-50): (1-200): (1-200).
10. The method for preparing high temperature oxidation resistant ceramic aerogel according to claim 5, characterized in that: In S1, the drying temperature is 30-150° C.; the high temperature heat treatment temperature is 1350-1650° C., and the high temperature heat treatment is performed in a nitrogen atmosphere; In S2 and S3, the temperature of the first curing treatment and the second curing treatment is 150-300° C., and the first curing treatment and the second curing treatment are performed under an inert atmosphere.
Citation Information
Patent Citations
Silicon nitride nanoribbon aerogel and preparation method thereof
CN109704781A
Lightweight high-strength elastic ceramic and preparation method thereof
CN113999015A
Impedance gradient layered gradient composite aerogel as well as preparation method and application thereof
CN116217253A
Aerogel composite material capable of being ceramized in situ and having excellent thermal protection performance as well as preparation method and application of aerogel composite material