Antioxidant composite ceramic aerogel and preparation method thereof

By coating mullite and copper-nickel metal coatings on the nanostructure of silicon nitride aerogel, the anti-oxidation composite ceramic aerogel is solved, and the problem of stable service and insufficient anti-oxidation performance in high-temperature aerobic environment is achieved. Low-cost, large-scale preparation and efficient high-temperature anti-oxidation properties.

CN118955166AActive Publication Date: 2024-11-15SHAANXI UNIV OF SCI & TECH
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202411024550.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-29
Publication Date
2024-11-15
Estimated Expiration
2044-07-29

AI Technical Summary

Technical Problem

The prior art is difficult to prepare silicon nitride ceramic aerogels that are stable in service in high-temperature aerobic environments at low cost and batch-based, and their oxidation resistance is insufficient and cannot meet the needs of high-temperature applications.

Method used

The combined nanostructure of one-dimensional silicon nitride nanowires and two-dimensional silicon nitride nanoribbons is adopted, and the surface is successively coated with mullite and copper-nickel metal coatings to form an antioxidant composite ceramic aerogel, which is improved by this method. Its antioxidant properties and temperature resistance.

Benefits of technology

It significantly improves the antioxidant properties and temperature resistance of silicon nitride aerogel, enables it to serve stably in high-temperature aerobic environment, extends its service life, and achieves low-cost and large-scale preparation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118955166A_ABST
    Figure CN118955166A_ABST
Patent Text Reader

Abstract

The invention discloses antioxidant composite ceramic aerogel and a preparation method thereof, and belongs to the technical field of composite ceramic aerogel. The main body of the antioxidant composite ceramic aerogel is silicon nitride aerogel, and the nanostructure of the silicon nitride aerogel is one or a combination of two of a one-dimensional silicon nitride nanowire and a two-dimensional silicon nitride nanobelt. The nano structure of the silicon nitride aerogel is sequentially coated with a mullite coating and a copper-nickel metal coating from inside to outside. The technical problem that the silicon nitride ceramic aerogel stably serving in the high-temperature aerobic environment cannot be prepared in batches at low cost in the prior art can be solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of composite ceramic aerogels, and in particular relates to an anti-oxidation composite ceramic aerogel and a preparation method thereof. Background Art

[0002] Ceramic aerogel has ultra-low density, ultra-high porosity, ultra-low thermal conductivity and high temperature resistance, and is a new generation of thermal insulation materials with great potential. At present, ceramic aerogels are mainly divided into two categories: oxide ceramic aerogels and non-oxide ceramic aerogels (such as nitrides, carbides, borides, etc.). Due to the high-temperature crystallization embrittlement and high-temperature structural collapse of oxide aerogels, its service temperature is difficult to exceed 1000°C. In contrast, among non-oxidative ceramic aerogels, silicon nitride aerogels exhibit excellent mechanical flexibility and high-temperature resistance, but silicon nitride aerogels have two major problems: one is that the existing preparation technology has high preparation costs and is not suitable for large-scale production; the other is that there is an oxidation failure problem in an aerobic environment above 1100°C, and it cannot be stably served for a long time. For example, the magazine "Materials Research Express" (2019, 1250c4) reported that Yang et al. found that silicon nitride nanowires will quickly oxidize and fail in an aerobic environment above 1100°C, and will be completely converted into silicon dioxide at 1500°C. Only by solving these two problems can we achieve large-scale preparation of ceramic aerogels with higher temperature resistance.

[0003] At present, there are few reports on patents and papers that simultaneously achieve low-cost large-scale preparation of silicon nitride aerogels and improved antioxidant properties. For example, the Chinese invention patent with publication number CN 108328586 A - a compressible and recoverable silicon nitride aerogel and its preparation, uses siloxane as a raw material, first prepares a silicon nitride nanowire film on graphite paper, and then tears the film off the graphite paper, and then stacks it layer by layer to form a silicon nitride aerogel. This method is not suitable for large-scale preparation of aerogels. And the Chinese invention patent with publication number CN 113929470 A - a silicon nitride nanobelt aerogel and its preparation method, short carbon fibers and polysiloxane are mixed and cured, and heated in nitrogen to prepare silicon nitride nanofiber aerogel. This method is a large-scale preparation method of silicon nitride aerogel, but the prepared aerogel will fail due to oxidation in an aerobic environment at 1100°C. The Chinese invention patent with publication number CN 113929470 A - a method for preparing anisotropic porous silicon nitride ceramics and aerogels with nanoarray directional arrangement, obtains silicon nitride aerogels by chemical treatment, freeze drying and carbon thermal reduction of natural wood. Although this method uses low-cost natural wood as raw material, the freeze drying process consumes a lot of energy, the preparation cost is high, and the use temperature of the prepared aerogel in an aerobic environment does not exceed 1100°C. The Chinese invention patent with publication number CN 112047742 A - a low-cost preparation method for large-size silicon nitride nanobelt aerogels, uses low-cost silicon powder and nitrogen as raw materials to directly synthesize silicon nitride. Although low-cost preparation can be achieved, the oxidation resistance temperature of the prepared aerogel is only 1000°C. The Chinese invention patent with publication number CN 111205106 A - A silicon nitride @ carbon absorbing foam and its preparation method and application and the journal "ACS Nano" (2024, 4c03816) reported a method of coating pyrolytic carbon on the surface of silicon nitride aerogel by hydrothermal method and chemical vapor deposition method. Although the two methods have improved the heat resistance temperature of silicon nitride aerogel in an inert atmosphere to a certain extent, the pyrolytic carbon coating will be rapidly oxidized in an aerobic environment above 400°C.

[0004] In summary, the current research on low-cost and large-scale preparation of silicon nitride ceramic aerogels that can serve stably in high-temperature aerobic environments is still in a technical gap. Summary of the invention

[0005] In order to overcome the shortcomings of the above-mentioned prior art, the purpose of the present invention is to provide an antioxidant composite ceramic aerogel and a preparation method thereof, so as to solve the technical problem that silicon nitride ceramic aerogels that can stably serve in high-temperature aerobic environments cannot be prepared at low cost and in batches.

[0006] In order to achieve the above object, the present invention adopts the following technical solutions:

[0007] The present invention provides an antioxidant composite ceramic aerogel, wherein the main body of the antioxidant composite ceramic aerogel is silicon nitride aerogel, and the nanostructure of the silicon nitride aerogel is one of a one-dimensional silicon nitride nanowire and a two-dimensional silicon nitride nanobelt, or a combination of the two nanostructures;

[0008] The nanostructure of the silicon nitride aerogel is sequentially coated with a mullite coating and a copper-nickel metal coating from the inside to the outside.

[0009] In one embodiment, after the melting temperature of silica is reached, the silica in the mullite coating forms a flowing silica molten liquid, and the aluminum oxide nanoparticles in the mullite coating, the copper oxide nanoparticles and the nickel oxide nanoparticles formed by oxidation of the copper-nickel metal coating are dissolved in the silica molten liquid to form an oxide film together.

[0010] In one embodiment, the element composition of the oxidation resistant composite ceramic aerogel is nitrogen, silicon, aluminum, oxygen, copper and nickel.

[0011] The present invention also provides a method for preparing the antioxidant composite ceramic aerogel, comprising the following steps:

[0012] S1: mixing polysiloxane sol, plant sugar, foaming agent, metal catalyst and water, stirring, standing and solidifying, and then performing a first drying to form a xerogel, and then performing a first heat treatment to obtain silicon nitride aerogel;

[0013] S2: preparing a mullite mixed sol, immersing the silicon nitride aerogel in the mullite mixed sol, taking it out after saturation adsorption, drying it for the second time, and performing a second heat treatment to obtain a mullite / silicon nitride composite ceramic aerogel;

[0014] S3: Evenly mix the copper-containing compound, the nickel-containing compound and water to obtain a mixed solution, immerse the mullite / silicon nitride composite ceramic aerogel in the mixed solution, take it out after adsorption saturation, dry it for the third time, and perform a third heat treatment to obtain the copper-nickel / mullite / silicon nitride composite ceramic aerogel.

[0015] In one embodiment, in S1, the mass ratio of the polysiloxane sol, plant sugar, foaming agent, metal catalyst and water is (1-30): (1-30): (1-8): (1-5): (80-200).

[0016] In one embodiment, in S1, the plant sugar is one or a combination of glucose, sucrose, starch, fructose, maltose and xylose;

[0017] The foaming agent is one or a combination of animal protein foaming agent, plant protein foaming agent, sodium bicarbonate, nitrosamine and sodium dodecyl sulfate;

[0018] The metal catalyst is one or a combination of platinum catalyst, palladium catalyst, copper catalyst and nickel catalyst.

[0019] In one embodiment, in S2, the mullite mixed sol is prepared from aluminum nitrate, tetraethyl orthosilicate, boric acid and deionized water;

[0020] The mass ratio of the aluminum nitrate, tetraethyl orthosilicate, boric acid and deionized water is (0.1-1): (1-10): (0.05-1): (100-300).

[0021] In one embodiment, in S3, the mass ratio of the copper-containing compound, the nickel-containing compound and water is (0.1-10):(1-10):(50-200).

[0022] In one embodiment, in S3, the copper-containing compound is one or a combination of copper nitrate, copper chloride, and copper sulfate; the nickel compound is one or a combination of nickel nitrate, nickel chloride, and nickel sulfate.

[0023] In one embodiment, in S1, the temperature of the first drying is 30 to 150°C;

[0024] The temperature of the first heat treatment is 1350-1650° C., and the first heat treatment is performed in a nitrogen-containing atmosphere;

[0025] In S2, the temperature of the second drying is 40-200° C.; the temperature of the second heat treatment is 500-1200° C., and the second heat treatment is performed in an air atmosphere;

[0026] In S3, the temperature of the third drying is 35-180°C; the temperature of the third heat treatment is 600-1200°C, and the third heat treatment is performed under a reducing atmosphere.

[0027] Compared with the prior art, the present invention has the following beneficial effects:

[0028] On the one hand, the present invention provides an antioxidant composite ceramic aerogel, the main component of the aerogel is silicon nitride, and the structural elements constituting the silicon nitride aerogel are one-dimensional silicon nitride nanowires and two-dimensional silicon nitride nanobelts. Compared with granular and nanosheet structural elements, these large aspect ratio nanowires and nanobelts have higher mechanical deformation ability, giving the silicon nitride aerogel excellent compression rebound and anti-bending ability. Further, the nanostructured surface of the silicon nitride aerogel is coated with a mullite coating and a copper-nickel metal coating (mullite and copper-nickel metal dual antioxidant coating) from the inside to the outside, and the external copper-nickel metal coating uses the sweating cooling of the metal to achieve active thermal protection, effectively reducing the direct damage of the high temperature to the aerogel structure; at the same time, the uniformly coated mullite coating inside can block the contact between oxygen and silicon nitride, prevent it from being oxidized and causing the performance to decline, and effectively improve the high temperature antioxidant performance of the aerogel, and the antioxidant temperature is increased by 300°C compared with the pure silicon nitride aerogel. Therefore, the antioxidant composite ceramic aerogel prepared by the present invention has higher temperature resistance and antioxidant performance, and can serve stably in a high-temperature aerobic environment.

[0029] During actual use, the silica in the mullite coating will form a flowing molten liquid. The nano-alumina particles in the mullite and the copper oxide and nickel oxide nano-particles formed by the oxidation of the metal coating will dissolve in the molten liquid and act as nails, which can increase the viscosity of the silica molten liquid. The molten liquid not only enhances the bonding between the coating and silicon nitride, but also enables the coating to have a certain self-healing ability, which can fill some uncoated areas, thereby better protecting the silicon nitride. In addition, the nano-alumina particles in the mullite and the nano-particles formed by the oxidation of the metal coating will form a dense composite oxide film together with the molten silica, thereby improving its ability to resist the impact of high-temperature airflow or high-temperature flames.

[0030] On the other hand, the present invention provides a method for preparing an antioxidant composite ceramic aerogel, wherein a precursor skeleton containing a carbon source and a silicon source of any size can be prepared by foaming low-cost plant sugars and polysiloxanes, and a silicon nitride aerogel can be prepared quickly and efficiently by a carbon thermal reduction method; a mullite and metal copper-nickel dual antioxidant coating is coated on the surface of the silicon nitride nanostructure by a precursor impregnation pyrolysis method, and the prepared aerogel has a good adsorption effect on the precursor solution or sol of the coating due to its high porosity, which is beneficial to the efficient coating of the coating, that is, it is beneficial to the large-scale preparation of composite ceramic aerogels. In summary, the preparation method provided by the present invention has the advantages of low cost and large-scale preparation. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] Figure 1 This is an optical photograph of the antioxidant composite ceramic aerogel prepared in Example 1 of the present invention;

[0032] Figure 2This is an EDS spectrum analysis diagram of the antioxidant composite ceramic aerogel prepared in Example 1 of the present invention;

[0033] Figure 3 The middle figure (a) is an optical photograph of the antioxidant composite ceramic aerogel prepared in Example 1 after being flushed with a butane spray gun (about 1300°C); Figures (b-f) are infrared thermal imaging photographs of the antioxidant composite ceramic aerogel prepared in Example 1 after being flushed with a butane spray gun (about 1300°C) for 1, 5, 10, 15, and 20 minutes, respectively;

[0034] Figure 4 The SEM comparison diagram of the silicon nitride aerogel and the antioxidant composite ceramic aerogel prepared in Example 1 of the present invention after being oxidized at 1400°C for 30 minutes; wherein, Figure a is the SEM of the silicon nitride aerogel after being oxidized at 1400°C for 30 minutes; Figure b is the SEM of the antioxidant composite ceramic aerogel after being oxidized at 1400°C for 30 minutes;

[0035] Figure 5 This is a TGA comparison chart of the silicon nitride aerogel and the antioxidant composite ceramic aerogel prepared in Example 1 of the present invention. DETAILED DESCRIPTION

[0036] In order to enable those skilled in the art to understand the characteristics and effects of the present invention, the following is a general description and definition of the terms and expressions mentioned in the specification and claims. Unless otherwise specified, all technical and scientific terms used in the text are the common meanings understood by those skilled in the art for the present invention. In the event of a conflict, the definition in this specification shall prevail.

[0037] The theories or mechanisms described and disclosed herein, whether correct or incorrect, should not limit the scope of the present invention in any way, that is, the present invention can be implemented without being limited by any specific theory or mechanism.

[0038] Herein, all features such as values, quantities, contents and concentrations defined in the form of numerical ranges or percentage ranges are for simplicity and convenience only. Accordingly, the description of numerical ranges or percentage ranges should be considered to have included and specifically disclosed all possible secondary ranges and individual values ​​within the range (including integers and fractions).

[0039] In this document, unless otherwise specified, “includes,” “including,” “contains,” “has,” or similar terms cover the meanings of “consisting of” and “mainly consisting of,” for example, “A includes a” covers the meanings of “A includes a and other” and “A only includes a.”

[0040] In this document, in order to make the description concise, not all possible combinations of various technical features in various embodiments or examples are described. Therefore, as long as there is no contradiction in the combination of these technical features, the various technical features in various embodiments or examples can be combined arbitrarily, and all possible combinations should be considered to be within the scope of this specification.

[0041] The invention provides an antioxidant composite ceramic aerogel and a preparation method thereof.

[0042] On one hand, the present invention provides an antioxidant composite ceramic aerogel, wherein the main body of the antioxidant composite ceramic aerogel is silicon nitride aerogel, and the surface of the nanostructure of the silicon nitride aerogel is coated with a copper-nickel metal and mullite dual antioxidant coating.

[0043] More specifically, the structural components of silicon nitride aerogel are one-dimensional silicon nitride nanowires and two-dimensional silicon nitride nanobelts; in other words, the nanostructure of silicon nitride aerogel is one or a combination of one-dimensional silicon nitride nanowires and two-dimensional silicon nitride nanobelts. In addition, the nanostructure of silicon nitride aerogel is coated with a mullite coating and a copper-nickel metal coating in sequence from the inside to the outside. The main elements of the above-mentioned antioxidant composite ceramic aerogel are nitrogen, silicon, aluminum, oxygen, copper and nickel.

[0044] In one embodiment, an antioxidant composite ceramic aerogel is provided, the main component of which is silicon nitride, and the structural components constituting the silicon nitride aerogel are one-dimensional silicon nitride nanowires and two-dimensional silicon nitride nanobelts; in the antioxidant composite ceramic aerogel, the copper-nickel metal and mullite dual antioxidant coating are uniformly coated on the surface of the nanostructure of the silicon nitride aerogel. The main elements of the antioxidant composite ceramic aerogel are nitrogen, silicon, aluminum, oxygen, copper, and nickel. The above-mentioned antioxidant composite ceramic aerogel has an extremely low thermal conductivity of 0.025 to 0.042 W / mk; the antioxidant composite ceramic aerogel has excellent antioxidant properties, and its microscopic morphology does not change significantly after being treated in an aerobic environment at 1400°C for 30 minutes.

[0045] In one embodiment, if Figure 1 As shown, the antioxidant composite ceramic aerogel is a gray-white three-dimensional block with a density of 15 to 50 mg / cm 3 .

[0046] The invention provides a method for preparing an antioxidant composite ceramic aerogel, which comprises the following steps: preparing a polysiloxane sol, mixing the sol with plant sugar, a foaming agent, a metal catalyst and water in a certain proportion, stirring and standing to solidify, drying to form a dry gel, and subjecting to high-temperature heat treatment to obtain a silicon nitride aerogel; immersing the prepared silicon nitride aerogel in a mullite mixed sol, taking it out, drying, and subjecting to high-temperature heat treatment to obtain a mullite / silicon nitride composite ceramic aerogel; uniformly mixing a copper-containing compound, a nickel-containing compound and water in a certain proportion, immersing the prepared mullite / silicon nitride composite ceramic aerogel in the mixed solution, taking it out, drying, and subjecting to high-temperature heat treatment to obtain a copper-nickel / mullite / silicon nitride composite ceramic aerogel, i.e., an antioxidant composite ceramic aerogel.

[0047] The specific steps of the above preparation method are as follows:

[0048] Step 1) prepare polysiloxane sol, mix the sol with plant sugar, foaming agent, metal catalyst and water in a certain proportion, stir for 30 minutes, let it stand and solidify for 24 hours, dry at 30-150° C. to form a dry gel, and then perform high-temperature heat treatment at 1350-1650° C. in a nitrogen atmosphere to obtain silicon nitride aerogel.

[0049] Step 2) preparing a mullite mixed sol, immersing the silicon nitride aerogel prepared in step 1 into the mixed sol, taking it out, drying it at 40-200° C., and heat treating it at 500-1200° C. in an air atmosphere to obtain a mullite / silicon nitride composite ceramic aerogel.

[0050] Step 3) The copper-containing compound, the nickel-containing compound and water are uniformly mixed in a certain proportion, and the mullite / silicon nitride composite ceramic aerogel prepared in step 2 is immersed in the mixed solution. After being taken out, it is dried at 35-180° C. and heat-treated at 600-1200° C. in a reducing atmosphere to obtain the copper-nickel / mullite / silicon nitride composite ceramic aerogel, i.e., the antioxidant composite ceramic aerogel.

[0051] The specific dosage and process conditions are as follows:

[0052] In step 1), the process of preparing the polysiloxane sol is as follows: silicone resin, ethanol and water are uniformly mixed in a mass ratio of 3:10:8 to obtain the polysiloxane sol.

[0053] In step 1), the mass ratio of the polysiloxane, plant sugar, foaming agent, metal catalyst and water is (1-30): (1-30): (1-8): (1-5): (80-200); the plant sugar can be one or a combination of glucose, sucrose, starch, fructose, maltose and xylose; the foaming agent can be one or a combination of animal protein foaming agent, plant protein foaming agent, sodium bicarbonate, nitrosamine and sodium dodecyl sulfate; the metal catalyst can be one or a combination of platinum catalyst, palladium catalyst, copper catalyst and nickel catalyst; the nitrogen-containing atmosphere can be one or a combination of nitrogen and ammonia; the temperature of the high-temperature heat treatment is 1350-1650°C.

[0054] In step 2), the mullite mixed sol is prepared from aluminum nitrate, tetraethyl orthosilicate, boric acid and deionized water; the mass ratio of aluminum nitrate, tetraethyl orthosilicate, boric acid and water in the mullite mixed sol is (0.1-1): (1-10): (0.05-1): (100-300).

[0055] In step 3), the copper-containing compound may be: a composite of one or more of copper nitrate, copper chloride, and copper sulfate; the nickel-containing compound may be: a composite of one or more of nickel nitrate, nickel chloride, and nickel sulfate; the ratio of the copper-containing compound, the nickel-containing compound, and water is: (0.1-10): (1-10): (50-200).

[0056] The present invention will be further described below in conjunction with specific embodiments. It should be understood that these embodiments are only used to illustrate the present invention and are not intended to limit the scope of the present invention. In addition, it should be understood that after reading the content taught by the present invention, those skilled in the art can make various changes or modifications to the present invention, and these equivalent forms fall within the scope limited by the appended claims of the application equally.

[0057] The following examples use conventional instruments and equipment in the art. The experimental methods in the following examples where specific conditions are not specified are usually carried out under conventional conditions or under conditions recommended by the manufacturer. The various raw materials used in the following examples are conventional commercial products unless otherwise specified, and their specifications are conventional specifications in the art. In the specification of the present invention and the following examples, unless otherwise specified, "%" means weight percentage, "part" means weight part, and ratio means weight ratio.

[0058] Embodiment 1:

[0059] Step 1) Prepare 8 g of polysiloxane sol, mix the sol with 10 g of glucose, 5 g of animal protein foaming agent, 3 g of platinum catalyst and 180 g of water, stir for 30 min, let stand and cure for 24 h, dry at 100 ° C to form a xerogel, and then heat treat at 1550 ° C in a nitrogen atmosphere to obtain silicon nitride aerogel.

[0060] Step 2) 0.5 g of aluminum nitrate, 5 g of tetraethyl orthosilicate, 0.2 g of boric acid and 150 g of water are mixed evenly to prepare a mullite mixed sol, and the silicon nitride aerogel prepared in step 1 is immersed in the mixed sol. After being taken out, it is dried at 160° C. and heat-treated at 900° C. in an air atmosphere to obtain a mullite / silicon nitride composite ceramic aerogel.

[0061] Step 3) 1 g of copper chloride, 3 g of nickel nitrate and 180 g of water are mixed evenly, and the mullite / silicon nitride composite ceramic aerogel prepared in step 2 is immersed in the mixed solution. After being taken out, it is dried at 80° C. and heat-treated at 1000° C. in an argon-hydrogen mixed atmosphere to obtain a copper-nickel / mullite / silicon nitride composite ceramic aerogel, i.e., an antioxidant composite ceramic aerogel.

[0062] The density of the prepared antioxidant composite ceramic aerogel is 20 mg / cm 3 , the thermal conductivity at room temperature is 0.028W / mk. Figure 1 It can be seen that the antioxidant composite ceramic aerogel is gray-white three-dimensional block. Figure 2 It can be seen that the main elements of the antioxidant composite ceramic aerogel are nitrogen, silicon, aluminum, oxygen, copper and nickel. Figure 3 It can be seen that the antioxidant composite ceramic aerogel still maintains excellent thermal insulation performance under the 1300℃ butane flame erosion, and the back temperature of the aerogel is stabilized at 95℃ after 20 minutes of erosion. Figure 4 It can be seen that the microstructure of the antioxidant composite ceramic aerogel does not change after being treated in an aerobic environment at 1400°C for 30 min. Figure 4 Comparison between Figure (a) and Figure (b) shows that the microscopic components of the silicon nitride aerogel without the antioxidant coating melt and deform (i.e., silicon nitride nanowires or silicon nitride nanobelts are oxidized to silicon dioxide in a high-temperature aerobic environment, and silicon dioxide melts into a liquid at high temperature), while the aerogel coated with the antioxidant coating (i.e., antioxidant composite ceramic aerogel) can still maintain its original microscopic morphology after heat treatment in the same high-temperature aerobic environment. The reason is that the mullite and metal copper-nickel dual antioxidant coating coated on the surface of the nanostructure of the silicon nitride aerogel have an antioxidant effect.

[0063] Figure 5This is a comparison of the thermogravimetric curves of silicon nitride aerogel and antioxidant composite ceramic aerogel (i.e. silicon nitride aerogel coated with an antioxidant coating). It can be seen that pure silicon nitride aerogel undergoes rapid oxidation in an aerobic environment above 1100°C, while the antioxidant composite ceramic aerogel remains unoxidized at 1500°C (the oxidation at 300-900°C is the oxidation process of the copper-nickel coating). This figure can be compared with Figure 4 The combination proves that the antioxidant composite ceramic aerogel has better high-temperature antioxidant properties than pure silicon nitride aerogel.

[0064] Embodiment 2:

[0065] Step 1) 8 g of polysiloxane sol was prepared, and the sol was mixed with 15 g of sucrose, 3 g of vegetable protein foaming agent, 3 g of copper catalyst and 120 g of water, stirred for 30 min, left to cure for 24 h, dried at 120° C. to form a xerogel, and then heat treated at 1500° C. in a nitrogen atmosphere to obtain silicon nitride aerogel.

[0066] Step 2) 0.5 g aluminum nitrate, 8 g ethyl orthosilicate, 0.3 g boric acid and 180 g water are mixed evenly to prepare a mullite mixed sol, and the silicon nitride aerogel prepared in step 1 is immersed in the mixed sol. After being taken out, it is dried at 120° C. and heat-treated at 1100° C. in an air atmosphere to obtain a mullite / silicon nitride composite ceramic aerogel.

[0067] Step 3) 0.5g of copper chloride, 4g of nickel nitrate and 120g of water are mixed evenly, and the mullite / silicon nitride composite ceramic aerogel prepared in step 2 is immersed in the mixed solution. After being taken out, it is dried at 75°C and heat treated at 1000°C in an argon-hydrogen mixed atmosphere to obtain a copper-nickel / mullite / silicon nitride composite ceramic aerogel, that is, an antioxidant composite ceramic aerogel.

[0068] Embodiment 3:

[0069] Step 1) 15 g of polysiloxane sol was prepared, and the sol was mixed with 20 g of fructose, 6 g of sodium bicarbonate, 1 g of platinum catalyst and 140 g of water, stirred for 30 min, and then allowed to stand for curing for 24 h, dried at 130° C. to form a xerogel, and then heat treated at 1450° C. in a nitrogen atmosphere to obtain a silicon nitride aerogel.

[0070] Step 2) 1 g of aluminum nitrate, 6 g of tetraethyl orthosilicate, 0.1 g of boric acid and 200 g of water are mixed evenly to prepare a mullite mixed sol, and the silicon nitride aerogel prepared in step 1 is immersed in the mixed sol. After being taken out, it is dried at 100° C. and heat-treated at 800° C. in an air atmosphere to obtain a mullite / silicon nitride composite ceramic aerogel.

[0071] Step 3) 4 g of copper chloride, 4 g of nickel nitrate and 180 g of water are mixed evenly, and the mullite / silicon nitride composite ceramic aerogel prepared in step 2 is immersed in the mixed solution. After being taken out, it is dried at 150° C. and heat-treated at 700° C. in an argon-hydrogen mixed atmosphere to obtain a copper-nickel / mullite / silicon nitride composite ceramic aerogel, i.e., an antioxidant composite ceramic aerogel.

[0072] Embodiment 4:

[0073] Step 1) prepare 10g of polysiloxane sol, mix the sol with 20g of xylose, 4g of plant protein foaming agent, 3g of nickel catalyst and 100g of water, stir for 30min, let stand and cure for 24h, dry at 60°C to form a xerogel, and then heat treat at 1580°C in a nitrogen atmosphere to obtain silicon nitride aerogel.

[0074] Step 2) 0.6 g aluminum nitrate, 3 g ethyl orthosilicate, 0.3 g boric acid and 220 g water are mixed evenly to prepare a mullite mixed sol, and the silicon nitride aerogel prepared in step 1 is immersed in the mixed sol. After being taken out, it is dried at 120° C. and heat-treated at 750° C. in an air atmosphere to obtain a mullite / silicon nitride composite ceramic aerogel.

[0075] Step 3) 4 g of copper chloride, 10 g of nickel nitrate and 150 g of water are mixed evenly, and the mullite / silicon nitride composite ceramic aerogel prepared in step 2 is immersed in the mixed solution. After being taken out, it is dried at 80° C. and heat-treated at 700° C. in an argon-hydrogen mixed atmosphere to obtain a copper-nickel / mullite / silicon nitride composite ceramic aerogel, i.e., an antioxidant composite ceramic aerogel.

[0076] Embodiment 5:

[0077] Step 1) 1 g of polysiloxane sol was prepared, and the sol was mixed with 10 g of maltose, 1 g of sodium dodecyl sulfate, 1 g of nickel catalyst and 80 g of water, stirred for 30 min, and then allowed to stand for curing for 24 h, dried at 30° C. to form a xerogel, and then heat treated at 1350° C. in a nitrogen atmosphere to obtain a silicon nitride aerogel.

[0078] Step 2) 0.1 g of aluminum nitrate, 1 g of tetraethyl orthosilicate, 0.05 g of boric acid and 100 g of water are mixed evenly to prepare a mullite mixed sol, and the silicon nitride aerogel prepared in step 1 is immersed in the mixed sol. After being taken out, it is dried at 40° C. and heat-treated at 500° C. in an air atmosphere to obtain a mullite / silicon nitride composite ceramic aerogel.

[0079] Step 3) 0.1 g of copper sulfate, 1 g of nickel chloride and 50 g of water are mixed evenly, and the mullite / silicon nitride composite ceramic aerogel prepared in step 2 is immersed in the mixed solution. After being taken out, it is dried at 35° C. and heat-treated at 600° C. in an argon-hydrogen mixed atmosphere to obtain a copper-nickel / mullite / silicon nitride composite ceramic aerogel, i.e., an antioxidant composite ceramic aerogel.

[0080] Embodiment 6:

[0081] Step 1) 30 g of polysiloxane sol was prepared, and the sol was mixed with 30 g of starch, 8 g of nitrosamine, 5 g of palladium catalyst and 200 g of water, stirred for 30 min, and then allowed to stand for curing for 24 h, dried at 150° C. to form a xerogel, and then heat treated at 1650° C. in a nitrogen atmosphere to obtain silicon nitride aerogel.

[0082] Step 2) 1 g of aluminum nitrate, 10 g of tetraethyl orthosilicate, 1 g of boric acid and 300 g of water are mixed evenly to prepare a mullite mixed sol, and the silicon nitride aerogel prepared in step 1 is immersed in the mixed sol. After being taken out, it is dried at 200° C. and heat-treated at 1200° C. in an air atmosphere to obtain a mullite / silicon nitride composite ceramic aerogel.

[0083] Step 3) 10 g of copper nitrate, 10 g of nickel sulfate and 200 g of water are evenly mixed, and the mullite / silicon nitride composite ceramic aerogel prepared in step 2 is immersed in the mixed solution. After being taken out, it is dried at 180° C. and heat-treated at 1200° C. in an argon-hydrogen mixed atmosphere to obtain a copper-nickel / mullite / silicon nitride composite ceramic aerogel, i.e., an antioxidant composite ceramic aerogel.

[0084] In summary, the antioxidant composite ceramic aerogel prepared by the present invention has excellent compression resilience and bending resistance, thermal insulation performance and antioxidant performance, and can be prepared at low cost and on a large scale. It has great application potential in thermal insulation fields such as aerospace, high-temperature kilns and fire protection engineering.

[0085] The above contents are only for explaining the technical idea of ​​the present invention and cannot be used to limit the protection scope of the present invention. Any changes made on the basis of the technical solution in accordance with the technical idea proposed by the present invention shall fall within the protection scope of the claims of the present invention.

Claims

1. An antioxidant composite ceramic aerogel, characterized in that: The main body of the anti-oxidation composite ceramic aerogel is silicon nitride aerogel, and the nanostructure of the silicon nitride aerogel is one of one-dimensional silicon nitride nanowires and two-dimensional silicon nitride nanobelts, or a combination of the two nanostructures; The nanostructure of the silicon nitride aerogel is sequentially coated with a mullite coating and a copper-nickel metal coating from the inside to the outside.

2. The antioxidant composite ceramic aerogel according to claim 1, characterized in that: After reaching the melting temperature of silicon dioxide, the silicon dioxide in the mullite coating forms a flowing silicon dioxide molten liquid, and the aluminum oxide nanoparticles in the mullite coating, the copper oxide nanoparticles and the nickel oxide nanoparticles formed by oxidation of the copper-nickel metal coating are dissolved in the silicon dioxide molten liquid to form an oxide film together.

3. The antioxidant composite ceramic aerogel according to claim 1, characterized in that: The elements of the anti-oxidation composite ceramic aerogel are nitrogen, silicon, aluminum, oxygen, copper and nickel.

4. A method for preparing the antioxidant composite ceramic aerogel according to any one of claims 1 to 3, characterized in that: The following steps are involved: S1: mixing polysiloxane sol, plant sugar, foaming agent, metal catalyst and water, stirring, standing and solidifying, and then performing a first drying to form a xerogel, and then performing a first heat treatment to obtain silicon nitride aerogel; S2: preparing a mullite mixed sol, immersing the silicon nitride aerogel in the mullite mixed sol, taking it out and then drying it for a second time, and performing a second heat treatment to obtain a mullite / silicon nitride composite ceramic aerogel; S3: Evenly mix the copper-containing compound, the nickel-containing compound and water to obtain a mixed solution, immerse the mullite / silicon nitride composite ceramic aerogel in the mixed solution, take it out and then dry it for the third time, and perform a third heat treatment to obtain the copper-nickel / mullite / silicon nitride composite ceramic aerogel.

5. The method for preparing the antioxidant composite ceramic aerogel according to claim 4, characterized in that: In S1, the mass ratio of the polysiloxane sol, plant sugar, foaming agent, metal catalyst and water is (1-30): (1-30): (1-8): (1-5): (80-200).

6. The method for preparing the antioxidant composite ceramic aerogel according to claim 4, characterized in that: In S1, the plant sugar is one or a combination of glucose, sucrose, starch, fructose, maltose and xylose; The foaming agent is one or a combination of animal protein foaming agent, plant protein foaming agent, sodium bicarbonate, nitrosamine and sodium dodecyl sulfate; The metal catalyst is one or a combination of platinum catalyst, palladium catalyst, copper catalyst and nickel catalyst.

7. The method for preparing the antioxidant composite ceramic aerogel according to claim 4, characterized in that: In S2, the mullite mixed sol is prepared from aluminum nitrate, tetraethyl orthosilicate, boric acid and deionized water; The mass ratio of the aluminum nitrate, tetraethyl orthosilicate, boric acid and deionized water is (0.1-1): (1-10): (0.05-1): (100-300).

8. The method for preparing the antioxidant composite ceramic aerogel according to claim 4, characterized in that: In S3, the mass ratio of the copper-containing compound, the nickel-containing compound and water is (0.1-10):(1-10):(50-200).

9. The method for preparing the antioxidant composite ceramic aerogel according to claim 4, characterized in that: In S3, the copper-containing compound is one or a combination of copper nitrate, copper chloride, and copper sulfate; the nickel compound is one or a combination of nickel nitrate, nickel chloride, and nickel sulfate.

10. The method for preparing the antioxidant composite ceramic aerogel according to claim 4, characterized in that: In S1, the temperature of the first drying is 30 to 150° C.; The temperature of the first heat treatment is 1350-1650° C., and the first heat treatment is performed in a nitrogen-containing atmosphere; In S2, the temperature of the second drying is 40-200° C.; the temperature of the second heat treatment is 500-1200° C., and the second heat treatment is performed in an air atmosphere; In S3, the temperature of the third drying is 35-180°C; the temperature of the third heat treatment is 600-1200°C, and the third heat treatment is performed under a reducing atmosphere.

Citation Information

Patent Citations

  • Silicon nitride nanoribbon aerogel and preparation method thereof

    CN109704781A

  • Metal coating-based high temperature-resistant structural wave absorbing material and preparation method thereof

    CN109720027A

  • Preparation method of high-temperature-resistant light silicon nitride aerogel material

    CN110028048A

  • Reversible self-repair thermoplastic polymer nanofiber membrane or aerogel material and preparation method thereof

    CN110258127A

  • Production of mullite-silicon carbide combined ceramics

    JP1994219828A