High-thermal-conductivity insulating epoxy resin with biological characteristics, cured product, and preparation method and application of high-thermal-conductivity insulating epoxy resin and cured product

By introducing biphenyl structure and organic silicon compounds into epoxy resin and combining inorganic fillers to form a crosslinking network, the problem of synergistic improvement of thermal conductivity and breakdown strength of epoxy resin composite materials is solved, and high thermal conductivity and high insulation are achieved It has low dielectric loss performance, meets the high-performance needs of power equipment, and has the characteristics of green and environmental protection.

CN118955550APending Publication Date: 2024-11-15NINGBO INST OF MATERIALS TECH & ENG CHINESE ACAD OF SCI
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202411227651.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-03
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

When existing epoxy resin composites improve thermal conductivity and breakdown strength, it is difficult to coordinately improve thermal conductivity and dielectric loss performance, and traditional petroleum-based epoxy resins do not have enough environmental friendliness requirements.

Method used

Epoxy resin is prepared by bio-based compound Magnolia , biphenyl structure and organic silicon compounds are introduced , cross-linking network is formed through hydrogen silicon addition reaction and acid anhydride curing agent , and combined with micron-scale inorganic fillers to improve thermal conductivity and breakdown strength , while reducing dielectric loss.

Benefits of technology

The cured epoxy resin substance with high thermal conductivity, high insulation, excellent mechanical and heat resistance is achieved, meeting the dual needs of green and environmental protection and high performance, solving the contradiction between thermal conductivity and insulation performance, and improving the multi-dimensional performance of electrical equipment.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118955550A_ABST
    Figure CN118955550A_ABST
Patent Text Reader

Abstract

The invention discloses a bio-intrinsic high-thermal-conductivity insulating epoxy resin, a cured product, a preparation method of the cured product and an application of the cured product, and belongs to the technical field of high polymer materials, and the structural formula of the bio-intrinsic high-thermal-conductivity insulating epoxy resin is shown in the formula (I), the preparation method comprises the following steps: carrying out a two-step reaction on a bio-based compound magnolol and epoxy halogenated propane to prepare magnolol epoxy resin, and carrying out a hydrosilylation reaction on the magnolol epoxy resin and organic silicon to obtain the magnolol epoxy resin. The epoxy resin cured product obtained by curing the biologic intrinsic high-thermal-conductivity insulating epoxy resin and an aryl-containing anhydride curing agent has outstanding thermal conductivity, breakdown strength, mechanical property and heat resistance at the same time, the problem of contradiction between thermal conductivity and insulating property is solved, and the resource and environment problems faced by the existing electrical insulating epoxy resin are solved; wide application prospects are realized. # imgabs0 #
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of epoxy resins, and in particular to a biologically basic high thermal conductivity insulating epoxy resin, a cured product, and a preparation method and application thereof. Background Art

[0002] Epoxy resin has excellent mechanical properties, thermal properties, bonding properties and insulation properties, and is widely used in electronic packaging materials, coatings, adhesives, power equipment materials and other fields. The growing global demand for clean energy has prompted the transformation of traditional petroleum-based epoxy resins to environmentally friendly materials. Therefore, it is necessary to develop green, low-carbon and environmentally friendly epoxy resins to replace existing petroleum-based epoxy resins.

[0003] In recent years, insulating parts with epoxy resin as dielectric have been widely used in the power industry, especially in the insulation of electrical equipment and insulation packaging of microelectronic equipment. With the development of power systems towards high frequency, high capacity and compactness, higher requirements are placed on the insulation, heat resistance and mechanical properties of epoxy resins used in power equipment, especially the need for high breakdown strength, high thermal conductivity and low dielectric loss performance. However, the optimization of the multi-dimensional performance of epoxy resin cured products is a complex multi-objective optimization problem, which is difficult to improve in a coordinated manner.

[0004] For example, a Chinese patent document with publication number CN109206849A discloses a high thermal conductivity insulating epoxy resin composition and a preparation method thereof. In the invention, thermal conductive insulating fillers and microspheres are added to the epoxy resin prepolymer so that it has both good thermal conductivity and electrical insulation properties; a Chinese patent document with publication number CN109535658A discloses a preparation method for a high thermal conductivity hexagonal boron nitride / epoxy resin composite material. The invention improves the thermal conductivity of the composite material by introducing hexagonal boron nitride and a specific process; a Chinese patent document with publication number CN116200006A discloses a high thermal conductivity epoxy resin composite material and a preparation method thereof. The invention improves the thermal conductivity of the epoxy resin-based composite material by adding dopamine-coated boron nitride / copper nanowires having a one-dimensional and two-dimensional heterogeneous structure; however, although the above method improves the thermal conductivity of the epoxy resin composite material, it may have an adverse effect on the breakdown strength and dielectric loss performance.

[0005] The Chinese patent document with publication number CN117820813A discloses a high-insulation epoxy resin material and a preparation method. The invention improves the electrical breakdown strength, dielectric properties and resistivity by adding core-shell particles (copolymer with polybutyl acrylate as the core and a composition of polyalkoxystyrene and polymethyl methacrylate as the shell) and wollastonite. The Chinese patent document with publication number CN116462874A discloses a method for improving the breakdown strength of epoxy resin materials. The invention performs a short-term high-temperature heat treatment on the cured epoxy resin, thereby promoting the epoxy resin to form a dense oxide film on the surface, thereby hindering the charge transport in the body and improving the breakdown performance of epoxy insulating materials. The Chinese patent document with publication number CN107163293A discloses a method for improving the breakdown strength and energy storage density of dielectric composite materials. The invention effectively improves the problem that the electrical breakdown performance of the composite film deteriorates with the increase of fillers by inorganic nanofillers coated with surface modifiers. However, none of the above inventions pays attention to thermal conductivity.

[0006] In summary, while ensuring the excellent mechanical and heat resistance of epoxy resin cured products, synergistically improving thermal conductivity and breakdown strength is an urgent problem to be solved. Therefore, it is necessary to develop an environmentally friendly epoxy resin with high thermal conductivity, high insulation, and excellent mechanical and heat resistance to meet the dual needs of "green environmental protection" and "high performance". Summary of the invention

[0007] In order to solve the deficiencies in the prior art, the present invention provides a bio-based high thermal conductivity insulating epoxy resin, whose cured product has high thermal conductivity, high insulation, low dielectric, and excellent mechanical and heat resistance properties.

[0008] The specific technical solutions adopted are as follows:

[0009] A biologically basic high thermal conductivity insulating epoxy resin, the structural formula of which is shown in formula (I):

[0010]

[0011] In the formula, 0≤n≤3, R is an organosilicon compound residue, the organosilicon compound structure contains a silicon-hydrogen bond, and is selected from at least one of 1,1,5,5-tetramethyl-3,3-diphenyltrisiloxane, 1,2-bis(dimethylsilyl)benzene, diphenylsilane, tetramethyldisilazane, 1,1,3,3-tetramethyldisiloxane, phenyltri(dimethylsiloxy)silane, and 2,4,6,8-tetramethylcyclotetrasiloxane.

[0012] Preferably, the weight average molecular weight of the bio-basic high thermal conductive insulating epoxy resin is 700-1500 g / mol, and the epoxy value is 0.26-0.62 eq / 100 g.

[0013] The present invention also provides a method for preparing the biological basic characteristic high thermal conductive insulating epoxy resin, comprising the following steps:

[0014] (1) Under the protection of an inert gas, magnolol, an epoxyhalopropane and a first catalyst are fully mixed, reacted at 55 to 80° C. for 4 to 10 hours, then cooled to 20 to 50° C., a basic compound solution is added dropwise, and then the reaction is continued for 10 to 24 hours, and magnolol epoxy resin is obtained through post-treatment;

[0015] (2) Under the protection of an inert gas, magnolol epoxy resin, a second catalyst, and the organosilicon compound (containing silicon-hydrogen bonds) are reacted in an organic solvent system at 50 to 90° C. for 5 to 12 hours, and the bio-basic high thermal conductive insulating epoxy resin is obtained through post-treatment.

[0016] The inert gas is nitrogen atmosphere, argon atmosphere, etc.

[0017] Preferably, in step (1), the mass ratio of magnolol, epihalopropane, the first catalyst and the alkaline compound is 100:250-520:0.5-2:30-36;

[0018] And / or, in step (2), the mass ratio of magnolol epoxy resin, the second catalyst, and the organosilicon compound is 4 to 12:1×10 -5 ~8×10 -4 :1.

[0019] Optionally, the epihalohydrin includes epichlorohydrin and / or epibromohydrin;

[0020] And / or, the first catalyst comprises at least one of tetrabutylammonium bromide, benzyltriethylammonium chloride, benzyltrimethylammonium chloride, tetramethylammonium chloride, sodium hydroxide and potassium hydroxide;

[0021] And / or, the alkaline compound includes at least one of sodium hydroxide, potassium hydroxide and calcium hydroxide;

[0022] And / or, the second catalyst is a platinum catalyst, which can be chloroplatinic acid, Custer catalyst or platinum dioxide;

[0023] And / or, the organic solvent includes at least one of toluene, xylene, 1,4-dioxane, methyl isobutyl ketone, acetonitrile, chloroform, dichloromethane, tetrahydrofuran, isobutanol and isopropanol.

[0024] The invention also provides a high thermal conductivity insulating epoxy resin composition, comprising the biological basic characteristics high thermal conductivity insulating epoxy resin, anhydride curing agent, inorganic filler and accelerator.

[0025] Preferably, the high thermal conductive insulating epoxy resin composition comprises, by weight, 100 parts of the bio-based high thermal conductive insulating epoxy resin, 50-120 parts of anhydride curing agent, 0-400 parts (further 200-400 parts) of inorganic filler and 0.4-1 part of accelerator.

[0026] Optionally, the anhydride curing agent is selected from at least one of phthalic anhydride, tetrahydrophthalic anhydride, 2,2'-biphenyl dicarboxylic anhydride, 1,4,5,8-naphthalenetetracarboxylic anhydride, 1,8-naphthalene dicarboxylic anhydride, methyltetrahydrophthalic anhydride, tetrahydrophthalic anhydride, 3,4,5,6-tetrafluorophthalic anhydride, 3-fluorophthalic anhydride, 4,4'-(hexafluoroisopropylene) diphthalic anhydride, 4,4'-oxydiphthalic anhydride, 2,3-naphthalene dicarboxylic anhydride, 1,2-cyclohexane anhydride, 1-phenyl-2,3-naphthalene dicarboxylic anhydride, benzoxanthenyl anhydride, and 2,3-biphenyl maleic anhydride;

[0027] And / or, the inorganic filler comprises at least one of alumina, silicon dioxide, boron nitride, aluminum hydroxide, diamond, silicon carbide, zinc oxide, titanium dioxide, aluminum nitride, and barium titanate, and the median particle size of the inorganic filler is 8 to 30 μm;

[0028] And / or, the accelerator includes a first accelerator and a second accelerator, the first accelerator is at least one of N,N-dimethylbenzylamine, 2,4,6-tris(dimethylaminomethyl)phenol, 2-methylimidazole, triethanolamine, and boron trifluoride complex, and the second accelerator is dibenzoyl peroxide or dilauroyl peroxide.

[0029] The use of an aromatic anhydride curing agent can increase the benzene ring content in the composition. A large number of benzene rings form an ordered microstructure through π-π interactions, which is beneficial to improving the thermal conductivity of the cured product. The use of a first accelerator can promote the epoxy-anhydride reaction, and the use of a second accelerator can promote the free radical polymerization reaction of the allyl group. The combined use of the accelerators can form two cross-linking structures, which is beneficial to increase the cross-linking density of the cured product and improve the mechanical strength.

[0030] The invention also provides a high thermal conductivity insulating epoxy resin cured product, which is obtained by curing the high thermal conductivity insulating epoxy resin composition.

[0031] The present invention also provides a method for preparing the highly thermally conductive insulating epoxy resin cured product, comprising:

[0032] The biological basic characteristics high thermal conductivity insulating epoxy resin, anhydride curing agent, and inorganic filler are mixed and vacuum stirred at 80-140° C. for 30-60 minutes, and then an accelerator is added and vacuum stirred at 80-140° C. for 5-10 minutes to obtain a mixture; the mixture is first cured at 80-140° C. for 2-5 hours, and then cured at 140-180° C. for 8-16 hours to obtain a high thermal conductivity insulating epoxy resin cured product.

[0033] The present invention also provides the application of the biological basic characteristics high thermal conductivity insulating epoxy resin, the high thermal conductivity insulating epoxy resin composition or the high thermal conductivity insulating epoxy resin cured product in the field of electrical insulation.

[0034] Compared with the prior art, the present invention has the following beneficial effects:

[0035] (1) The present invention uses the bio-based compound magnolia officinalis as a raw material to prepare magnolia officinalis epoxy resin, introduces a biphenyl structure into the epoxy resin cured product, and simultaneously selects an acid anhydride curing agent with an aromatic group to increase the benzene ring content in the cross-linked network, and utilizes the π-π interaction of the benzene ring to self-assemble in the cured network to form a microscopic ordered structure, thereby promoting phonon propagation and improving the intrinsic thermal conductivity of the epoxy resin. The thermal conductivity of the pure epoxy resin cured product can reach 0.3 to 0.4 W / (m·K), and the thermal conductivity of the epoxy resin cured product after being compounded with a micron-sized inorganic filler can reach 1.1 to 2.1 W / (m·K).

[0036] (2) The present invention introduces an organosilicon structure into the epoxy resin cured product through the allylic double bond of magnolol and the Si-H bond of the organosilicon compound to form a localized energy difference by combining the high LUMO energy level of the organosilicon structure with the low LUMO energy level of the biphenyl structure, thereby constructing a molecular charge trap, thereby inhibiting charge migration, improving breakdown strength and reducing dielectric loss. The AC breakdown strength of the pure epoxy resin cured product can reach 36 to 39 kV / mm, and the dielectric loss is less than 0.003; the AC breakdown strength of the epoxy resin cured product compounded with micron inorganic fillers can reach 34 to 39 kV / mm, and the dielectric loss is less than 0.005.

[0037] (3) The high thermal conductivity insulating epoxy resin cured product of the present invention has both high thermal conductivity and excellent electrical insulation performance, solving the problem of the contradiction between thermal conductivity and insulation performance. At the same time, the high thermal conductivity insulating epoxy resin composition of the present invention undergoes a free radical polymerization reaction including epoxy-anhydride reaction and allyl group during curing, so that the cured product has a tight cross-linked network structure, improves the mechanical and heat resistance of the cured product, solves the problem of the difficulty in synergistically improving the electrical, mechanical and thermal multi-dimensional performance of epoxy resin composite materials, and can meet the performance requirements of current power equipment manufacturing.

[0038] (4) The bio-basic high thermal conductive insulating epoxy resin of the present invention is directly prepared by Si-H addition reaction, which has the characteristics of mild reaction conditions, simple process and easy industrial production.

[0039] (5) Magnolia officinalis is derived from biomass raw materials and is a green and environmentally friendly product that solves the resource and environmental problems faced by existing electrical insulating epoxy resins. BRIEF DESCRIPTION OF THE DRAWINGS

[0040] Figure 1 This is the hydrogen nuclear magnetic resonance spectrum of the biological basic high thermal conductive insulating epoxy resin EP-A prepared in Example 1;

[0041] Figure 2 The temperature-time curves of the high thermal conductive insulating epoxy resin cured product prepared in Example 5 and the traditional epoxy resin cured product on the heating plate. DETAILED DESCRIPTION

[0042] The present invention will be further described below in conjunction with the examples and drawings. It should be understood that these examples are intended only to illustrate the present invention and are not intended to limit the scope of the present invention. The operating methods in the following examples that do not specify specific conditions are usually carried out under conventional conditions or under conditions recommended by the manufacturer. Contents not described in detail in this specification belong to prior art known to professionals and technicians in the field.

[0043] Example 1

[0044] Preparation of biological basic characteristics high thermal conductivity insulating epoxy resin EP-A:

[0045] The specific reaction route is as follows:

[0046]

[0047] (1) Under the protection of nitrogen, 100 g of magnolol, 347.7 g of epichlorohydrin (ECH) and 1.69 g of tetrabutylammonium bromide were fully mixed, reacted at 70° C. for 5 h, then cooled to 25° C., 63.2 g of a 50 wt % sodium hydroxide aqueous solution was added dropwise for 2 h, and then the reaction was continued for 12 h. After washing, solvent removal by rotary evaporation and drying, magnolol epoxy resin was obtained;

[0048] (2) Under the protection of nitrogen, 100g of magnolol epoxy resin and 1.2g of Pt catalyst (2000ppm) were mixed, stirred at 60°C for 5min, and then 40g of 50wt% 1,1,5,5-tetramethyl-3,3-diphenyltrisiloxane toluene solution was added dropwise. After the reaction was continued at 60°C for 8h, the solvent was evaporated to obtain a biological basic high thermal conductivity insulating epoxy resin EP-A. The epoxy value of EP-A resin is 0.38eq / 100g, the weight average molecular weight is 1088g / mol, 0≤n≤1, and the hydrogen nuclear magnetic resonance spectrum is as follows: Figure 1 shown.

[0049] Example 2

[0050] Preparation of biological basic characteristics high thermal conductivity insulating epoxy resin EP-B:

[0051] (1) Under the protection of nitrogen, 100 g of magnolol, 417.3 g of epichlorohydrin and 1.69 g of benzyltriethylammonium chloride were fully mixed, reacted at 70° C. for 5 h, then cooled to 25° C., 66.5 g of 50% mass concentration sodium hydroxide aqueous solution was added dropwise for 2 h, and then the reaction was continued for 12 h. After washing, the solvent was removed by rotary evaporation and dried, magnolol epoxy resin was obtained;

[0052] (2) Under the protection of nitrogen, 100g of magnolol epoxy resin and 1.1g of Pt catalyst (2000ppm) were mixed, stirred at 60°C for 5min, and then 18.7g of 50wt% 1,1,3,3-tetramethyldisiloxane toluene solution was added dropwise, and the reaction was continued at 60°C for 8h, and the solvent was removed by rotary evaporation to obtain a biological basic high thermal conductivity insulating epoxy resin EP-B. The epoxy value of EP-B resin is 0.43eq / 100g, the weight average molecular weight is 890g / mol, and 0≤n≤1.

[0053] Example 3

[0054] Preparation of high thermal conductivity insulating epoxy resin cured product (without inorganic filler):

[0055] (1) 100 g of the bio-based high thermal conductive insulating epoxy resin EP-A prepared in Example 1 and 56.3 g of phthalic anhydride (PA) were stirred at 120° C. in a vacuum atmosphere for 30 min, followed by addition of 0.6 g of N,N-dimethylbenzylamine and 0.4 g of dilauroyl peroxide, and the mixture was stirred at 120° C. in a vacuum atmosphere for 5 min to obtain a casting material mixture;

[0056] (2) The casting material is poured into a preheated 120°C mold, cured at 120°C for 3 hours, and then further cured at 140°C for 10 hours to obtain a highly thermally conductive insulating epoxy resin EP-A cured product.

[0057] Example 4

[0058] The high thermal conductive insulating epoxy resin cured product in this embodiment does not contain inorganic filler, and the preparation method of the high thermal conductive insulating epoxy resin cured product in this embodiment is different from that in Example 3 in that the raw material is the biological basic high thermal conductive insulating epoxy resin EP-B prepared in Example 2, the amount of PA is 63.6 g, and the other processes and parameters are the same.

[0059] Example 5

[0060] Preparation of bio-based high thermal conductivity insulating epoxy resin cured product (including inorganic filler):

[0061] (1) 100 g of the bio-based high thermal conductive insulating epoxy resin EP-A prepared in Example 1, 56.3 g of phthalic anhydride (PA) and 300 g of micronized alumina (median particle size of 12.6 μm) were mixed and stirred at 120° C. under vacuum for 40 min; then 0.6 g of N,N-dimethylbenzylamine and 0.4 g of dilauroyl peroxide were added and stirred at 120° C. under vacuum for 5 min to obtain a casting material mixture;

[0062] (2) The casting material is poured into a preheated 120°C mold, cured at 120°C for 4 hours, and then further cured at 150°C for 16 hours to obtain a cured product of a highly thermally conductive insulating epoxy resin EP-A.

[0063] Example 6

[0064] The high thermal conductive insulating epoxy resin cured product in this embodiment contains inorganic filler, and the preparation method of the high thermal conductive insulating epoxy resin cured product in this embodiment is different from that in Example 5 in that the raw material is the biological basic high thermal conductive insulating epoxy resin EP-B prepared in Example 2, the amount of PA is 63.6 g, and the other processes and parameters are the same.

[0065] Example 7

[0066] The high thermal conductive insulating epoxy resin cured material in this embodiment contains inorganic filler, and the preparation method of the high thermal conductive insulating epoxy resin cured material in this embodiment is different from that in Example 5 in that the anhydride curing agent is tetrahydrophthalic anhydride THPA, the amount of THPA used is 57.8 g, and the other processes and parameters are the same.

[0067] Example 8

[0068] The high thermal conductive insulating epoxy resin cured material in this embodiment contains an inorganic filler, and the preparation method of the high thermal conductive insulating epoxy resin cured material in this embodiment is different from that in Example 5 in that the inorganic filler is boron nitride (median particle size is 14.1 μm), and the other processes and parameters are the same.

[0069] Comparative Example 1

[0070] Preparation of petroleum-based bisphenol A epoxy resin cured product (without inorganic filler):

[0071] (1) 100 g of petroleum-based bisphenol A epoxy resin DGEBA and 76.9 g of phthalic anhydride (PA) were stirred at 120° C. under vacuum for 30 min, and then 0.6 g of N,N-dimethylbenzylamine was added and stirred at 120° C. under vacuum for 5 min to obtain a casting material mixture;

[0072] (2) The casting material is poured into a preheated 120°C mold, cured at 120°C for 3 hours, and then further cured at 140°C for 10 hours to obtain a petroleum-based bisphenol A epoxy resin cured product.

[0073] Comparative Example 2

[0074] Preparation of petroleum-based bisphenol A epoxy resin cured product (containing inorganic filler):

[0075] (1) 100 g of petroleum-based bisphenol A epoxy resin DGEBA, 76.9 g of phthalic anhydride (PA) and 300 g of micronized alumina (median particle size of 12.6 μm) were mixed and stirred at 120° C. under vacuum for 40 min; then 0.6 g of N,N-dimethylbenzylamine was added and stirred at 120° C. under vacuum for 5 min to obtain a casting material mixture;

[0076] (2) The casting material is poured into a preheated 120°C mold, cured at 120°C for 4 hours, and then further cured at 150°C for 16 hours to obtain a petroleum-based bisphenol A epoxy resin cured product.

[0077] Comparative Example 3

[0078] The petroleum-based bisphenol A epoxy resin cured product in this comparative example contains an inorganic filler, and the preparation method of the petroleum-based bisphenol A epoxy resin cured product in comparative example 2 is different only in that the inorganic filler is boron nitride (median particle size is 14.1 μm), and the other processes and parameters are the same.

[0079] Sample analysis

[0080] The performance test of the samples prepared in the embodiments and comparative examples is carried out as follows:

[0081] Breakdown strength test: Use a stainless steel ball-ball electrode with a diameter of 20mm, place a solidified sample with a diameter of 100mm and a thickness of 1mm in the middle of the electrode, and place the electrode and the sample in insulating oil. Apply AC and DC voltages with a voltage increase rate of 2kV / s to the electrodes respectively until breakdown occurs, record the breakdown voltage, and use formula E b=U / d to calculate the breakdown strength, where U is the breakdown voltage of the sample and d is the thickness of the sample. Each sample was tested 10 times, and the 10 data were processed by Weibull distribution, and the value with a Weibull distribution probability of 63.2% was taken as the breakdown strength.

[0082] Thermal conductivity test: The thermal conductivity was tested using a laser thermal conductivity meter (Netzsch LFA457) using the laser thermal conductivity method.

[0083] Glass transition temperature (T g ) Test: Differential scanning calorimeter (DSC 214) was used to test T g , the temperature range is 30-200℃, and the heating rate is 10℃ / min.

[0084] Dielectric constant and dielectric loss test: Under the conditions of temperature of 20°C and relative humidity of 50%, the dielectric constant and dielectric loss at an industrial frequency of 50Hz were tested using a high-voltage bridge (QS 87 type) with an applied voltage of 1kV.

[0085] Temperature rise test: Place epoxy resin cured samples on a 50°C heating plate and use an infrared thermal imager to record the temperature-time curve of the samples.

[0086] The high thermal conductivity insulating epoxy resin cured products prepared in Examples 3 to 8 and the petroleum-based bisphenol A epoxy resin cured products prepared in Comparative Examples 1 to 3 were tested for thermal conductivity, AC breakdown strength, dielectric constant and dielectric loss, tensile strength, T g Test, the test results are shown in Table 1;

[0087] Table 1 Test results of samples prepared in Examples 3 to 8 and Comparative Examples 1 to 3

[0088]

[0089] As can be seen from Table 1, compared with Comparative Examples 1 to 3, Examples 3 to 8 show that the cured product prepared using the bio-based high thermal conductivity insulating epoxy resin as a raw material has higher thermal conductivity, AC breakdown strength, lower dielectric constant and dielectric loss than the cured product prepared using the petroleum-based bisphenol A epoxy resin DGEBA. In addition, the tensile strength and glass transition temperature remain substantially the same. This shows that the bio-based high thermal conductivity insulating epoxy resin shown in formula (I) has excellent electrical, mechanical and thermal properties.

[0090] By comparing Examples 3 and 4 with Comparative Example 1, it can be concluded that the biologically basic high thermal conductivity insulating epoxy resin shown in Formula (I) has the advantages of intrinsic high thermal conductivity, high insulation and low dielectric constant.

[0091] Comparing Examples 5 and 7 with Comparative Example 2, it can be concluded that the biological basic characteristics high thermal conductive insulating epoxy resin shown in formula (I) has a good effect when cured with different anhydride curing agents (phthalic anhydride, tetrahydrophthalic anhydride).

[0092] Comparing Examples 5 to 8 with Comparative Examples 2 and 3, it can be concluded that after adding different inorganic fillers, the biological basic characteristics high thermal conductive insulating epoxy resin shown in formula (I) all have very good effects.

[0093] from Figure 2 It can also be seen that Example 5 has a faster temperature rise than Comparative Example 2, indicating that the high thermal conductive insulating epoxy resin has a good heat dissipation effect as a raw material for casting or packaging of power equipment.

[0094] The embodiments described above provide a detailed description of the technical solutions of the present invention. It should be understood that the above are only specific embodiments of the present invention and are not intended to limit the present invention. Any modifications, supplements or similar substitutions made within the scope of the principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A biological basic high thermal conductivity insulating epoxy resin, characterized in that: The structural formula is shown in formula (I): In the formula, 0≤n≤3, R is an organosilicon compound residue, the organosilicon compound structure contains a silicon-hydrogen bond, and is selected from at least one of 1,1,5,5-tetramethyl-3,3-diphenyltrisiloxane, 1,2-bis(dimethylsilyl)benzene, diphenylsilane, tetramethyldisilazane, 1,1,3,3-tetramethyldisiloxane, phenyltri(dimethylsiloxy)silane, and 2,4,6,8-tetramethylcyclotetrasiloxane.

2. The biological basic high thermal conductive insulating epoxy resin according to claim 1, characterized in that: The weight average molecular weight of the biological basic characteristic high thermal conductive insulating epoxy resin is 700-1500 g / mol, and the epoxy value is 0.26-0.62 eq / 100 g.

3. The method for preparing the biologically basic high thermal conductive insulating epoxy resin according to claim 1 or 2, characterized in that: The following steps are involved: (1) Under the protection of an inert gas, magnolol, an epoxyhalopropane and a first catalyst are fully mixed, reacted at 55 to 80° C. for 4 to 10 hours, then cooled to 20 to 50° C., a basic compound solution is added dropwise, and then the reaction is continued for 10 to 24 hours, and magnolol epoxy resin is obtained through post-treatment; (2) Under the protection of an inert gas, magnolol epoxy resin, a second catalyst, and the organosilicon compound are reacted in an organic solvent system at 50 to 90° C. for 5 to 12 hours, and the bio-basic high thermal conductive insulating epoxy resin is obtained through post-treatment.

4. The method for preparing the biologically basic high thermal conductive insulating epoxy resin according to claim 3, characterized in that: In step (1), the mass ratio of magnolol, epihalopropane, the first catalyst and the alkaline compound is 100:250-520:0.5-2:30-36; And / or, in step (2), the mass ratio of magnolol epoxy resin, the second catalyst, and the organosilicon compound is 4 to 12:1×10 -5 ~8×10 -4 :

1.

5. The method for preparing the biologically basic high thermal conductive insulating epoxy resin according to claim 3, characterized in that: The epihalohydrin includes epichlorohydrin and / or epibromohydrin; And / or, the first catalyst comprises at least one of tetrabutylammonium bromide, benzyltriethylammonium chloride, benzyltrimethylammonium chloride, tetramethylammonium chloride, sodium hydroxide and potassium hydroxide; And / or, the alkaline compound includes at least one of sodium hydroxide, potassium hydroxide and calcium hydroxide; And / or, the second catalyst is a platinum catalyst; And / or, the organic solvent includes at least one of toluene, xylene, 1,4-dioxane, methyl isobutyl ketone, acetonitrile, chloroform, dichloromethane, tetrahydrofuran, isobutanol and isopropanol.

6. A high thermal conductive insulating epoxy resin composition, characterized in that: The invention comprises the biological basic characteristic high thermal conductive insulating epoxy resin as claimed in claim 1 or 2, an acid anhydride curing agent, an inorganic filler and an accelerator.

7. The high thermal conductive insulating epoxy resin composition according to claim 6, characterized in that: Calculated by mass, it comprises 100 parts of the biological basic characteristics high thermal conductivity insulating epoxy resin, 50-120 parts of anhydride curing agent, 0-400 parts of inorganic filler and 0.4-1 part of accelerator; The anhydride curing agent is selected from at least one of phthalic anhydride, tetrahydrophthalic anhydride, 2,2'-biphenyl dicarboxylic anhydride, 1,4,5,8-naphthalenetetracarboxylic anhydride, 1,8-naphthalene dicarboxylic anhydride, methyltetrahydrophthalic anhydride, tetrahydrophthalic anhydride, 3,4,5,6-tetrafluorophthalic anhydride, 3-fluorophthalic anhydride, 4,4'-(hexafluoroisopropylene) diphthalic anhydride, 4,4'-oxydiphthalic anhydride, 2,3-naphthalene dicarboxylic anhydride, 1,2-cyclohexane anhydride, 1-phenyl-2,3-naphthalene dicarboxylic anhydride, benzoxanthenyl anhydride, and 2,3-biphenyl maleic anhydride; And / or, the inorganic filler comprises at least one of alumina, silicon dioxide, boron nitride, aluminum hydroxide, diamond, silicon carbide, zinc oxide, titanium dioxide, aluminum nitride, and barium titanate, and the median particle size of the inorganic filler is 8 to 30 μm; And / or, the accelerator includes a first accelerator and a second accelerator, the first accelerator is at least one of N,N-dimethylbenzylamine, 2,4,6-tris(dimethylaminomethyl)phenol, 2-methylimidazole, triethanolamine, and boron trifluoride complex, and the second accelerator is dibenzoyl peroxide or dilauroyl peroxide.

8. A highly thermally conductive insulating epoxy resin cured product, characterized in that: The invention is obtained by curing the high thermal conductive insulating epoxy resin composition according to claim 6 or 7.

9. The method for preparing a highly thermally conductive insulating epoxy resin cured product according to claim 8, characterized in that: include: The biological basic characteristics high thermal conductivity insulating epoxy resin, anhydride curing agent, and inorganic filler are mixed and vacuum stirred at 80-140° C. for 30-60 minutes, and then an accelerator is added and vacuum stirred at 80-140° C. for 5-10 minutes to obtain a mixture; the mixture is first cured at 80-140° C. for 2-5 hours, and then cured at 140-180° C. for 8-16 hours to obtain a high thermal conductivity insulating epoxy resin cured product.

10. Use of the high thermal conductivity insulating epoxy resin according to claim 1 or 2, the high thermal conductivity insulating epoxy resin composition according to claim 6 or 7, or the high thermal conductivity insulating epoxy resin cured product according to claim 8 in the field of electrical insulation.

Citation Information

Cited By

  • Copper profile for chip radiator base and processing technology of copper profile

    CN120679954A

  • Heat insulation coating containing rare earth and preparation method thereof

    CN121249219A