Multi-generation branched polyurethane antistatic finishing agent emulsion and preparation method thereof
Through the preparation of multi-generation branched polyurethane antistatic finishing agent, the problems of durable antistatic properties and hardening of the hand in the prior art are solved, and the durable antistatic effect and softness of synthetic fiber textiles are achieved. It is suitable for amino silicone oil The finished textiles are simple and safe.
Patent Information
- Application Number
- CN202411286995.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-13
- Publication Date
- 2024-11-15
AI Technical Summary
Existing water-based polyurethane antistatic finishing agents are difficult to last for synthetic fiber textiles, and are prone to deterioration of antistatic properties after washing, and are not suitable for textiles sorted with softeners such as amino silicone oil, and the fabric feels hard after finishing.
The preparation method of multi-generation branched polyurethane antistatic finishing agent emulsion is adopted. By constructing a multi-generation branched structure, polyether, polyester and end-hydroxyhydrocarbon-based polysiloxane are introduced, and partially active capping is carried out to improve the antistatic properties and Softness, acrylic fatty alcohol is used as the capping agent to increase the degree of crosslinking, combined with a mixture of high boiling point and low boiling point diluent to control the polymer structure.
It realizes the long-lasting anti-static effect of synthetic fiber textiles, gives the fabric good elasticity and smoothness, solves the problem of hardening of the fabric's hand and degradation of anti-static properties. It is suitable for textiles sorted with amino silicone oil, and has a simple process and energy-saving , safe and environmentally friendly.
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of antistatic finishing agent preparation, and in particular to a multi-generation branched polyurethane antistatic finishing agent emulsion and a preparation method thereof. Background Art
[0002] In the field of antistatic for synthetic fiber textiles, although there are reports on the preparation method of waterborne polyurethane antistatic finishing agent emulsion, the research is relatively early. The waterborne polyurethane antistatic finishing agent products based on the existing technology are usually polyether polyester block type waterborne polyurethane, and the antistatic property of the synthetic fiber after finishing is difficult to last; the closed waterborne polyether type polyurethane, the synthetic fiber after finishing is easy to change color, feel hard, and the finishing agent is not convenient to store; or the former two are respectively compounded with cationic quaternary ammonium salts, and the initial antistatic property of the synthetic fiber after finishing is good, but the antistatic performance is seriously reduced after washing; and the three types of waterborne polyurethane antistatic finishing agents are not suitable for synthetic fiber textiles after finishing with softeners such as amino silicone oil.
[0003] At present, the preparation methods of durable waterborne polyurethane antistatic finishing agents include the following:
[0004] 1. A method for preparing a polyether polyester block type waterborne polyurethane antistatic finishing agent, wherein the raw materials include polymerization monomers, end-capping agents, auxiliary agents and water, wherein the polymerization monomers include polyester diols, polyethylene glycol, terminal hydroxyl hydrocarbon polysiloxanes, and diol chain extenders; the end-capping agents are monofunctional and trifunctional compounds; and the auxiliary agents include polymerization catalysts and diluents.
[0005] For example, patent application CN109403044B discloses a method for preparing a polyester polyether type water-based polyurethane hydrophilic antistatic finishing agent, in which the polymerization monomers in the raw materials are toluene diisocyanate, poly(hexanediol phthalate), terminal hydroxyl polydimethylsiloxane, polyoxyethylene ethylpropylene glycol methyl ether, and N-methyldiethanolamine; the end-capping agents include methyl ethyl ketone oxime and glycerol; and the auxiliary agents include polymerization catalysts such as stannous octoate, glacial acetic acid, and N-ethylpyrrolidone. The polyester polyether type waterborne polyurethane antistatic finishing agent prepared by the method has a common segment structure with polyester fibers, and can be melted and intercalated with the amorphous regions of polyester fibers during high-temperature baking. However, its structural design molecular weight is relatively small, and the polyether segment accounts for more than 60% of the polymer long chain ratio, and is extremely hydrophilic. In addition, the scheme uses a large proportion of triols as end-capping agents, which makes it difficult to increase the molecular weight of the polymer and further cross-link after the oxime end-capping agent is unblocked. The finishing agent is difficult to remain fixed on synthetic fiber textiles after multiple washings, and cannot form a lasting antistatic effect.
[0006] 2. A method for preparing a closed water-based polyether polyurethane, the raw materials of which include polymerizable monomers, end-capping monomers, auxiliary agents and water, wherein: the polymerizable monomers include polyethylene glycol, dibasic acid, and isocyanate; the end-capping monomer is sodium bisulfite; and the auxiliary agents are diluents and compounding auxiliary agents.
[0007] For example, the preparation method of the blocked waterborne polyurethane compound durable antistatic finishing agent disclosed in "Development of blocked waterborne polyurethane antistatic agent for polyester and antistatic finishing" (Journal of Hunan Institute of Engineering (Natural Science Edition) No. 4, 2006) by Liu Yongjun, Peng Jian, Zhan Shixiong and others, the polymerizing monomers in the raw materials are 2,4-toluene diisocyanate, polyethylene glycol 400, and oxalic acid; the blocking monomer is sodium hydrogen sulfite; the auxiliary agent includes the diluent acetone; the compound auxiliary agent includes the surfactant alkyl polyoxyethylene ether alcohol (JFC), the crosslinking agent 3-(methacryloyloxy)propyl trimethoxysilane (KH570) and hydroxymethyl cellulose. Compared with the non-durable waterborne polyurethane antistatic finishing agent, the blocked waterborne polyurethane hydrophilic finishing agent prepared by this method takes into account the possibility of the waterborne polyurethane antistatic finishing agent forming a film on the surface of the finished fabric. However, in the compounding test, the cross-linking agent hydroxymethyl cellulose with a weight ratio of more than 16% and the weight ratio of more than 66% of 3-(methacryloyloxy)propyltrimethoxysilane to the water-based polyurethane antistatic finishing agent are used to strengthen the cross-linking film-forming property of the polymer, which will inevitably cause the fabric to feel harder due to the introduction of a large amount of hydroxymethyl cellulose, a monomer with a high glass transition temperature and excellent planar structure; a large amount of sodium sulfite is unblocked during high-temperature thermosetting, resulting in a violent reaction between isocyanate and water, hydroxymethyl cellulose hydroxyl group, etc. to generate urea groups, resulting in obvious yellowing of the finished fabric and a decrease in whiteness.
[0008] 3. A method for preparing a water-based polyurethane and cationic quaternary ammonium salt compound antistatic finishing agent, wherein the raw materials include polymerization monomers, chain extension monomers, auxiliary agents, compounding monomers and water, wherein: the polymerization monomers are polyether diols and isocyanates; the chain extension monomers are small molecule diols; the auxiliary agents include diluents and neutralizers; and the compounding monomers are fatty amine polyoxyethylene ether quaternary ammonium salt derivatives.
[0009] For example, the preparation method of water-based polyurethane antistatic finishing agent disclosed in "Development of Water-based Polyurethane Antistatic Agent" (China Adhesives, Vol. 16, No. 3, 2007) written by Bao Junjie, Wang Lechun, Xu Gewen, etc., the polymerization monomers in its raw materials are polyethylene glycol 210 and 2,4-toluene diisocyanate; the chain extension monomers are 1,4-butanediol and dimethylol propionic acid; the auxiliary agents include diluent acetone and neutralizer triethylamine; the compounding monomer is octadecyl diethanolamine octyl quaternary ammonium salt. The water-based polyurethane antistatic finishing agent prepared by this method is compounded with a long-chain alkyl quaternary ammonium salt to perform antistatic finishing on textiles. It uses the negative charge of anionic polyurethane and quaternary ammonium salt cations to form ionic bonds on the fabric surface, which can increase the durability of the antistatic finishing. However, after the nitrogen cations in the quaternary ammonium salt derivatives of fatty amine polyoxyethylene ether combine with the negatively charged carboxyl groups in the polyurethane molecules, the antistatic properties originally provided by the positive charge are bound to be greatly weakened. As described in the article, only when the amount of quaternary ammonium salt is sufficient can the finished fabric have good antistatic properties. Moreover, the long hydrophobic alkyl chains introduced by the quaternary ammonium salt derivatives will further reduce the antistatic properties of the textiles finished with this technology. In addition, when finishing the fabric, cationic quaternary ammonium salts need to be compounded with anionic water-based polyurethanes, which are prone to form gels or precipitation and are difficult to apply on a large scale. Summary of the invention
[0010] The purpose of the present invention is to overcome the above problems existing in the prior art and to provide a multi-generation branched polyurethane antistatic finishing agent emulsion and a preparation method thereof.
[0011] In order to achieve the above object, the present invention provides a method for preparing a multi-generation branched polyurethane antistatic finishing agent emulsion, which comprises the following steps:
[0012] (1) Raw material preparation: the raw materials include polymerizable monomers, branching monomers, end-capping agents, auxiliary agents and water; wherein the polymerizable monomers include diisocyanate, polyester diol, polyethylene glycol and hydroxyl-terminated polysiloxane, and the auxiliary agents include polymerization catalysts, olefin inhibitors and diluents;
[0013] The diisocyanate is toluene diisocyanate, isophorone diisocyanate or diphenylmethane diisocyanate;
[0014] The molecular weight of the polyester diol is 2000-4000, and the polyester diol is a polyester diol of phthalic anhydride and 1,6-hexanediol or a polyester diol of dimethyl terephthalate and ethylene glycol;
[0015] The molecular weight of polyethylene glycol is 1000-8000;
[0016] The terminal hydroxyl polysiloxane is a terminal hydroxyl polydimethylsiloxane having a molecular weight of 2000 to 6000;
[0017] The branching monomer is glycerol or trimethylolpropane;
[0018] The end-capping agent is hydroxyethyl methacrylate, hydroxyethyl acrylate, hydroxypropyl acrylate or hydroxybutyl methacrylate;
[0019] The polymerization catalyst is stannous octoate, dibutyltin dilaurate or triethylamine;
[0020] The olefin polymerization inhibitor is p-hydroxyanisole, hydroquinone or 2,5-di-tert-butylhydroquinone;
[0021] The diluent is a mixture of a high boiling point diluent and a low boiling point diluent, wherein the high boiling point diluent is propylene glycol methyl ether acetate or dipropylene glycol dimethyl ether, and the low boiling point diluent is methyl ethyl ketone or acetone;
[0022] The molar fractions of the components are: diisocyanate 18, polyethylene glycol 3.5-6.5, polyester diol 1.5-3.5, and the sum of the molar fractions of terminal hydroxyl polysiloxane, polyethylene glycol and polyester diol is 9, branching monomer 4, and end-capping agent 2-5;
[0023] The amount of the polymerization catalyst used is 0.06 to 0.09 wt% of the total weight of the polymerization monomers;
[0024] The amount of olefin polymerization inhibitor used is 0.01 to 0.05 wt% of the total weight of the polymerization monomers;
[0025] The total amount of the diluent is 150-200 wt% of the total weight of the polymerized monomers, and the weight ratio of the high boiling point diluent to the low boiling point diluent is 1:2-7;
[0026] (2) a step of pre-treating polyethylene glycol, polyester diol and hydroxyl-terminated polysiloxane, wherein the polyethylene glycol, polyester diol and hydroxyl-terminated polysiloxane are pre-treated by dehydration under vacuum and heating conditions;
[0027] (3) a prepolymerization step, in which the polyester diol after dehydration pretreatment, the polyethylene glycol after dehydration pretreatment, the terminal hydroxyl polysiloxane after dehydration pretreatment, part of the diluent and the diisocyanate are subjected to a prepolymerization reaction under the catalytic action of part of the polymerization catalyst to obtain a multi-generation branched polyurethane antistatic finishing agent prepolymer;
[0028] (4) a first-generation branching step, in which the multi-generation branched polyurethane antistatic finishing agent prepolymer is subjected to a branching reaction with a portion of a branching monomer and a portion of a diluent to obtain a multi-generation branched polyurethane antistatic finishing agent branched intermediate;
[0029] (5) a second generation branching step, in which the remaining branching monomer, a portion of the diluent, the remaining polymerization catalyst and the multi-generation branched polyurethane antistatic finishing agent intermediate are reacted to obtain the multi-generation branched polyurethane antistatic finishing agent intermediate;
[0030] (6) an end-capping step, in which the multi-generation branched polyurethane antistatic finishing agent intermediate is reacted with an end-capping agent, an olefin polymerization inhibitor, and a remaining diluent to obtain a multi-generation branched polyurethane antistatic finishing agent polymer;
[0031] (7) an emulsification step, in which the multi-generation branched polyurethane antistatic finishing agent polymer and water are mixed and emulsified to prepare a multi-generation branched polyurethane antistatic finishing agent intermediate emulsion.
[0032] (8) Removal of solvent: removing part of the diluent from the multi-generation branched polyurethane antistatic finishing agent emulsion product under vacuum and heating conditions to obtain a multi-generation branched polyurethane antistatic finishing agent emulsion with a solid content of 8-14wt%.
[0033] Preferably, the specific process of step (2) includes:
[0034] (2.1) adding polyethylene glycol, polyester diol and hydroxyl-terminated polysiloxane into a reactor;
[0035] (2.2) Heat the material to 110-120°C and treat it under a vacuum condition of -0.100 to -0.098 MPa for 90-150 min.
[0036] Preferably, the specific process of step (3) includes:
[0037] (3.1) Cooling the material obtained in step (2) to 70-75°C;
[0038] (3.2) Add diisocyanate and keep stirring, control the temperature of the reaction system to 75-85°C, and keep stirring for 30-50 minutes;
[0039] (3.3) maintaining the temperature of the reaction system at 75-85° C., adding a total amount of 60-80 wt % of a polymerization catalyst at a uniform rate within 10-15 min;
[0040] (3.4) raising the temperature of the reaction system to 80-90° C. and maintaining the temperature for 100-120 min. During the temperature maintenance period, a diluent in an amount of 10-20 wt % is added to prepare a multi-generation branched polyurethane antistatic finishing agent prepolymer.
[0041] Preferably, the specific process of step (4) includes:
[0042] (4.1) Cooling the reaction system obtained in step (3) to 75-85°C;
[0043] (4.2) Add 75 wt% of branched monomers and 40-70 wt% of diluents and maintain stirring, control the temperature of the reaction system to 75-90° C., maintain stirring for 90-120 min, and obtain a multi-generation branched polyurethane antistatic finishing agent branched intermediate.
[0044] Preferably, the specific process of step (5) includes:
[0045] (5.1) maintaining the reaction system obtained in step (4) at 75-85° C.;
[0046] (5.2) Add the remaining branched monomer, the remaining polymerization catalyst, and a total amount of 10 to 40 wt% of a diluent and maintain stirring, control the temperature of the reaction system to 75 to 90° C., maintain stirring for 90 to 120 minutes, and obtain a multi-generation branched polyurethane antistatic finishing agent intermediate.
[0047] Preferably, the specific process of step (6) includes:
[0048] (6.1) Add the remaining diluent to the reaction system obtained in step (5) and cool the system to 60-65° C.;
[0049] (6.2) Add the end-capping agent, maintain the system temperature at 60-65°C, and continue stirring the reaction for 30-60 minutes;
[0050] (6.3) Add olefin polymerization inhibitor, control the temperature of the reaction system to 60-75°C, maintain stirring reaction for 15-60 minutes, and obtain multi-generation branched polyurethane antistatic finishing agent polymer.
[0051] Preferably, the specific process of step (7) includes:
[0052] (7.1) The reaction system obtained in step (6) is stirred and cooled to 50-60° C., and the material is pumped into an emulsifier;
[0053] (7.2) The stirring rate of the emulsifier is adjusted to 1000-1200 r / min, and water at 20-35° C. is added to the emulsifier within 20-30 min, and the system temperature is maintained at 40-60° C. and stirred for 30-60 min to obtain a multi-generation branched polyurethane antistatic finishing agent intermediate emulsion.
[0054] Preferably, the specific process of step (8) includes:
[0055] (8.1) maintaining the emulsified system obtained in step (7) at 50-60° C.;
[0056] (8.2) The stirring rate of the emulsifier is adjusted to 300-500 r / min, the vacuum system and the condensing heat exchanger are opened, part of the diluent is recovered, the vacuum system is closed and the system is cooled to obtain a multi-generation branched polyurethane antistatic finishing agent emulsion with a solid content of 8-14 wt%.
[0057] Preferably, the water is soft water with a total hardness of less than 50 ppm CaO.
[0058] The second aspect of the present invention provides a multi-generation branched polyurethane antistatic finishing agent emulsion prepared according to the method described above.
[0059] The invention constructs a multi-generation branched structure in the multi-generation branched polyurethane antistatic finishing agent molecule, introduces polyether, polyester and an appropriate amount of terminal hydroxyl polysiloxane into the branched chain, and performs partial active end-capping, thereby specifically improving the durable antistatic property of synthetic fibers treated with softening finishing agents such as amino silicone oil, and can give the synthetic fibers excellent elasticity and smoothness, and has good applicability for antistatic finishing of synthetic fibers; has good market prospects; the product is energy-saving and consumption-reducing, has low usage, is safe and environmentally friendly, and is easy to use.
[0060] Compared with the prior art, the present invention has the following advantages and characteristics:
[0061] 1. The multi-generation branched polyurethane antistatic finishing agent provided by the present invention has a simple polymer structure control and good functional segment adjustability. The multi-branched structure can make the hydrophilic polyether segment easier to migrate to the surface of the synthetic fiber textile during high-temperature treatment, thereby increasing the specific surface area of the polymer segment for absorbing moisture in the air. It has low dependence on the amount of polyether used and can give the fabric good antistatic properties.
[0062] 2. In the preparation method of the multi-generation branched polyurethane antistatic finishing agent provided by the present invention, acrylic fatty alcohol is preferably used as a partial end-capping agent and distributed at the end of the polymer branch chain. When treated at high temperature, the olefins distributed at the end of the polymer branch chain are more likely to undergo thermal polymerization reaction, thereby increasing the degree of cross-linking of the polymer; in addition, there are still some uncapped isocyanate groups at the end of the polymer, which can undergo cross-linking reaction with water, further promoting the multi-generation branched polyurethane antistatic finishing agent to form high-density chemical crosslinks on the surface of synthetic fibers, which can solve the problem that general end-capped polyurethanes cannot effectively form chemical crosslinks on the surface of fabrics, and endow synthetic fibers with excellent and long-lasting antistatic properties.
[0063] 3. The polysiloxane flexible chain segments introduced into the multi-generation branched polyurethane antistatic finishing agent polymer provided by the present invention account for a relatively high proportion, which can solve the problem of hardened feel caused by the increase in polymer cross-linking density or the use of externally added cross-linking agents (such as hydroxymethyl cellulose, etc.) with good planarity and high glass transition temperature; at the same time, it can effectively reduce the surface tension of the multi-generation branched polyurethane antistatic finishing agent, making it easier to adsorb on the surface of synthetic fibers, and during the high-temperature treatment process, it undergoes molecular entanglement and rearrangement with the original hydrophobic amino silicone oil on the fiber surface, reducing the continuous distribution of the hydrophobic amino silicone oil, giving the finished fabric excellent antistatic properties while also giving the fabric excellent elasticity and smoothness.
[0064] 4. The step-by-step branching reaction process and the design of mixing high-boiling point and low-boiling point solvents in the method of the present invention can conveniently and effectively control the multi-generation branching structure of the polymer, ensuring that the product has a reliable branching and cross-linking structure and the mobility of the polyether chain segments.
[0065] 5. The preparation method of the multi-generation branched polyurethane antistatic finishing agent provided by the present invention is easy to implement and control, has a smooth process, and has no special requirements for production equipment; the product does not contain an emulsifier, has good emulsion stability, low solvent content, is safe and environmentally friendly, and is easy to use; the product has good application performance and a wide range of uses. DETAILED DESCRIPTION
[0066] The specific embodiments of the present invention are described in detail below. It should be understood that the specific embodiments described herein are only used to illustrate and explain the present invention, and are not used to limit the present invention.
[0067] The endpoints and any values of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values should be understood to include values close to these ranges or values. For numerical ranges, the endpoint values of each range, the endpoint values of each range and the individual point values, and the individual point values can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.
[0068] In one aspect, the present invention provides a method for preparing a multi-generation branched polyurethane antistatic finishing agent emulsion, the method comprising the following steps:
[0069] (1) Raw material preparation: the raw materials include polymerizable monomers, branching monomers, end-capping agents, auxiliary agents and water; wherein the polymerizable monomers include diisocyanate, polyester diol, polyethylene glycol and hydroxyl-terminated polysiloxane, and the auxiliary agents include polymerization catalysts, olefin inhibitors and diluents;
[0070] The diisocyanate is toluene diisocyanate, isophorone diisocyanate or diphenylmethane diisocyanate;
[0071] The molecular weight of the polyester diol is 2000-4000, and the polyester diol is a polyester diol of phthalic anhydride and 1,6-hexanediol or a polyester diol of dimethyl terephthalate and ethylene glycol;
[0072] The molecular weight of polyethylene glycol is 1000-8000;
[0073] The terminal hydroxyl polysiloxane is a terminal hydroxyl polydimethylsiloxane having a molecular weight of 2000 to 6000;
[0074] The branching monomer is glycerol or trimethylolpropane;
[0075] The end-capping agent is hydroxyethyl methacrylate, hydroxyethyl acrylate, hydroxypropyl acrylate or hydroxybutyl methacrylate;
[0076] The polymerization catalyst is stannous octoate, dibutyltin dilaurate or triethylamine;
[0077] The olefin polymerization inhibitor is p-hydroxyanisole, hydroquinone or 2,5-di-tert-butylhydroquinone;
[0078] The diluent is a mixture of a high boiling point diluent and a low boiling point diluent, wherein the high boiling point diluent is propylene glycol methyl ether acetate or dipropylene glycol dimethyl ether, and the low boiling point diluent is methyl ethyl ketone or acetone;
[0079] The molar fractions of the components are: diisocyanate 18, polyethylene glycol 3.5-6.5, polyester diol 1.5-3.5, and the sum of the molar fractions of terminal hydroxyl polysiloxane, polyethylene glycol and polyester diol is 9, branching monomer 4, and end-capping agent 2-5;
[0080] The amount of the polymerization catalyst used is 0.06 to 0.09 wt% of the total weight of the polymerization monomers;
[0081] The amount of olefin polymerization inhibitor used is 0.01 to 0.05 wt% of the total weight of the polymerization monomers;
[0082] The total amount of the diluent is 150-200 wt% of the total weight of the polymerized monomers, and the weight ratio of the high boiling point diluent to the low boiling point diluent is 1:2-7;
[0083] (2) a step of pre-treating polyethylene glycol, polyester diol and hydroxyl-terminated polysiloxane, wherein the polyethylene glycol, polyester diol and hydroxyl-terminated polysiloxane are pre-treated by dehydration under vacuum and heating conditions;
[0084] (3) a prepolymerization step, in which the polyester diol after dehydration pretreatment, the polyethylene glycol after dehydration pretreatment, the terminal hydroxyl polysiloxane after dehydration pretreatment, part of the diluent and the diisocyanate are subjected to a prepolymerization reaction under the catalytic action of part of the polymerization catalyst to obtain a multi-generation branched polyurethane antistatic finishing agent prepolymer;
[0085] (4) a first-generation branching step, in which the multi-generation branched polyurethane antistatic finishing agent prepolymer is subjected to a branching reaction with a portion of a branching monomer and a portion of a diluent to obtain a multi-generation branched polyurethane antistatic finishing agent branched intermediate;
[0086] (5) a second generation branching step, in which the remaining branching monomer, a portion of the diluent, the remaining polymerization catalyst and the multi-generation branched polyurethane antistatic finishing agent intermediate are reacted to obtain the multi-generation branched polyurethane antistatic finishing agent intermediate;
[0087] (6) an end-capping step, in which the multi-generation branched polyurethane antistatic finishing agent intermediate is reacted with an end-capping agent, an olefin polymerization inhibitor, and a remaining diluent to obtain a multi-generation branched polyurethane antistatic finishing agent polymer;
[0088] (7) an emulsification step, in which the multi-generation branched polyurethane antistatic finishing agent polymer and water are mixed and emulsified to prepare a multi-generation branched polyurethane antistatic finishing agent intermediate emulsion.
[0089] (8) Removal of solvent: removing part of the diluent from the multi-generation branched polyurethane antistatic finishing agent emulsion product under vacuum and heating conditions to obtain a multi-generation branched polyurethane antistatic finishing agent emulsion with a solid content of 8-14%.
[0090] In the method of the present invention, the terminal hydroxyl polydimethylsiloxane refers to hydroxyl silicone oil. For example, hydroxyl silicone oil with the brand name UC-3667 can be used.
[0091] According to some specific embodiments of the present invention, based on the molar fraction of diisocyanate being 18, the molar fraction of polyethylene glycol can be 3.5, 4, 5, 6 or 6.5.
[0092] In a preferred embodiment, the specific process of step (2) includes:
[0093] (2.1) adding polyethylene glycol, polyester diol and hydroxyl-terminated polysiloxane into a reactor;
[0094] (2.2) Heat the material to 110-120°C and treat it under a vacuum condition of -0.100 to -0.098 MPa for 90-150 min.
[0095] In a preferred embodiment, the specific process of step (3) includes:
[0096] (3.1) Cooling the material obtained in step (2) to 70-75°C;
[0097] (3.2) Add diisocyanate and keep stirring, control the temperature of the reaction system to 75-85°C, and keep stirring for 30-50 minutes;
[0098] (3.3) maintaining the temperature of the reaction system at 75-85° C., adding a total amount of 60-80 wt % of a polymerization catalyst at a uniform rate within 10-15 min;
[0099] (3.4) raising the temperature of the reaction system to 80-90° C. and maintaining the temperature for 100-120 min. During the temperature maintenance period, a diluent in an amount of 10-20 wt % is added to prepare a multi-generation branched polyurethane antistatic finishing agent prepolymer.
[0100] In the method of the present invention, in step (3.4), the diluent can be added in multiple times during the heat preservation reaction to control the viscosity of the reaction system.
[0101] In a preferred embodiment, the specific process of step (4) includes:
[0102] (4.1) Cooling the reaction system obtained in step (3) to 75-85°C;
[0103] (4.2) Add 75 wt% of branched monomers and 40-70 wt% of diluents and maintain stirring, control the temperature of the reaction system to 75-90° C., maintain stirring for 90-120 min, and obtain a multi-generation branched polyurethane antistatic finishing agent branched intermediate.
[0104] In a preferred embodiment, the specific process of step (5) includes:
[0105] (5.1) maintaining the reaction system obtained in step (4) at 75-85° C.;
[0106] (5.2) Add the remaining branched monomer, the remaining polymerization catalyst, and a total amount of 10 to 40 wt% of a diluent and maintain stirring, control the temperature of the reaction system to 75 to 90° C., maintain stirring for 90 to 120 minutes, and obtain a multi-generation branched polyurethane antistatic finishing agent intermediate.
[0107] In a preferred embodiment, the specific process of step (6) includes:
[0108] (6.1) Add the remaining diluent to the reaction system obtained in step (5) and cool the system to 60-65° C.;
[0109] (6.2) Add the end-capping agent, maintain the system temperature at 60-65°C, and continue stirring the reaction for 30-60 minutes;
[0110] (6.3) Add olefin polymerization inhibitor, control the temperature of the reaction system to 60-75°C, maintain stirring reaction for 15-60 minutes, and obtain multi-generation branched polyurethane antistatic finishing agent polymer.
[0111] In a preferred embodiment, the specific process of step (7) includes:
[0112] (7.1) The reaction system obtained in step (6) is stirred and cooled to 50-60° C., and the material is pumped into an emulsifier;
[0113] (7.2) Adjust the stirring rate of the emulsifier to 1000-1200 r / min, add water at 20-35° C. into the emulsifier within 20-30 min, maintain the system temperature at 40-60° C., and continue stirring for 30-60 min to obtain a multi-generation branched polyurethane antistatic finishing agent intermediate emulsion.
[0114] In a preferred embodiment, the specific process of step (8) includes:
[0115] (8.1) maintaining the emulsified system obtained in step (7) at 50-60° C.;
[0116] (8.2) The stirring rate of the emulsifier is adjusted to 300-500 r / min, the vacuum system and the condensing heat exchanger are opened, part of the diluent is recovered, the vacuum system is closed and the system is cooled to obtain a multi-generation branched polyurethane antistatic finishing agent emulsion with a solid content of 8-14 wt%.
[0117] In the method of the present invention, in step (8), the emulsified system obtained in step (7) is heated to remove part of the diluent, so that the solid content of the obtained multi-generation branched polyurethane antistatic finishing agent emulsion can be 8-14wt%.
[0118] In a preferred embodiment, the water is soft water with a total hardness of less than 50 ppm CaO (ie, 5 degrees).
[0119] In the method of the present invention, there is no special requirement for the amount of water used, as long as the solid content of the finally prepared emulsion is 8-14 wt%.
[0120] The second aspect of the present invention provides a multi-generation branched polyurethane antistatic finishing agent emulsion prepared according to the method described above.
[0121] The multi-generation branched polyurethane antistatic finishing agent emulsion product prepared by the method described in the present invention will not cause the synthetic fiber to have a reduced feel or a change in color. Its unique branched structure can reduce the amount of finishing agent used and give the finished fabric a good smooth feeling and lasting antistatic performance. It is particularly suitable for the lasting antistatic finishing of synthetic fiber textiles with a high specific surface area after finishing with softeners such as amino silicone oil, and is an energy-saving, efficient and feasible solution. The product must be sealed and stored in a cool and dry place.
[0122] The present invention will be described in detail below through examples, but the protection scope of the present invention is not limited thereto.
[0123] Example 1
[0124] The preparation of multi-generation branched polyurethane antistatic finishing agent emulsion S1 comprises the following steps:
[0125] (1) Raw material preparation: the raw materials include polymerizable monomers, branching monomers, end-capping agents, auxiliary agents and water; wherein the polymerizable monomers include diisocyanate, polyester diol, polyethylene glycol and hydroxyl-terminated polysiloxane, and the auxiliary agents include polymerization catalysts, olefin polymerization inhibitors and diluents (composed of high-boiling-point diluents and low-boiling-point diluents);
[0126] Diisocyanate: isophorone diisocyanate 18.0 mol (4001.0 g);
[0127] Polyester diol: 3.3 mol (6600.0 g) of polyester diol of dimethyl terephthalate and ethylene glycol with a molecular weight of 2000; wherein, it is prepared by dimethyl terephthalate and ethylene glycol in a molar ratio of 10:11;
[0128] Polyethylene glycol: molecular weight 4000, 4.5 mol (18000.0 g);
[0129] Hydroxyl-terminated polysiloxane: 1.2 mol (6000.0 g) of hydroxyl-terminated polydimethylsiloxane with a molecular weight of 5000;
[0130] Branching monomer: trimethylolpropane 4.0 mol (536.7 g);
[0131] Capping agent: 4.0 mol (464.5 g) of hydroxyethyl acrylate;
[0132] Polymerization catalyst: dibutyltin dilaurate (28.5 g);
[0133] Olefin polymerization inhibitor: p-hydroxyanisole (7.1 g);
[0134] High boiling point diluent: propylene glycol methyl ether acetate (20293.3g);
[0135] Low boiling point diluent: methyl ethyl ketone (47350.9 g);
[0136] Water: Soft water with a total hardness of less than 50 ppm CaO (266624.9 g);
[0137] (2) a step of pre-treating polyethylene glycol, polyester diol and hydroxyl-terminated polysiloxane, wherein the polyethylene glycol, polyester diol and hydroxyl-terminated polysiloxane are pre-treated by dehydration under vacuum and heating conditions; specifically:
[0138] (2.1) adding polyethylene glycol, polyester diol and hydroxyl-terminated polysiloxane into a reactor;
[0139] (2.2) heating the material to 115-120°C and treating it under a vacuum degree of -0.100 to -0.098 MPa for 120 min;
[0140] (3) a prepolymerization step, in which the polyester diol after dehydration pretreatment, the polyethylene glycol after dehydration pretreatment, the terminal hydroxyl polysiloxane after dehydration pretreatment, part of the diluent and the diisocyanate are subjected to a prepolymerization reaction under the catalytic action of part of the polymerization catalyst to obtain a multi-generation branched polyurethane antistatic finishing agent prepolymer; specifically:
[0141] (3.1) Cooling the material obtained in step (2.2) to 75°C;
[0142] (3.2) Add diisocyanate and keep stirring, control the temperature of the reaction system to 75°C, and keep stirring for 45 minutes;
[0143] (3.3) maintaining the temperature of the reaction system at 75°C, adding 70 wt% of the polymerization catalyst at a uniform rate within 15 minutes;
[0144] (3.4) raising and controlling the temperature of the reaction system to 85° C., maintaining the temperature for 100 min, and adding a diluent in an amount of 10 wt % in a timely manner in multiple times to control the viscosity of the reaction system, thereby preparing a multi-generation branched polyurethane antistatic finishing agent prepolymer;
[0145] (4) a first generation branching step, wherein the multi-generation branched polyurethane antistatic finishing agent prepolymer is subjected to a branching reaction with a total amount of 75 wt% of a branching monomer and a portion of a diluent to obtain a multi-generation branched polyurethane antistatic finishing agent branched intermediate; specifically:
[0146] (4.1) Cooling the reaction system of step (3.4) to 80°C;
[0147] (4.2) adding 75 wt% of branched monomers and 50 wt% of diluents and maintaining stirring, controlling the temperature of the reaction system to 85° C., maintaining stirring and reacting for 100 min, and obtaining a multi-generation branched polyurethane antistatic finishing agent branched intermediate;
[0148] (5) A second generation branching step, in which the remaining branching monomer, part of the diluent, the remaining polymerization catalyst and the multi-generation branched polyurethane antistatic finishing agent branched intermediate are reacted to obtain a multi-generation branched polyurethane antistatic finishing agent intermediate; specifically:
[0149] (5.1) maintaining the reaction system of step (4.2) at 83-85°C;
[0150] (5.2) adding the remaining branched monomer, the remaining polymerization catalyst, and a total amount of 30 wt% of a diluent and maintaining stirring, controlling the temperature of the reaction system to 83-85° C., maintaining stirring and reacting for 120 min, and obtaining a multi-generation branched polyurethane antistatic finishing agent intermediate;
[0151] (6) an end-capping step, in which the multi-generation branched polyurethane antistatic finishing agent intermediate is reacted with an end-capping agent, an olefin polymerization inhibitor, and a remaining diluent to obtain a multi-generation branched polyurethane antistatic finishing agent polymer; specifically:
[0152] (6.1) Add the remaining diluent to the reaction system of step (5.2) and cool the system to 60-65°C;
[0153] (6.2) Add the end-capping agent, maintain the system temperature at 62-64°C, and continue stirring the reaction for 60 minutes;
[0154] (6.3) adding olefin polymerization inhibitor at one time, controlling the temperature of the reaction system to 65° C., maintaining stirring and reacting for 20 minutes, and obtaining a multi-generation branched polyurethane antistatic finishing agent polymer;
[0155] (7) an emulsification step, in which the multi-generation branched polyurethane antistatic finishing agent polymer and water are mixed and emulsified to prepare a multi-generation branched polyurethane antistatic finishing agent intermediate emulsion; specifically:
[0156] (7.1) The reaction system of step (6.3) is stirred and cooled to 50-60°C, and the material is pumped into an emulsifier;
[0157] (7.2) Increase the stirring rate of the emulsifier to 1200 r / min, add water at 20-35°C into the emulsifier within 20 minutes, maintain the system temperature at 50°C, and stir for 60 minutes to obtain a multi-generation branched polyurethane antistatic finishing agent intermediate emulsion.
[0158] (8) Removal of solvent: removing part of the diluent from the multi-generation branched polyurethane antistatic finishing agent emulsion product under vacuum and heating conditions to obtain a multi-generation branched polyurethane antistatic finishing agent emulsion product with a solid content of 8-14%; specifically:
[0159] (8.1) Maintaining the emulsified system in step (7.2) at 55°C;
[0160] (8.2) The emulsifier maintains medium-low speed stirring (stirring rate is 400r / min), opens the vacuum system and the condensing heat exchanger, recovers part of the diluent, closes the vacuum system and cools the system to obtain a multi-generation branched polyurethane antistatic finishing agent emulsion product with a solid content of 8-14wt%.
[0161] The multi-generation branched polyurethane antistatic finishing agent emulsion product prepared in this embodiment can be used for durable antistatic finishing of synthetic fiber textiles such as polyester, vinylon, nylon and spandex after softening with amino silicone oil or the like. The product is a self-emulsifying aqueous polymer emulsion, which can significantly improve the hydrophilicity of synthetic fiber textile products. For synthetic fiber textiles with large specific surface area (friction charging voltage greater than 10,000V), after impregnation finishing with commercially available products, the friction charging voltage can be reduced to 7,000V after washing 5 times; after impregnation finishing with this product, the friction charging voltage can be reduced to below 3,000V after washing 5 times. In addition, this product has no effect on the feel of large specific surface area polyester long-pile blankets, and its fluffiness is tested by Fast style instrument (compressibility expression), and the compressibility of the fabric is increased by 5% after finishing, which has no adverse effect on the feel of the fabric; it has good market prospects; the product is safe, environmentally friendly and easy to use.
[0162] Example 2
[0163] The preparation of multi-generation branched polyurethane antistatic finishing agent emulsion S2 comprises the following steps:
[0164] (1) Raw material preparation: the raw materials include polymerizable monomers, branching monomers, end-capping agents, auxiliary agents and water; wherein the polymerizable monomers include diisocyanate, polyester diol, polyethylene glycol and hydroxyl-terminated polysiloxane, and the auxiliary agents include polymerization catalysts, olefin polymerization inhibitors and diluents (composed of high-boiling-point diluents and low-boiling-point diluents);
[0165] Diisocyanate: 2,4-toluene diisocyanate 18.0 mol (3134.9 g);
[0166] Polyester diol: 3.0 mol (6000.0 g) of polyester diol of dimethyl terephthalate and ethylene glycol with a molecular weight of 2000; wherein, it is prepared by dimethyl terephthalate and ethylene glycol in a molar ratio of 10:11;
[0167] Polyethylene glycol: molecular weight 6000, 4.0 mol (24000.0 g);
[0168] Hydroxyl-terminated polysiloxane: 2.0 mol (4000.0 g) of hydroxyl-terminated polydimethylsiloxane with a molecular weight of 2000;
[0169] Branching monomer: trimethylolpropane 4.0 mol (536.7 g);
[0170] Capping agent: hydroxypropyl acrylate 2.0 mol (260.3 g);
[0171] Polymerization catalyst: stannous octoate (32.3 g);
[0172] Olefin polymerization inhibitor: 2,5-di-tert-butylhydroquinone (17.1 g);
[0173] High boiling point diluent: propylene glycol methyl ether acetate (12896.8g);
[0174] Low boiling point diluent: acetone (51587.30 g);
[0175] Water: Soft water with a total hardness of less than 50 ppm CaO (214201.1 g);
[0176] (2) a step of pre-treating polyethylene glycol, polyester diol and hydroxyl-terminated polysiloxane, wherein the polyethylene glycol, polyester diol and hydroxyl-terminated polysiloxane are pre-treated by dehydration under vacuum and heating conditions; specifically:
[0177] (2.1) adding polyethylene glycol, polyester diol and hydroxyl-terminated polysiloxane into a reactor;
[0178] (2.2) heating the material to 120°C and treating it under a vacuum degree of -0.100 to -0.098 MPa for 150 min;
[0179] (3) a prepolymerization step, in which the polyester diol after dehydration pretreatment, the polyethylene glycol after dehydration pretreatment, the terminal hydroxyl polysiloxane after dehydration pretreatment, the diluent and the diisocyanate are subjected to a prepolymerization reaction under the catalytic action of a partial polymerization catalyst to obtain a multi-generation branched polyurethane antistatic finishing agent prepolymer; specifically:
[0180] (3.1) Cooling the material in step (2.2) to 70-75°C;
[0181] (3.2) Add diisocyanate and keep stirring, control the temperature of the reaction system to 85°C, and keep stirring for 30 minutes;
[0182] (3.3) maintaining the temperature of the reaction system at 85°C, adding 65 wt% of the polymerization catalyst at a uniform rate within 10 to 15 minutes;
[0183] (3.4) raising and controlling the temperature of the reaction system to 85° C., maintaining the temperature for 120 min, and adding a diluent in an amount of 20 wt % in multiple times during the reaction to control the viscosity of the reaction system, thereby preparing a multi-generation branched polyurethane antistatic finishing agent prepolymer;
[0184] (4) a first generation branching step, in which the multi-generation branched polyurethane antistatic finishing agent prepolymer is subjected to a branching reaction with a total amount of 75 wt% of a branching monomer and a portion of a diluent to obtain a multi-generation branched polyurethane antistatic finishing agent branched intermediate; specifically:
[0185] (4.1) Cooling the reaction system of step (3.4) to 80-85°C;
[0186] (4.2) adding 75 wt% of branched monomers and 60 wt% of diluents and maintaining stirring, controlling the temperature of the reaction system to 85° C., maintaining stirring and reacting for 90 min, and obtaining a multi-generation branched polyurethane antistatic finishing agent branched intermediate;
[0187] (5) a second generation branching step, wherein the remaining branching monomer, diluent, and remaining polymerization catalyst react with the multi-generation branched polyurethane antistatic finishing agent branched intermediate to obtain a multi-generation branched polyurethane antistatic finishing agent intermediate; specifically:
[0188] (5.1) maintaining the reaction system of step (4.2) at 80-85°C;
[0189] (5.2) adding the remaining branched monomer, the remaining polymerization catalyst, and a total amount of 15 wt% of a diluent and maintaining stirring, controlling the temperature of the reaction system to 85° C., and maintaining stirring for 120 min to obtain a multi-generation branched polyurethane antistatic finishing agent intermediate;
[0190] (6) an end-capping step, in which the branched intermediate of the multi-generation branched polyurethane antistatic finishing agent is reacted with an end-capping agent, an olefin polymerization inhibitor, and a remaining diluent to obtain a multi-generation branched polyurethane antistatic finishing agent polymer; specifically:
[0191] (6.1) Add the remaining diluent to the reaction system obtained in step (5.2) and cool the system to 60-65° C.;
[0192] (6.2) Add the end-capping agent, maintain the system temperature at 62-64°C, and continue stirring the reaction for 60 minutes;
[0193] (6.3) Adding olefin polymerization inhibitor at one time, controlling the temperature of the reaction system to 60° C., maintaining stirring and reacting for 30 minutes, and obtaining a multi-generation branched polyurethane antistatic finishing agent polymer;
[0194] (7) an emulsification step, in which the multi-generation branched polyurethane antistatic finishing agent polymer and water are mixed and emulsified to prepare a multi-generation branched polyurethane antistatic finishing agent intermediate emulsion; specifically:
[0195] (7.1) The reaction system in step (6.2) is stirred and cooled to 50-60°C, and the material is pumped into an emulsifier;
[0196] (7.2) increasing the stirring rate of the emulsifier to 1100 r / min, adding water at 20 to 35° C. into the emulsifier within 20 to 30 minutes, maintaining the system temperature at 50° C., and stirring for 45 minutes to obtain a multi-generation branched polyurethane antistatic finishing agent intermediate emulsion;
[0197] (8) Removal of solvent: removing the low boiling point diluent from the multi-generation branched polyurethane antistatic finishing agent emulsion product under vacuum and heating conditions to obtain a multi-generation branched polyurethane antistatic finishing agent emulsion product with a solid content of 8-14%; specifically:
[0198] (8.1) Maintaining the emulsified system in step (7.2) at 60°C;
[0199] (8.2) The emulsifier maintains medium-low speed stirring (stirring rate is 400r / min), opens the vacuum system and the condensing heat exchanger, recovers part of the diluent, closes the vacuum system and cools the system to obtain a multi-generation branched polyurethane antistatic finishing agent emulsion product with a solid content of 8-14%.
[0200] The multi-generation branched polyurethane antistatic finishing agent emulsion product prepared in this embodiment can be used for durable antistatic finishing of synthetic fiber textiles such as polyester, vinylon, nylon and spandex after softening with amino silicone oil or the like. The product is a self-emulsifying aqueous polymer emulsion, which can significantly improve the hydrophilicity of synthetic fiber textile products. For synthetic fiber textiles with large specific surface area (friction charging voltage greater than 10000V), after impregnation finishing with commercially available products, the friction charging voltage can be reduced to 7000V after washing 5 times; after impregnation finishing with this product, the friction charging voltage can be reduced to below 2500V after washing 5 times. In addition, this product has no effect on the feel of large specific surface area polyester long-pile blankets, and its fluffiness is tested by Fast style instrument (compressibility expression), and the compressibility of the fabric is increased by 7% after finishing, which has no adverse effect on the feel of the fabric; it has good market prospects; the product is safe, environmentally friendly and easy to use.
[0201] Example 3
[0202] The preparation of multi-generation branched polyurethane antistatic finishing agent emulsion S3 comprises the following steps:
[0203] (1) Raw material preparation: the raw materials include polymerizable monomers, branching monomers, end-capping agents, auxiliary agents and water; wherein the polymerizable monomers include diisocyanate, polyester diol, polyethylene glycol and hydroxyl-terminated polysiloxane, and the auxiliary agents include polymerization catalysts, olefin polymerization inhibitors and diluents (composed of high-boiling-point diluents and low-boiling-point diluents);
[0204] Diisocyanate: Isophorone diisocyanate 18.0 mol (4001.0 g)
[0205] Polyester diol: 2.0 mol (6000.0 g) of polyester diol of phthalic anhydride with a molecular weight of 3000 and 1,6-hexanediol; wherein, the polyester diol is prepared by phthalic anhydride and 1,6-hexanediol in a molar ratio of 12:13;
[0206] Polyethylene glycol: molecular weight 2000, 6.0 mol (12000.0 g);
[0207] Hydroxyl-terminated polysiloxane: 1.0 mol (5000.0 g) of hydroxyl-terminated polydimethylsiloxane with a molecular weight of 5000;
[0208] Branching monomer: glycerol 4.0 mol (368.4 g);
[0209] Capping agent: hydroxyethyl acrylate 3.0 mol (348.4 g);
[0210] Polymerization catalyst: dibutyltin dilaurate (19.4 g);
[0211] Olefin polymerization inhibitor: p-hydroxyanisole (8.3 g);
[0212] High boiling point diluent: dipropylene glycol dimethyl ether (6236.5 g);
[0213] Low boiling point diluent: methyl ethyl ketone (35340.1 g);
[0214] Water: Soft water with a total hardness of less than 50 ppm CaO (188702.5 g);
[0215] (2) a step of pre-treating polyethylene glycol, polyester diol and hydroxyl-terminated polysiloxane, wherein the polyethylene glycol, polyester diol and hydroxyl-terminated polysiloxane are pre-treated by dehydration under vacuum and heating conditions; specifically:
[0216] (2.1) adding polyethylene glycol, polyester diol and hydroxyl-terminated polysiloxane into a reactor;
[0217] (2.2) Heat the material to 115°C and treat it at a vacuum degree of -0.100 to -0.098 MPa for 150 min.
[0218] (3) a prepolymerization step, in which the polyester diol after dehydration pretreatment, the polyethylene glycol after dehydration pretreatment, the hydroxyl polysiloxane after dehydration pretreatment, the diluent and the diisocyanate are subjected to a prepolymerization reaction under the catalytic action of a partial polymerization catalyst to obtain a multi-generation branched polyurethane antistatic finishing agent prepolymer; specifically:
[0219] (3.1) Cooling the material obtained in step (2.2) to 70-75°C;
[0220] (3.2) Add diisocyanate and keep stirring, control the temperature of the reaction system to 80°C, and keep stirring for 45 minutes;
[0221] (3.3) maintaining the temperature of the reaction system at 80°C, adding 75 wt% of the polymerization catalyst at a uniform rate within 15 minutes;
[0222] (3.4) Raise the temperature of the reaction system to 90° C. and keep the temperature to react for 100 min. During this time, add a diluent in an amount of 20 wt % in multiple times to control the viscosity of the reaction system, thereby preparing a multi-generation branched polyurethane antistatic finishing agent prepolymer.
[0223] (4) a first generation branching step, in which the multi-generation branched polyurethane antistatic finishing agent prepolymer is subjected to a branching reaction with a total amount of 75 wt% of a branching monomer and a portion of a diluent to obtain a multi-generation branched polyurethane antistatic finishing agent branched intermediate; specifically:
[0224] (4.1) Cooling the reaction system obtained in step (3.4) to 80-85°C;
[0225] (4.2) adding 75 wt% of branched monomers and 60 wt% of diluents and maintaining stirring, controlling the temperature of the reaction system to 85° C., maintaining stirring and reacting for 100 min, and obtaining a multi-generation branched polyurethane antistatic finishing agent branched intermediate;
[0226] (5) a second generation branching step, wherein the remaining branching monomer, part of the diluent, the remaining polymerization catalyst and the multi-generation branched polyurethane antistatic finishing agent branched intermediate react to obtain a multi-generation branched polyurethane antistatic finishing agent intermediate; specifically:
[0227] (5.1) maintaining the reaction system of step (4.2) at 85°C;
[0228] (5.2) adding the remaining branched monomer, the remaining polymerization catalyst, and a total amount of 10 wt% of a diluent and maintaining stirring, controlling the temperature of the reaction system to 85° C., maintaining stirring and reacting for 100 min, and obtaining a multi-generation branched polyurethane antistatic finishing agent intermediate;
[0229] (6) an end-capping step, in which the multi-generation branched polyurethane antistatic finishing agent intermediate is reacted with an end-capping agent, an olefin polymerization inhibitor, and a remaining diluent to obtain a multi-generation branched urethane antistatic finishing agent polymer; specifically:
[0230] (6.1) Add the remaining diluent to the reaction system obtained in step (5) and cool the system to 60-65° C.;
[0231] (6.2) Add the end-capping agent, maintain the system temperature at 62-64°C, and continue stirring the reaction for 60 minutes;
[0232] (6.3) Add olefin polymerization inhibitor all at once, control the temperature of the reaction system to 65°C, maintain stirring reaction for 30 minutes, and obtain multi-generation branched polyurethane antistatic finishing agent polymer.
[0233] (7) an emulsification step, in which the multi-generation branched polyurethane antistatic finishing agent polymer and water are mixed and emulsified to prepare a multi-generation branched polyurethane antistatic finishing agent intermediate emulsion; specifically:
[0234] (7.1) The reaction system of step (6.2) is stirred and cooled to 50-60°C, and the material is pumped into an emulsifier;
[0235] (7.2) increasing the stirring rate of the emulsifier to 1200 r / min, adding water at 20-35° C. into the emulsifier within 30 min, maintaining the system temperature at 45° C., stirring for 60 min, and preparing a multi-generation branched polyurethane antistatic finishing agent intermediate emulsion;
[0236] (8) Removal of solvent: removing the low boiling point diluent from the multi-generation branched polyurethane antistatic finishing agent emulsion product under vacuum and heating conditions to obtain a multi-generation branched polyurethane antistatic finishing agent emulsion product with a solid content of 8-14%; specifically:
[0237] (8.1) heating the emulsified system in step (7.2) to 50-60°C;
[0238] (8.2) The emulsifier is maintained at a medium-low speed stirring (stirring rate is 300r / min), the vacuum system and the condensing heat exchanger are turned on, part of the diluent is recovered, the vacuum system is turned off and the system is cooled to obtain a multi-generation branched polyurethane antistatic finishing agent emulsion product with a solid content of 8-14wt%.
[0239] The multi-generation branched polyurethane antistatic finishing agent emulsion product prepared in this embodiment can be used for durable antistatic finishing of synthetic fiber textiles such as polyester, vinylon, nylon and spandex after softening with amino silicone oil or the like. The product is a self-emulsifying aqueous polymer emulsion, which can significantly improve the hydrophilicity of synthetic fiber textile products. For synthetic fiber textiles with large specific surface area (friction charging voltage greater than 10000V), after impregnation finishing with commercially available products, the friction charging voltage can be reduced to 7000V after washing 5 times; after impregnation finishing with this product, the friction charging voltage can be reduced to below 2600V after washing 5 times. In addition, this product has no effect on the feel of large specific surface area polyester long-pile blankets, and its fluffiness is tested by Fast style instrument (compressibility expression). After the fabric is finished, the compressibility is increased by 5%, which has no adverse effect on the feel of the fabric; it has good market prospects; the product is safe, environmentally friendly and easy to use.
[0240] The preferred embodiments of the present invention are described in detail above, but the present invention is not limited thereto. Within the technical concept of the present invention, the technical solution of the present invention can be subjected to a variety of simple modifications, including the combination of various technical features in any other suitable manner, and these simple modifications and combinations should also be regarded as the contents disclosed by the present invention and belong to the protection scope of the present invention.
Claims
1. A method for preparing a multi-generation branched polyurethane antistatic finishing agent emulsion, characterized in that: The method comprises the following steps: (1) Raw material preparation: the raw materials include polymerizable monomers, branching monomers, end-capping agents, auxiliary agents and water; wherein the polymerizable monomers include diisocyanate, polyester diol, polyethylene glycol and hydroxyl-terminated polysiloxane, and the auxiliary agents include polymerization catalysts, olefin inhibitors and diluents; The diisocyanate is toluene diisocyanate, isophorone diisocyanate or diphenylmethane diisocyanate; The molecular weight of the polyester diol is 2000-4000, and the polyester diol is a polyester diol of phthalic anhydride and 1,6-hexanediol or a polyester diol of dimethyl terephthalate and ethylene glycol; The molecular weight of polyethylene glycol is 1000-8000; The terminal hydroxyl polysiloxane is a terminal hydroxyl polydimethylsiloxane having a molecular weight of 2000 to 6000; The branching monomer is glycerol or trimethylolpropane; The end-capping agent is hydroxyethyl methacrylate, hydroxyethyl acrylate, hydroxypropyl acrylate or hydroxybutyl methacrylate; The polymerization catalyst is stannous octoate, dibutyltin dilaurate or triethylamine; The olefin polymerization inhibitor is p-hydroxyanisole, hydroquinone or 2,5-di-tert-butylhydroquinone; The diluent is a mixture of a high boiling point diluent and a low boiling point diluent, wherein the high boiling point diluent is propylene glycol methyl ether acetate or dipropylene glycol dimethyl ether, and the low boiling point diluent is methyl ethyl ketone or acetone; The molar fractions of the components are: 18 of diisocyanate, 3.5-6.5 of polyethylene glycol, 1.5-3.5 of polyester diol, the sum of the molar fractions of terminal hydroxyl hydrocarbon polysiloxane, polyethylene glycol and polyester diol is 9, 4 of branching monomer, and 2-5 of end-capping agent; The amount of the polymerization catalyst used is 0.06 to 0.09 wt% of the total weight of the polymerization monomers; The amount of olefin polymerization inhibitor used is 0.01 to 0.05 wt% of the total weight of the polymerization monomers; The total amount of the diluent is 150-200 wt% of the total weight of the polymerized monomers, and the weight ratio of the high boiling point diluent to the low boiling point diluent is 1:2-7; (2) a step of pre-treating polyethylene glycol, polyester diol and hydroxyl-terminated polysiloxane, wherein the polyethylene glycol, polyester diol and hydroxyl-terminated polysiloxane are pre-treated by dehydration under vacuum and heating conditions; (3) a prepolymerization step, in which the polyester diol after dehydration pretreatment, the polyethylene glycol after dehydration pretreatment, the terminal hydroxyl polysiloxane after dehydration pretreatment, part of the diluent and the diisocyanate are subjected to a prepolymerization reaction under the catalytic action of part of the polymerization catalyst to obtain a multi-generation branched polyurethane antistatic finishing agent prepolymer; (4) a first-generation branching step, in which the multi-generation branched polyurethane antistatic finishing agent prepolymer is subjected to a branching reaction with a portion of a branching monomer and a portion of a diluent to obtain a multi-generation branched polyurethane antistatic finishing agent branched intermediate; (5) a second generation branching step, in which the remaining branching monomer, a portion of the diluent, the remaining polymerization catalyst and the multi-generation branched polyurethane antistatic finishing agent intermediate are reacted to obtain the multi-generation branched polyurethane antistatic finishing agent intermediate; (6) an end-capping step, in which the multi-generation branched polyurethane antistatic finishing agent intermediate is reacted with an end-capping agent, an olefin polymerization inhibitor, and a remaining diluent to obtain a multi-generation branched polyurethane antistatic finishing agent polymer; (7) an emulsification step, in which the multi-generation branched polyurethane antistatic finishing agent polymer and water are mixed and emulsified to prepare a multi-generation branched polyurethane antistatic finishing agent intermediate emulsion; (8) Removal of solvent: removing part of the diluent from the multi-generation branched polyurethane antistatic finishing agent emulsion product under vacuum and heating conditions to obtain a multi-generation branched polyurethane antistatic finishing agent emulsion with a solid content of 8-14wt%.
2. The preparation method according to claim 1, characterized in that: The specific process of step (2) includes: (2.1) adding polyethylene glycol, polyester diol and hydroxyl-terminated polysiloxane into a reactor; (2.2) Heat the material to 110-120°C and treat it under a vacuum condition of -0.100 to -0.098 MPa for 90-150 min.
3. The preparation method according to claim 1 or 2, characterized in that: The specific process of step (3) includes: (3.1) Cooling the material obtained in step (2) to 70-75°C; (3.2) Add diisocyanate and keep stirring, control the temperature of the reaction system to 75-85°C, and keep stirring for 30-50 minutes; (3.3) maintaining the temperature of the reaction system at 75-85° C., adding a total amount of 60-80 wt % of a polymerization catalyst at a uniform rate within 10-15 min; (3.4) raising the temperature of the reaction system to 80-90° C. and maintaining the temperature for 100-120 min. During the temperature maintenance period, a diluent in an amount of 10-20 wt % is added to prepare a multi-generation branched polyurethane antistatic finishing agent prepolymer.
4. The preparation method according to claim 1, characterized in that: The specific process of step (4) includes: (4.1) Cooling the reaction system obtained in step (3) to 75-85°C; (4.2) Add 75 wt% of branched monomers and 40-70 wt% of diluents and maintain stirring, control the temperature of the reaction system to 75-90° C., maintain stirring for 90-120 min, and obtain a multi-generation branched polyurethane antistatic finishing agent branched intermediate.
5. The preparation method according to claim 1, characterized in that: The specific process of step (5) includes: (5.1) maintaining the reaction system obtained in step (4) at 75-85° C.; (5.2) Add the remaining branched monomer, the remaining polymerization catalyst, and a total amount of 10 to 40 wt% of a diluent and maintain stirring, control the temperature of the reaction system to 75 to 90° C., maintain stirring for 90 to 120 minutes, and obtain a multi-generation branched polyurethane antistatic finishing agent intermediate.
6. The preparation method according to claim 1, characterized in that: The specific process of step (6) includes: (6.1) Add the remaining diluent to the reaction system obtained in step (5) and cool the system to 60-65° C.; (6.2) Add the end-capping agent, maintain the system temperature at 60-65°C, and continue stirring the reaction for 30-60 minutes; (6.3) Add olefin polymerization inhibitor, control the temperature of the reaction system to 60-75°C, maintain stirring reaction for 15-60 minutes, and obtain multi-generation branched polyurethane antistatic finishing agent polymer.
7. The preparation method according to claim 1 or 6, characterized in that: The specific process of step (7) includes: (7.1) The reaction system obtained in step (6) is stirred and cooled to 50-60° C., and the material is pumped into an emulsifier; (7.2) The stirring rate of the emulsifier is adjusted to 1000-1200 r / min, and water at 20-35° C. is added to the emulsifier within 20-30 min, and the system temperature is maintained at 40-60° C. and stirred for 30-60 min to obtain a multi-generation branched polyurethane antistatic finishing agent intermediate emulsion.
8. The preparation method according to claim 1, characterized in that: The specific process of step (8) includes: (8.1) maintaining the emulsified system obtained in step (7) at 50-60° C.; (8.2) The stirring rate of the emulsifier is adjusted to 300-500 r / min, the vacuum system and the condensing heat exchanger are opened, part of the diluent is recovered, the vacuum system is closed and the system is cooled to obtain a multi-generation branched polyurethane antistatic finishing agent emulsion with a solid content of 8-14 wt%.
9. The preparation method according to claim 1, characterized in that: The water is soft water with a total hardness of less than 50 ppm CaO.
10. A multi-generation branched polyurethane antistatic finishing agent emulsion prepared by the method described in any one of claims 1 to 9.