Cracking photo-thermal coating as well as preparation method and application thereof

By introducing cracked structures into the photothermal coating, relieving tension stress and improving evaporation efficiency, the problem of poor stability of existing photothermal coatings during extrusion and long-term use is solved, and efficient seawater evaporation and desalination treatment is achieved .

CN118955998APending Publication Date: 2024-11-15NANCHANG UNIV
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202410989111.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-23
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

The existing photothermal coatings are prone to nanospheres falling off during external force extrusion and long-term use, resulting in reduced hydrophilicity and photothermal performance, reduced evaporation rate, and inability to achieve long-term operation.

Method used

By using the preparation method of cracked photothermal coating, the pre-wetted porous matrix is ​​immersed in a modified solution dissolved with polyphenols and silane coupling agent, and then immersed in an iron ion solution to react to form a photothermal coating with cracks. to relieve tension stress and improve evaporation efficiency.

Benefits of technology

It improves the stability and evaporation efficiency of the coating, enhances the limiting capillary effect on moisture, and ensures stability during the extrusion process and efficient performance in long-term use.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118955998A_ABST
    Figure CN118955998A_ABST
Patent Text Reader

Abstract

The invention provides a preparation method and application of a cracked metal-polyphenol photo-thermal coating, and belongs to the field of functional coating technologies and seawater desalination. According to the preparation method of the cracked metal-polyphenol photo-thermal coating, the photo-thermal coating with a unique nano crack structure is formed on the surface of a porous material under a specific concentration condition by regulating and controlling the concentration of reactants. When the photo-thermal material is extruded by external force, the nano crack can be used as a buffer area to relieve tensile stress generated in the extrusion process, so that the stability of the coating is improved, and the problem that the stability of the metal-polyphenol nano sphere coating is insufficient is solved. Besides, a crack structure of the cracked metal-polyphenol coating can generate a strong confinement capillary action, and water can spontaneously diffuse along cracks and be transported upwards instead of filling pores of the sponge, so that the evaporation rate is greatly increased. The metal-polyphenol photo-thermal coating modified sponge has the advantages of being high in evaporation efficiency, economical, environmentally friendly and the like.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of functional coatings, and in particular to a cracked photothermal coating and a preparation method and application thereof. Background Art

[0002] How to obtain fresh water resources sustainably is one of the biggest challenges facing the sustainable development of human society, and desalination of seawater, which accounts for about 97% of the earth's reserves, is a feasible idea. The current seawater desalination technologies mainly include distillation, reverse osmosis, electrodialysis and ion exchange. Among them, distillation and reverse osmosis are the two most mature and widely used methods. However, distillation consumes a lot of energy, and reverse osmosis is difficult to treat high-salinity wastewater.

[0003] Therefore, in recent years, the solar-driven seawater evaporation, collection, and desalination technology based on photothermal materials has shown great application potential due to its simple process and green environmental protection. The core of the technology is that the photothermal material captures light, efficiently converts light energy into heat energy and concentrates it on an interface, reducing heat loss and driving seawater evaporation. This technology has the characteristics of zero carbon dioxide emissions and is very attractive and practical. In order to achieve solar-driven seawater evaporation, the photothermal material needs to be stably adhered to a porous substrate as an evaporator. Among them, metal polyphenol networks (MPNs) have attracted widespread attention due to their porous structure and strong affinity for various substrates. Metal ions are coordinated with abundant natural phenolic ligands, which makes MPNs have a wide range of and adjustable physical and chemical properties, especially photothermal properties and selective wettability.

[0004] For example, a Chinese invention patent with publication number CN116020279A provides a fast, green and universal method for modifying a polyphenol coating, in which a hydrophobic material pre-moistened with ethanol is immersed in a polyphenol-containing substance, a silane coupling agent having an amino group and deionized water for super-hydrophilic modification, thereby forming a polyphenol-modified super-hydrophilic film on the surface of the hydrophobic material, and the surface of the polyphenol-modified super-hydrophilic film has a layered nanosphere structure; another example is a Chinese invention patent with publication number CN114835183A that provides a three-dimensional solar evaporator, in which a melamine sponge is immersed in a Tric-HCl mixed solution containing tannic acid and 3-aminopropyltriethoxysilane to react to obtain a super-hydrophilic sponge, and then immersed in an iron ion solution to react to obtain a super-hydrophobic sponge, both of which form a layered nanosphere structure on the melamine surface.

[0005] However, the nanospheres stacked in the polyphenol coating are prone to fall off when squeezed by external forces and during long-term use, which will lead to reduced hydrophilicity and photothermal performance of the photothermal material, thereby causing a decrease in the evaporation rate. The thin layer of hydrogel is attached to the surface of the sponge through hydrogen bonds and is also prone to fall off during long-term use, making long-term operation impossible. Therefore, there is an urgent need to provide a solution to improve the above problems. Summary of the invention

[0006] The purpose of the present invention is to provide a cracked photothermal coating and a preparation method and application thereof. By forming a cracked photothermal coating with cracks, the tensile stress generated during the extrusion process can be absorbed, thereby improving the stability of the coating and improving the evaporation efficiency.

[0007] In the first aspect, the present invention provides a method for preparing a cracked photothermal coating, comprising immersing a pre-wetted porous substrate into a modified solution in which polyphenols and silane coupling agents are dissolved to obtain a modified substrate after adsorption; immersing the modified substrate into an iron ion solution to react to obtain a photothermal material having a cracked photothermal coating formed on the surface; wherein the silane coupling agent has an amino group, and the mass ratio of polyphenols, silane coupling agents and iron ion solutes in the iron ion solution is 4:4:1.

[0008] The photothermal coating prepared by the preparation method provided by the present invention has a cracked structure. When subjected to external force extrusion, the cracks of the cracked photothermal coating can serve as a buffer zone, thereby alleviating the tensile stress generated during the extrusion process, thereby improving the stability of the coating on the surface of the porous substrate. In addition, the cracks can also produce a strong confined capillary effect, and water can diffuse spontaneously along the cracks, thereby improving the evaporation efficiency.

[0009] Optionally, the polyphenols include one of tannic acid, gallic acid, caffeic acid and a mixture thereof.

[0010] Optionally, the silane coupling agent is 3-aminopropyltriethoxysilane.

[0011] Optionally, the iron ion solution includes one of a ferric sulfate solution and a ferric chloride solution.

[0012] Optionally, the modified solution is a deionized water solution of polyphenol and a silane coupling agent.

[0013] Optionally, the method includes the following steps: pre-wetting the porous substrate by immersing it in ethanol; immersing the pre-wetted porous substrate in a modification solution for adsorption and reaction to obtain a modified substrate; washing the modified substrate and then immersing it in an iron ion solution for reaction to obtain a photothermal material having a cracked photothermal coating formed on the surface.

[0014] Optionally, the porous matrix includes a porous sponge, and the porous sponge includes one of polyurethane sponge, polyimide sponge, polystyrene sponge, melamine sponge, polyvinyl chloride sponge, and polyethylene sponge.

[0015] Optionally, the polyphenol concentration in the modified solution is 2-12 mg / mL.

[0016] Optionally, the concentration of the silane coupling agent in the modified solution is 2-12 mg / mL.

[0017] Optionally, the iron ion concentration in the iron ion solution is 0.05-3 mg / mL.

[0018] Optionally, after the porous matrix is ​​immersed in ethanol for pre-wetting, the adsorption amount of ethanol by the porous matrix is ​​less than or equal to 1.60 g / g.

[0019] Optionally, the pre-wetted porous substrate is placed into the modified solution for adsorption and reaction for 50-70 minutes to obtain the modified substrate.

[0020] Optionally, the modified substrate is washed and then immersed in an iron ion solution for reaction for 20-40 minutes to obtain a photothermal material with a cracked photothermal coating formed on the surface.

[0021] Optionally, the whole process is carried out in a stirring environment at 100-200 rpm.

[0022] In a second aspect, the present invention also provides a cracked photothermal coating prepared by any of the above optional preparation methods, wherein the coating has smooth nanocracks.

[0023] In a third aspect, the present invention also provides the use of a cracked photothermal coating prepared by any of the above optional preparation methods in solar evaporation materials, photothermal seawater desalination materials, salt-containing wastewater purification materials, sewage purification materials, and oil-water emulsion separation materials. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 A flowchart of the method for preparing the cracked photothermal coating provided by the present invention;

[0025] Figure 2 A schematic diagram of the mechanism of the cracked photothermal coating provided by the present invention after being formed on the surface of a porous substrate;

[0026] Figure 3 A schematic diagram of the preparation process of the cracked photothermal coating provided by the present invention;

[0027] Figure 4 The scanning electron microscope images of the modified porous sponge and polyurethane sponge prepared in Examples 1 to 4 of the present invention and the test images when conducting a water contact angle test;

[0028] Figure 5 The modified porous sponge prepared in Example 3 of the present invention and Comparative Example 1 is shown in the photographs before and after extrusion, the mass weighing, the scanning electron microscope image and the water contact angle change image;

[0029] Figure 6 This is a schematic diagram of the structure of an evaporation device when the modified porous sponge prepared in Example 3 of the present invention is tested for evaporation rate;

[0030] Figure 7This is a graph of the evaporation efficiency of the modified porous sponge prepared in Example 3 of the present invention when conducting an evaporation rate test, wherein the abscissa is time (min) and the ordinate is mass change (kg / m 2 );

[0031] Figure 8 This is a graph showing the evaporation efficiency of the modified porous sponge prepared in Example 3 of the present invention when placed in an outdoor continuous light environment, where the horizontal axis is days (d) and the left vertical axis is the evaporation rate (kg / m 2 h), the right ordinate is the humidity change (%);

[0032] Fig. 9 This is a graph showing changes in ion concentration in condensed water of the modified porous sponge prepared in Example 3 of the present invention before and after the evaporation test, where the abscissa represents the type of ions and the ordinate represents the ion concentration (mg / L). DETAILED DESCRIPTION

[0033] In order to make the purpose, technical solutions and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention. Unless otherwise defined, the technical terms or scientific terms used herein should be the common meanings understood by people with general skills in the field to which the present invention belongs.

[0034] The present invention provides a method for preparing a cracked photothermal coating, comprising: immersing a pre-wetted porous substrate into a modified solution in which polyphenols and a silane coupling agent are dissolved, and then adsorbing the solution to obtain a modified substrate; immersing the modified substrate into an iron ion solution to react and obtain a photothermal material with a cracked photothermal coating formed on the surface.

[0035] In fact, after the porous substrate is immersed in the modification solution, the polyphenols and the silane coupling agent will react on the surface of the porous substrate, thereby surface coating and modifying the porous substrate. In addition, after being immersed in the iron ion solution, the polyphenols react with the iron ions and form a smooth coating on the surface of the porous substrate. During the drying process, the coating loses water and shrinks to produce cracks.

[0036] Specifically, the morphology of the coating formed on the surface of the porous substrate can be adjusted by regulating the concentration of polyphenols and iron ions. Specifically, the silane coupling agent has an amino group, and the mass ratio of polyphenols, silane coupling agent and iron ion solute in the iron ion solution is 4:4:1. The nano-crack structure formed in this way is more stable and has a good buffering effect. It can well relieve the tensile stress generated during the extrusion process and effectively improve the adhesion stability of the photothermal coating.

[0037] In some embodiments, the polyphenol in the modified solution may specifically include tannic acid (TA), the silane coupling agent may specifically include 3-aminopropyltriethoxysilane (APTES), and the iron ion solution may include one of a ferric sulfate solution and a ferric chloride solution. Specifically, the modified solution is a deionized water solution of the polyphenol and the silane coupling agent.

[0038] In some embodiments, see Figure 1 When preparing the cracking photothermal coating, the following steps are included:

[0039] S1, immersing the porous substrate in ethanol for pre-wetting;

[0040] S2, immersing the pre-wetted porous substrate into the modified solution for adsorption and reaction to obtain a modified substrate;

[0041] S3. After washing the modified substrate, immersing it in an iron ion solution for reaction, rinsing and drying it to obtain a photothermal material with a cracked photothermal coating formed on the surface.

[0042] In fact, when performing step S1, the porous substrate is soaked in anhydrous ethanol until the porous substrate is saturated with adsorption, and then the porous substrate is squeezed to squeeze out excess ethanol, so that the loading amount of ethanol on the porous substrate is less than or equal to 1.60 g / g. In fact, pre-wetting the porous substrate with ethanol is conducive to the adsorption of polyphenols and silane coupling agents in the modified solution.

[0043] Specifically, when the silane coupling agent in the modified solution is 3-aminopropyltriethoxysilane, since the hydrolysis product of 3-aminopropyltriethoxysilane is ethanol, squeezing out the ethanol in the porous matrix as much as possible can effectively promote the hydrolysis of 3-aminopropyltriethoxysilane, thereby improving the reaction efficiency.

[0044] In some embodiments, the porous matrix used in step S1 includes a porous sponge, and the porous sponge includes one of polyurethane sponge, polyimide sponge, polystyrene sponge, melamine sponge, polyvinyl chloride sponge, and polyethylene sponge.

[0045] In some embodiments, the polyphenol concentration in the modified solution is 2-12 mg / mL, for example, 2 mg / mL, 4 mg / mL, 8 mg / mL, or 12 mg / mL.

[0046] In some embodiments, the concentration of the silane coupling agent in the modified solution is 2-12 mg / mL.

[0047] In some embodiments, the concentration of iron ions in the iron ion solution is 0.5-3 mg / mL.

[0048] Specifically, the pre-wetted porous substrate is placed into the modified solution for adsorption and reaction for 50-70 minutes to obtain the modified substrate.

[0049] Specifically, the modified substrate is washed and then immersed in an iron ion solution for reaction for 20-40 minutes to obtain a photothermal material with a cracked photothermal coating formed on the surface.

[0050] In fact, the whole process is carried out in a stirring environment at 100-200 rpm.

[0051] Example 1

[0052] Embodiment 1 of the present invention provides a method for preparing a porous sponge modified by a cracked photothermal coating, comprising the following steps:

[0053] S1. Wash a 1cm×1cm×1cm polyurethane sponge with anhydrous ethanol, immerse it in anhydrous ethanol for pre-wetting, take out the polyurethane sponge and squeeze out the excess anhydrous ethanol, so that the polyurethane sponge has a loading capacity of 1.57 gg of anhydrous ethanol. -1 about;

[0054] S2. Dissolve 50 mg of tannic acid (TA) in 25 mL of deionized water to obtain a tannic acid solution, add 200 μL of 3-aminopropyltriethoxysilane (APTES) to the tannic acid solution and evenly disperse the mixture to obtain a modified solution; immerse the pre-moistened polyurethane sponge in the modified solution, adsorb and react for 1 h at 25° C. and a shaking speed of 140 rpm, then take out the polyurethane sponge and wash it with deionized water to obtain a modified matrix;

[0055] S3. The modified substrate was immersed in a 2 mg / mL ferric sulfate solution for reaction for 30 min, and then taken out and dried to constant weight to obtain a modified porous sponge (Sp@MPN1).

[0056] Example 2 to Example 4

[0057] Embodiments 2 to 4 of the present invention respectively provide a method for preparing a porous sponge modified by a cracked photothermal coating, which is different from Embodiment 1 in that the concentration of the tannic acid solution in step S2 is different, as shown in Table 1 below.

[0058] Table 1 Tannic acid solution concentration in Examples 1 to 4

[0059] Tannic acid dosage / mg Deionized water usage / mL Modified porous sponge Example 1 50 25 <![CDATA[Sp@MPN1]]> Example 2 100 25 <![CDATA[Sp@MPN2]]> Example 3 200 25 <![CDATA[Sp@MPN3]]> Example 4 300 25 <![CDATA[Sp@MPN4]]>

[0060] Comparative Example 1

[0061] Comparative Example 1 of the present invention is based on the publication number CN114835183A, and provides a method for preparing a porous sponge modified by a metal-polyphenol nanosphere photothermal coating, comprising the following steps:

[0062] D1, same as Example 1;

[0063] D2, immersing the pre-wetted polyurethane sponge in a modified solution (tannic acid concentration 2 mg / mL, 3-aminopropyltriethoxysilane concentration 2 mg / mL, solvent is Tris-HCl solution with pH = 8.5), adsorbing and reacting for 12 hours at 25° C. and a shaker speed of 140 rpm, taking out the polyurethane sponge and washing it with deionized water to obtain a modified matrix;

[0064] D3. The modified substrate was immersed in a 2 mg / mL ferric sulfate solution for reaction for 2 h, taken out and dried to constant weight to obtain a modified porous sponge (Sp@MPNP).

[0065] Performance Testing

[0066] The polyurethane sponge and the modified porous sponge prepared in Examples 1 to 4 were observed using a scanning electron microscope and tested for hydrophilicity. The results are as follows: Figure 4 As shown; after the surface of the modified porous sponge prepared in Example 3 and Comparative Example 1 was observed using a scanning electron microscope, a 20g weight was used to squeeze 100 times, and then the scanning electron microscope was used to observe, and the water contact angle before and after squeezing was tested. The results are shown as follows Figure 5 shown.

[0067] See also Figure 6 The modified porous sponge prepared in Example 3 is placed on the top of the insulation board 1, and a container 2 is set at the bottom of the insulation board 1. The container 2 contains a sodium chloride solution 3 with a concentration of 3.5wt.%, and a water supply column 4 is passed through the middle of the insulation board 1. One end of the water supply column 4 is in contact with the modified porous sponge, and the other end is inserted into the bottom of the sodium chloride solution 3. A xenon lamp is used to simulate 1kw / m 2 After the whole device is irradiated with the radiation power, the relationship between the mass change and time during the evaporation process is detected. Figure 7 shown.

[0068] The modified porous sponge shown in Example 3 was placed Figure 6 After the devices were installed, they were placed outdoors with 9 hours of sunlight per day for 23 days. The evaporation rate and humidity were tested every hour of the day. The results are as follows: Figure 8 Prepare a 3.5 wt.% simulated seawater solution and use Figure 6 After the device shown in the figure evaporates under outdoor light, the condensed water is collected and the ion content in the condensed water is measured. The results are as follows Fig. 9 shown.

[0069] Results Analysis

[0070] from Figure 4It can be seen that the surface of the modified porous sponge prepared in Example 3 has a nano-crack structure, which can produce a strong confined capillary effect, forming a thin water layer on the surface of the sponge skeleton, and limiting the water to the surface of the sponge skeleton instead of filling the entire sponge pores, thereby increasing the gas escape area during the evaporation process, thereby increasing the evaporation rate. From the hydrophilicity test, it can be seen that its hydrophilic angle is 0°, which has super hydrophilicity.

[0071] from Figure 5 (a) and Figure 5 As can be seen from Figure (c), the weight loss rate of Sp@MPN3 prepared in Example 3 after extrusion is only 0.1%, while the weight loss rate of Sp@MPNP prepared in Comparative Example 1 (such as Figure 5 (b) and Figure 5 (d) shows that the weight loss rate after extrusion is as high as 12.85%. From the photos before and after extrusion, it can be seen that Sp@MPNP has obviously faded and a large amount of powder appears on the periphery. This is because the nanosphere structure on the surface of Sp@MPNP peels off after extrusion.

[0072] In addition, from Figure 5 (a) and Figure 5 From the scanning electron micrographs before and after extrusion in (c), it can be seen that the nanocracks on the surface of Sp@MPN3 still exist after extrusion, and are slightly wider than those before extrusion. This indicates that the nanocracks can serve as a buffer during the extrusion process, relieving the tensile stress generated during the extrusion process and improving the stability of the surface photothermal coating. However, the nanospheres on the surface of Sp@MPNP after extrusion are difficult to adapt to the polyurethane sponge due to the tensile stress, resulting in shedding (e.g. Figure 5 (b) and Figure 5 (d)).

[0073] from Figure 7 It can be seen that the evaporation rate of Sp@MPN3 prepared in Example 3 is stable at 3.2 kg / (m 2 h) With balanced evaporation performance under light, water can diffuse quickly in the cracked coating instead of filling the pores of the polyurethane sponge. Figure 8 It can be seen that when continuous light evaporation is carried out in an outdoor environment, the evaporation rate of Sp@MPN3 is basically 3.0 kg / (m 2 h) fluctuated steadily, and the evaporation rate did not decrease during the 23-day continuous test. Fig. 9 It can be seen that the concentration of each ion in the condensed water after the evaporation test dropped significantly by several orders of magnitude, which shows that Sp@MPN3 provided in Example 3 has an excellent water purification effect.

[0074] Although the embodiments of the present invention are described in detail above, it is obvious to those skilled in the art that various modifications and variations can be made to these embodiments. However, it should be understood that such modifications and variations are within the scope and spirit of the present invention as described in the claims. Moreover, the present invention described herein may have other embodiments and may be implemented or realized in a variety of ways.

Claims

1. A method for preparing a cracked photothermal coating, It is characterized in that The pre-wetted porous substrate is immersed in a modification solution containing polyphenol and silane coupling agent for adsorption to obtain a modified substrate; The modified substrate is immersed in an iron ion solution for reaction to obtain a photothermal material with a cracked photothermal coating formed on the surface; wherein the silane coupling agent has an amino group, and the mass ratio of polyphenol, silane coupling agent and iron ion solute in the iron ion solution is 4:4:

1.

2. The preparation method according to claim 1, It is characterized in that The polyphenol includes tannic acid; and / or the silane coupling agent includes 3-aminopropyltriethoxysilane; and / or the iron ion solution includes one of a ferric sulfate solution and a ferric chloride solution; and / or the modified solution is a deionized water solution of polyphenol and a silane coupling agent.

3. The preparation method according to claim 1, It is characterized in that The following steps are involved: The porous substrate is immersed in ethanol for pre-wetting; The pre-wetted porous substrate is immersed in a modification solution for adsorption and reaction to obtain a modified substrate; The modified substrate is washed, immersed in an iron ion solution for reaction, and then rinsed and dried to obtain a photothermal material with a cracked photothermal coating formed on the surface.

4. The preparation method according to claim 3, It is characterized in that The porous matrix includes a porous sponge, and the porous sponge includes one of polyurethane sponge, polyimide sponge, polystyrene sponge, melamine sponge, polyvinyl chloride sponge, and polyethylene sponge.

5. The preparation method according to claim 3, It is characterized in that The polyphenol concentration in the modified solution is 2-12 mg / mL; and / or, the silane coupling agent concentration in the modified solution is 2-12 mg / mL; and / or, the iron ion concentration in the iron ion solution is 0.05-3 mg / mL.

6. The preparation method according to claim 3, It is characterized in that After the porous matrix is ​​immersed in ethanol for pre-wetting, the adsorption amount of ethanol by the porous matrix is ​​less than or equal to 1.60 g / g.

7. The preparation method according to claim 3, It is characterized in that The pre-wetted porous substrate is placed in the modified solution for adsorption and reaction for 50-70 minutes to obtain a modified substrate; and / or, the modified substrate is washed and immersed in an iron ion solution for reaction for 20-40 minutes to obtain a photothermal material with a cracked photothermal coating formed on the surface; and / or, the whole process is carried out in a stirring environment of 100-200rpm.

8. A cracked photothermal coating prepared by the preparation method according to any one of claims 1 to 7, It is characterized in that The coating has smooth nanocracks.

9. An application of a cracked photothermal coating prepared by the preparation method according to any one of claims 1 to 7 in solar evaporation materials, photothermal seawater desalination materials, saline wastewater purification materials, sewage purification materials, and oil-water emulsion separation materials.

Citation Information

Cited By

  • Three-dimensional carbon nitride photocatalyst with tip structure as well as preparation method and application of three-dimensional carbon nitride photocatalyst