Preparation method of high-calibration-rate EBSD sample for 7-series aluminum alloy material

Through the combination of mechanical polishing and SiO2 sol polishing, the problem of lack of universal electrolytic polishing technology and sample surface corrosion pits in the preparation of 7-series aluminum alloy is solved, and the preparation of EBSD samples with high calibration rate and high imaging quality is achieved. , 7-Series aluminum alloy material suitable for a variety of heat treatment processes.

CN118961337AActive Publication Date: 2024-11-15HARBIN INST OF TECH

Patent Information

Application Number
CN202411071695.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-06
Publication Date
2024-11-15
Estimated Expiration
2044-08-06

AI Technical Summary

Technical Problem

The existing 7-Series aluminum alloy EBSD sample preparation methods lack universal electrolytic polishing technology, which leads to corrosion pits on the surface of the sample, affecting the generation of diffraction patterns, especially when the material contains a large amount of precipitation phase or has a large deformation amount. The parameters are difficult to stabilize, resulting in a low calibration rate.

Method used

Using a combination of mechanical polishing and SiO2 sol polishing, the samples are gradually polished and polished through metallographic sandpaper coarse grinding, anhydrous ethanol cleaning, diamond spray polishing and SiO2 sol polishing, so as to ensure smooth surface without scratches and remove stress layers. , improve the quality of diffraction patterns.

Benefits of technology

The high calibration rate preparation of 7-Series aluminum alloy EBSD specimens is realized, and the process flow is simplified. It is suitable for materials for various heat treatment processes, especially materials containing a large number of precipitation phases or large deformations, which significantly improves imaging quality and analysis accuracy. sex.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118961337A_ABST
    Figure CN118961337A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of a high-calibration-rate EBSD sample for a 7-series aluminum alloy material, and relates to a preparation method of a high-calibration-rate EBSD sample for an aluminum alloy material. The invention aims to solve the technical problems that no universal electrolytic polishing process exists in the preparation process of the existing 7-series aluminum alloy EBSD sample, corrosion pits are easy to appear on the surface of the sample, and the generation of diffraction patterns is seriously influenced. According to the method, SiO2 sol polishing is further adopted on the basis of mechanical polishing, a stress layer generated on the surface of the sample in the mechanical polishing process can be removed, and generation of a strong Kikuchi pattern in the EBSD test is facilitated; the SiO2 sol can polish structures and precipitated phases with different hardness, so that the surface of a sample is smoother, the extrusion deformation effect of the hard second phase on an aluminum matrix in the mechanical polishing process is relieved, the imaging quality of EBSD is further improved, and research and analysis of the microstructure and the texture of the 7-series aluminum alloy in the preparation processing heat treatment process are facilitated.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to an EBSD sample preparation method with a high calibration rate for an aluminum alloy material. Background Art

[0002] The 7 series aluminum alloy has attracted much attention for its excellent comprehensive mechanical properties, especially its extremely high specific strength, good corrosion resistance and outstanding high temperature impact performance, which makes it have great potential in load-bearing parts with strict lightweight requirements, especially in the aerospace field. In the context of current scientific and technological progress, further improving the comprehensive performance of the 7 series aluminum alloy has become an important research topic. In order to achieve this goal, heat treatment of 7 series aluminum alloy is considered to be one of the most effective methods. During the heat treatment process, researchers focus on exploring how the microstructure of the material affects its mechanical properties. This research direction is crucial to optimizing the performance of the alloy, especially in improving its strength, corrosion resistance and toughness.

[0003] In order to effectively explore the evolution of interfaces and textures of 7-series aluminum alloys during heat treatment, EBSD analysis of the materials is required. EBSD technology can take into account the crystal structure and orientation information of materials, and its role in the fields of metals, semiconductors, minerals and ceramic materials is becoming increasingly important, and it has gradually become a very important characterization method in material organization and texture analysis technology. The traditional EBSD sample preparation method for 7-series aluminum alloys is completed through two steps: mechanical polishing and electrolytic polishing. In the electrolytic polishing process, the cathode material is usually a platinum sheet, and the electrolyte is a mixed solution of HClO4 and CH3CH2OH, with a volume ratio of generally 1:9. The traditional EBSD sample electrolytic polishing preparation method can prepare EBSD samples that meet the requirements under appropriate process parameters. However, due to the diverse heat treatment states of 7-series aluminum alloys, 7-series aluminum alloy materials with different heat treatment states require different electrolytic polishing process parameters. At present, there is no universal electrolytic polishing process that can obtain a surface with a high calibration rate (the calibration rate is the ratio of the number of Kikuchi pattern points accurately calibrated by the computer to the total number of collected points). Especially when the material contains a large amount of precipitated phases or the deformation is large, it often takes a lot of time to explore the process; in addition, when the electrolytic polishing method is used to prepare EBSD samples, corrosion pits caused by unstable process parameters are also prone to appear on the sample surface, which will seriously affect the generation of diffraction patterns. The above problems will bring many inconveniences to researchers. Therefore, it is urgent to develop a simple, easy-to-operate and high-calibration polishing method suitable for 7-series aluminum alloys. Summary of the invention

[0004] The present invention aims to solve the technical problems that there is no universal electrolytic polishing process in the preparation process of the existing 7 series aluminum alloy EBSD samples, and corrosion pits are easily formed on the sample surface, which seriously affects the generation of diffraction patterns, and to provide an EBSD sample preparation method with a high calibration rate for 7 series aluminum alloy materials.

[0005] The EBSD sample preparation method for 7 series aluminum alloy materials with high calibration rate of the present invention is carried out according to the following steps:

[0006] 1. Sample preparation:

[0007] Cut the 7 series aluminum alloy material into small rectangular pieces. If the sample size is small, it can be inlaid to obtain the original sample of 7 series aluminum alloy electron backscatter diffraction analysis;

[0008] 2. Rough grinding of samples:

[0009] Use different types of metallographic sandpaper to preliminarily grind the sample prepared in step 1. During the grinding process, the grinding direction should be constantly changed to make the force in each direction uniform until the surface of the sample is flat after rough grinding and the scratch direction is consistent;

[0010] 3. Anhydrous ethanol cleaning:

[0011] The roughly ground sample was ultrasonically cleaned in anhydrous ethanol for 5 to 10 minutes to prevent the debris generated during the grinding process from affecting the subsequent polishing;

[0012] 4. Mechanical polishing:

[0013] After cleaning, the sample is blown dry, and then mechanically polished with diamond spray polishing agent. During the polishing process, the sample needs to be rotated 90° horizontally every 3min to 5min. The total polishing time is 10min to 15min. After polishing, the surface of the sample needs to be bright and scratch-free.

[0014] 5. Anhydrous ethanol cleaning:

[0015] The mechanically polished samples were ultrasonically cleaned with anhydrous ethanol for 5 to 10 minutes to remove the residual diamond polishing agent on the surface of the samples;

[0016] 6. SiO2 sol polishing:

[0017] The sample cleaned in step 5 is subjected to final polishing on a rubber polishing disc using SiO2 sol. During the polishing process, anhydrous ethanol is sprayed for lubrication. During the polishing process, the sample is horizontally rotated 90° every 3 to 5 minutes. The total polishing time is 10 to 20 minutes, and finally a sample with a bright surface and no scratches is obtained;

[0018] 7. Anhydrous ethanol cleaning: Place the polished sample in anhydrous ethanol for ultrasonic cleaning for 5 to 10 minutes, and then blow dry and store;

[0019] In steps two, four and six, the same surface of the sample is polished.

[0020] The beneficial effects of the present invention are:

[0021] 1) The present invention further adopts SiO2 sol polishing on the basis of mechanical polishing, which can remove the stress layer generated on the sample surface during the mechanical polishing process, which is conducive to generating strong diffraction patterns during EBSD testing; in addition, SiO2 sol can polish the structures and precipitated phases of different hardness at the same time, so as to make the sample surface smoother, alleviate the extrusion deformation effect of the hard second phase on the aluminum substrate during the mechanical polishing process, thereby further improving the imaging quality of EBSD, and facilitating the research and analysis of the microstructure and texture of 7 series aluminum alloys during the preparation, processing and heat treatment process;

[0022] 2) The method of the present invention is simple to operate, easy to control, and has good effect. It is suitable for the preparation of EBSD specimens of 7 series aluminum alloys of various types or heat treatment processes, especially for 7 series aluminum alloy materials with more precipitated phases, a large amount of second phases, and a large amount of deformation. Its effect is significantly better than electrolytic polishing. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 The grain morphology orientation map and inverse pole figure obtained by EBSD analysis of the sample prepared in Experiment 1;

[0024] Figure 2 The grain morphology orientation map and inverse pole figure obtained by EBSD analysis of the sample prepared in Experiment 2;

[0025] Figure 3 The grain morphology orientation map and inverse pole figure obtained by EBSD analysis of the same aluminum alloy sample as in Experiment 2 prepared by conventional electrolytic polishing;

[0026] Figure 4 Grain morphology orientation map and inverse pole figure of the samples prepared for experiment three. DETAILED DESCRIPTION

[0027] Specific implementation method 1: This implementation method is a method for preparing EBSD samples with high calibration rate for 7 series aluminum alloy materials, which is specifically carried out in the following steps:

[0028] 1. Sample preparation:

[0029] The 7 series aluminum alloy material is cut into rectangular small pieces to obtain the original sample for electron backscatter diffraction analysis of the 7 series aluminum alloy;

[0030] 2. Rough grinding of samples:

[0031] Use different types of metallographic sandpaper to preliminarily grind the sample prepared in step 1. During the grinding process, the grinding direction should be constantly changed to make the force in each direction uniform until the surface of the sample is flat after rough grinding and the scratch direction is consistent;

[0032] 3. Anhydrous ethanol cleaning:

[0033] The roughly ground sample was ultrasonically cleaned in anhydrous ethanol for 5 to 10 minutes to prevent the debris generated during the grinding process from affecting the subsequent polishing;

[0034] 4. Mechanical polishing:

[0035] After cleaning, the sample is blown dry, and then mechanically polished with diamond spray polishing agent. During the polishing process, the sample needs to be rotated 90° horizontally every 3min to 5min. The total polishing time is 10min to 15min. After polishing, the surface of the sample needs to be bright and scratch-free.

[0036] 5. Anhydrous ethanol cleaning:

[0037] The mechanically polished samples were ultrasonically cleaned with anhydrous ethanol for 5 to 10 minutes to remove the residual diamond polishing agent on the surface of the samples;

[0038] 6. SiO2 sol polishing:

[0039] The sample cleaned in step 5 is subjected to final polishing on a rubber polishing disc using SiO2 sol. During the polishing process, anhydrous ethanol is sprayed for lubrication. During the polishing process, the sample is horizontally rotated 90° every 3 to 5 minutes. The total polishing time is 10 to 20 minutes, and finally a sample with a bright surface and no scratches is obtained;

[0040] 7. Anhydrous ethanol cleaning: Place the polished sample in anhydrous ethanol for ultrasonic cleaning for 5 to 10 minutes, and then blow dry and store;

[0041] In steps two, four and six, the same surface of the sample is polished.

[0042] Specific implementation method 2: This implementation method is different from specific implementation method 1 in that in step 2, the sample prepared in step 1 is preliminarily polished using 600#, 800#, 1000#, 1500#, 2000# and 3000# metallographic sandpapers in sequence. The rest is the same as specific implementation method 1.

[0043] Specific implementation method 3: This implementation method is different from specific implementation method 1 or 2 in that: in step 3, the roughly ground sample is ultrasonically cleaned in anhydrous ethanol for 5 minutes. The rest is the same as specific implementation method 1 or 2.

[0044] Specific embodiment 4: This embodiment is different from specific embodiments 1 to 3 in that the diamond spray polishing agent described in step 4 is W0.5 diamond spray polishing agent. The rest is the same as specific embodiments 1 to 3.

[0045] Specific implementation method 5: This implementation method is different from specific implementation method 4 in that: in step 4, the sample needs to be rotated horizontally by 90° every 3 minutes during the polishing process. The rest is the same as specific implementation method 4.

[0046] Specific implementation example 6: This implementation example is different from specific implementation example 5 in that the total polishing time in step 4 is 12 minutes. The rest is the same as specific implementation example 5.

[0047] Specific implementation example 7: This implementation example is different from specific implementation example 6 in that: in step 5, the sample after mechanical polishing is ultrasonically cleaned with anhydrous ethanol for 5 minutes. The rest is the same as specific implementation example 6.

[0048] Specific embodiment 8: This embodiment is different from specific embodiment 7 in that the particle size of the SiO2 sol described in step 6 is 30nm to 50nm. The rest is the same as specific embodiment 7.

[0049] Specific embodiment 9: This embodiment is different from specific embodiment 8 in that: in step 6, the sample is horizontally rotated 90° every 3 minutes during the polishing process, and the total polishing time is 15 minutes. Other aspects are the same as specific embodiment 8.

[0050] Specific embodiment 10: This embodiment differs from specific embodiment 9 in that the rotation speed of the polishing disc during polishing in step 6 is 200 r / min to 300 r / min, and the rubber polishing disc in step 6 is a porous chloroprene rubber polishing disc. The rest is the same as specific embodiment 9.

[0051] The present invention is verified by the following tests:

[0052] Experiment 1: This experiment is a method for preparing EBSD samples with high calibration rate for 7 series aluminum alloy materials. The specific steps are as follows:

[0053] 1. Sample preparation:

[0054] The O-state 7075 aluminum alloy material with a thickness of 5 mm was cut into rectangular small pieces (length and width were 1 cm) to obtain the original sample of the O-state 7075 aluminum alloy electron backscatter diffraction analysis;

[0055] 2. Rough grinding of samples:

[0056] Use 600#, 800#, 1000#, 1500#, 2000# and 3000# metallographic sandpaper to grind the sample prepared in step 1. During the grinding process, the grinding direction should be constantly changed to make the force in each direction uniform until the surface of the sample is flat after rough grinding and the scratch direction is consistent;

[0057] 3. Anhydrous ethanol cleaning:

[0058] The roughly ground samples were ultrasonically cleaned in anhydrous ethanol for 5 min to prevent the debris generated during the grinding process from affecting the subsequent polishing;

[0059] 4. Mechanical polishing:

[0060] After cleaning, the sample was blown dry, and then mechanically polished with W0.5 diamond spray polishing agent. During the polishing process, the sample was rotated 90° horizontally every 3 minutes. The total polishing time was 12 minutes. After polishing, the surface of the sample must be bright and scratch-free.

[0061] 5. Anhydrous ethanol cleaning:

[0062] After mechanical polishing, the sample was ultrasonically cleaned with anhydrous ethanol for 5 min to remove the residual diamond polishing agent on the surface of the sample;

[0063] 6. SiO2 sol polishing:

[0064] The sample cleaned in step 5 is subjected to final polishing on a porous chloroprene rubber polishing disc with SiO2 sol. During the polishing process, SiO2 should not be added too much. During the polishing process, anhydrous ethanol is appropriately sprayed for lubrication. During the polishing process, the sample is horizontally rotated 90° every 3 minutes. The total polishing time is 15 minutes. The polishing disc speed is 300r / min, and finally a sample with a bright surface and no scratches is obtained. The particle size of the SiO2 sol is 50nm;

[0065] 7. Anhydrous ethanol cleaning: Place the polished sample in anhydrous ethanol for ultrasonic cleaning for 5 minutes, and then blow dry and store;

[0066] In steps two, four and six, the same surface of the sample is polished.

[0067] Experiment 2: This experiment is a method for preparing EBSD samples with high calibration rate for 7 series aluminum alloy materials. The specific steps are as follows:

[0068] 1. Sample preparation:

[0069] The cold-rolled 7075 aluminum alloy material with a thickness of 6.35 mm was cut into rectangular small pieces (length and width were 1 cm) to obtain the original sample of cold-rolled 7075 aluminum alloy electron backscatter diffraction analysis;

[0070] 2. Rough grinding of samples:

[0071] Use 600#, 800#, 1000#, 1500#, 2000# and 3000# metallographic sandpaper to grind the sample prepared in step 1. During the grinding process, the grinding direction should be constantly changed to make the force in each direction uniform until the surface of the sample is flat after rough grinding and the scratch direction is consistent;

[0072] 3. Anhydrous ethanol cleaning:

[0073] The roughly ground samples were ultrasonically cleaned in anhydrous ethanol for 5 min to prevent the debris generated during the grinding process from affecting the subsequent polishing;

[0074] 4. Mechanical polishing:

[0075] After cleaning, the sample was blown dry, and then mechanically polished with W0.5 diamond spray polishing agent. During the polishing process, the sample was rotated 90° horizontally every 3 minutes. The total polishing time was 15 minutes. After polishing, the sample surface must be bright and scratch-free.

[0076] 5. Anhydrous ethanol cleaning:

[0077] After mechanical polishing, the sample was ultrasonically cleaned with anhydrous ethanol for 5 min to remove the residual diamond polishing agent on the surface of the sample;

[0078] 6. SiO2 sol polishing:

[0079] The sample cleaned in step 5 is subjected to final polishing on a porous chloroprene rubber polishing disc with SiO2 sol. During the polishing process, not too much SiO2 should be added. During the polishing process, anhydrous ethanol is appropriately sprayed for lubrication. During the polishing process, the sample is horizontally rotated 90° every 3 minutes. The total polishing time is 21 minutes. The polishing disc speed is 300 r / min, and finally a sample with a bright surface and no scratches is obtained. The particle size of the SiO2 sol is 50 nm.

[0080] 7. Anhydrous ethanol cleaning: Place the polished sample in anhydrous ethanol for ultrasonic cleaning for 5 minutes, and then blow dry and store;

[0081] In steps two, four and six, the same surface of the sample is polished.

[0082] Experiment 3: This experiment is a method for preparing EBSD samples with high calibration rate for 7 series aluminum alloy materials. The specific steps are as follows:

[0083] 1. Sample preparation:

[0084] The T6 aged 7075 aluminum alloy material with a thickness of 4.75 mm was cut into rectangular small pieces (length and width were 1 cm) to obtain the original sample of the T6 aged 7075 aluminum alloy electron backscatter diffraction analysis;

[0085] 2. Rough grinding of samples:

[0086] Use 600#, 800#, 1000#, 1500#, 2000# and 3000# metallographic sandpaper to grind the sample prepared in step 1. During the grinding process, the grinding direction should be constantly changed to make the force in each direction uniform until the surface of the sample is flat after rough grinding and the scratch direction is consistent;

[0087] 3. Anhydrous ethanol cleaning:

[0088] The roughly ground samples were ultrasonically cleaned in anhydrous ethanol for 5 min to prevent the debris generated during the grinding process from affecting the subsequent polishing;

[0089] 4. Mechanical polishing:

[0090] After cleaning, the sample was blown dry, and then mechanically polished with W0.5 diamond spray polishing agent. During the polishing process, the sample was rotated 90° horizontally every 3 minutes. The total polishing time was 12 minutes. After polishing, the surface of the sample must be bright and scratch-free.

[0091] 5. Anhydrous ethanol cleaning:

[0092] After mechanical polishing, the sample was ultrasonically cleaned with anhydrous ethanol for 5 min to remove the residual diamond polishing agent on the surface of the sample;

[0093] 6. SiO2 sol polishing:

[0094] The sample cleaned in step 5 is subjected to final polishing on a porous chloroprene rubber polishing disc with SiO2 sol. During the polishing process, SiO2 should not be added too much. During the polishing process, anhydrous ethanol is appropriately sprayed for lubrication. During the polishing process, the sample is horizontally rotated 90° every 3 minutes. The total polishing time is 12 minutes. The polishing disc speed is 200r / min, and finally a sample with a bright surface and no scratches is obtained. The particle size of the SiO2 sol is 50nm;

[0095] 7. Anhydrous ethanol cleaning: Place the polished sample in anhydrous ethanol for ultrasonic cleaning for 5 minutes, and then blow dry and store;

[0096] In steps two, four and six, the same surface of the sample is polished.

[0097] Figure 1 The grain morphology orientation map and inverse pole figure (IPF, Figure 1 In the figure in the upper right corner, the 7075 aluminum alloy was treated in the O state. It can be seen from the figure that a large amount of second phases were precipitated in its structure, indicating that the method of the present invention can be applied to the preparation of EBSD samples of 7 series aluminum alloy materials containing a large amount of precipitated phases.

[0098] Figure 2 The grain morphology orientation map and inverse pole figure (IPF, Figure 2 The upper right corner of the picture), Figure 3 The grain morphology orientation map and inverse pole figure obtained by EBSD analysis of the same aluminum alloy sample prepared by traditional electrolytic polishing as in Experiment 2. The cold-rolled 7075 aluminum alloy contains not only a large amount of MgZn2 second phase ( Figure 2 and Figure 3 The black area in the figure), and the deformation of the grains is also large. The large deformation and the presence of the second phase will have a serious impact on the preparation of aluminum alloy EBSD samples. By comparing the images obtained by the two different preparation methods, it can be seen that the traditional electrolytic polishing preparation method cannot obtain a grain morphology orientation map with a high calibration rate when dealing with such materials. It also proves the superiority of the method of the present invention in the preparation of EBSD samples of 7 series aluminum alloy materials containing a large amount of second phases and large deformation.

[0099] Figure 4 The grain morphology orientation diagram and inverse pole figure of the sample prepared for Experiment 3 are intended to verify that the method of the present invention can also obtain high-quality EBSD samples when applied to 7 series aluminum alloy materials with less second phase content, indicating that the present invention has wide applicability.

Claims

1. A method for preparing EBSD samples with high calibration rate for 7 series aluminum alloy materials. Features The EBSD sample preparation method for 7 series aluminum alloy materials with high calibration rate is carried out in the following steps:

1. Sample preparation: The 7 series aluminum alloy material is cut into rectangular small pieces to obtain the original sample for electron backscatter diffraction analysis of the 7 series aluminum alloy; 2. Rough grinding of samples: Use different types of metallographic sandpaper to preliminarily grind the sample prepared in step 1. During the grinding process, the grinding direction should be constantly changed to make the force in each direction uniform until the surface of the sample is flat after rough grinding and the scratch direction is consistent; 3. Anhydrous ethanol cleaning: The roughly ground sample was ultrasonically cleaned in anhydrous ethanol for 5 to 10 minutes to prevent the debris generated during the grinding process from affecting the subsequent polishing; 4. Mechanical polishing: After cleaning, the sample is blown dry, and then mechanically polished with diamond spray polishing agent. During the polishing process, the sample needs to be rotated 90° horizontally every 3min to 5min. The total polishing time is 10min to 15min. After polishing, the surface of the sample needs to be bright and scratch-free.

5. Anhydrous ethanol cleaning: The mechanically polished samples were ultrasonically cleaned with anhydrous ethanol for 5 to 10 minutes to remove the residual diamond polishing agent on the surface of the samples; 6. SiO 2 Sol polishing: The sample cleaned in step 5 was washed with SiO 2 The sol was final polished on a rubber polishing disc. During the polishing process, anhydrous ethanol was sprayed for lubrication. During the polishing process, the sample was horizontally rotated 90° every 3 to 5 minutes. The total polishing time was 10 to 20 minutes. Finally, a sample with a bright surface and no scratches was obtained.

7. Anhydrous ethanol cleaning: Place the polished sample in anhydrous ethanol for ultrasonic cleaning for 5 to 10 minutes, and then blow dry and store; In steps two, four and six, the same surface of the sample is polished.

2. The EBSD sample preparation method for 7 series aluminum alloy materials with high calibration rate according to claim 1, Features In step 2, the sample prepared in step 1 is preliminarily polished using 600#, 800#, 1000#, 1500#, 2000# and 3000# metallographic sandpaper in sequence.

3. The EBSD sample preparation method for 7 series aluminum alloy materials with high calibration rate according to claim 1, Features In step 3, the coarsely ground sample is ultrasonically cleaned in anhydrous ethanol for 5 minutes.

4. The EBSD sample preparation method for 7 series aluminum alloy materials with high calibration rate according to claim 1, Features The diamond spray polishing agent described in step 4 is W0.5 diamond spray polishing agent.

5. The EBSD sample preparation method for 7 series aluminum alloy materials with high calibration rate according to claim 1, Features In step 4, the sample needs to be rotated horizontally 90° every 3 minutes during the polishing process.

6. The EBSD sample preparation method for 7 series aluminum alloy materials with high calibration rate according to claim 5, Features The total polishing time in step 4 is 12 minutes.

7. The EBSD sample preparation method for 7 series aluminum alloy materials with high calibration rate according to claim 1, Features After mechanical polishing in step 5, the sample was ultrasonically cleaned with anhydrous ethanol for 5 minutes.

8. The EBSD sample preparation method for 7 series aluminum alloy materials with high calibration rate according to claim 1, Features SiO2 as described in step 6 2 The particle size of the sol is 30nm to 50nm.

9. The EBSD sample preparation method for 7 series aluminum alloy materials with high calibration rate according to claim 1, Features During the polishing process in step 6, the sample was rotated horizontally by 90° every 3 minutes, and the total polishing time was 15 minutes.

10. The EBSD sample preparation method for 7 series aluminum alloy materials with high calibration rate according to claim 1, Features During polishing in step 6, the rotation speed of the polishing disc is 200 r / min to 300 r / min; the rubber polishing disc described in step 6 is a porous chloroprene rubber polishing disc.

Citation Information

Patent Citations

  • Preparation method of test sample for testing EBSD of annealed aluminum-steel composite plate interface

    CN108107064A

  • Preparation method for high-nitrogen nickel-free austenitic stainless steel EBSD sample

    CN109030134A

  • Tin-lead and composite material or alloy electron back scattering diffraction sample manufacturing technology

    CN109839393A

  • Method for grinding, polishing and cleaning section of component containing soft metal structure

    CN114720220A

  • Preparation method of aluminum alloy free processing state EBSD sample

    CN116718621A

Cited By

  • Measurement method of high-temperature alloy texture

    CN119936088A