Positive electrode active material and preparation method thereof, positive electrode plate, secondary battery and electric device

By controlling the particle size distribution in the positive electrode active material, the negative impact of micropowder and ultra-large single crystal particles on the circulation performance is solved, the cycle life and stability of the material are improved, and better electrochemical performance is achieved.

CN118969975APending Publication Date: 2024-11-15CONTEMPORARY AMPEREX TECHNOLOGY CO LTD +1
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202311021582.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-15
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

The micropowders and super-large single crystal particles present in existing olivine phosphate-based cathode active materials affect their cyclic performance, resulting in a decay of cycle life, making it difficult to achieve effective separation and improvement in high yields.

Method used

Provide a phosphate-based positive electrode active material, by controlling the primary particle size of 80 nm or more and 180 nm or less, and the particle size distribution of the secondary particles meets (Dv90-Dv10)/ Dv50≤3, to reduce cycle life attenuation and improve mechanical integrity.

Benefits of technology

It significantly improves the cycle life and high-temperature storage performance of the positive electrode active material, slows down the side reaction rate between the micro powder and the electrolyte, and enhances the chemical mechanical stability and electrochemical performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118969975A_ABST
    Figure CN118969975A_ABST
Patent Text Reader

Abstract

The invention provides a positive active material and a preparation method thereof, a positive pole piece, a secondary battery and an electric device. The positive electrode active material comprises at least one of compounds shown as a general formula LizFexMn (1-x-y) MyPO4 (at) C, z is greater than or equal to 1 and less than or equal to 1.1, x is greater than or equal to 0.5 and less than or equal to 1, and y is greater than or equal to 0 and less than or equal to 0.1; m is selected from at least one of Ti, V and Mg; at least one part of the positive electrode active material comprises primary particles, and the particle size distribution of the primary particles with the primary particle size of more than 80 nm and less than 180 nm in the positive electrode active material is less than or equal to 10%; and the number of primary particles with the primary particle size of more than 1500nm in the area of (250 + / -5) mu m < 2 > in the cut section after the positive electrode active material is prepared into a pole piece is not more than 15. The primary particle size distribution concentration ratio of the positive electrode active material provided by the invention is remarkably improved, and the cycle performance of the battery is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of secondary batteries, and in particular to a positive electrode active material and a preparation method thereof, an electrolyte, a secondary battery and an electrical device. Background Art

[0002] Olivine phosphate-based cathode materials have stable structures and good cycle life performance. They are widely used cathode active materials in secondary batteries. As the performance requirements of secondary batteries in energy storage applications increase, how to improve the cycle performance of olivine phosphate-based cathode active materials is a scientific and technological problem that needs to be solved in the current energy storage application field. One of the factors that affect the cycle performance of cathode active materials is the presence of fine powder in the cathode active materials. Due to the rapid decay of cycle life, it restricts the further improvement of the cycle performance of cathode active materials.

[0003] At present, the most common method to improve the powder in the positive electrode active material is to optimize the production process and equipment to reduce the generation of small powder particles during the mixing or transportation of the material. Although the generation of small powder particles can be reduced to a certain extent, the effect is minimal; or, by using a cyclone separation device to remove the small powder particles in the material, but the effect is not good, especially for nanomaterials of lithium iron phosphate or lithium manganese iron phosphate, it is difficult to achieve effective separation at a high yield.

[0004] In addition, the presence of ultra-large single crystal particles in the positive electrode active material affects the mechanical integrity of the positive electrode active material particles and also affects the cycle performance of the positive electrode active material.

[0005] Therefore, it is urgent to improve the content of micropowder and super-large single crystal particles in the positive electrode active material to improve the particle uniformity of the positive electrode active material. Summary of the invention

[0006] The present application aims to solve at least one of the technical problems existing in the background technology. To this end, one purpose of the present application is to provide a phosphate-based positive electrode active material, which has a significant difference in primary particle distribution compared with the current conventional phosphate-based positive electrode active nanomaterials, is evenly distributed, and has a small proportion of micropowder and large particles, which can improve the cycle and high temperature storage performance of the phosphate-based positive electrode active material.

[0007] The first aspect of the present application is to provide a positive electrode active material, including a general formula Li z Fe x Mn (1-x-y) M yAt least one of the compounds shown in PO4@C, wherein 0.5≤x≤1, 0≤y≤0.1, 1≤z≤1.1; M is selected from at least one of Ti, V, and Mg; at least a portion of the positive electrode active material includes primary particles, and the particle size distribution of the primary particles with a primary particle size of more than 80nm and less than 180nm in the positive electrode active material is less than or equal to 10%.

[0008] In the positive electrode active material provided in the present application, the particle size distribution of primary particles with a primary particle size of more than 80nm and less than 180nm in the positive electrode active material powder is controlled within an appropriate range, which helps to reduce or slow down the cycle life decay of small particle positive electrode active substances in the positive electrode active material, slow down the rate of side reactions between the surface of the micropowder and the electrolyte, and thus improve the cycle life of the positive electrode active material.

[0009] In some embodiments, the particle size distribution of primary particles with a primary particle size of 80 nm or more and 180 nm or less in the positive electrode active material is less than or equal to 8.5%, and optionally less than 8%, 6%, 5%, or 2%.

[0010] In some embodiments, the primary particles with a primary particle size of 1500 nm or more in the positive electrode active material are substantially 250 μm in the cross section cut after the positive electrode active material is prepared into a pole piece. 2 The number of particles in the area does not exceed 15, optionally, in the basic 250μm 2 The number of particles in the area does not exceed 12, 8 or 6, optionally 250 μm 2 When measuring, it can have 5μm 2 The region is selected from the cross-sectional end face of the positive electrode active material after it is prepared into a pole piece, and the method of preparing the positive electrode active material into a pole piece is well known in the art.

[0011] Primary particles with a primary particle size of more than 1500nm are prone to particle crushing or pulverization during the circulation of positive electrode active materials, reducing the mechanical integrity of the positive electrode active material particles, thereby causing active material loss. Controlling the particle size distribution of primary particles with a primary particle size of more than 1500nm in the positive electrode active material powder within an appropriate range helps to improve the chemical mechanical stability of the positive electrode active material and improve the electrochemical performance, thereby improving the cycle stability of the positive electrode active material. Excessively large primary particle sizes cause particles to break during the circulation process, resulting in the loss of electrical contact between the crushed particles, which is also an important reason for capacity decay during battery use.

[0012] In some embodiments, the positive electrode active material includes secondary particles, and the particle size distribution of the secondary particles satisfies: (Dv90-Dv10) / Dv50≤3.

[0013] In the positive electrode active material, the particle size distribution of the secondary particles is within a suitable range, which helps to improve the particle size uniformity of the positive electrode active material.

[0014] In some embodiments, the Dv50 of the secondary particles is 0.45 - 1.5 μm, and optionally 0.6 - 1.5 μm.

[0015] In the positive electrode active material, the particle size of the secondary particles is within a suitable range. During charge and discharge, the secondary particles will not or reduce the structural damage caused by excessive lithium deintercalation / insertion, or reduce the polarization degree of the secondary particles during charge and discharge, which helps to make the current density on the surface of the secondary particles more uniform, thereby enabling the positive electrode active material to fully exert its capacity.

[0016] In some embodiments, in the general formula of the positive electrode active material provided in the present application, 0.6 < x ≤ 1, 0 ≤ y < 0.1, 1 ≤ z ≤ 1.1, and optionally 0.8 ≤ x ≤ 1, 0.004 ≤ y ≤ 0.008, 1 ≤ z ≤ 1.08.

[0017] In some embodiments, in the positive electrode active material provided in the present application, the mass content of the M element in the positive electrode active material is 1000 ppm - 6000 ppm, and optionally 1500 ppm - 5000 ppm.

[0018] The mass content of the M element in the positive electrode active material within a suitable range helps to improve the structural stability of the positive electrode active material.

[0019] The second aspect of the present application provides a method for preparing a positive electrode active material. The positive electrode active material prepared by the method includes at least one of the compounds represented by the general formula Li z Fe x Mn (1-x-y) M y PO4@C, where 0.5 ≤ x ≤ 1, 0 ≤ y ≤ 0.1, 1 ≤ z ≤ 1.1; M is selected from at least one of Ti, V, and Mg; at least a part of the positive electrode active material includes primary particles, and the particle size distribution of the primary particles with a primary particle size above 80 nm and below 180 nm in the positive electrode active material is less than or equal to 10%.

[0020] Controlling the particle size distribution of the primary particles with a primary particle size above 80 nm and below 180 nm within the above range in the positive electrode active material powder helps to reduce or slow down the cycle life decay of the small particle positive electrode active substance in the positive electrode active material, thereby improving the cycle life of the positive electrode active material.

[0021] In some embodiments, the particle size distribution of primary particles with a primary particle size of 80 nm or more and 180 nm or less in the positive electrode active material is less than or equal to 8.5%, and may be 8%, 6%, 5%, 4%, or less than 2%. The smaller the particle size distribution of primary particles with a primary particle size of 80 nm or more and 180 nm or less in the positive electrode active material, the more conducive it is to improving the cycle life of the positive electrode active material, and to maintaining the stability of the cycle life of the positive electrode active material.

[0022] In some embodiments, in the positive electrode active material prepared by the method, the primary particles with a primary particle size of 1500 nm or more are (250±5) μm in the cross section cut after the positive electrode active material is prepared into a pole piece. 2 The number of particles in the area does not exceed 15, optionally, in the basic 250μm 2 The number of particles in the area does not exceed 12, 8 or 6.

[0023] Controlling the particle size distribution of primary particles with a primary particle size of more than 1500 nm in the positive electrode active material powder within the above range helps to improve the chemical mechanical stability of the positive electrode active material and improve the electrochemical performance, thereby improving the cycle stability of the positive electrode active material.

[0024] In some embodiments, the preparation method comprises the following steps:

[0025] The raw materials including lithium source, iron source, manganese source, phosphorus source, carbon source, M source and molding aid are compacted and granulated to obtain compacted particles with an average particle size of 3mm-30mm, optionally 5mm-15mm.

[0026] Compacting the formed particles within a suitable range helps to improve the uniformity of different raw materials inside the particles. At the same time, the pores between the particles are conducive to removing the reducing gas produced by the decomposition of the carbon source during the preparation process, and the uniformity of carbon at different positions of the sintering device (such as the sagger) is improved.

[0027] In some embodiments, the compacted shaped particles have a compacted density of 1.0 g / cm 3 Above, optional 1.2-3.0g / cm 3 .

[0028] The compaction density of the compacted particles is controlled within a suitable range, which helps to increase the filling amount during the preparation process, thereby increasing the sintering capacity.

[0029] In some embodiments, the preparation method comprises: filling the compacted particles to a filling height of 5 cm to 30 cm, and sintering the compacted particles to obtain secondary particles;

[0030] Optionally, the filling height is 8cm-20cm.

[0031] The filling height of the compacted particles during the sintering process is within an appropriate range, which helps to timely discharge the reducing gas generated by the decomposition of the carbon source during the sintering process, while accelerating heat transfer and avoiding uneven decomposition of the carbon source in the compacted particles at different positions in the sintering device, thereby improving the consistency of particle growth while taking into account production capacity.

[0032] In some embodiments, the preparation method includes: crushing the secondary particles to make their Dv50 0.45 μm-1.5 μm, optionally 0.6 μm-1.5 μm. When the secondary particles are crushed to a particle size within the range, the secondary particles will not or will reduce structural damage caused by excessive lithium extraction during the charge and discharge process, or reduce the polarization degree of the secondary particles during the charge and discharge process, which helps to give full play to the capacity of the positive electrode active material.

[0033] In some embodiments, the preparation method comprises: crushing the secondary particles so that their particle size distribution satisfies:

[0034] (Dv90-Dv10) / Dv50≤3; Optionally, the secondary particles are crushed to make their particle size distribution satisfy: 1≤Dv90-Dv10) / Dv50≤3. Crushing the secondary particles to make their particle size distribution within the range helps to improve the particle size uniformity of the positive electrode active material and the cycle stability of the positive electrode active material.

[0035] In some embodiments, the preparation method does not include multiple compaction granulation.

[0036] In some embodiments, the preparation method does not include pre-sintering. Optionally, no pre-sintering process is performed before the compaction and granulation process.

[0037] The preparation method provided in the present application has a simple process flow, high reproducibility, and relatively low cost, which is conducive to industrial mass production.

[0038] The third aspect of the present application provides a positive electrode plate, which includes the positive electrode active material provided in the first aspect of the present application, or includes the positive electrode active material prepared by the method provided in the second aspect of the present application.

[0039] The fourth aspect of the present application provides a secondary battery, comprising a negative electrode plate and the positive electrode plate provided in the third aspect of the present application.

[0040] The fifth aspect of the present application provides an electrical device, comprising the secondary battery provided in the fourth aspect of the present application.

[0041] The above description is only an overview of the technical solution of the present application. In order to more clearly understand the technical means of the present application, it can be implemented in accordance with the contents of the specification. In order to make the above and other purposes, features and advantages of the present application more obvious and easy to understand, the specific implementation methods of the present application are listed below. BRIEF DESCRIPTION OF THE DRAWINGS

[0042] In the accompanying drawings, unless otherwise specified, the same reference numerals throughout the multiple drawings represent the same or similar parts or elements. These drawings are not necessarily drawn to scale. It should be understood that these drawings only depict some embodiments disclosed in the present application and should not be regarded as limiting the scope of the present application.

[0043] Figure 1 is a schematic diagram of sintering of compacted particles in a sintering device in the present application;

[0044] Figure 2 is a scanning electron microscope (SEM) photograph of the positive electrode active material in Example 1 of the present application;

[0045] Figure 3 This is a scanning electron microscope photograph of the cross section of the positive electrode active material after being prepared into a positive electrode sheet in Example 1 of the present application; Figure 3 The electron microscopic scale in A is 2 μm; Figure 3 The electron microscopic scale in B is 500 nm;

[0046] Figure 4 This is a scanning electron microscope photograph of the cross section of the positive electrode active material after being prepared into a positive electrode sheet in Comparative Example 1 of the present application; Figure 4 The electron microscope scale in A is 1 μm; Figure 4 The electron microscopic scale in B is 200 nm;

[0047] Figure 5 It is the cycle performance test curve of the secondary battery in Example 1 and Comparative Example 1 of the present application at 25° C. and 60° C.;

[0048] Figure 6 is a schematic diagram of a secondary battery cell according to an embodiment of the present application;

[0049] Figure 7 yes Figure 6 An exploded view of a secondary battery cell according to an embodiment of the present application is shown;

[0050] Figure 8 is a schematic diagram of a battery module according to an embodiment of the present application;

[0051] Fig. 9 is a schematic diagram of a battery pack according to an embodiment of the present application;

[0052] Fig.10yes Fig. 9 An exploded view of a battery pack according to an embodiment of the present application is shown;

[0053] Fig.11 is a schematic diagram of an electrical device using a secondary battery according to an embodiment of the present application as a power source;

[0054] Fig.12 is a SEM photograph of a cross section of a secondary battery in one embodiment of the present application;

[0055] Description of reference numerals:

[0056] 1 battery pack; 2 upper box; 3 lower box; 4 battery module; 5 secondary battery; 51 shell; 52 electrode assembly; 53 cover plate; 6 compacted particles; 7 sagger. DETAILED DESCRIPTION

[0057] The following embodiments of the technical solution of the present application are described in detail in conjunction with the accompanying drawings. The following embodiments are only used to more clearly illustrate the technical solution of the present application, and are therefore only used as examples, and cannot be used to limit the scope of protection of the present application.

[0058] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by technicians in the technical field to which this application belongs; the terms used herein are only for the purpose of describing specific embodiments and are not intended to limit this application; the terms "including" and "having" in the specification and claims of this application and the above-mentioned figure descriptions and any variations thereof are intended to cover non-exclusive inclusions.

[0059] Reference to "embodiments" herein means that a particular feature, structure, or characteristic described in conjunction with the embodiments may be included in at least one embodiment of the present application. The appearance of the phrase in various locations in the specification does not necessarily refer to the same embodiment, nor is it an independent or alternative embodiment that is mutually exclusive with other embodiments. It is explicitly and implicitly understood by those skilled in the art that the embodiments described herein may be combined with other embodiments.

[0060] In the description of the embodiments of the present application, the term "and / or" is only a description of the association relationship of the associated objects, indicating that there may be three relationships. For example, A and / or B can represent: A exists alone, A and B exist at the same time, and B exists alone. In addition, the character " / " in this article generally indicates that the associated objects before and after are in an "or" relationship.

[0061] "Scope" disclosed in the present application is limited in the form of lower limit and upper limit, and a given range is limited by selecting a lower limit and an upper limit, and the selected lower limit and upper limit define the boundary of a special range. The scope limited in this way can be including end values ​​or not including end values, and can be arbitrarily combined, that is, any lower limit can be combined with any upper limit to form a scope. For example, if the scope of 60-120 and 80-110 is listed for a specific parameter, it is understood that the scope of 60-110 and 80-120 is also expected. In addition, if the minimum range values ​​1 and 2 are listed, and if the maximum range values ​​3, 4 and 5 are listed, the following scope can be all expected: 1-3, 1-4, 1-5, 2-3, 2-4 and 2-5. In the present application, unless otherwise specified, the numerical range "ab" represents the abbreviation of any real number combination between a and b, wherein a and b are real numbers. For example, the numerical range "0-5" means that all real numbers between "0-5" are listed in this document, and "0-5" is just an abbreviation of these numerical combinations. In addition, when a parameter is expressed as an integer ≥ 2, it is equivalent to disclosing that the parameter is, for example, an integer of 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, etc.

[0062] If there is no special explanation, all steps of the present application can be performed sequentially or randomly, preferably sequentially. For example, the method includes steps (a) and (b), which means that the method may include steps (a) and (b) performed sequentially, or may include steps (b) and (a) performed sequentially. For example, the method may further include step (c), which means that step (c) may be added to the method in any order. For example, the method may include steps (a), (b) and (c), or may include steps (a), (c) and (b), or may include steps (c), (a) and (b), etc.

[0063] If there is no special explanation, the "include" and "comprising" mentioned in this application are open-ended or closed-ended. For example, the "include" and "comprising" may mean that other components not listed may also be included or only the listed components may be included or only the listed components may be included.

[0064] Positive electrode active material

[0065] Multiple factors can affect the cycle performance of positive electrode active materials, such as the residual alkali content on the surface of the material, the integrity of the crystal structure of the material, the content of micropowder in the material, and the water content adsorbed on the surface of the material. Among them, the content of micropowder, that is, the proportion of small particles in all particles, is an important factor restricting the further improvement of battery cyclability. This is because in the synthesis reaction of positive electrode active materials, the embedding energy barrier of lithium ions in particles with smaller particle sizes is lower and the reaction activity is higher, resulting in the transition of lithium ions into lithium in micropowders, excessive Li content in small micropowder particles, and insufficient Li content in other particles with particle sizes larger than the micropowder particle size, that is, uneven lithium distribution. During the charging process, due to polarization, small particles are always over-de-lithiated and the structure is destroyed, and the side reactions of small particles in the charged state with the electrolyte are more intense, which is more obvious at high temperatures, resulting in a faster decay of the cycle life of small particles. Therefore, controlling the content of micropowder in positive electrode active materials helps to improve the cycle performance in energy storage devices (e.g., secondary batteries).

[0066] The present application provides a carbon-coated (@C) phosphate-based positive electrode active material, including a general formula Li z Fe x Mn (1-x-y) M y At least one of the compounds shown in PO4@C, wherein 0.5≤x≤1, 0≤y≤0.1, 1≤z≤1.1; M is selected from at least one of Ti, V, and Mg; at least a portion of the positive electrode active material includes primary particles, and the particle size distribution of the primary particles with a primary particle size of more than 80nm and less than 180nm in the positive electrode active material is less than or equal to 10%.

[0067] In some embodiments, the particle size distribution of primary particles with a primary particle size of greater than 80 nm and less than 180 nm in the positive electrode active material is less than or equal to 9.5%, 9%, 8.5%, 8%, 7%, 6%, 5%, 4%, 3%, 2% or 1%, or the particle size distribution of primary particles with a primary particle size of greater than 80 nm and less than 180 nm in the positive electrode active material is selected from 0.1%-10%, 0.5%-10%, 1%-10%, 0.1%-8%, 0.1%-6%, 0.1%-4%, 0.1%-3%, 0.1%-2%, 0.1%-1%, 0.3%-5%, 0.8%-3%, or 0.1%-1.5%.

[0068] The term "primary particle" is also called a single crystal particle, and usually a single fine grain is called a primary particle. In some cases, even if it is an amorphous particle, when there are primary particles and agglomerated particles, the primary particles can also be called primary particles.

[0069] Agglomerated particles formed by agglomeration of multiple primary particles or primary particles are called "secondary particles". The force for agglomeration between particles can be physical bonding (such as van der Waals force) or chemical bonding (such as bridging oxygen bond); the method for agglomeration between particles can be external pressure or other substances (such as sticky chemicals) to assist agglomeration. The particle size of secondary particles is called "secondary particle size".

[0070] Herein, the term "primary particle size" refers to the particle size of primary particles.

[0071] In the present application, the terms "micropowder", "small particles" and "micropowder small particles" have the same meaning, and refer to particles with a particle size of more than 80 nm and less than 180 nm, and the particles include primary particles and secondary particles.

[0072] The term "particle size distribution" refers to the percentage of particles within a certain particle size or a certain particle size range in the total number of powder particles.

[0073] The particle size distribution can be determined by a commonly used detection method in the art, such as a laser particle size analyzer, to determine the particle size distribution of powder particles.

[0074] The particle size distribution can also be measured by the long diameter statistical method, which can measure the particle size of the active material in the electrode membrane. In some embodiments, the electrode can be cut by an argon ion beam perpendicular to the electrode plane (for example, a plane with a relatively large area), and the exposed section is photographed using a scanning electron microscope. The longer diameter in the particle cross section is used as the long diameter of the particle, and the particle size of the particle is measured and counted. Particles below 80nm are difficult to distinguish one by one when taking pictures using a scanning electron microscope. In this case, particles below 80nm can be excluded from the statistics when the particle size distribution is determined using the long diameter statistical method.

[0075] In the positive electrode active material provided in the present application, the particle size distribution of primary particles with a primary particle size of more than 80nm and less than 180nm in the positive electrode active material powder is controlled within 10%, which helps to reduce the number of micropowders whose structures are destroyed due to excessive delithiation during charging, reduce the side reactions between micropowders and electrolytes, delay the cycle life attenuation of the positive electrode active material, and thus improve the cycle life of the positive electrode active material.

[0076] As mentioned above, the high activity of micropowder in the reaction leads to uneven distribution of lithium in the positive electrode active material, which also affects the surface state of the positive electrode active material. When the powder content is too high, the alkalinity of the positive electrode active material increases due to the high lithium content, and the side reaction of the binder increases, which deteriorates the processing performance of the slurry and causes the slurry viscosity to increase rapidly. In severe cases, gelation may occur. Controlling the particle size distribution of micropowder within an appropriate range also helps to improve the processing performance of the positive electrode active material.

[0077] In some embodiments, in the positive electrode active material, the primary particle size of the particles is 1500 nm or more and the primary particle size is substantially 250 μm. 2 The number of particles in the area does not exceed 15, optionally, in the area of ​​250 μm 2 The number of particles in the area does not exceed 12, 10, 9, 8, 7, 6, 5, 4, 3, or 2. "Basic" indicates the measurement error or the degree of fluctuation during measurement, which can be selected as 5μm 2 The "region" refers to the region in the cross section after the positive electrode active material is prepared into a pole piece, and the region is used to measure the number of large particles. The method of preparing a positive electrode active material into a pole piece is well known in the art.

[0078] In some embodiments, the positive electrode active material can be prepared into a pole piece according to the method disclosed in Example 1. In some embodiments, the positive electrode material powder and polyvinylidene fluoride (PVDF) binder can be mixed in a mass ratio of 95:5, and N-methylpyrrolidone is used as a solvent to prepare a pole piece, and cold pressed to a compaction density of 2.2 g / cm 3 .

[0079] In some embodiments, in the positive electrode active material, the primary particles with a primary particle size of 1500 nm or more are substantially 250 μm. 2 The number of particles in the area does not exceed 0-2, 0-3, 1-2, 1-3, 2-3, 0-4, 2-4, 3-4, 0-5, 2-5, 0-6, 5-6, 6-8, 8-14.

[0080] The number of particles with a primary particle size of more than 1500nm can be counted by scanning electron microscopy (SEM), for example, by using an argon ion beam to cut the pole piece perpendicular to the large surface of the pole piece to expose the end face, taking a picture of the end face with SEM, and using the long diameter statistical method to count the particle size. The number of large particles can be determined by a single measurement, or by taking the average value of multiple measurements.

[0081] Primary particles with a primary particle size of more than 1500nm are also called "large particles", "super-large single crystal particles" or "super-large primary particles". During the cycle process, the positive electrode material undergoes a deformation process of repeated expansion and contraction. Super-large primary particles undergo intergranular cracks due to deformation during the cycle process, which in turn causes severe pulverization of the super-large primary particles. This seriously reduces the mechanical integrity of the primary and secondary particles, aggravates the penetration of the electrolyte, and leads to a large loss of positive electrode active materials (for example, lithium ions). At the same time, the presence of intergranular cracks also causes electrical contact failure, aggravating capacity polarization losses. Correspondingly, the continuous generation of new electrode / electrolyte interfaces also leads to a sharp deterioration in the chemical and mechanical properties of the positive electrode active materials during long cycles.

[0082] Controlling the particle size distribution of primary particles with a primary particle size of more than 1500nm in the cathode active material powder within an appropriate range can effectively prevent particle breakage, alleviate surface degradation, and inhibit intergranular cracking, thereby enhancing chemical mechanical stability and improving electrochemical performance. Interface degradation and overall mechanical disintegration effects are inhibited, chemical mechanical stability is enhanced, and the cycle stability of the cathode active material can be improved.

[0083] In some embodiments, the positive electrode active material includes secondary particles, and the particle size distribution of the secondary particles satisfies: (Dv90-Dv10) / Dv50≤3, optionally, less than or equal to 2.9, 2.8, 2.6, 2.5, 2.4, 2.3, 2.2, 1.4, 1.5 or 1.2. Optionally, 1≤(Dv90-Dv10) / Dv50≤3.

[0084] In the positive electrode active material, the particle size distribution of the secondary particles is within a suitable range, which helps to improve the particle size uniformity of the positive electrode active material and further improve the cycle performance.

[0085] In some embodiments, the Dv50 of the secondary particles is 0.45-1.5 μm, optionally 0.5-1.5 μm, 0.8-1.5 μm, 0.7-1.5 μm, 1-1.5 μm, 0.45-1.3 μm, 0.45-1.0 μm, 0.5-1.0 μm, 0.6-1.5 μm or 0.7-1.5 μm, or any value within the range.

[0086] In the positive electrode active material, the particle size of the secondary particles is within a suitable range, and during the charge and discharge process, the secondary particles will not or will reduce structural damage caused by excessive lithium extraction. In addition, it helps to reduce the polarization degree of the secondary particles during the charge and discharge process, and helps to make the current density on the surface of the secondary particles more uniform, so as to give full play to the capacity of the positive electrode active material and improve the cycle performance.

[0087] In the positive electrode active material provided by the present application, while reducing the particle size distribution of fine powder and large particles, the particle size distribution concentration of the positive electrode active material is significantly improved.

[0088] In some embodiments, the positive electrode active material may be one or more of lithium iron phosphate or lithium iron manganese phosphate with an olivine structure and their modified compounds, which can improve the rate performance of the battery while enhancing the cycle performance and storage performance of the battery. The working voltage of the battery using these positive electrode active materials is not high, generally ≤ 4.35V, so the cycle performance and storage performance of the battery can be further improved.

[0089] In some embodiments, in the positive electrode active material provided by the present application, 0.6 < x ≤ 1, 0 ≤ y < 0.1, 1 ≤ z ≤ 1.1, and optionally 0.8 ≤ x ≤ 1, 0.004 ≤ y ≤ 0.008, 1 ≤ z ≤ 1.08.

[0090] In some embodiments, in the positive electrode active material provided by the present application, the mass content of the M element in the positive electrode active material is selected from 1000 ppm - 6000 ppm, and optionally 1000 ppm - 5500 ppm, 1000 ppm - 5000 ppm, 1500 ppm - 6000 ppm, 1500 ppm - 5000 ppm, 2000 ppm - 6000 ppm, 2500 ppm - 6000 ppm, or 2000 ppm - 5500 ppm, or any value within the range.

[0091] In some embodiments, the M includes Ti. In some embodiments, the M includes V. In some embodiments, the M includes Mg.

[0092] The main body of the anion part of the positive electrode active material is a phosphate matrix, and the metal matrix is mainly composed of iron, manganese or a combination of both. By introducing divalent or multivalent M cations, the lithium ions are inserted and extracted in the olivine structure matrix composed of cations including M and anions including phosphoric acid, which helps to improve the structural stability of the positive electrode active material.

[0093] Preparation method of positive electrode active material

[0094] The present application provides a preparation method of a carbon-coated (@C) phosphate-based positive electrode active material, and the positive electrode active material includes at least one of the compounds represented by the general formula Li z Fe x Mn (1-x-y) M y PO4@C, where 0.5 ≤ x ≤ 1, 0 ≤ y ≤ 0.1, 1 ≤ z ≤ 1.1; M is selected from at least one of Ti, V, and Mg.

[0095] In the cathode active material of some embodiments, 0.6 < x ≤ 1, 0 ≤ y < 0.1, optionally 0.8 ≤ x ≤ 1,

[0096] 0.004 ≤ y ≤ 0.008, 1 ≤ z ≤ 1.08. In some embodiments, the M is selected from Ti. In some embodiments, the M is selected from V. In some embodiments, the M is selected from Mg.

[0097] In the cathode active material of some embodiments, the mass content of the M element in the cathode active material is 1000 ppm - 6000 ppm, optionally 1000 ppm - 5500 ppm, 1000 ppm - 5000 ppm, 1500 ppm - 6000 ppm, 1500 ppm - 5000 ppm, 2000 ppm - 6000 ppm, 2500 ppm - 6000 ppm, or 2000 ppm - 5500 ppm, or any value within the range.

[0098] The main body of the anion part of the cathode active material is a phosphate matrix, and the metal matrix is mainly composed of iron, manganese, or a combination of both. By introducing divalent or polyvalent M cations, lithium ions are intercalated and deintercalated in the olivine - structured matrix composed of M - containing cations and phosphate - containing anions, which helps to improve the structural stability of the cathode active material.

[0099] In some embodiments, the cathode active material can be one or more of lithium iron phosphate or lithium iron manganese phosphate with an olivine structure and their modified compounds, which can improve the rate performance of the battery while enhancing the cycle performance and storage performance of the battery. The working voltage of the battery using these cathode active materials is not high, generally ≤ 4.35V, so the cycle performance and storage performance of the battery can be further improved.

[0100] The preparation method provided by this application includes the following steps:

[0101] Compacting and granulating the raw materials including a lithium source, an iron source, a manganese source, a phosphorus source, a carbon source, an M source, and a shaping aid to obtain compacted and formed particles.

[0102] Generally speaking, a compacted particle is an actual particle group composed of particles of different sizes and shapes. Compared with an imaginary particle group composed of uniform spherical particles, if the total length of the particle diameter of the two is the same, the diameter of the spherical particle is the average particle diameter of the actual particle group (compacted particle). For spherical particles, there is no doubt that the spherical diameter is the particle diameter of the particle, but in fact, there are no real spherical particles, and the shape of the actual particles is very complex. For convenience, this application uses an equivalent particle diameter to describe the particle size (particle size) or average particle diameter of irregular particles. It can be understood that when the physical properties or physical behavior of a particle is closest to a homogeneous sphere of a certain diameter, the diameter (or combination) of the sphere is taken as the equivalent particle diameter of the measured particle.

[0103] The average particle size can be determined by a particle size determination method or instrument commonly used in the art, including but not limited to a laser particle size analyzer and an ultrasonic particle size analyzer. The average particle size can be a linear average diameter, an area average diameter, a volume average diameter, a weight average diameter, or a specific surface average diameter. The average particle size in this application refers to a volume average diameter. When an equivalent particle size is used to describe the particle size, the average particle size in this application can also be a volume equivalent diameter.

[0104] In some embodiments, the lithium source includes at least one of lithium carbonate, lithium hydroxide, lithium phosphate, lithium dihydrogen phosphate, lithium oxide, lithium chloride, lithium nitrate, and lithium sulfate. Optionally, the lithium source includes lithium carbonate.

[0105] In some embodiments, the iron source includes at least one of ferric phosphate, ferrous hydroxide, ferrous nitrate, ferrous phosphate, ferrous pyrophosphate, ferrous carbonate, ferrous chloride, ferrous oxalate, ferric chloride, ferric hydroxide, ferric nitrate, ferric citrate, and ferric oxide. Optionally, the iron source includes ferric oxide.

[0106] In some embodiments, the manganese source includes at least one of manganese dioxide, manganese trioxide, manganese tetraoxide, manganese oxalate, manganese acetate, or manganese nitrate.

[0107] In some embodiments, the phosphorus source includes at least one of phosphoric acid, diammonium hydrogen phosphate, ammonium dihydrogen phosphate, iron phosphate, lithium dihydrogen phosphate, and lithium phosphate. Optionally, the phosphorus source includes ammonium dihydrogen phosphate.

[0108] In some embodiments, the carbon source includes at least one of sucrose, glucose, citric acid, fructose, lactose, porous graphene, activated carbon, activated carbon fiber, mesoporous carbon, carbon nanotubes, carbon molecular sieves, asphalt and polyethylene glycol. Optionally, the carbon source includes sucrose.

[0109] In some embodiments, the M source is selected from at least one of oxides, hydroxides, oxalates, acetates, chlorides, nitrates or phosphates of Ti, V, and Mg elements. Optionally, the M source includes one or more of titanium dioxide, magnesium hydroxide, and vanadium pentoxide.

[0110] The molding aid is selected from a high molecular substance that can be dissolved or dispersed in water or alcohol. In some embodiments, the molding aid includes at least one of polypropylene, starch, phenolic resin, polyurethane, melamine resin, polyethylene, stearic acid, PVC, polyacrylonitrile, natural rubber, styrene-butadiene rubber, and butadiene rubber. Optionally, the molding aid includes starch.

[0111] The molding aid can further improve the integrity of the compacted particles during the sintering process, enhance the mechanical stability of the compacted particles during the sintering process, and avoid structural collapse of the particles during the sintering process.

[0112] In some embodiments, raw materials including lithium source, iron source, manganese source, phosphorus source, carbon source, M source and molding aid are ground; optionally, the raw materials are ground to a Dv50 of 0.3-1.5 μm, 0.3-1.0 μm, 0.3-0.8 μm, 0.35-0.6 μm, or 0.35-0.9 μm. The raw materials can be ground using a grinding device such as a ball mill, a sand mill, or a mechanical mill.

[0113] In some embodiments, water, alcohol solvents or a uniform and stable mixed solution of the two can be added, mixed evenly with the raw materials and then ground. The alcohol solvents include but are not limited to methanol, ethanol, and ethylene glycol, and can be used after mixing one or more different alcohol solvents.

[0114] In some embodiments, the molding aid in the raw material can be dissolved or dispersed in water, alcohol solvent or a uniform and stable mixed solution of the two, and mixed with other components in the raw material as the solvent or solution is added.

[0115] After grinding, the particle size of the super-large primary particles becomes smaller, reducing the content of super-large primary particles in the raw materials, which helps to reduce the particle size distribution of super-large primary particles in the prepared positive electrode active material; reducing the particle size of different raw materials, which helps to obtain nano-level primary particles with more uniform particle size. At the same time, the uniformity of mixing different raw materials is improved, which helps to improve the uniformity of different components in the prepared positive electrode active material.

[0116] In some embodiments, the ground raw material is dried, and optionally, the ground raw material is spray dried. In some embodiments, the microsphere particle size Dv50 formed by spray drying is 5-50 μm, optionally, 5-40 μm, 8-30 μm, 10-25 μm, or 10-20 μm.

[0117] The raw materials treated by spray drying are spherical in shape with good fluidity, and there are suitable pores between the raw material particles, which are conducive to the discharge of reducing gases generated by the decomposition of the carbon source during the sintering process.

[0118] In some embodiments, the raw material after the spray drying process is compacted and granulated.

[0119] In some embodiments, raw materials including lithium source, iron source, manganese source, phosphorus source, carbon source, M source and molding aid are compacted and granulated to obtain compacted particles with an average particle size of 3mm-30mm, optionally 5mm-25mm, 5mm-20mm, 5mm-15mm, 10mm-15mm, 10mm-20mm, 10mm-25mm. The average particle size can also be selected from any value of 7.5mm, 12.5mm, 17.5mm, 22.5mm, 27.5mm, or a range between any two values.

[0120] When the average particle size of the compacted particles is less than 3 mm, the pores formed by the bridges between the particles are small, and the improvement in gas removal is not obvious; when the average particle size of the compacted particles is greater than 30 mm, the uniformity of the nanoparticles inside a single compacted particle cannot be guaranteed, and the exhaust capacity of a single compacted particle is significantly reduced. Compacted particles within a suitable range help improve the uniformity of different raw materials inside the particles, and the pores between the particles are conducive to removing the reducing gas generated by the decomposition of the carbon source during the preparation process.

[0121] In some embodiments, the compacted granules obtained by compaction granulation have a compaction density of 1.0 g / cm 3 Above, optional 1.2-3.0g / cm 3 .

[0122] The compaction density of the compacted particles is controlled within a suitable range, which helps to increase the filling amount during the preparation process, thereby increasing the sintering capacity.

[0123] In some embodiments, the preparation method comprises: filling the compacted particles to a filling height of 5 cm to 30 cm, and sintering the compacted particles to obtain secondary particles. Optionally, the filling height is 8 cm to 30 cm.

[0124] 8cm-20cm, 5cm-25cm, 5cm-20cm, 10cm-30cm, 10cm-25cm or 10cm-20cm.

[0125] Figure 1 The schematic diagram of sintering the compacted particles in a filling component of a sintering device, such as a sagger, is shown. The sagger 7 is generally made of graphite and is used to hold the compacted particles 6. At this time, pores can be formed between the compacted particles 6. The reducing gas and other gaseous substances generated by the decomposition of the carbon source during the sintering process can be discharged from the pores to the sagger. Figure 1 The gas rises and transfers heat to the compacted particles 6 on the top layer of the sagger 7. When the gas is not discharged smoothly, the temperature of each part of the sagger 7 is uneven, which may also lead to a high content of reducing gas on the top layer of the sagger 7. The filling height of the compacted particles within a suitable range helps to timely discharge reducing gas and other gaseous unexpected substances during the sintering process, accelerates heat transfer, and avoids uneven decomposition of carbon sources in the compacted particles at different positions in the sintering device, which can improve the consistency of particle growth and take into account production capacity at the same time.

[0126] In some embodiments, after filling and compacting the shaped particles, the porosity between the particles is 5%-20%, optionally, the porosity is selected from 5%-15%, 10%-20%, 10%-15%, 8%-20%, 12%-20% or 8%-17%.

[0127] In some embodiments, the compacted particles are sintered in an inert gas atmosphere, and the inert gas may include one or more of nitrogen, carbon dioxide, and helium. Optionally, the inert gas is selected from nitrogen.

[0128] In some embodiments, the compacted particles are sintered within a sintering temperature range of 600°C-800°C. Optionally, the sintering temperature is selected from 650°C-800°C, 680°C-800°C, 700°C-800°C, 600°C-780°C, 600°C-750°C, 620°C-800°C or 640°C-720°C.

[0129] In some embodiments, the compacted particles are sintered at a sintering temperature range of 600°C-800°C for 2-12 hours, optionally, sintered at the sintering temperature for 2-10 hours, 4-12 hours, 2-10 hours, 4-8 hours, 6-12 hours, 6-10 hours or 6-8 hours.

[0130] In some embodiments, during the sintering process, the heating rate is controlled at 1°C-5°C / min to the sintering temperature. Optionally, the heating rate is selected from 2°C-5°C / min, 3°C-5°C / min, 2°C-4°C / min or 2°C-3°C / min; or, the heating rate is selected from 2°C / min, 2.5°C / min, 3°C / min, 3.5°C / min, or a range between any two of the values.

[0131] In the preparation method provided by the present application, the raw material mixture is compacted and granulated before sintering, which is conducive to the timely discharge of reducing gas from the decomposition of the carbon source during the sintering process, avoiding uneven decomposition of the carbon source at different positions of the sintering device; at the same time, the compacted particles at different positions of the sintering device are heated evenly. After sintering, the carbon content in the surface, middle, and bottom particles tends to be at a consistent level, and the carbon content tends to be consistent, which has a basically consistent effect on the growth inhibition of the raw material particles during the sintering reduction process, and the uniformity of the carbon content of the primary particle nanomaterial is improved.

[0132] In some embodiments, the preparation method includes: crushing the secondary particles obtained after sintering so that their Dv50 is 0.45μm-1.5μm, optionally, crushing to a Dv50 selected from 0.5-1.5μm, 0.8-1.5μm, 0.7-1.5μm, 1-1.5μm, 0.45-1.3μm, 0.45-1.0μm, 0.5-1.0μm, 0.6-1.5μm or 0.7-1.5μm.

[0133] If DV50 is too small, the overall particle size is low, the proportion of small particles increases, and the surface stability of the material decreases; if DV50 is too large, the overall particle size is low, the proportion of large particles increases, and the particle breakage effect increases during the circulation process, both of which are not conducive to improving material stability.

[0134] The particle size of the secondary particles is crushed to a suitable range, and during the charge and discharge process, the secondary particles will not or will reduce the structural damage caused by excessive lithium extraction. In addition, it helps to reduce the polarization degree of the secondary particles during the charge and discharge process, helps to make the current density on the surface of the secondary particles more uniform, and helps to improve the stability of the material, thereby giving full play to the capacity of the positive electrode active material and improving the cycle performance.

[0135] In some embodiments, the preparation method comprises: crushing the secondary particles so that their particle size distribution satisfies:

[0136] (Dv90-Dv10) / Dv50≤3, optionally, less than or equal to 2.9, 2.8, 2.6, 2.5, 2.4, 2.3, 2.2, 2, 1.8, 1.4, 1.2 or 1.5. Optionally, the secondary particles are crushed to have a particle size distribution that satisfies: 1≤(Dv90-Dv10) / Dv50≤3.

[0137] In the positive electrode active material, the particle size distribution of the secondary particles is within a suitable range, which helps to improve the particle size uniformity of the positive electrode active material and further improve the cycle performance.

[0138] In some embodiments, the preparation method includes crushing the sintered secondary particles so that at least a portion of the obtained positive electrode active material includes primary particles, and the particle size distribution of primary particles with a primary particle size of more than 80nm and less than 180nm in the positive electrode active material is less than or equal to 10%.

[0139] In some embodiments, the particle size distribution of primary particles with a primary particle size of greater than 80 nm and less than 180 nm in the positive electrode active material is less than or equal to 9.5%, 9%, 8.5%, 8%, 7%, 6%, 5%, 4%, 3%, 2% or 1%, or the particle size distribution of primary particles with a primary particle size of greater than 50 nm and less than 200 nm in the positive electrode active material is selected from 0.1%-10%, 0.5%-10%, 1%-10%, 0.1%-8%, 0.1%-6%, 0.1%-4%, 0.1%-3%, 0.1%-2%, 0.1%-1%, 0.3%-5%, 0.8%-3%, or 0.1%-1.5%.

[0140] In the positive electrode active material prepared by the preparation method provided in the present application, the particle size distribution of the micropowder is significantly reduced, the side reaction between the micropowder and the electrolyte is reduced, the cycle life attenuation of the positive electrode active material is delayed, and the cycle life of the positive electrode active material is improved.

[0141] At the same time, the positive electrode active material prepared by the method reduces the particle size distribution of the micropowder, reduces the side reaction between the positive electrode active material and the binder, and improves the processing performance of the positive electrode active material.

[0142] In some embodiments, the secondary particles are crushed so that in the obtained positive electrode active material, the particles with a primary particle size of 1500 nm or more are substantially 250 μm. 2 The number of particles in the area does not exceed 15, optionally within 250 μm 2 The number of particles in the area does not exceed 12, 10, 9, 8, 7, 6, 5, 4, 3 or 2.

[0143] In the positive electrode active material prepared by the method, the particle size distribution of the super-large primary particles is significantly reduced, the mechanical integrity of the primary particles and the secondary particles is improved, and the penetration of the electrolyte into the positive electrode active material and the loss of the positive electrode active material (for example, lithium ions) are delayed during the cycle. At the same time, the electrical contact failure and capacity polarization loss caused by intercrystalline cracks of the super-large primary particles are reduced, and the chemical mechanical properties and cycle performance of the positive electrode active material are improved.

[0144] In some embodiments, the preparation method does not include multiple compaction granulation.

[0145] In some embodiments, the preparation method does not include pre-sintering. Optionally, the mixed raw materials are not subjected to sintering or pre-sintering before compaction and granulation.

[0146] The preparation method provided in the present application has a simple process flow, high reproducibility, and relatively low cost, which is conducive to industrial mass production.

[0147] In some embodiments, the preparation method comprises:

[0148] The raw materials including lithium source, iron source, manganese source, phosphorus source, carbon source and molding aid are mixed with water, alcohol or mixed solvent, ground, dried and compacted to obtain compacted particles; the compacted particles are filled, sintered and crushed to obtain positive electrode active materials.

[0149] In some embodiments, the preparation method comprises:

[0150] The raw materials including lithium source, iron source, manganese source, phosphorus source, carbon source and molding aid are mixed with water, alcohol or mixed solvent, ground, dried and compacted to obtain compacted particles with an average particle size controlled in the range of 3 mm to 30 mm;

[0151] Filling the compacted particles to a filling height of 5 cm to 30 cm, with a porosity of 5% to 20%, and sintering;

[0152] The secondary particles obtained by pulverizing and sintering are pulverized to a Dv50 of 0.45 μm-1.5 μm and / or 1≤(Dv90-Dv10) / Dv50≤3 to obtain a positive electrode active material.

[0153] The present application also provides a positive electrode active material prepared by the method.

[0154] The present application also provides the use of the positive electrode active material prepared by the method in a secondary battery.

[0155] Secondary battery

[0156] The present application provides a secondary battery, which includes a positive electrode sheet, a separator, a negative electrode sheet, and an electrolyte in any embodiment.

[0157] In the secondary battery of the present application, the positive electrode sheet includes a positive electrode current collector and a positive electrode film layer disposed on at least one surface of the positive electrode current collector and including a positive electrode active material. For example, the positive electrode current collector has two surfaces opposite to each other in its thickness direction, and the positive electrode film layer is disposed on any one or both of the two opposite surfaces of the positive electrode current collector.

[0158] In the secondary battery of the present application, the positive electrode film layer generally comprises a positive electrode active material and an optional binder and an optional conductive agent. The positive electrode film layer is generally formed by coating the positive electrode slurry on the positive electrode current collector, drying and cold pressing. The positive electrode slurry is generally formed by dispersing the positive electrode active material, the optional conductive agent, the optional binder and any other components in a solvent and stirring them evenly. The solvent may be N-methylpyrrolidone (NMP), but is not limited thereto. The type and content of the conductive agent and the binder are not specifically limited and can be selected according to actual needs. As an example, the binder may include one or more of polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), vinylidene fluoride-tetrafluoroethylene-propylene terpolymer, vinylidene fluoride-hexafluoropropylene-tetrafluoroethylene terpolymer, tetrafluoroethylene-hexafluoropropylene copolymer, and fluorine-containing acrylate resin. As an example, the conductive agent may include one or more of superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers.

[0159] In the secondary battery of the present application, the positive electrode current collector may be a metal foil or a composite current collector. As an example of a metal foil, the positive electrode current collector may be an aluminum foil. The composite current collector may include a polymer material base layer and a metal material layer formed on at least one surface of the polymer material base layer. As an example, the metal material may be selected from one or more of aluminum, aluminum alloy, nickel, nickel alloy, titanium, titanium alloy, silver, and silver alloy. As an example, the polymer material base layer may be selected from polypropylene, polyethylene terephthalate, polybutylene terephthalate, polystyrene, polyethylene, etc.

[0160] In some embodiments, the negative electrode active material includes at least one of artificial graphite, natural graphite, soft carbon, hard carbon, mesophase microcarbon beads, silicon-based materials, and tin-based materials.

[0161] In the secondary battery of the present application, the negative electrode film layer generally comprises a negative electrode active material, an optional binder, an optional conductive agent and other optional additives. The negative electrode film layer is generally formed by coating the negative electrode slurry on the negative electrode current collector, drying and cold pressing. The negative electrode slurry coating is generally formed by dispersing the negative electrode active material, the optional conductive agent, the optional binder, and other optional additives in a solvent and stirring them evenly. The solvent may be N-methylpyrrolidone (NMP) or deionized water, but is not limited thereto. Among them, the type and content of the conductive agent and the binder are not specifically limited and can be selected according to actual needs. As an example, the conductive agent may include one or more of superconducting carbon, carbon black (such as acetylene black, Ketjen black, etc.), carbon dots, carbon nanotubes, graphene and carbon nanofibers. As an example, the binder may include one or more of styrene-butadiene rubber (SBR), water-soluble unsaturated resin SR-1B, water-based acrylic resin (e.g., polyacrylic acid PAA, polymethacrylic acid PMAA, sodium polyacrylate PAAS), polyacrylamide (PAM), polyvinyl alcohol (PVA), sodium alginate (SA) and carboxymethyl chitosan (CMCS). Other optional additives may include thickeners (e.g., sodium carboxymethyl cellulose CMC-Na), PTC thermistor materials, etc.

[0162] In the secondary battery of the present application, the negative electrode film layer can be arranged on one side of the negative electrode current collector, or can be arranged on both sides of the negative electrode current collector at the same time. For example, the negative electrode current collector has two opposite sides in its own thickness direction, and the negative electrode film layer is arranged on any one side or both sides of the two opposite sides of the negative electrode current collector.

[0163] In the secondary battery of the present application, the type of the negative electrode current collector is not specifically limited and can be selected according to actual needs.

[0164] In the secondary battery of the present application, the negative electrode current collector may be a metal foil or a composite current collector. As an example of a metal foil, the negative electrode current collector may be a copper foil. The composite current collector may include a polymer material base layer and a metal material layer formed on at least one surface of the polymer material base layer. As an example, the metal material may be selected from one or more of copper, copper alloy, nickel, nickel alloy, titanium, titanium alloy, silver, and silver alloy. As an example, the polymer material base layer may be selected from polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), polyethylene (PE), etc.

[0165] It should be noted that the parameters of the negative electrode film layer (such as thickness, compaction density, etc.) given in this application refer to the parameters of the negative electrode film layer on one side of the negative electrode current collector. When the negative electrode film layer is arranged on both sides of the negative electrode current collector, the parameters of the negative electrode film layer on either side meet the requirements of this application and are considered to fall within the protection scope of this application. The ranges of the thickness and compaction density of the negative electrode film layer described in this application refer to the parameters of the negative electrode film layer after cold pressing and used to assemble the battery.

[0166] In addition, in the secondary battery of the present application, the negative electrode plate does not exclude other additional functional layers in addition to the negative electrode film layer. For example, in some embodiments, the negative electrode plate described in the present application may also include a conductive primer layer (e.g., composed of a conductive agent and a binder) disposed between the negative electrode current collector and the negative electrode film layer. In some other embodiments, the negative electrode plate described in the present application also includes a protective layer covering the surface of the negative electrode film layer.

[0167] The electrolyte plays the role of conducting ions between the positive electrode and the negative electrode. The present application has no specific restrictions on the type of electrolyte, which can be selected according to needs. For example, the electrolyte can be liquid, gel or all-solid.

[0168] In some embodiments, the electrolyte is an electrolyte solution, which includes an electrolyte salt and a solvent.

[0169] In some embodiments, the electrolyte salt can be selected from at least one of lithium hexafluorophosphate, lithium tetrafluoroborate, lithium perchlorate, lithium hexafluoroarsenate, lithium bis(fluorosulfonyl)imide, lithium bis(trifluoromethanesulfonyl)imide, lithium trifluoromethanesulfonate, lithium difluorophosphate, lithium difluorooxalatoborate, lithium dioxalatoborate, lithium difluorodioxalatophosphate, and lithium tetrafluorooxalatophosphate.

[0170] In some embodiments, the solvent can be selected from at least one of ethylene carbonate, propylene carbonate, ethyl methyl carbonate, diethyl carbonate, dimethyl carbonate, dipropyl carbonate, methyl propyl carbonate, ethyl propyl carbonate, butylene carbonate, fluoroethylene carbonate, methyl formate, methyl acetate, ethyl acetate, propyl acetate, methyl propionate, ethyl propionate, propyl propionate, methyl butyrate, ethyl butyrate, 1,4-butyrolactone, cyclopentane sulfone, dimethyl sulfone, methyl ethyl sulfone and diethyl sulfone.

[0171] In some embodiments, the electrolyte may further include additives, such as negative electrode film-forming additives, positive electrode film-forming additives, and additives that can improve certain battery properties, such as additives that improve battery overcharge performance, additives that improve battery high or low temperature performance, etc.

[0172] In the secondary battery of the present application, there is no particular restriction on the type of the separator, and any known porous structure separator with good chemical stability and mechanical stability can be selected.

[0173] In some embodiments, the material of the isolation membrane can be selected from at least one of glass fiber, non-woven fabric, polyethylene, polypropylene and polyvinylidene fluoride. The isolation membrane can be a single-layer film or a multi-layer composite film, without particular limitation. When the isolation membrane is a multi-layer composite film, the materials of each layer can be the same or different, without particular limitation.

[0174] In some embodiments, the outer packaging of the secondary battery may be a hard shell, such as a hard plastic shell, an aluminum shell, a steel shell, etc. The outer packaging of the secondary battery may also be a soft package, such as a bag-type soft package. The material of the soft package may be plastic, and examples of the plastic include polypropylene, polybutylene terephthalate, and polybutylene succinate.

[0175] The present application has no particular limitation on the shape of the battery, which may be cylindrical, square or any other shape. For example, Figure 6 The secondary battery 5 is a square structure as an example.

[0176] In some embodiments, reference Figure 7 , the outer packaging may include a shell 51 and a cover plate 53. Among them, the shell 51 may include a bottom plate and a side plate connected to the bottom plate, and the bottom plate and the side plate enclose a receiving cavity. The shell 51 has an opening connected to the receiving cavity, and the cover plate 53 can be covered on the opening to close the receiving cavity. The positive electrode sheet, the negative electrode sheet and the isolation membrane can form an electrode assembly 52 through a winding process or a lamination process. The electrode assembly 52 is encapsulated in the receiving cavity. The electrolyte is infiltrated in the electrode assembly 52. ​​The number of electrode assemblies 52 contained in the secondary battery 5 can be one or more, and those skilled in the art can select according to specific actual needs.

[0177] In some embodiments, secondary batteries may be assembled into a battery module. The number of secondary batteries contained in the battery module may be one or more, and the specific number may be selected by those skilled in the art according to the application and capacity of the battery module.

[0178] Figure 8 4 is an example of a battery module. Figure 8 In the battery module 4, the plurality of secondary batteries 5 may be arranged in sequence along the length direction of the battery module 4. Of course, they may also be arranged in any other manner. Further, the plurality of secondary batteries 5 may be fixed by fasteners.

[0179] Optionally, the battery module 4 may further include a housing having a receiving space, and the plurality of secondary batteries 5 are received in the receiving space.

[0180] In some embodiments, the battery modules described above may also be assembled into a battery pack. The battery pack may contain one or more battery modules, and the specific number may be selected by those skilled in the art according to the application and capacity of the battery pack.

[0181] Fig. 9 and Fig.10 1 is a battery pack 1 as an example. Fig. 9 and Fig.10 The battery pack 1 may include a battery box and a plurality of battery modules 4 disposed in the battery box. The battery box includes an upper box body 2 and a lower box body 3. The upper box body 2 can cover the lower box body 3 and form a closed space for accommodating the battery modules 4. The plurality of battery modules 4 can be arranged in the battery box in any manner.

[0182] Electrical devices

[0183] The present application also provides an electrical device, which includes at least one of the secondary battery, battery module, or battery pack provided in the present application. The secondary battery, battery module, or battery pack can be used as a power source for the electrical device, and can also be used as an energy storage unit for the electrical device. The electrical device may include mobile devices (such as mobile phones, laptops, etc.), electric vehicles (such as pure electric vehicles, hybrid electric vehicles, plug-in hybrid electric vehicles, electric bicycles, electric scooters, electric golf carts, electric trucks, etc.), electric trains, ships and satellites, energy storage systems, etc., but are not limited thereto.

[0184] As the electrical device, a secondary battery, a battery module or a battery pack may be selected according to its usage requirements.

[0185] Fig.11 The power consumption device is taken as an example. The power consumption device is a pure electric vehicle, a hybrid electric vehicle, or a plug-in hybrid electric vehicle. In order to meet the high power and high energy density requirements of the power consumption device for the secondary battery, a battery pack or a battery module can be used.

[0186] Another example of a device may be a mobile phone, a tablet computer, a notebook computer, etc. Such a device is usually required to be thin and light, and a secondary battery may be used as a power source.

[0187] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present application, rather than to limit them; although the present application has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein by equivalents; and these modifications or replacements do not make the essence of the corresponding technical solutions deviate from the scope of the technical solutions of the embodiments of the present application, and they should all be included in the scope of the claims and specification of the present application. In particular, as long as there is no conflict, the various technical features mentioned in the various embodiments can be combined in any way. The present application is not limited to the specific embodiments disclosed herein, but includes all technical solutions that fall within the scope of the claims.

[0188] Example

[0189] Hereinafter, the embodiments of the present application will be described. The embodiments described below are exemplary and are only used to explain the present application, and should not be construed as limiting the present application. If no specific techniques or conditions are indicated in the embodiments, the techniques or conditions described in the literature in this area or the product specifications are used. If the manufacturer is not indicated in the reagents or instruments used, they are all conventional products that can be obtained commercially.

[0190] 1. Preparation of batteries

[0191] Example 1

[0192] 1) Preparation of positive electrode active materials

[0193] Weigh lithium carbonate, ferric oxide, ammonium dihydrogen phosphate and titanium dioxide respectively, so that the mass ratio of Li:Fe:P elements is 1.01:0.99:1.01, and the mass ratio of titanium dioxide to lithium carbonate is 1:105. Add water and mix well to obtain a slurry, and add 8% of sucrose by mass in all solid raw materials and 1% of starch by mass in all solid raw materials. The solid content in the slurry is 40%.

[0194] The mixed slurry is ground by a ball mill to a Dv50 of about 0.5 μm, and then spray dried (the negative pressure of the high-speed spray dryer is -650 to -200 pa, the inlet temperature is 300°C to 360°C, and the outlet temperature is 100°C to 140°C). The powder obtained by spray drying is compacted and granulated by a granulator, and the average particle size is about 10 mm, and the compacted density of the particles is 1.2 to 1.5 g / cm 3. The granulated reactants are loaded into a graphite sagger, and the loading depth of the materials is 12 cm. The sagger filled with the reaction materials is placed in a kiln for sintering, and the heating rate is controlled at 3°C / min, the insulation temperature is controlled at 750°C, and the insulation time is 6-8 hours. After the materials are cooled, the materials are crushed by a jet mill or a mechanical mill until the Dv50 is about 1.1μm, and the positive electrode active material LiFe 0.995 Ti 0.005 PO4@C, where the Ti element content in the positive electrode active material is 1500ppm.

[0195] 2) Preparation of positive electrode

[0196] Fully dissolve 2.0wt% polyvinylidene fluoride binder in N-methylpyrrolidone (NMP), then add 1.0wt% Super P, 0.5wt% carbon nanotubes and 96.5wt% of the above positive electrode active materials and stir and mix evenly to obtain positive electrode slurry. Apply the slurry evenly on the surface of the current collector aluminum foil, and then transfer it to a vacuum drying oven for complete drying. Roll and punch the dried electrode to obtain a positive electrode sheet with a compaction density of 2.35g / cm 3 .

[0197] 3) Preparation of negative electrode sheet

[0198] The active material artificial graphite, the conductive agent carbon black, the binder styrene-butadiene rubber (SBR), and the thickener sodium carboxymethyl cellulose (CMC-Na) are dissolved in the solvent deionized water in a weight ratio of 96.7:1.3:0.8:1.2, and the mixture is evenly mixed to prepare a negative electrode slurry; the negative electrode slurry is evenly coated on the negative electrode collector copper foil once or multiple times, and the negative electrode sheet is obtained after drying, cold pressing, and slitting.

[0199] 4) Electrolyte

[0200] In an argon atmosphere glove box (H2O<0.1ppm, O2<0.1ppm), organic solvents ethylene carbonate (EC) and ethyl methyl carbonate (EMC) were evenly mixed in a volume ratio of 3:7, and LiPF6 lithium salt was dissolved in the organic solvent to prepare a solution with a mass content of 12.5% ​​to obtain an electrolyte.

[0201] 5) Isolation film

[0202] Polypropylene film is used as the isolation film.

[0203] 6) Preparation of batteries

[0204] The positive electrode sheet, the isolation film, and the negative electrode sheet are stacked in order, so that the isolation film is placed between the positive and negative electrode sheets to play an isolating role, and then they are wound to obtain an electrode assembly; the electrode assembly is placed in a battery casing, and after drying, the electrolyte is injected, and then the steps of standing, hot and cold pressing, formation, shaping, and capacity testing are sequentially performed to obtain the lithium battery product of Example 1.

[0205] The preparation methods of Examples 2 to 10 are similar to those of Example 1, and the specific parameter adjustments are shown in Table 1.

[0206] The preparation method of Example 11 is similar to that of Example 1, but magnesium hydroxide is used as an adjustment, and the mass ratio of magnesium hydroxide to lithium carbonate is 0.73:105.

[0207] The preparation method of Example 12 is similar to that of Example 1, but vanadium pentoxide is used as an adjustment, and the mass ratio of vanadium pentoxide to lithium carbonate is 1.138:105.

[0208] The preparation method of Example 13 is similar to that of Example 1, but no doping elements are added to the raw materials. Specific parameters are shown in Table 1.

[0209] Comparative Example 1

[0210] The preparation method of the battery of Comparative Example 1 is similar to that of the battery of Example 1, except that no compaction molding is performed and no molding additives are added, and the sintering reaction is directly performed after the spraying is completed.

[0211] Comparative Example 2

[0212] The preparation method of the battery of Comparative Example 2 is similar to that of the battery of Example 1, but the difference from Example 1 is that no compaction molding additive is added.

[0213] The preparation methods of Comparative Examples 3 to 6 are similar to those of Example 1, and the specific parameter adjustments are shown in Table 1.

[0214] 2. Performance Test

[0215] 1. Volume average particle size Dv10, D50, Dv90 test

[0216] Equipment model: Malvern 2000 (MasterSizer 2000) laser particle size analyzer, reference standard process: GB / T19077-2016 / ISO 13320:2009.

[0217] Specific test process: Take an appropriate amount of the sample to be tested (the sample concentration is sufficient to ensure 8-12% shading), add 20ml of deionized water, and ultrasonicate for 5min (53KHz / 120W) to completely disperse the sample, and then measure the sample according to GB / T19077-2016 / ISO 13320:2009 standard.

[0218] 2. Morphology test

[0219] The positive electrode active materials prepared in the examples and comparative examples were tested using a ZEISS sigma 300 scanning electron microscope, and the sample morphology was observed with reference to the standard JY / T010-1996.

[0220] 3. Determination method of primary particle size in positive electrode sheet

[0221] The pole piece is cut open perpendicularly to the large surface of the pole piece by using an argon ion beam to expose the cross section, which is then photographed by SEM, and the particle size of the nanoparticles is counted by the length diameter statistical method.

[0222] by Fig.12 For example, Fig.12 The SEM image of the cross section of the electrode piece is shown. The double arrows in the figure indicate the long diameter of the primary particles in the positive electrode piece, and the particle size of the primary particles is measured and counted.

[0223] 4. Battery performance test

[0224] 1) Capacity retention test at 25°C

[0225] The capacity retention rate test process is as follows: at 25°C, the prepared battery is charged to 3.65V at a constant current of 1C, then charged at a constant voltage of 3.65V until the current drops to 0.05C, and then discharged to 2.5V at 1C. The obtained capacity is recorded as the initial capacity (C0). Repeat the above steps for the same battery, and record the discharge capacity (Cn) of the battery after the nth cycle at the same time. The battery capacity retention rate after each cycle is Pn = Cn / C0×100%. The capacity retention rate after 1000 cycles is measured under the above measurement conditions.

[0226] 2) Capacity retention test at 60°C

[0227] The capacity retention rate test process is as follows: at 60°C, the prepared battery is charged to 3.65V at a constant current of 1C, then charged at a constant voltage of 3.65V until the current drops to 0.05C, and then discharged to 2.5V at 1C, and the obtained capacity is recorded as the initial capacity (C0). Repeat the above steps for the same battery, and record the discharge capacity (Cn) of the battery after the nth cycle at the same time, then the battery capacity retention rate after each cycle Pn = Cn / C0×100%, and the capacity retention rate after 1000 cycles is measured under the above measurement conditions.

[0228] 5. Determination of the content of doping elements Ti, V, and Mg

[0229] According to methods known in the art, a mixed acid of HF, HNO3 and HCl is prepared for sample dissolution so that titanium, vanadium and Mg in the positive electrode material are fully dissolved in the solution, and inductively coupled plasma atomic emission spectroscopy is used to determine the Ti, V and Mg elements.

[0230] 6. Evaluation of carbon distribution uniformity

[0231] Take the material that has not been crushed after sintering and cooling, and divide it into three layers according to the height of the material filled in the graphite sagger. Take samples, and determine the carbon content with reference to the determination method of carbon content in GB / T 33822-2017 (infrared carbon-sulfur tester). Calculate the average carbon content in the upper, middle and lower layers of materials, and calculate the range (i.e. the difference between the maximum and minimum values) based on the average carbon content in the upper, middle and lower layers of materials.

[0232] The sintered, cooled and pulverized material was taken, and the carbon content of the prepared positive electrode active material was determined by referring to the carbon content determination method in GB / T 33822-2017 (infrared carbon-sulfur tester).

[0233] When the ratio of the extreme difference to the carbon content of the positive electrode active material does not exceed 10%, the uniformity of the carbon distribution is judged to be good; when the ratio of the two is greater than 10% and not more than 20%, the uniformity of the carbon distribution is judged to be good; when the ratio of the two is greater than 20% and not more than 30%, the uniformity of the carbon distribution is judged to be poor; when the ratio of the two is greater than 30%, the uniformity of the carbon distribution is judged to be poor.

[0234] III. Analysis of test results of various embodiments and comparative examples

[0235] Figure 2 The SEM image of the positive electrode active material prepared in Example 1 is shown, and it can be seen that the primary particle size distribution of the positive electrode active material is very uniform, and the content of micro powder and large particles is low.

[0236] Figure 3 A and Figure 3 B shows a scanning electron microscope photo of the argon ion beam cut section of the positive electrode sheet prepared in Example 1. It can be clearly observed that the uniform particle size distribution is very low. The content of micropowder and large particles in the positive electrode active material is extremely low. The number of nanoparticles with a diameter of less than 80nm accounts for less than 2%, and the number of particles with a diameter of more than 1500nm accounts for less than 250μm. 2 The quantity inside is 2 pcs.

[0237] Figure 4 A and Figure 4 B shows a scanning electron microscope photograph of the argon ion beam cut section of the positive electrode sheet prepared in Comparative Example 1, where a large number of micropowders and oversized primary particles can be clearly observed.

[0238] Table 1 shows the parameters of the positive electrode active materials and batteries prepared in each embodiment and comparative example, and Table 2 shows the particle size Dv50 (μm) of the positive electrode active materials in Table 1, the particle size distribution concentration (Dv90-Dv10) / Dv50, the particle size distribution of the micropowder (the percentage of the particle size of the micropowder with a particle size of 80-180nm), the number of large particles (250μm 2 The results of the evaluation of carbon distribution uniformity and the test results of the capacity retention rate of secondary batteries after 1000 cycles at 25°C and 60°C were used.

[0239] Table 1

[0240]

[0241] Table 2

[0242]

[0243] According to the above results, the particle size distribution of large particles and small particles in the positive electrode active materials of Examples 1 to 13 is reduced, and the uniformity of the charge and discharge reaction and the cycle performance of the positive electrode active materials are significantly improved.

[0244] Figure 5 The cycle curves of Example 1 and Comparative Example 1 at 25°C and 60°C are shown (two samples were measured in parallel). It can be seen that the cycle performance of the secondary battery prepared in Example 1 is significantly improved under normal temperature and high temperature conditions compared with the secondary battery prepared in Comparative Example 1.

[0245] In Examples 1 to 3, the average particle size of compaction granulation was adjusted. Compared with Comparative Examples 3 to 4, the average particle size of compaction granulation was within the range of 3-30 mm, the material had good air permeability during sintering, the particles were heated evenly, the carbon content was uniform, and the battery cycle performance was significantly improved. If the average particle size of compaction granulation is too small or too large, it is not conducive to the control of the particle size distribution of micro powder and the number of large particles.

[0246] In Examples 4 and 5, the height of the compacted particles during the sintering process is adjusted. The filling height is within the range of 5-30 cm. The material has good air permeability during the sintering process, the particles are heated evenly, the carbon is evenly distributed, the particle growth consistency is good, and the battery cycle performance is significantly improved; and it is conducive to obtaining good production capacity.

[0247] Examples 6 to 8 adjusted the Dv50 value of the positive electrode active material after the pulverization treatment. Compared with Comparative Example 6, the Dv50 value is in the range of 0.45-1.5 μm, and the particle size of the positive electrode active material is small, which contains at least some nano-scale primary particles, which is beneficial to the release and embedding of active material lithium ions; at the same time, the (Dv90-Dv10) / Dv50 of the obtained positive electrode active material powder is less than 3, and the particle size distribution concentration is high. Both too small and too high Dv50 can lead to deterioration of cycle performance. If Dv50 is too small, the overall particle size is low, the proportion of small particles increases, and the surface stability of the material decreases; if Dv50 is too large, the overall particle size is low, the proportion of large particles increases, and the particle crushing effect increases during the cycle, which is not conducive to improving the stability of the material.

[0248] The compaction density of the compaction granulation was adjusted in Examples 9 and 10, and the compaction density was 1-2.5 g / cm 3 Compared with Comparative Examples 1 and 2, the compaction density is too low or no compaction molding process is performed, which is not conducive to the uniformity of particle size and carbon distribution.

[0249] Examples 11 to 13 adjust the reaction raw materials of the doping elements. It can be seen that the preparation method provided in this application can be applied to phosphate-based positive electrode active materials with different doping elements and without doping elements. The doped phosphate-based positive electrode active material prepared using magnesium hydroxide and vanadium pentoxide has a particle size distribution and electrical properties similar to those of the doped phosphate-based positive electrode active material prepared using titanium dioxide. The phosphate-based positive electrode active material without doping elements prepared in the examples also has good particle size distribution and electrical properties.

[0250] Compared with Comparative Example 1, the positive electrode active materials prepared without compaction and granulation treatment in Examples 1 to 13 have low particle size distribution concentration and poor carbon content uniformity. Compared with Comparative Example 5, adding a molding aid to the raw materials helps to improve the particle size distribution concentration, and due to the improvement of chemical mechanical properties, it also helps to improve the cycle performance of the battery.

[0251] It should be noted that the present application is not limited to the above-mentioned embodiments. The above-mentioned embodiments are only examples, and the embodiments having the same structure as the technical idea and exerting the same effect within the scope of the technical solution of the present application are all included in the technical scope of the present application. In addition, without departing from the scope of the main purpose of the present application, various modifications that can be thought of by those skilled in the art to the embodiments and other methods of combining some of the constituent elements in the embodiments are also included in the scope of the present application.

Claims

1. A positive electrode active material, characterized in that: Including the general formula Li z Fe x Mn (1-x-y) M y At least one of the compounds shown in PO4@C, wherein 1≤z≤1.1, 0.5≤x≤1, 0≤y≤0.1; M is selected from at least one of Ti, V, and Mg; At least a portion of the positive electrode active material includes primary particles, and the particle size distribution of the primary particles with a primary particle size of 80 nm or more and 180 nm or less in the positive electrode active material is less than or equal to 10%; The primary particles with a primary particle size of more than 1500nm are (250±5)μm in the cross section cut after the positive electrode active material is prepared into a pole piece. 2 The number of particles in the area does not exceed 15; The positive electrode active material includes secondary particles, and the particle size distribution of the secondary particles satisfies: 1≤(Dv90-Dv10) / Dv50≤3; The Dv50 of the secondary particles is 0.45-1.5 μm.

2. The positive electrode active material according to claim 1, characterized in that The particle size distribution of primary particles with a primary particle size of 80 nm or more and 180 nm or less in the positive electrode active material is 1.9-8.5%, optionally 1.9-8% or 1.9-7%.

3. The positive electrode active material according to claim 1 or 2, characterized in that: In the positive electrode active material, the primary particles with a primary particle size of 1500 nm or more are (250±5) μm in the cross section cut after the positive electrode active material is prepared into a pole piece. 2 The number of particles in the area does not exceed 12, and can be selected as 10, 8 or 7.

4. The positive electrode active material according to any one of claims 1 to 3, characterized in that The positive electrode active material includes secondary particles, and the particle size distribution of the secondary particles satisfies: 1.2≤(Dv90-Dv10) / Dv50≤2.9, which can be 1.2≤(Dv90-Dv10) / Dv50≤2.3 or 1.2≤(Dv90-Dv10) / Dv50≤1.

5.

5. The positive electrode active material according to any one of claims 1 to 4, characterized in that The Dv50 of the secondary particles is 1-1.5 μm, and can be optionally 1.3-1.5 μm.

6. The positive electrode active material according to any one of claims 1 to 5, characterized in that 0.6 <x≤1,0≤y<0.1,1≤z≤1.1; The mass content of the M element in the positive electrode active material is 1000ppm-6000ppm.

7. A method for preparing a positive electrode active material, characterized in that: The positive electrode active material comprises the general formula, Li z Fe x Mn (1-x-y) M y At least one of the compounds shown in PO4@C, wherein 0.5≤x≤1, 0≤y≤0.1, 1≤z≤1.1; M is selected from at least one of Ti, V, and Mg; The preparation method comprises the following steps: The raw materials including lithium source, iron source, manganese source, phosphorus source, carbon source, M source and molding aid are compacted and granulated to obtain compacted particles, the compacted particles are filled, and the compacted particles are sintered to obtain secondary particles.

8. The preparation method according to claim 7, characterized in that: The method comprises mixing raw materials including a lithium source, an iron source, a manganese source, a phosphorus source, a carbon source and a molding aid with water, alcohol or a mixed solvent, grinding, drying and compacting to obtain compacted particles; and filling the compacted particles, sintering and crushing to obtain a positive electrode active material.

9. The preparation method according to claim 7 or 8, characterized in that: The average particle size of the compacted particles is 3 mm to 30 mm, and can be optionally 10 mm to 30 mm.

10. The preparation method according to any one of claims 7 to 9, characterized in that: The compacted density of the compacted particles is 1.2-3.0 g / cm 3 , optional 1.2-2.5g / cm 3 .

11. The preparation method according to any one of claims 7 to 10, characterized in that: The preparation method comprises: filling the compacted particles to a filling height of 5 cm-30 cm, which may be 8 cm-30 cm or 5 cm-25 cm; or, the filling porosity of the compacted particles is 5%-20%.

12. The preparation method according to any one of claims 7 to 11, characterized in that: The molding aid comprises at least one of polypropylene, starch, phenolic resin, polyurethane, melamine resin, polyethylene, stearic acid, PVC, polyacrylonitrile, natural rubber, styrene-butadiene rubber and butadiene rubber.

13. A positive electrode plate, characterized in that: The positive electrode sheet includes the positive electrode active material according to any one of claims 1 to 6 or includes the positive electrode active material prepared by the method according to any one of claims 7 to 12.

14. A secondary battery, characterized in that: It comprises a negative electrode plate, a separator, an electrolyte and the positive electrode plate according to claim 13.

15. An electrical device, characterized in that: Includes the secondary battery as claimed in claim 14.

Citation Information

Cited By

  • Secondary battery and preparation method thereof, battery pack, energy storage system and electric equipment

    CN119920887A