NASICON type solid electrolyte and preparation method and application thereof

By introducing NASICON type solid electrolytes with S elements and specific metal elements, the problems of insufficient interface stability and ionic conductivity in solid-state batteries are solved, and the performance of solid-state batteries is significantly improved, including capacity, cycling performance and rate performance.

CN118970154APending Publication Date: 2024-11-15BEIJING EASPRING MATERIAL TECH CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411046831.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2024-05-31
Filing Date
2024-07-31
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

Existing solid-state batteries have challenges in high energy density, especially the lack of interface stability and ionic conductivity of oxide and sulfide solid-state electrolyte materials, resulting in poor cycling and rate performance.

Method used

Using NASICON type solid electrolyte, the LixM1yM2zM3uM4v(PO4)w1(PS4)w2 structure is formed by introducing S elements and specific metal elements, which improves its interface stability and ionic conductivity, and coats it on the matrix of the positive electrode active material to reduce the Space charge layer and interface side reaction.

Benefits of technology

It significantly improves the capacity, cycle performance and rate performance of solid-state batteries, reduces the impedance of solid-state batteries, and enhances interface stability and ionic conductivity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118970154A_ABST
    Figure CN118970154A_ABST
Patent Text Reader

Abstract

The invention discloses an NASICON type solid electrolyte and a preparation method and application thereof, the NASICON type solid electrolyte comprises Li < x > M < 1 > < y > M < 2 > < z > M < 3 > M < 4 > < v > (PO4) < w1 > (PO4) < w2 >, y + z + u + v = 2, and w1 + w2 = 3, 0 lt; xlt; 0 < = y < = 0.5, 0lt; z < = 1, 0lt; u, u; wherein, 1 < = v < = 3, 2 < = v < = 3, 1 < = w1 < = 3, M1 includes at least one of Mg, Na, K and Zn, M2 includes at least one of Al, Ga, In, Y, Sc, La and Ce, M3 includes at least one of Ti, Zr, Hf and Ge, and M4 includes at least one of Cr, Mo, Ca, Fe, Si, W, Nb, Sm, V and B. Therefore, the NASICON type solid-state electrolyte has excellent interface stability and ionic conductivity, so that when the NASICON type solid-state electrolyte is coated on a positive electrode active material substrate and is applied to a solid-state battery, the side reaction of a space charge layer and an interface between the positive electrode active material substrate and a solid-state electrolyte layer and the impedance of the solid-state battery can be reduced; and the capacity, the cycle performance and the rate capability of the solid-state battery are improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of batteries, and in particular relates to a NASICON type solid electrolyte and a preparation method and application thereof. Background Art

[0002] Liquid lithium-ion batteries have been the main energy storage technology since they were first commercialized in 1991, but are now gradually approaching their energy density limit and have certain safety risks. Solid-state batteries (SSBs) that use solid electrolytes (SEs) instead of organic flammable liquid electrolytes (LEs) can fundamentally solve safety issues and are expected to improve key battery performance indicators.

[0003] Solid-state batteries mainly include solid electrolytes and positive and negative electrode sheets. The most promising negative electrode active materials for achieving high energy density are metallic lithium and silicon. According to the roadmap, metallic lithium has the highest technical potential as a negative electrode active material, followed by silicon, but the market application potential of silicon is higher than that of metallic lithium. Although alloy negative electrodes such as Li-In and Li-Al have good compatibility with solid electrolyte materials in laboratory studies, they are not discussed in the roadmap. For positive electrode active materials (CAMs), the roadmap points out that traditional layered oxide materials (such as lithium nickel manganese cobalt oxide (NMC), lithium nickel cobalt aluminum oxide (NCA), lithium cobalt oxide (LCO)) have the highest technical potential for application in SSBs, followed by medium-priced and medium-performance materials such as lithium iron phosphate (LFP) or high-voltage materials such as Li(Mn, Ni)2O4 (LMNO). Among them, due to the low cost and high safety of LFP, its market application potential is comparable to that of layered oxide materials.

[0004] For solid electrolyte materials, garnet-type SEs are the most promising class of oxide SEs due to their wide electrochemical stability window. For sulfide SEs, argyrodite electrolytes represented by Li6PS5Cl have the most potential due to their high ionic conductivity and high kinetic stability to lithium metal. So far, no SEs can meet all the requirements of high energy density SSBs, and solid electrolytes still face many challenges. For oxide and sulfide solid electrolytes, processability and (electro)chemical compatibility are their main challenges, respectively. In addition to problems with the solid electrolyte itself (such as interface stability and ionic conductivity, etc.), most of the problems occur at the interface between different components. At the CAM / SEs interface, poor contact and interfacial side reactions during cycling are two major problems.

[0005] Therefore, existing solid-state batteries need to be improved. Summary of the invention

[0006] The present invention aims to solve one of the technical problems in the related art to at least a certain extent. To this end, one object of the present invention is to provide a NASICON type solid electrolyte and a preparation method and application thereof, wherein the NASICON type solid electrolyte has excellent interface stability and ionic conductivity, so that it is coated on a positive electrode active material matrix and applied to a solid-state battery, which can reduce the space charge layer and interface side reactions between the positive electrode active material matrix and the solid electrolyte layer and the impedance of the solid-state battery, and improve the capacity, cycle performance and rate performance of the solid-state battery.

[0007] In one aspect of the present invention, the present invention provides a NASICON type solid electrolyte. According to an embodiment of the present invention, the NASICON type solid electrolyte comprises: Li x M1 y M2 z M3 u M4 v (PO4) w1 (PS4) w2 , where y+z+u+v=2, w1+w2=3, 0 <x<2,0≤y≤0.5,0<z≤1,0<u<2,0≤v≤3,1≤w1≤3,

[0008] 0.0001≤w2≤0.3, M1 includes at least one of Mg, Na, K and Zn, M2 includes at least one of Al, Ga, In, Y, Sc, La and Ce, M3 includes at least one of Ti, Zr, Hf and Ge, and M4 includes at least one of Cr, Mo, Ca, Fe, Si, W, Nb, Sm, V and B.

[0009] According to the NASICON type solid electrolyte of the embodiment of the present invention, its main elements include Li, M1, M2, M3, M4 (M1 includes at least one of Mg, Na, K and Zn, M2 includes at least one of Al, Ga, In, Y, Sc, La and Ce, M3 includes at least one of Ti, Zr, Hf and Ge, M4 includes at least one of Cr, Mo, Ca, Fe, Si, W, Nb, Sm, V and B), which can improve the ionic conductivity of the solid electrolyte, and at the same time, the introduction of S element can improve the interface stability of the solid electrolyte. Thus, the NASICON type solid electrolyte has excellent interface stability and ionic conductivity, so that it is coated on the positive electrode active material matrix, and applied to the solid-state battery, which can reduce the space charge layer and interface side reactions between the positive electrode active material matrix and the solid electrolyte layer, as well as the impedance of the solid-state battery, and improve the capacity, cycle performance and rate performance of the solid-state battery.

[0010] In addition, the NASICON solid electrolyte according to the above embodiment of the present invention may also have the following additional technical features:

[0011] In some embodiments of the present invention, the NASICON solid electrolyte satisfies at least one of the following conditions:

[0012] 0.6≤x≤3.2, preferably 1≤x≤2;

[0013] 0≤y≤0.3, preferably 0≤y≤0.1;

[0014] 0.2≤z≤0.7, preferably 0.2≤z≤0.4;

[0015] 0.9≤u<2, preferably 1.4≤u<2;

[0016] 0.2≤v≤2, preferably 0.5≤v≤1.

[0017] Thereby, the interface stability and ionic conductivity of the NASICON-type solid electrolyte can be further improved.

[0018] In some embodiments of the present invention, the XRD spectrum of the NASICON solid electrolyte has a (113) characteristic peak, a (104) characteristic peak, a (024) characteristic peak and a (012) characteristic peak.

[0019] The peak position of the characteristic peak (113) is 24.490°-24.880°, and the full width at half maximum is 0.195°-0.290°;

[0020] The peak position of the characteristic peak (104) is 20.850°-21.110°, and the full width at half maximum is 0.200°-0.300°;

[0021] The peak position of the (024) characteristic peak is 29.640°-30.010°, and the full width at half maximum is 0.180°-0.320°;

[0022] The peak position of the (012) characteristic peak is 14.680°-15.990°, and the full width at half maximum is 0.165°-0.315°;

[0023] Therefore, the solid electrolyte of the present invention is a NASICON-type solid electrolyte, and thus has excellent interface stability and ion conductivity.

[0024] In some embodiments of the present invention, the NASICON solid electrolyte satisfies at least one of the following conditions:

[0025] Volume average particle size Dv 500.01 μm-0.2 μm, preferably 0.05 μm-0.1 μm;

[0026] pH 7.2-9;

[0027] Ionic conductivity 1.0×10 -4 S / cm-1.5×10 -3 S / cm;

[0028] The electronic conductivity is 1.0×10 -10 S / cm-1.0×10 -8 S / cm.

[0029] Thereby, the ionic conductivity and interface stability of the NASICON-type solid electrolyte can be further improved.

[0030] In a second aspect of the present invention, the present invention provides a method for preparing a NASICON type solid electrolyte. According to an embodiment of the present invention, the method comprises:

[0031] (1) mixing and sintering a lithium-containing compound, an M1-containing compound, an M2-containing compound, an M3-containing compound, an M4-containing compound and a phosphorus-containing compound to obtain a solid electrolyte;

[0032] (2) The solid electrolyte is dispersed in a second solvent and ground to obtain a nanoscale slurry, and a sulfide is added to the nanoscale slurry, mixed, and then dried to obtain a NASICON type solid electrolyte.

[0033] Therefore, the method can be used to prepare the above-mentioned NASICON-type solid electrolyte with excellent interface stability and ionic conductivity, and then it can be coated on the positive electrode active material matrix to reduce the impedance of the solid-state battery and improve the capacity, cycle performance and rate performance of the solid-state battery.

[0034] In addition, the preparation of NASICON solid electrolyte according to the above embodiment of the present invention may also have the following additional technical features:

[0035] In some embodiments of the present invention, step (1) is performed according to the following method:

[0036] (1-1) mixing a lithium-containing compound, an M1-containing compound, an M2-containing compound, an M3-containing compound, an M4-containing compound, a phosphorus-containing compound, an organic monomer, a first solvent, an initiator, and a catalyst to obtain a mixture;

[0037] (1-2) heating the mixture to initiate a polymerization reaction to obtain a bulk solid electrolyte precursor;

[0038] (1-3) pre-sintering the block-shaped solid electrolyte precursor and crushing it to obtain a powder-shaped solid electrolyte precursor;

[0039] (1-4) The solid electrolyte precursor in powder form is sintered and crushed to obtain a solid electrolyte.

[0040] In some embodiments of the present invention, step (1-1) satisfies at least one of the following conditions:

[0041] The organic monomer includes at least one of acrylamide, methylene bisacrylamide, styrene, butadiene and methyl methacrylate;

[0042] The first solvent includes at least one of water, N-methyl-2-pyrrolidone, phthalate, dibasic lipid, long-chain alcohol and pyrrolidone;

[0043] The initiator includes at least one of benzoyl peroxide, (NH4)2S2O8 and K2S2O8;

[0044] The catalyst includes at least one of N,N,N′N′-tetramethylethylenediamine, N,N,N′,N′-tetramethyl-1,6-hexanediamine, N,N-diisopropylethylamine, and N-(3-aminopropyl)-N-dodecyl-1,3-propylenediamine;

[0045] In some embodiments of the present invention, in step (1-2), the polymerization reaction temperature is 80°C-200°C, preferably 90°C-150°C, and more preferably 96°C-120°C.

[0046] In some embodiments of the present invention, in step (1-3), the pre-sintering temperature is 300°C-600°C, preferably 350°C-575°C, and more preferably 380°C-560°C; and / or the pre-sintering duration is 2 hours-6 hours, preferably 2 hours-5 hours, and more preferably 2 hours-4 hours.

[0047] In some embodiments of the present invention, in step (1-4), the sintering temperature is 650°C-900°C, preferably 700°C-875°C, and more preferably 730°C-860°C; and / or the sintering duration is 4 hours to 10 hours, preferably 5 hours to 9 hours, and more preferably 6 hours to 8 hours.

[0048] In some embodiments of the present invention, in step (2), the volume average particle size Dv50 of the slurry is 5nm-500nm, preferably 10nm-200nm, more preferably 50nm-100nm, and the second solvent includes at least one of n-heptane, toluene and dimethyl ether.

[0049] In some embodiments of the present invention, in step (2), the amount of sulfide added is 0.1wt%-3wt% of the solid electrolyte, preferably 0.1wt%-1wt%.

[0050] In some embodiments of the present invention, in step (2), the drying temperature is 120°C-600°C, preferably 150°C-500°C.

[0051] In a third aspect of the present invention, the present invention provides a positive electrode active material. According to an embodiment of the present invention, the positive electrode active material comprises:

[0052] A cathode active material matrix;

[0053] A coating layer is formed on at least a portion of the surface of the positive electrode active material matrix, and the coating layer includes the NASICON type solid electrolyte described in the first aspect of the present invention or the NASICON type solid electrolyte obtained by the method described in the second aspect of the present invention.

[0054] According to the positive electrode active material of the embodiment of the present invention, by forming a coating layer containing the above-mentioned NASICON type solid electrolyte on the surface of the positive electrode active material matrix and applying it to a solid-state battery, the space charge layer and interface side reactions between the positive electrode active material matrix and the solid electrolyte layer and the impedance of the solid-state battery can be reduced, thereby improving the capacity, cycle performance and rate performance of the solid-state battery.

[0055] In addition, the positive electrode active material according to the above embodiment of the present invention may also have the following additional technical features:

[0056] In some embodiments of the present invention, based on the total amount of the cathode active material matrix, the mass proportion of the NASICON solid electrolyte is 0.05%-1%, preferably 0.3%-0.9%, and more preferably 0.4%-0.8%. Thus, the interface stability and ionic conductivity of the cathode active material can be further improved.

[0057] In some embodiments of the present invention, the positive electrode active material matrix includes at least one of lithium nickel oxide, lithium cobalt oxide, lithium manganese oxide, lithium nickel manganese oxide, lithium nickel cobalt manganese oxide, lithium nickel cobalt aluminum oxide, lithium nickel cobalt manganese aluminum oxide, lithium manganese-rich layered oxides and their derivatives, lithium iron phosphate and lithium manganese iron phosphate.

[0058] In some embodiments of the present invention, the positive electrode active material undergoes acid-base titration treatment to produce a phosphate characteristic titration peak at pH=5-8.

[0059] In a fourth aspect of the present invention, the present invention provides a method for preparing the above-mentioned positive electrode active material. According to an embodiment of the present invention, the method comprises:

[0060] The positive electrode active material matrix and the NASICON type solid electrolyte are mixed and heat-treated to form a coating layer including the NASICON type solid electrolyte on at least a portion of the surface of the positive electrode active material matrix.

[0061] Wherein, the NASICON-type solid electrolyte includes the NASICON-type solid electrolyte described in the first aspect of the present invention or the NASICON-type solid electrolyte obtained by the method described in the second aspect of the present invention.

[0062] Therefore, this method can be used to prepare the above-mentioned positive electrode active material with high interface stability and ionic conductivity. Applying it to solid-state batteries can reduce the space charge layer and interface side reactions between the positive electrode active material matrix and the solid electrolyte layer and the impedance of the solid-state battery, thereby improving the capacity, cycle performance and rate performance of the solid-state battery.

[0063] In some embodiments of the present invention, the heat treatment temperature is 300-700° C., preferably 375-625° C., more preferably 420-580° C. The heat treatment duration is 2-10 hours, preferably 4-10 hours, more preferably 5-10 hours.

[0064] In a fifth aspect of the present invention, the present invention provides a positive electrode plate, comprising the positive electrode active material described in the third aspect of the present invention or the positive electrode active material obtained by the method described in the fourth aspect of the present invention.

[0065] In a sixth aspect of the present invention, the present invention provides a solid-state battery, comprising the positive electrode sheet according to the fifth aspect of the present invention. Thus, the solid-state battery has higher capacity, cycle performance and rate performance.

[0066] In the seventh aspect of the present invention, the present invention proposes an electrical device, including the solid-state battery described in the sixth aspect of the present invention.

[0067] Additional aspects and advantages of the present invention will be given in part in the following description and in part will be obvious from the following description, or will be learned through practice of the present invention. BRIEF DESCRIPTION OF THE DRAWINGS

[0068] The above and / or additional aspects and advantages of the present invention will become apparent and easily understood from the description of the embodiments in conjunction with the following drawings, in which:

[0069] Figure 1 It is a schematic flow chart of a method for preparing a NASICON type solid electrolyte according to an embodiment of the present invention;

[0070] Figure 2is a schematic structural diagram of a positive electrode active material according to an embodiment of the present invention;

[0071] Figure 3 This is the EDS test mapping diagram of the NASICON solid electrolyte phase prepared in Example 1;

[0072] Figure 4 The XRD spectra of Example 1 and Comparative Example 1 are shown in FIG.

[0073] Figure 5 The XRD spectra of Example 1 and Comparative Example 1 are shown in FIG.

[0074] Figure 6 The first charge and discharge curves of the batteries of Example 1 and Comparative Example 1;

[0075] Figure 7 This is the EDS test mapping diagram of the positive electrode material in Example 3. DETAILED DESCRIPTION

[0076] Embodiments of the present invention are described in detail below, examples of which are shown in the accompanying drawings, wherein the same or similar reference numerals throughout represent the same or similar elements or elements having the same or similar functions. The embodiments described below with reference to the accompanying drawings are exemplary and are intended to be used to explain the present invention, and should not be construed as limiting the present invention.

[0077] The endpoints and any values ​​of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of each range, the endpoint values ​​of each range and the individual point values, and the individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.

[0078] In one aspect of the present invention, the present invention provides a NASICON type solid electrolyte. According to an embodiment of the present invention, the NASICON type solid electrolyte comprises: Li x M1 y M2 z M3 u M4 v (PO4) w1 (PS4) w2 , where y+z+u+v=2, w1+w2=3, 0 <x<2,0≤y≤0.5,0<z≤1,0<u<2,0≤v≤3,1≤w1≤3,

[0079] 0.0001 ≤ w2 ≤ 0.3, M1 includes at least one of Mg, Na, K, and Zn, M2 includes at least one of Al, Ga, In, Y, Sc, La, and Ce, M3 includes at least one of Ti, Zr, Hf, and Ge, and M4 includes at least one of Cr, Mo, Ca, Fe, Si, W, Nb, Sm, V, and B.

[0080] For the NASICON-type solid electrolyte according to an embodiment of the present invention, introducing S element enables the active free cations on the material surface to be reduced and a dispersed inert phase to precipitate on the surface, making it resistant to further corrosion in a strong reducing environment of S. 2- In subsequent applications to sulfide all-solid-state battery systems, it can improve the interfacial stability of the solid electrolyte. The main elements include Li, M1, M2, M3, M4 (M1 includes at least one of Mg, Na, K, and Zn, M2 includes at least one of Al, Ga, In, Y, Sc, La, and Ce, M3 includes at least one of Ti, Zr, Hf, and Ge, and M4 includes at least one of Cr, Mo, Ca, Fe, Si, W, Nb, Sm, V, and B), which can improve the ionic conductivity of the solid electrolyte. Thus, this NASICON-type solid electrolyte has excellent interfacial stability and ionic conductivity. By coating it on the cathode active material matrix and applying it to a solid-state battery, it can reduce the space charge layer and interfacial side reactions between the cathode active material matrix and the solid electrolyte layer as well as the impedance of the solid-state battery, and improve the capacity, cycling performance, and rate performance of the solid-state battery.

[0081] According to an embodiment of the present invention, the Li x M1 y M2 z M3 u M4 v (PO4) w1 (PS4) w2 In it, 0 < x < 2, for example, 0.001 ≤ x ≤ 4.999, 0.005 ≤ x ≤ 4.9, 0.01 ≤ x ≤ 4.9, 0.05 ≤ x ≤ 4.9, 0.1 ≤ x ≤ 4.9, 0.5 ≤ x ≤ 4.5, 0.7 ≤ x ≤ 4.2, 1 ≤ x ≤ 4, 1.5 ≤ x ≤ 3.5, 1.7 ≤ x ≤ 3.2, 2 ≤ x ≤ 3, 2.2 ≤ x ≤ 2.8, 2.5 ≤ x ≤ 2.8, etc. According to a specific embodiment of the present invention, the Li x M1 y M2 z M3 u M4 v (PO4) w1 (PS4) w2 In it, 0.6 ≤ x ≤ 3.2, and further, 1 ≤ x ≤ 2.

[0082] According to an embodiment of the present invention, the Li x M1 y M2 z M3 u M4 v (PO4) w1 (PS4) w2 In, 0 ≤ y ≤ 0.5, for example, 0.001 ≤ y ≤ 0.49, 0.005 ≤ y ≤ 0.49, 0.01 ≤ y ≤ 0.49, 0.05 ≤ y ≤ 0.49, 0.1 ≤ y ≤ 0.49, 0.15 ≤ y ≤ 0.49, 0.18 ≤ y ≤ 0.45, 0.2 ≤ y ≤ 0.42, 0.22 ≤ y ≤ 0.4, 0.25 ≤ y ≤ 0.38, 0.28 ≤ y ≤ 0.35, 0.3 ≤ y ≤ 0.32, etc. According to a specific embodiment of the present invention, the Li x M1 y M2 z M3 u M4 v (PO4) w1 (PS4) w2 In, 0 ≤ y ≤ 0.3, further, 0 ≤ y ≤ 0.1.

[0083] According to an embodiment of the present invention, the Li x M1 y M2 z M3 u M4 v (PO4) w1 (PS4) w2 In, 0 < z ≤ 1, for example, 0.001 ≤ z ≤ 1, 0.005 ≤ z ≤ 1, 0.01 ≤ z ≤ 1, 0.05 ≤ z ≤ 1, 0.1 ≤ z ≤ 1, 0.1 ≤ z ≤ 0.9, 0.2 ≤ z ≤ 0.8, 0.3 ≤ z ≤ 0.7, 0.4 ≤ z ≤ 0.6, 0.5 ≤ z ≤ 0.6, etc. According to a specific embodiment of the present invention, the Li x M1 y M2 z M3 u M4 v (PO4) w1 (PS4) w2 In, 0.2 ≤ z ≤ 0.7, further, 0.2 ≤ z ≤ 0.4.

[0084] According to an embodiment of the present invention, the Li x M1 y M2 z M3 u M4 v (PO4) w1 (PS4) w2where 0 < u < 2, for example 0.001 ≤ u ≤ 1.9, 0.005 ≤ u ≤ 1.9, 0.01 ≤ u ≤ 1.9, 0.05 ≤ u ≤ 1.9, 0.07 ≤ u ≤ 1.9, 0.1 ≤ u ≤ 1.9, 0.3 ≤ u ≤ 1.7, 0.5 ≤ u ≤ 1.5, 0.7 ≤ u ≤ 1.2, 1 ≤ u ≤ 1.2, etc. According to a specific embodiment of the present invention, the Li x M1 y M2 z M3 u M4 v (PO4) w1 (PS4) w2 where 0.9 ≤ u < 2, and further 1.4 ≤ u < 2.

[0085] According to an embodiment of the present invention, the Li x M1 y M2 z M3 u M4 v (PO4) w1 (PS4) w2 where 0 ≤ v ≤ 3, for example 0.001 ≤ v ≤ 3, 0.005 ≤ v ≤ 3, 0.01 ≤ v ≤ 3, 0.05 ≤ v ≤ 3, 0.1 ≤ v ≤ 3, 0.5 ≤ v ≤ 3, 0.7 ≤ v ≤ 3, 1 ≤ v ≤ 3, 1.2 ≤ v ≤ 2.8, 1.5 ≤ v ≤ 2.5, 1.7 ≤ v ≤ 2.2, 1.7 ≤ v ≤ 2, etc. According to a specific embodiment of the present invention, the Li x M1 y M2 z M3 u M4 v (PO4) w1 (PS4) w2 where 0.2 ≤ v ≤ 2, and further 0.5 ≤ v ≤ 1.

[0086] According to an embodiment of the present invention, the Li x M1 y M2 z M3 u M4 v (PO4) w1 (PS4) w2 where 1 ≤ w1 ≤ 3, for example 1.2 ≤ w1 ≤ 2.7, 1.5 ≤ w1 ≤ 2.5, 1.7 ≤ w1 ≤ 2.3, 2 ≤ w1 ≤ 2.1, etc.

[0087] According to an embodiment of the present invention, the Li x M1 y M2 z M3 u M4 v(PO4) w1 (PS4) w2 , 0.0001≤w2≤0.3, for example, 0.0005≤w2≤0.3, 0.001≤w2≤0.3, 0.005≤w2≤0.3, 0.01≤w2≤0.3, 0.05≤w2≤0.3, 0.07≤w2≤0.3, 0.1≤w2≤0.3, 0.15≤w2≤0.25, 0.17≤w2≤0.22, 0.17≤w2≤0.2, etc.

[0088] In the present invention, the elemental composition of the NASICON solid electrolyte can be determined by instruments and methods known in the art, such as inductively coupled plasma emission spectrometry: the instrument standard refers to EPA6010D-2014 "Inductively Coupled Plasma Atomic Emission Spectrometry". The sample is treated by chemical methods to be digested into a solution, atomized into plasma and excited to produce characteristic spectral lines of the elements, and the element content is qualitatively and quantitatively analyzed according to the wavelength and intensity of the spectral lines (proportional to the concentration).

[0089] According to an embodiment of the present invention, the XRD spectrum of the NASICON solid electrolyte has a (113) characteristic peak, a (104) characteristic peak, a (024) characteristic peak and a (012) characteristic peak.

[0090] The peak position of the characteristic peak (113) is 24.490°-24.880°, and the full width at half maximum is 0.195°-0.290°;

[0091] The peak position of the characteristic peak (104) is 20.850°-21.110°, and the full width at half maximum is 0.200°-0.300°;

[0092] The peak position of the (024) characteristic peak is 29.640°-30.010°, and the full width at half maximum is 0.180°-0.320°;

[0093] The peak position of the (012) characteristic peak is 14.680°-15.990°, and the full width at half maximum is 0.165°-0.315°;

[0094] Specifically, the appearance of the above crystal structure information means that the elements in the corresponding NASICON solid electrolyte are doped into the unit cell to form a solid solution (according to Vegard's law), and the introduction of M1, M2, M3 and M4 elements and S elements is inconsistent with the chemical composition and element valence of conventional NASICON solid electrolytes, which will cause the charge balance to be maintained in the solid electrolyte in the form of point defects (for example, one atom is missing at a certain position in the unit cell). Such point defects, especially vacancy defects, will increase the transmission channel of lithium ions and improve ion conductivity. Some will cause the reconstruction of the electric field in the unit cell and improve electronic conductivity. The introduction of S element reduces the active free cations on the surface of the material and precipitates a dispersed inert phase on the surface, making it tolerant to S. 2- The further corrosion of the strong reducing environment can improve the interfacial stability of the solid electrolyte when it is subsequently applied to the sulfide all-solid-state battery system.

[0095] In the present invention, the phase testing method of the above-mentioned NASICON solid electrolyte includes: using the spectrum obtained by X-ray diffraction test (XRD) to perform target phase composition analysis and diffraction peak quantitative analysis; its basic working principle is based on the lattice interference phenomenon between the periodic arrangement of material lattice atoms and the incident high-energy X-ray particles, so that it can receive a specific strong interference signal. Different lattice materials have different lattice interference signals, which can be used for qualitative or quantitative analysis. The test target is Cu and analyzed under Cu Kα radiation. The tube voltage of the equipment is set to 40kV, the tube current is set to 200mA, the test angle range of the sample is 5° to 120°, the scanning rate is 1° / min, and the scanning step is 0.02°.

[0096] According to an embodiment of the present invention, the volume average particle size Dv of the NASICON type solid electrolyte is 50 is 0.01 μm-0.2 μm, for example, 0.05 μm-0.2 μm, 0.1 μm-0.2 μm, 0.12 μm-0.17 μm, 0.15 μm-0.17 μm, etc. According to a specific embodiment of the present invention, the volume average particle size Dv of the NASICON type solid electrolyte is 50 Therefore, the present invention adopts NASICON solid electrolyte with this particle size range, and after coating the positive electrode active material matrix, the two have better corresponding contact performance and higher contact point density, which is conducive to lithium ion transmission at the interface.

[0097] In the present invention, Dv50 refers to the particle size corresponding to when the cumulative volume distribution percentage reaches 50%, and is measured with reference to the standard GB / T19077-2016 using a laser particle size analyzer (eg, Malvern Master Size 3000).

[0098] In the present application, the specific surface area of ​​the NASICON solid electrolyte can be measured using instruments and methods known in the art. For example, it can be tested by referring to the following method: using the American Micromeritics multi-station fully automatic specific surface area and pore analyzer GeminiVII2390, take about 7g of the sample and put it into a 9cc long tube with a bulb, degas at 200°C for 2h, and then put it into the host for testing to obtain the BET specific surface area data of the positive electrode active material 1000.

[0099] According to an embodiment of the present invention, the pH of the NASICON solid electrolyte is 7.2-9, such as 7.5-8.7, 7.8-8.5, 8-8.2, etc. Therefore, the present invention controls the pH of the NASICON solid electrolyte to be within the above range, so that it can be chemically stable when matching the positive electrode active material in a high alkaline environment, thereby reducing corrosion to the positive electrode active material.

[0100] In the present invention, the pH test method of the NASICON solid electrolyte comprises: weighing 5 grams of the sample to be tested and placing it in 95 grams of deionized water at room temperature and stirring for 5 minutes, filtering the stirred slurry through a Buchner funnel with filter paper to obtain a filtrate, and titrating the obtained filtrate in a Metrohm 888 potentiometric titrator at room temperature or directly testing it using a pH meter.

[0101] According to an embodiment of the present invention, the ionic conductivity of the NASICON solid electrolyte is 1.0×10 -4 S / cm-1.5×10 -3 S / cm, for example 1.5×10 -4 S / cm-5×10 -3 S / cm, 3.0×10 -4 S / cm-1.0×10 -3 S / cm, 4.0×10 - 4 S / cm-1.0×10 -3 S / cm, 5.0×10 -4 S / cm-1.0×10 -3 S / cm,7.0×10 -4 S / cm-1.1×10 -3 S / cm,9×10 -4 S / cm-1.1×10 -3 S / cm, etc.

[0102] According to an embodiment of the present invention, the electronic conductivity of the NASICON solid electrolyte is 1.0×10 -10 S / cm-1.0×10 -8S / cm, for example 5×10 -10 S / cm-1.0×10 -8 S / cm, 1.0×10 -9 S / cm-1.0×10 -8 S / cm, 5.0×10 -9 S / cm-1.0×10 -8 S / cm,7.0×10 -9 S / cm-1.0×10 -8 S / cm.

[0103] Therefore, the present invention controls the ionic conductivity and electronic conductivity of the NASICON solid electrolyte within the above range, which can reduce the impedance of the solid-state battery and improve the power performance and cycle performance of the battery.

[0104] In the present invention, the test method for the ionic conductivity and electronic conductivity of the NASICON solid electrolyte is to use an electrochemical workstation to perform electrochemical impedance spectroscopy (EIS) test and direct current polarization (DC) test. The frequency range of the electrical signal of the EIS test is 0.01Hz to 10000000Hz, and the disturbance amplitude of the AC voltage is 10mV. The constant voltage of the DC test is 1.0V, which lasts for 3000s. σ=L / RS is used to calculate the ionic conductivity and electronic conductivity, where R is the resistance value, L is the thickness, and S is the area of ​​the particles. Specifically, the test of the ionic conductivity and electronic conductivity of the above-mentioned NASICON solid electrolyte is tested at the mold battery level, and the specific composition of the mold battery is: stainless steel electrode / / conductive carbon / / solid electrolyte / / conductive carbon / / stainless steel electrode. The assembly method of the test mold battery device is: pre-press about 100 mg of solid electrolyte sample, add conductive carbon on both sides of the sample, press it into a battery cell under 300 MPa, and place the battery cell between two stainless steel electrodes to assemble the mold battery.

[0105] In a second aspect of the present invention, the present invention provides a method for preparing a NASICON type solid electrolyte. According to an embodiment of the present invention, reference Figure 1 , the method comprising:

[0106] S100: Mix and sinter the lithium-containing compound, the M1-containing compound, the M2-containing compound, the M3-containing compound, the M4-containing compound and the phosphorus-containing compound

[0107] In this step, the lithium-containing compound, the M1-containing compound, the M2-containing compound, the M3-containing compound, the M4-containing compound and the phosphorus-containing compound are mixed and sintered to obtain a solid electrolyte.

[0108] According to an embodiment of the present invention, the lithium-containing compound, the M1-containing compound, the M2-containing compound, the M3-containing compound, and the M4-containing compound may include but are not limited to oxides, hydroxides, oxalates, organic alcohol salts or carbonates of the corresponding elements, and the phosphorus-containing compound may be phosphoric acid or phosphates. At the same time, the lithium-containing compound, the M1-containing compound, the M2-containing compound, the M3-containing compound, and the M4-containing compound may also be phosphates of the corresponding elements, and when at least one of the lithium-containing compound, the M1-containing compound, the M2-containing compound, the M3-containing compound, and the M4-containing compound is a phosphate of the corresponding element, it is not necessary to add the phosphorus-containing compound separately.

[0109] According to an embodiment of the present invention, the mixed sintering of the lithium-containing compound, the M1-containing compound, the M2-containing compound, the M3-containing compound, the M4-containing compound and the phosphorus-containing compound and the mixed sintering of the phosphorus-containing compound can be performed by the following steps:

[0110] (1-1) A lithium-containing compound, an M1-containing compound, an M2-containing compound, an M3-containing compound, an M4-containing compound, a phosphorus-containing compound, an organic monomer, a first solvent, an initiator, and a catalyst are mixed to obtain a mixture.

[0111] As an example, the organic monomer includes but is not limited to at least one of acrylamide, methylenebisacrylamide, styrene, butadiene and methyl methacrylate; the first solvent includes but is not limited to at least one of water, N-methyl-2-pyrrolidone, phthalate, dibasic lipid, long-chain alcohol and pyrrolidone; the initiator includes but is not limited to at least one of benzoyl peroxide, (NH4)2S2O8 and K2S2O8; the catalyst includes at least one of N,N,N′N′-tetramethylethylenediamine, N,N,N',N'-tetramethyl-1,6-hexanediamine, N,N-diisopropylethylamine, N-(3-aminopropyl)-N-dodecyl-1,3-propylenediamine;

[0112] (1-2) The mixture is heated to initiate a polymerization reaction to obtain a bulk solid electrolyte precursor.

[0113] According to an embodiment of the present invention, in step (1-2), the polymerization reaction temperature is 80°C-200°C, such as 100°C-200°C, 120°C-170°C, 150°C-160°C, etc. Therefore, at the polymerization temperature, the organic monomer undergoes a polymerization reaction under the action of the initiator, so that the raw material elements of the NASICON material can be evenly combined at the molecular level. After subsequent sintering, the polymer is oxidized and volatilized, and the raw materials react to each other to easily form a uniform NASICON phase.

[0114] According to a specific embodiment of the present invention, the temperature of the polymerization reaction is 90°C-150°C, and further, the temperature of the polymerization reaction is 96°C-120°C.

[0115] (1-3) The block-like solid electrolyte precursor is pre-sintered and crushed to obtain a powder-like solid electrolyte precursor.

[0116] According to an embodiment of the present invention, the bulk solid electrolyte precursor obtained above is pre-sintered to remove organic polymers in the solid electrolyte precursor to prevent organic residues from affecting electrical performance, and then crushed to obtain a powdered solid electrolyte precursor.

[0117] According to an embodiment of the present invention, in step (1-3), the pre-sintering temperature is 300°C-600°C, such as 350°C-550°C, 400°C-500°C, 450°C-500°C, etc. According to a specific embodiment of the present invention, the pre-sintering temperature is 350°C-575°C, and further, the pre-sintering temperature is 380°C-560°C.

[0118] According to an embodiment of the present invention, in step (1-3), the duration of the pre-sintering is 2 hours to 6 hours, such as 2.5 hours to 5.5 hours, 3 hours to 5 hours, 3.5 hours to 4.5 hours, 3.5 hours to 4 hours, etc. According to a specific embodiment of the present invention, the duration of the pre-sintering is 2 hours to 5 hours, and further, the pre-sintering time is 2 hours to 4 hours.

[0119] Therefore, the present invention adopts the above-mentioned pre-sintering conditions to significantly remove the organic polymer in the solid electrolyte precursor to prevent the residual organic matter from affecting the electrical performance.

[0120] (1-4) The powdered solid electrolyte precursor is sintered and crushed to obtain a micrometer-sized solid electrolyte.

[0121] According to an embodiment of the present invention, in step (1-4), the sintering temperature is 650°C-900°C, such as 700°C-850°C, 750°C-800°C, etc. According to a specific embodiment of the present invention, the sintering temperature is 700°C-875°C, and further, the sintering temperature is 730°C-860°C.

[0122] According to an embodiment of the present invention, in step (1-4), the duration of the sintering is 4 hours to 10 hours, such as 5 hours to 9 hours, 6 hours to 8 hours, 6.5 hours to 7.5 hours, etc. According to a specific embodiment of the present invention, the duration of the sintering is 5 hours to 9 hours, and further, the sintering time is 6 hours to 8 hours.

[0123] S200: dispersing the solid electrolyte in a second solvent and grinding it to obtain a nanoscale slurry, adding sulfide to the nanoscale slurry, mixing and drying

[0124] In this step, the solid electrolyte is dispersed in the second solvent and ground to obtain a nanoscale slurry, sulfide is added to the nanoscale slurry and mixed, and then dried in a vacuum or other inert atmosphere to obtain a powdery, nanoscale NASICON solid electrolyte. Sulfide is added to the slurry with nanoscale particles for full mixing and contact. During the drying process, the sulfide raw material and the second solvent undergo sublimation. During the transformation from the solid phase to the gas phase, the sulfide has high reactivity, and sulfur is introduced on the surface of the nanoscale solid electrolyte with a high specific surface area. The gaseous sulfide and the second solvent are discharged with the tail gas. This method has high sulfur introduction efficiency and good impurity removal effect.

[0125] According to an embodiment of the present invention, the volume average particle size Dv50 of the slurry is 5nm-500nm, for example, 10nm-500nm, 50nm-500nm, 100nm-450nm, 150nm-400nm, 200nm-350nm, 250nm-300nm. According to a specific embodiment of the present invention, the volume average particle size Dv50 of the slurry is 10nm-200nm, and further, the volume average particle size of the slurry is 50nm-100nm. Therefore, the present invention can make the solid electrolyte have high reactivity and good dispersibility by controlling the volume average particle size Dv50 of the slurry to be within the above range, and can achieve good physical and chemical contact with the positive electrode active material matrix and uniform and dense coating during the coating process of the positive electrode active material matrix.

[0126] As an example, the second solvent includes but is not limited to at least one of n-heptane, toluene and dimethyl ether, and the sulfide includes but is not limited to phosphorus pentasulfide, lithium sulfide, thiourea, sulfur and other sulfur-containing compounds with low sublimation temperature (for example, sublimation temperature 100°C-300°C).

[0127] According to an embodiment of the present invention, the amount of the sulfide added is 0.1wt%-3wt% of the solid electrolyte, such as 0.5wt%-3wt%, 0.7wt%-3wt%, 1wt%-3wt%, 1.5wt%-2.5wt%, 1.7wt%-2wt%, etc. Specifically, during the heating process, the sulfur element will be lost, so the amount of sulfide added in this process is excessive compared to the sulfur content in the NASICON solid electrolyte composition. According to a specific embodiment of the present invention, the amount of the sulfide added is 0.1wt%-1wt% of the solid electrolyte.

[0128] According to an embodiment of the present invention, the drying temperature is 120°C-600°C, for example, 150°C-580°C, 170°C-550°C, 200°C-520°C, 230°C-500°C, 250°C-480°C, 270°C-450°C, 300°C-420°C, 320°C-400°C, 350°C-380°C, etc. According to a specific embodiment of the present invention, the drying temperature is 150°C-500°C.

[0129] Thus, the NASICON type solid electrolyte obtained by the method of the present invention, its transition metal (M1-M4) is introduced during the thermal polymerization process to achieve atomic-level uniform mixing of elements, sulfur elements are introduced during the nano-heating process to achieve thio-introduction, the prepared solid electrolyte composition is uniform, the average particle size can reach the nanoscale, the presence of transition elements inside the lattice makes its structural stability excellent, and the prepared NASICON type solid electrolyte slurry and powder have a high specific surface area, have a strong specific surface energy, and are suitable for the preparation of composite solid electrodes and ceramic coated diaphragms. Thus, the method can be used to prepare the above-mentioned NASICON type solid electrolyte with excellent interface stability and ionic conductivity, which is coated on the positive active material matrix, and applied to solid-state batteries, which can reduce the space charge layer and interface side reactions between the positive active material matrix and the solid electrolyte layer and the impedance of the solid-state battery, and improve the capacity, cycle performance and rate performance of the solid-state battery.

[0130] It should be noted that the above-mentioned features and advantages of the “NASICON-type solid electrolyte” are also applicable to the method for preparing the NASICON-type solid electrolyte, and will not be described in detail here.

[0131] In the third aspect of the present invention, the present invention provides a positive electrode active material. According to an embodiment of the present invention, reference Figure 2 The positive electrode active material includes a positive electrode active material matrix 100 and a coating layer 200 .

[0132] As an example, the positive electrode active material matrix 100 includes but is not limited to at least one of lithium nickel oxide, lithium cobalt oxide, lithium manganese oxide, lithium nickel manganese oxide, lithium nickel cobalt manganese oxide, lithium nickel cobalt aluminum oxide, lithium nickel cobalt manganese aluminum oxide, lithium manganese-rich layered oxides and their derivatives, lithium iron phosphate and lithium manganese iron phosphate.

[0133] According to an embodiment of the present invention, the coating layer 200 is formed on at least a portion of the surface of the positive electrode active material matrix 100, and the coating layer 200 includes the NASICON type solid electrolyte described in the first aspect of the present invention or the NASICON type solid electrolyte obtained by the method described in the second aspect of the present invention.

[0134] According to the positive electrode active material of the embodiment of the present invention, by forming a coating layer 200 containing the above-mentioned NASICON type solid electrolyte on the surface of the positive electrode active material matrix 100, that is, when the positive electrode active material is assembled into a solid-state battery, the coating layer 200 containing the above-mentioned NASICON type solid electrolyte is located between the positive electrode active material matrix 100 and the solid electrolyte layer. On the one hand, it can buffer the large gradient effect of chemical potential energy between the positive electrode active material matrix 100 and the solid electrolyte layer, and on the other hand, it can inhibit the formation of a lithium depletion layer at the interface between the positive electrode active material matrix 100 and the solid electrolyte layer, which can effectively reduce the large interface resistance caused by the space charge layer, and also play a role in inhibiting interface side reactions. At the same time, because the NASICON type solid electrolyte has excellent interface stability and ionic conductivity, it can improve the interface stability of the positive electrode active material, so that it can be applied to solid-state batteries, which can reduce the space charge layer and interface side reactions between the positive electrode active material matrix 100 and the solid electrolyte layer and the impedance of the solid-state battery, and improve the capacity, cycle performance and rate performance of the solid-state battery.

[0135] According to an embodiment of the present invention, based on the total amount of the positive electrode active material matrix 100, the mass proportion of the NASICON type solid electrolyte is 0.05%-1%, such as 0.08%-1%, 0.1%-1%, 0.3%-1%, 0.5%-1%, 0.6%-1%, 0.7%-1%, 0.8%-1%, 0.9%-1%, etc. Therefore, the present invention controls the mass proportion of the NASICON type solid electrolyte within the above range, which can further improve the interface stability and ionic conductivity of the positive electrode active material, so that it can be applied to solid-state batteries, and the space charge layer and interface side reactions between the positive electrode active material matrix 100 and the solid electrolyte layer and the impedance of the solid-state battery can be reduced, thereby improving the capacity, cycle performance and rate performance of the solid-state battery.

[0136] According to an embodiment of the present invention, the positive electrode active material undergoes acid-base titration treatment and exhibits a phosphate characteristic titration peak between pH = 5 and 8. Specifically, the appearance of this characteristic titration peak means that phosphate is generated at the interface between the NASICON solid electrolyte and the positive electrode active material matrix 100 during the coating process, which can serve as a buffer layer to balance the potential difference between the NASICON solid electrolyte and the positive electrode active material, alleviate the generation of the space charge layer, and reduce the interface impedance, thereby better exerting the electrochemical performance of the positive electrode material.

[0137] In the present invention, the "characteristic titration peak" is obtained by acid-base titration test, and the specific steps are: weigh 5 grams of the sample to be tested and put it into 95 grams of deionized water at room temperature and stir for 5 minutes. The stirred slurry is filtered through a Buchner funnel with filter paper to obtain a filtrate. The obtained filtrate is titrated in a Metrohm 888 potentiometric titrator at room temperature to obtain a titration curve, and the pH value corresponding to the position of the characteristic titration peak in the curve is read.

[0138] PO4 in the solution to be tested 3- The potential corresponding to the stoichiometric ratio of the concentration of hydrochloric acid in the titration solution is the equivalence point potential. At this potential, there is a characteristic titration peak in the titration curve. The calculation of the equivalence point potential follows the following formula:

[0139] E 等 =E 终 +(E 初 -E 终 )*V 滴 / V 总

[0140] Where E 等 E is the equivalence point potential; 终 is the titration endpoint potential; E 初 is the titration starting potential; V 滴 V is the volume of the titrant added; 总 is the total volume of the titrant. The relationship between the titration endpoint potential and the titration start potential is inferred based on the volume of the titrant, and the equivalence point potential is further calculated. 初 -E 终 ) is so that every additional drop of titrant added to the volume contributes to the equivalence point potential.

[0141] It should be noted that the above-mentioned features and advantages of “NASICON-type solid electrolyte and preparation method thereof” are also applicable to the positive electrode active material and will not be elaborated here.

[0142] In a fourth aspect of the present invention, the present invention provides a method for preparing the above-mentioned positive electrode active material. According to an embodiment of the present invention, the method comprises:

[0143] The positive electrode active material matrix and the NASICON type solid electrolyte are mixed and heat-treated to form a coating layer including the NASICON type solid electrolyte on at least a portion of the surface of the positive electrode active material matrix.

[0144] Wherein, the NASICON-type solid electrolyte includes the NASICON-type solid electrolyte described in the first aspect of the present invention or the NASICON-type solid electrolyte obtained by the method described in the second aspect of the present invention.

[0145] Therefore, this method can be used to prepare the above-mentioned positive electrode active material with high interface stability and ionic conductivity, so that it can be applied to solid-state batteries, which can reduce the space charge layer and interface side reactions between the positive electrode active material matrix and the solid electrolyte layer and the impedance of the solid-state battery, and improve the capacity, cycle performance and rate performance of the solid-state battery.

[0146] According to an embodiment of the present invention, the temperature of the heat treatment is 300°C-700°C, such as 350°C-650°C, 400°C-600°C, 450°C-550°C, 450°C-500°C, etc. According to a specific embodiment of the present invention, the temperature of the heat treatment is 375°C-625°C, and further, the temperature of the heat treatment is 420°C-580°C.

[0147] According to an embodiment of the present invention, the duration of the heat treatment is 2 hours to 10 hours, such as 2 hours to 9 hours, 3 hours to 8 hours, 4 hours to 7 hours, 5 hours to 6 hours, etc. According to a specific embodiment of the present invention, the duration of the heat treatment is 4 hours to 10 hours, and further, the heat treatment time is 5 hours to 10 hours.

[0148] Therefore, the present invention adopts the above-mentioned heat treatment conditions to significantly improve the binding force of the coating layer containing the NASICON type solid electrolyte on the positive electrode active material matrix, thereby improving the stability of the positive electrode active material.

[0149] It should be noted that the above-mentioned features and advantages of the “positive electrode active material” are also applicable to the method for preparing the positive electrode active material, and will not be described in detail here.

[0150] In a fifth aspect of the present invention, the present invention provides a positive electrode plate, comprising the positive electrode active material described in the third aspect of the present invention or the positive electrode active material obtained by the method described in the fourth aspect of the present invention.

[0151] According to an embodiment of the present invention, the positive electrode plate includes a positive electrode collector and a positive electrode active material layer arranged on the positive electrode collector, the positive electrode active material layer includes the above-mentioned positive electrode active material, wherein the positive electrode collector can be a metal foil or a composite current collector (the metal material can be arranged on a polymer substrate to form a composite current collector), for example, the positive electrode collector can be aluminum foil.

[0152] According to some embodiments of the present invention, the positive electrode active material layer may further optionally include a binder. As an example, the binder may include at least one of polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), vinylidene fluoride-tetrafluoroethylene-propylene terpolymer, vinylidene fluoride-hexafluoropropylene-tetrafluoroethylene terpolymer, tetrafluoroethylene-hexafluoropropylene copolymer, or fluorine-containing acrylate resin.

[0153] According to some embodiments of the present invention, the positive electrode active material layer may further optionally include a conductive agent. As an example, the conductive agent may include at least one of superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene or carbon nanofibers.

[0154] According to some embodiments of the present invention, the positive electrode sheet can be prepared in the following manner: the components for preparing the positive electrode sheet, such as the positive electrode active material, the conductive agent, the binder and any other components are dispersed in a solvent (such as N-methylpyrrolidone) to form a positive electrode slurry; the positive electrode slurry is coated on the positive electrode collector, and after drying, cold pressing and other processes, the positive electrode sheet can be obtained.

[0155] It should be noted that the features and advantages described above for the positive electrode active material and the preparation method thereof are also applicable to the positive electrode plate and will not be described in detail here.

[0156] In a sixth aspect of the present invention, the present invention provides a solid-state battery. According to an embodiment of the present invention, the solid-state battery includes the above-mentioned positive electrode sheet.

[0157] As an example, a solid-state battery includes a positive electrode sheet, a negative electrode sheet, and a solid electrolyte layer, wherein the solid electrolyte layer is located between the positive electrode sheet and the negative electrode sheet.

[0158] According to an embodiment of the present invention, the negative electrode plate includes a negative electrode current collector and a negative electrode active material layer arranged on the negative electrode current collector, the negative electrode active material layer includes a negative electrode active material, wherein the negative electrode current collector can be a metal foil or a composite current collector (the metal material can be arranged on a polymer substrate to form a composite current collector), for example, the positive electrode current collector can be a copper foil.

[0159] According to an embodiment of the present invention, the negative electrode active material may include at least one of the following materials: artificial graphite, natural graphite, soft carbon, hard carbon, silicon-based materials, tin-based materials, lithium titanate, etc.

[0160] According to an embodiment of the present invention, the negative electrode active material layer may further include a conductive agent, which may include at least one of superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene or carbon nanofibers.

[0161] According to an embodiment of the present invention, the negative electrode active material layer may further optionally include other additives, such as a thickener (eg, sodium carboxymethyl cellulose (CMC-Na)).

[0162] According to an embodiment of the present invention, the negative electrode sheet can be prepared in the following manner: the components for preparing the negative electrode sheet, such as the negative electrode active material, the conductive agent, and the binder are dispersed in a solvent (such as deionized water) to form a negative electrode slurry; the negative electrode slurry is coated on the negative electrode collector, and after drying, cold pressing and other processes, the negative electrode sheet can be obtained.

[0163] According to an embodiment of the present invention, the negative electrode plate may include a metal lithium plate or a lithium alloy, such as a lithium-indium alloy.

[0164] According to an embodiment of the present invention, the solid electrolyte layer between the positive electrode sheet and the negative electrode sheet may include but is not limited to at least one of LiPSCl, LiGePS, LiSnPS, LiSiPSCl, LiSiPSBr and LiSiPSI.

[0165] It should be noted that the above-mentioned features and advantages described for the positive electrode plate are also applicable to the solid-state battery and will not be repeated here.

[0166] In a seventh aspect of the present invention, the present invention provides an electric device. According to an embodiment of the present invention. The electric device includes the above-mentioned solid-state battery. According to an embodiment of the present invention, the electric device may include but is not limited to a mobile phone, a laptop computer, an electric vehicle, etc.

[0167] It should be noted that the features and advantages described above for solid-state batteries are also applicable to the electrical equipment and will not be repeated here.

[0168] Below, the embodiment of the present invention is described. The embodiment described below is exemplary, is only used to explain the present invention, and cannot be interpreted as limiting the present invention. If no specific technology or conditions are indicated in the embodiment, the technology or conditions described in the literature in this field or the product instructions are used. If the manufacturer of the reagents or instruments is not indicated, they are all conventional products that can be obtained commercially.

[0169] Example 1

[0170] The method for preparing a NASICON type solid electrolyte comprises:

[0171] Step (1-1): weighing Li2CO3, Al2O3, ZnO, TiO2, and NH4H2PO4 compounds according to the stoichiometric ratio of NASICON solid electrolyte S1, adding a certain amount of pure water to mix, and then mixing and crushing them in a ball mill to obtain a mixed slurry A with a solid content of 50%; adding 50 weight% of acrylamide (monomer), (NH4)2S2O8 (initiator) and N,N,N′N′-tetramethylethylenediamine (TEMED) catalyst to the mixed slurry A, and dispersing them evenly in a stirring device to obtain a mixed slurry B;

[0172] Step (1-2): pouring the mixed slurry B into a sagger container and drying it in a 100° C. forced air oven to initiate a polymerization reaction of the substances in the mixed slurry B, and obtaining a bulk solid electrolyte precursor after 12 hours;

[0173] Step (1-3): pre-sinter the bulk solid electrolyte precursor obtained in step (1-2) at 500° C. in a muffle furnace for 2 hours, and crush the sintered product in a wall breaker for 5 minutes to obtain a powdered solid electrolyte precursor.

[0174] Step (1-4): Sinter the powdered solid electrolyte precursor obtained in step (1-3) at 750° C. in a muffle furnace for 6 hours, and crush the sintered product in a jet mill to obtain a powdered, micron-sized solid electrolyte.

[0175] Step (1-5): The solid electrolyte obtained in step (1-4) is dispersed in a solvent of n-heptane and then sand-milled at 2000 rpm in a sand mill for 2 hours to obtain a nanoscale slurry with a solid content of 50%, and then the slurry is mixed with P2S5 (the solid electrolyte and P2S5 are mixed in a mass ratio of 1:0.01) and dried under nitrogen protection at a drying temperature of 300°C, and the powder obtained after the heat treatment is further dissociated by a jet mill to obtain a NASICON type solid electrolyte.

[0176] The remaining embodiments and comparative examples are consistent with Example 1, except for the following differences:

[0177] Example 2

[0178] The difference from Example 1 is that the raw materials used in step (1-1) are LiOH, Al2O3, Y2O3, TiO2, and P2O5; step (1-4): the solid electrolyte precursor obtained in step (1-3) is sintered at 800°C in a muffle furnace for 6 hours; step (1-5): the solid electrolyte obtained in step (1-4) is dispersed in a solvent of dimethyl ether and then sand-milled at 2000 rpm in a sand mill for 2 hours to obtain a nanoscale slurry with a solid content of 55%, and then the slurry is mixed with Li2S (the solid electrolyte and Li2S are mixed in a mass ratio of 1:0.02) and dried under nitrogen protection at a drying temperature of 450°C.

[0179] Example 3

[0180] The difference from Example 1 is that the raw materials used in step (1-1) are Li3PO4, AlPO4, ZrO2, TiO2, and NH4H2PO4; step (1-4): step (1-4): the solid electrolyte precursor obtained in step (1-3) is sintered in a muffle furnace at 700°C for 6 hours; the solid electrolyte obtained in step (1-4) is dispersed in a solvent of n-heptane and then sand-milled in a sand mill at 2000 rpm for 2 hours to obtain a nanoscale slurry with a solid content of 55%, and then the slurry is mixed with Li7P3S 11 After mixing (solid electrolyte and Li7P3S 11 The mixture was mixed in a mass ratio of 1:0.05) and subjected to nitrogen protection spray drying at a drying temperature of 150°C.

[0181] Example 4

[0182] The difference from Example 1 is that the raw materials used in step (1-1) are C2H5OLi, C6H8Al2O 16 , TiO2, NH4H2PO4, C4H4NNbO9·xH2O; step (1-4): sintering the solid electrolyte precursor obtained in step (1-3) at 800°C in a muffle furnace for 6 hours; step (1-5): dispersing the solid electrolyte obtained in step (1-4) in a solvent of dimethyl ether and sand milling it at 2000rpm in a sand mill for 2 hours to obtain a nanoscale slurry with a solid content of 50%, and then mixing the slurry with Li3PS4 (the solid electrolyte and Li3PS4 are mixed in a mass ratio of 1:0.005) and performing nitrogen protection spray drying treatment, and the drying temperature is selected to be 200°C.

[0183] Example 5

[0184] The difference from Example 1 is that the raw materials used in step (1-1) are Li3PO4, AlPO4, GeO2, TiO2, NH4H2PO4, and H3BO3; step (1-5): the solid electrolyte obtained in step (1-4) is dispersed in a solvent of n-heptane and then sand-milled at 2000 rpm in a sand mill for 2 hours to obtain a nanoscale slurry with a solid content of 55%, and then the slurry is mixed with Li2S (the solid electrolyte and Li2S are mixed in a mass ratio of 1:0.02) and dried in a nitrogen-protected oven, and the drying temperature is selected to be 450°C.

[0185] Example 6

[0186] The difference from Example 1 is that the raw materials used in step (1-1) are Li3PO4, AlPO4, La2O3, TiO2, NH4H2PO4; WO3; step (1-5): the solid electrolyte obtained in step (1-4) is dispersed in solvent dimethyl ether and then sand-milled at 2000 rpm in a sand mill for 2 hours to obtain a nanoscale slurry with a solid content of 55%, and then the slurry is mixed with Li2S (the solid electrolyte and Li2S are mixed in a mass ratio of 1:0.01) and dried in a nitrogen protection oven, and the drying temperature is selected to be 450°C.

[0187] Example 7

[0188] The difference from Example 1 is that the raw materials used in step (1-1) are Li2CO3, Al2O3, MgO, TiO2, NH4H2PO4, and SiO2; step (1-5): the solid electrolyte obtained in step (1-4) is dispersed in a solvent of toluene and then sand-milled at 2000 rpm in a sand mill for 2 hours to obtain a nanoscale slurry with a solid content of 55%, and then the slurry is mixed with Li2S (the solid electrolyte and Li2S are mixed in a mass ratio of 1:0.02) and dried in a nitrogen-protected oven, and the drying temperature is selected to be 450°C.

[0189] Example 8

[0190] The difference from Example 1 is that the raw materials used in step (1-1) are Li2CO3, Al2O3, ZnO, TiO2, and NH4H2PO4; step (1-2): pouring the mixed slurry A into a sagger container and pre-sintering it at 500°C in a muffle furnace for 2 hours, crushing the sintered product in a wall breaker for 5 minutes to obtain a powdered solid electrolyte precursor; step (1-3): sintering the powdered solid electrolyte precursor obtained in step (1-3) at 750°C in a muffle furnace for 6 hours; step (1-4): dispersing the solid electrolyte obtained in step (1-3) in a solvent of n-heptane and sand milling it at 2000rpm in a sand mill for 2 hours to obtain a nanoscale slurry with a solid content of 50%, and then mixing the slurry with P2S5 (the solid electrolyte and P2S5 are mixed in a mass ratio of 1:0.01) and drying under nitrogen protection at a drying temperature of 300°C.

[0191] Example 9

[0192] The difference from Example 1 is that, in step (1-5), the solid electrolyte obtained in step (1-4) is dispersed in a solvent of dimethyl ether and then sand-milled at 2000 rpm in a sand mill for 2 hours to obtain a nanoscale slurry with a solid content of 55%, and then the slurry is mixed with Li2S (the solid electrolyte and Li2S are mixed in a mass ratio of 1:0.005) and dried under nitrogen protection at a drying temperature of 250°C.

[0193] Example 10

[0194] The difference from Example 1 is that, step (1-5): the solid electrolyte obtained in step (1-4) is dispersed in solvent dimethyl ether and then sand-milled in a sand mill at 2000 rpm for 2 hours to obtain a nanoscale slurry with a solid content of 55%, and then the slurry is mixed with P2S5 (the solid electrolyte and P2S5 are mixed in a mass ratio of 1:0.08) and dried under nitrogen protection at a drying temperature of 350°C.

[0195] Embodiment 11

[0196] The difference from Example 1 is that, step (1-5): the solid electrolyte obtained in step (1-4) is dispersed in a solvent of n-heptane and then sand-milled at 2000 rpm in a sand mill for 2 hours to obtain a nanoscale slurry with a solid content of 55%, and then the slurry is mixed with P2S5 (the solid electrolyte and P2S5 are mixed in a mass ratio of 1:0.1) and dried under nitrogen protection at a drying temperature of 350°C.

[0197] Example 12

[0198] The difference from Example 1 is that, step (1-5): the solid electrolyte obtained in step (1-4) is dispersed in a solvent of n-heptane and then sand-milled at 2000 rpm in a sand mill for 2 hours to obtain a nanoscale slurry with a solid content of 55%, and then the slurry is mixed with elemental sulfur (the solid electrolyte and S are mixed in a mass ratio of 1:0.2) and dried under nitrogen protection at a drying temperature of 450°C.

[0199] Example 13

[0200] The difference from Example 1 is that, step (1-5): the solid electrolyte obtained in step (1-4) is dispersed in a solvent of n-heptane and then sand-milled at 2000 rpm in a sand mill for 2 hours to obtain a nanoscale slurry with a solid content of 55%, and then the slurry is mixed with thiourea (the solid electrolyte and thiourea are mixed in a mass ratio of 1:0.3) and dried under nitrogen protection at a drying temperature of 400°C.

[0201] Embodiment 14

[0202] The difference from Example 1 is that, in step (1-5), the solid electrolyte obtained in step (1-4) is dispersed in a solvent of n-heptane and then sand-milled in a sand mill at 2000 rpm for 24 hours to obtain a nanoscale slurry with a solid content of 55%.

[0203] Embodiment 15

[0204] The difference from Example 1 is that the raw materials used in step (1-1) are LiOH, Al2O3, Y2O3, TiO2, and P2O5; step (1-5): the solid electrolyte obtained in step (1-4) is dispersed in a solvent of dimethyl ether and then sand-milled at 2000 rpm in a sand mill for 48 hours to obtain a nanoscale slurry with a solid content of 55%.

[0205] Comparative Example 1

[0206] The difference from Example 1 is that the raw materials used in step (1-1) are Li2CO3, Al2O3, TiO2, and NH4H2PO4; step (1-5): the solid electrolyte obtained in step (1-4) is combined with solvent water and sand-milled at 2000 rpm for 2 hours in a sand mill to obtain a nanoscale slurry with a solid content of 50%, and the slurry is spray-dried at a drying temperature of 120°C.

[0207] Comparative Example 2

[0208] The difference from Example 1 is that the raw materials used in step (1-1) are Li2CO3, Al2O3, ZnO, TiO2, and NH4H2PO4; step (1-5): the solid electrolyte obtained in step (1-4) is combined with solvent water and sand-milled at 2000 rpm for 2 hours in a sand mill to obtain a nanoscale slurry with a solid content of 50%, and the slurry is spray-dried at a drying temperature of 120°C.

[0209] Comparative Example 3

[0210] The difference from Example 1 is that the raw materials used in step (1-1) are Li2CO3, Al2O3, ZnO, TiO2, NH4H2PO4, and an excess of P2S5 compounds, which are weighed according to the stoichiometric ratio of NASICON solid electrolyte, a certain amount of pure water is added to mix, and then the mixture is mixed and crushed in a ball mill to obtain a mixed slurry A with a solid content of 50%; 50 weight% of acrylamide (monomer), (NH4)2S2O8 (initiator) and TEMED (catalyst) are added to the mixed slurry A, and the mixture is evenly dispersed in a stirring device to obtain a mixed slurry B;

[0211] Step (1-5): The solid electrolyte obtained in step (1-4) is mixed with solvent n-heptane in a sand mill at 2000 rpm for 2 hours to obtain a nanoscale slurry with a solid content of 50%. The slurry is dried in a nitrogen-protected oven at a drying temperature of 300°C.

[0212] Comparative Example 4

[0213] Only positive electrode active material is used, and the method for preparing the positive electrode active material includes:

[0214] The positive electrode active material LiNi0.93 Co 0.05 Mn 0.02 O2 was heat treated at 500℃ in an atmosphere furnace for 6 hours to obtain the heat-treated LiNi 0.93 Co 0.05 Mn 0.02 O2 material.

[0215] The positive electrode active material is prepared by using the aforementioned solid electrolyte, specifically,

[0216] Step (2-1): The NASICON solid electrolyte powder obtained in step (1-5) is mixed with the positive electrode active material matrix LiNi 0.93 Co 0.05 Mn 0.02 O2 was weighed at a mass ratio of 0.8:100 and put into a high-speed mixer to mix evenly to obtain NASICON solid electrolyte powder and positive electrode material matrix LiNi 0.93 Co 0.05 Mn 0.02 O2 mixture.

[0217] Step (2-2): The mixture obtained in step (2-1) is heat-treated at 500° C. in an atmosphere furnace for 6 hours to obtain a positive electrode active material coated with a NASICON type solid electrolyte.

[0218] The NASICON solid electrolytes of the above-mentioned embodiments and comparative examples were subjected to XRD, EIS, DC, pH and particle size tests, and the peak positions of the four strongest characteristic peaks (113), (104), (024) and (012) and the full width at half maximum (FWHM) were calculated and shown in Table 1. The chemical formula, ionic conductivity, electronic conductivity, pH value and particle size distribution results of the NASICON solid electrolyte are shown in Table 2.

[0219] like Figure 3 As shown, in the EDS test mapping diagram of the NASICON solid electrolyte phase prepared in Example 1, signal responses of elements Al, Ti, P, O, S, and Zn can be observed.

[0220] like Figure 4 and Figure 5 They are respectively the XRD patterns of Example 1 and Comparative Example 1, Figure 4 and Figure 5 It can be seen that the NASICON-type solid electrolyte S1 prepared in Example 1 has an obvious large-angle shift in peak position and an increase in the full width at half maximum FWHM in the XRD spectrum compared to the NASICON-type solid electrolyte M1 of Comparative Example 1.

[0221] like Figure 6As shown, the battery of Example 1 exhibits higher first cycle discharge capacity and first coulombic efficiency than those of Comparative Example 1.

[0222] like Figure 7 As shown, the signal responses of elements P, S, Ni, Co, and Mn can be observed in the EDS test mapping diagram of the positive electrode active material prepared in Example 3, indicating that the NASICON solid electrolyte is uniformly coated on the surface of the positive electrode active material.

[0223] Table 1

[0224]

[0225] Sulfur and other metal elements were introduced into the NASICON solid electrolytes in Examples 1-15, while Comparative Example 1 did not introduce any other elements except lithium aluminum titanium phosphorus oxygen, and Comparative Example 2 did not introduce S. In the process of preparing the NASICON solid electrolyte in Comparative Example 3, sulfur was introduced as a sulfur source in step (1-1). The positive electrode active material of Comparative Example 4 was not coated with a NASICON solid electrolyte. As shown in Table 1, compared with Comparative Examples 1-3, the peak positions of (113), (104), (024), and (012) in the XRD spectra of Examples 1-8 all underwent large angle shifts, and the full width at half maximum FWHM all increased. The four strongest peaks of the characteristic peaks of the NASICON-type solid electrolyte of Examples 1-18 are (113), (104), (024), and (012), and their peak positions are not less than 24.490°, 20.850°, 29.640°, and 14.680°; the corresponding full width at half maximum FWHM is greater than 0.165°, 0.160°, 0.180°, and 0.165°, indicating that the lattice collapse of the sulfur-modified NASICON-type solid electrolyte occurs.

[0226] Table 2

[0227]

[0228] As shown in Table 2, compared with Comparative Examples 1-3, the NASICON solid electrolytes of Examples 1-15 have higher ion conductivity, lower electronic conductivity, higher pH value, and a particle size Dv 50 Lower. Dv of Examples 1-15 50 All of them are less than 0.2μm, pH>7.2, ion conductivity>4.0×10 -4 S / cm, electronic conductivity <1.0×10 -8 S / cm. This indicates that the sulfur-modified NASICON solid electrolyte is a nanoscale raw material, weakly alkaline, and a good ion conductor and electronic insulator.

[0229] The positive electrode active materials obtained in Examples 1-8 and Comparative Examples 1-4 were subjected to acid-base titration, and the pH values ​​were as shown in Table 3. The positive electrode active materials were assembled into solid-state batteries, and the first discharge specific capacity, first coulomb efficiency, cycle performance, rate performance and interface stability of the solid-state batteries were characterized. The characterization results are shown in Table 3, where the cycle curves of the solid-state batteries in Example 1 and Comparative Example 1 are as shown in Table 3. Figure 6 shown.

[0230] Preparation of solid-state batteries:

[0231] The positive electrode active material, polyvinylidene fluoride binder, carbon black conductive agent and solid electrolyte sulfide Li6PS5Cl were fully dissolved in n-heptane (the mass ratio of positive electrode active material, binder, conductive agent and solid electrolyte was 70:0.5:1.5:28) to prepare a uniformly dispersed slurry, which was evenly coated on the surface of aluminum foil (loading amount was 36 mg / cm 2 ), and then transferred to a vacuum drying oven for complete drying, the obtained electrode sheet was roll-pressed, and then punched to obtain the positive electrode sheet.

[0232] Lithium-indium alloy is used as the negative electrode sheet, and 100 mg of sulfide Li6PS5Cl is used as the solid electrolyte, which is pressed into sheets under a pressure of 300 MPa to obtain a solid electrolyte layer, which is then stacked and assembled into a solid-state battery in the order of positive electrode sheet, solid electrolyte layer and negative electrode sheet.

[0233] All the above operations were carried out in a glove box filled with argon or in a laboratory with humidity controlled at a dew point of -40 °C.

[0234] Test of the real part of total impedance before cycling: Before cycling, the assembled solid-state battery is subjected to electrochemical impedance spectroscopy (EIS). The frequency range of the electrical signal of the EIS test is 0.01Hz to 10000000Hz, and the disturbance amplitude of the AC voltage is 10mV. The Nyquis graph obtained after the test is fitted by Zview software to obtain the real part of the total impedance of the battery before cycling. The smaller the real part of the total impedance, the better the chemical stability at the battery interface.

[0235] First discharge specific capacity, first cycle coulomb efficiency and cycle performance test: At 25°C, the solid-state battery was charged to 3.7V at a constant current of 0.1C to obtain the first charge specific capacity C0 of the solid-state battery, and then discharged to 2.0V at a constant current of 0.1C to obtain the first cycle discharge specific capacity C1 of the solid-state battery, and then charged and discharged at a constant current of 0.1C for 80 cycles, and the discharge specific capacity C of the 80th cycle was obtained. 80 . Battery first cycle coulombic efficiency = C1 / C0×100%. Battery capacity retention rate after 80 cycles = C 80 / C1×100%.

[0236] Rate performance test method: the solid-state battery is charged to 3.7V at a constant current of 0.33C, and then discharged to 2.0V at a constant current of 0.33C to obtain the first discharge specific capacity corresponding to 0.33C; then the solid-state battery is charged to 3.7V at a constant current of 0.5C, and then discharged to 2.0V at a constant current of 0.5C to obtain the discharge specific capacity corresponding to 0.5C; then the solid-state battery is charged to 3.7V at a constant current of 1C, and then discharged to 2.0V at a constant current of 1C to obtain the discharge specific capacity corresponding to 1C; finally, the solid-state battery is charged to 3.7V at a constant current of 0.33C, and then discharged to 2.0V at a constant current of 0.33C to obtain the second discharge specific capacity corresponding to 0.33C.

[0237] Table 3

[0238]

[0239]

[0240] In summary, it can be seen from Table 3 that the positive active materials corresponding to Examples 1-8 have a phosphate characteristic titration peak between pH = 5-8 after acid-base titration treatment, which means that NASICON solid electrolyte generates phosphate at the interface with the positive active material matrix during the coating process. The first discharge specific capacity, first cycle coulomb efficiency, 80-week cycle capacity retention rate, 0.33C corresponding to the first discharge specific capacity, 0.5C corresponding to the discharge specific capacity, 1.0C discharge specific capacity, 0.33C corresponding to the second discharge specific capacity of the solid-state battery of Examples 1-8 are all higher than those of Comparative Examples 1-4, and the real part value of the total impedance before the cycle is lower than that of Comparative Examples 1-4. This shows that the positive active material of the present invention uses a high-nickel material as a matrix, and forms a NASICON-type solid electrolyte coating layer on the surface of the matrix, has good chemical stability at the interface, and can improve the charge and discharge capacity and rate performance of the all-solid-state battery containing it, reduce the interface resistance, and improve the cycle capacity.

[0241] In the description of this specification, the description with reference to the terms "one embodiment", "some embodiments", "example", "specific example", or "some examples" etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representations of the above terms do not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described may be combined in any one or more embodiments or examples in a suitable manner. In addition, those skilled in the art may combine and combine the different embodiments or examples described in this specification and the features of the different embodiments or examples, without contradiction.

[0242] Although the embodiments of the present invention have been shown and described above, it is to be understood that the above embodiments are exemplary and are not to be construed as limitations of the present invention. A person skilled in the art may change, modify, replace and vary the above embodiments within the scope of the present invention.

Claims

1. A NASICON type solid electrolyte, characterized in that: include: Li x M1 y M2 z M3 u M4 v (PO4) w1 (PS4) w2 , wherein, y + z + u + v = 2, w1 + w2 = 3, 0 < x < 2, 0 ≤ y ≤ 0.5, 0 < z ≤ 1, 0 < u < 2, 0 ≤ v ≤ 3, 1 ≤ w1 ≤ 3, 0.0001 ≤ w2 ≤ 0.3, M1 includes at least one of Mg, Na, K, and Zn, M2 includes at least one of Al, Ga, In, Y, Sc, La, and Ce, M3 includes at least one of Ti, Zr, Hf, and Ge, and M4 includes at least one of Cr, Mo, Ca, Fe, Si, W, Nb, Sm, V, and B.

2. The NASICON solid electrolyte according to claim 1, characterized in that At least one of the following conditions is met: 0.6≤x≤3.2, preferably 1≤x≤2; 0≤y≤0.3, preferably 0≤y≤0.1; 0.2≤z≤0.7, preferably 0.2≤z≤0.4; 0.9≤u<2, preferably 1.4≤u<2; 0.2≤v≤2, preferably 0.5≤v≤1.

3. The NASICON solid electrolyte according to claim 1 or 2, characterized in that: The XRD spectrum of the NASICON solid electrolyte has a (113) characteristic peak, a (104) characteristic peak, a (024) characteristic peak and a (012) characteristic peak. The peak position of the characteristic peak (113) is 24.490°-24.880°, and the full width at half maximum is 0.195°-0.290°; The peak position of the characteristic peak (104) is 20.850°-21.110°, and the full width at half maximum is 0.200°-0.300°; The peak position of the (024) characteristic peak is 29.640°-30.010°, and the full width at half maximum is 0.180°-0.320°; The peak position of the (012) characteristic peak is 14.680°-15.990°, and the full width at half maximum is 0.165°-0.315°.

4. The NASICON solid electrolyte according to claim 1 or 2, characterized in that: The NASICON solid electrolyte satisfies at least one of the following conditions: Volume average particle size Dv 50 0.01 μm-0.2 μm, preferably 0.05 μm-0.1 μm; pH 7.2-9; Ionic conductivity 1.0×10 -4 S / cm-1.5×10 -3 S / cm; The electronic conductivity is 1.0×10 -10 S / cm-1.0×10 -8 S / cm.

5. A method for preparing the NASICON solid electrolyte according to any one of claims 1 to 4, characterized in that: include: (1) mixing and sintering a lithium-containing compound, an M1-containing compound, an M2-containing compound, an M3-containing compound, an M4-containing compound and a phosphorus-containing compound to obtain a solid electrolyte; (2) The solid electrolyte is dispersed in a second solvent and ground to obtain a nanoscale slurry, and a sulfide is added to the nanoscale slurry, mixed, and then dried to obtain a NASICON type solid electrolyte.

6. The method according to claim 5, characterized in that Step (1) is performed as follows: (1-1) mixing a lithium-containing compound, an M1-containing compound, an M2-containing compound, an M3-containing compound, an M4-containing compound, a phosphorus-containing compound, an organic monomer, a first solvent, an initiator, and a catalyst to obtain a mixture; (1-2) heating the mixture to initiate a polymerization reaction to obtain a bulk solid electrolyte precursor; (1-3) pre-sintering the block-shaped solid electrolyte precursor and crushing it to obtain a powder-shaped solid electrolyte precursor; (1-4) The solid electrolyte precursor in powder form is sintered and crushed to obtain a solid electrolyte.

7. The method according to claim 6, characterized in that Step (1-1) satisfies at least one of the following conditions: The organic monomer includes at least one of acrylamide, methylene bisacrylamide, styrene, butadiene and methyl methacrylate; The first solvent includes at least one of water, N-methyl-2-pyrrolidone, phthalate, dibasic lipid, long-chain alcohol and pyrrolidone; The initiator includes at least one of benzoyl peroxide, (NH4)2S2O8 and K2S2O8; The catalyst includes at least one of N,N,N'N'-tetramethylethylenediamine, N,N,N',N'-tetramethyl-1,6-hexanediamine, N,N-diisopropylethylamine, and N-(3-aminopropyl)-N-dodecyl-1,3-propylenediamine.

8. The method according to claim 6, characterized in that In step (1-2), the polymerization reaction temperature is 80°C-200°C, preferably 90°C-150°C, and more preferably 96°C-120°C.

9. The method according to claim 6, characterized in that In step (1-3), the pre-sintering temperature is 300°C-600°C, preferably 350°C-575°C, more preferably 380°C-560°C; and / or The duration of the pre-sintering is 2 hours to 6 hours, preferably 2 hours to 5 hours, and more preferably 2 hours to 4 hours.

10. The method according to claim 6, characterized in that In step (1-4), the sintering temperature is 650°C-900°C, preferably 700°C-875°C, more preferably 730°C-860°C; and / or The sintering duration is 4 hours to 10 hours, preferably 5 hours to 9 hours, and more preferably 6 hours to 8 hours.

11. The method according to claim 5, characterized in that In step (2), the volume average particle size Dv50 of the slurry is 5nm-500nm, preferably 10nm-200nm, more preferably 50nm-100nm; and / or The second solvent includes at least one of n-heptane, toluene and dimethyl ether.

12. The method according to claim 5 or 11, characterized in that: In step (2), the amount of sulfide added is 0.1wt%-3wt% of the solid electrolyte, preferably 0.1wt%-1wt%.

13. The method according to claim 5 or 11, characterized in that: In step (2), the drying temperature is 120°C-600°C, preferably 150°C-500°C.

14. A positive electrode active material, characterized in that: include: A cathode active material matrix; A coating layer is formed on at least a portion of the surface of the positive electrode active material matrix, and the coating layer comprises the NASICON type solid electrolyte according to any one of claims 1 to 4 or a NASICON type solid electrolyte obtained by the method according to any one of claims 5 to 13.

15. The positive electrode active material according to claim 14, characterized in that Based on the total amount of the positive electrode active material matrix, the mass proportion of the NASICON solid electrolyte is 0.05%-1%, preferably 0.3%-0.9%, and more preferably 0.4%-0.8%.

16. The positive electrode active material according to claim 14 or 15, characterized in that: The positive electrode active material matrix includes at least one of lithium nickel oxide, lithium cobalt oxide, lithium manganese oxide, lithium nickel manganese oxide, lithium nickel cobalt manganese oxide, lithium nickel cobalt aluminum oxide, lithium nickel cobalt manganese aluminum oxide, lithium-rich manganese-based layered oxides and their derivatives, lithium iron phosphate and lithium manganese iron phosphate.

17. The positive electrode active material according to claim 14 or 15, characterized in that: The positive electrode active material undergoes acid-base titration treatment and exhibits a phosphate characteristic titration peak between pH=5-8.

18. A method for preparing the positive electrode active material according to any one of claims 14 to 17, characterized in that: include: The positive electrode active material matrix and the NASICON type solid electrolyte are mixed and heat-treated to form a coating layer including the NASICON type solid electrolyte on at least a portion of the surface of the positive electrode active material matrix. Wherein, the NASICON-type solid electrolyte comprises the NASICON-type solid electrolyte described in any one of claims 1 to 4 or the NASICON-type solid electrolyte obtained by the method described in any one of claims 5 to 11.

19. The method according to claim 18, characterized in that The heat treatment temperature is 300°C-700°C, preferably 375°C-625°C, more preferably 420°C-580°C; and / or The duration of the heat treatment is 2 hours to 10 hours, preferably 4 hours to 10 hours, more preferably 5 hours to 10 hours.

20. A positive electrode sheet, characterized in that: The invention comprises the positive electrode active material described in claims 14 to 17 or the positive electrode active material obtained by the method described in claim 18 or 19.

21. A solid-state battery, characterized in that: Including the positive electrode sheet as described in claim 20.

22. An electrical equipment, characterized in that: Including the solid-state battery as described in claim 21.

Citation Information

Cited By

  • Coated high-nickel material as well as preparation method and application thereof

    CN119674046A