Solid electrolyte and preparation method thereof, positive active material and preparation method thereof, positive pole piece, solid-state battery and electric device
By introducing S element to optimize the unit cell structure of solid electrolyte and setting a solid electrolyte cladding layer on the surface of the positive electrode active material, the problem of insufficient structural stability and interface contact performance of solid electrolyte is solved, and the energy density and electrochemistry of lithium-ion batteries are improved performance.
Patent Information
- Application Number
- CN202411048198.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-31
- Publication Date
- 2024-11-15
AI Technical Summary
The existing solid electrolytes have problems with insufficient structural stability and interface contact performance in production and application, which makes it difficult to improve the energy density and safety of lithium-ion batteries.
By introducing S element, the unit cell structure of the solid electrolyte is optimized, its specific surface area and structural stability are improved, and a cladding layer containing solid electrolyte is provided on the surface of the positive electrode active material to reduce the space charge layer and interface side reactions.
It significantly improves the interface contact performance and structural stability of solid-state electrolytes, enhances the transmission path of lithium ions, and improves the capacity, circulation performance and rate performance of solid-state batteries.
Smart Images

Figure BDA0004974425060000171 
Figure BDA0004974425060000181 
Figure BDA0004974425060000182
Abstract
Description
Technical Field
[0001] The present application belongs to the field of batteries, and specifically relates to solid electrolytes and preparation methods thereof, positive electrode active materials and preparation methods thereof, positive electrode sheets, solid-state batteries, and electrical devices. Background Art
[0002] With the rapid development of electronic technology, smart grid and other industries, high energy density and high safety lithium-ion batteries have become an urgent need in the current market. All-solid-state lithium-ion batteries use solid electrolytes, so there is no need to worry about electrolyte leakage, which ensures the safety of the battery; at the same time, solid electrolytes have high hardness and strength, which can effectively prevent lithium dendrites from piercing the diaphragm, making the use of metal lithium negative electrodes possible, which in turn helps to improve the energy density of the battery. However, there are still many problems to be solved in the actual production and application of current solid electrolytes. Summary of the invention
[0003] In the first aspect of the present application, the present application proposes a solid electrolyte satisfying the chemical formula: Li 1+x A x D 2-x (PO 4-y S y )3, wherein A is at least one of Mg, B, Na, K, Zn, Ga, Sc, In, Y, Ce, Co, La, Cr, Mo, Mn, Fe, W, Si, Nb, Sm, Al, D is at least one of Ti, Zr, Hf and Ge, 0.01≤x≤5, 0.0001≤y≤0.3, wherein the unit cell parameter c / a of the solid electrolyte is 2.448-2.520. Thus, the unit cell structure of the solid electrolyte can be changed by the introduction of the S element, and the specific surface area and structural stability of the solid electrolyte can be increased. The unit cell parameter c / a value in the above range can improve the interface contact performance of the solid electrolyte.
[0004] In some embodiments, the lattice constants a, b, c, α, β, and γ of the solid electrolyte satisfy at least one of the following conditions: a is b is c is α is 90.005°-91.050°; β is 90.005°-91.050°; γ is 120.005°-120.050°. Therefore, the lattice constant of the solid electrolyte in the above range can improve the structural stability of the material.
[0005] In some embodiments, the solid electrolyte has a unit cell parameter c / a of 2.450-2.500. Thus, the solid electrolyte has a large specific surface area.
[0006] In some embodiments, the unit cell volume of the solid electrolyte is As a result, the solid electrolyte has a higher lattice stability and is less prone to structural collapse and self-degradation.
[0007] In some embodiments, the average grain radius of the solid electrolyte is And / or, the lattice distortion rate of the solid electrolyte is 0.05%-0.5%; and / or, the crystallinity of the solid electrolyte is 95.0%-99.5%. Thus, the effective sites of solid-phase contact can be increased.
[0008] In some embodiments, the solid electrolyte satisfies at least one of the following conditions: v50 Particle size is 0.01μm-0.2μm; specific surface area is 30m 2 / g-300m 2 / g; ionic conductivity is 4.0×10 -4 S / cm-1×10 -3 S / cm. Thus, the ionic conductivity and interface contact performance of the solid electrolyte can be further improved.
[0009] In the second aspect of the present application, the present application proposes a method for preparing the aforementioned solid electrolyte, comprising: S1: sintering a titanium source, a lithium source, a phosphorus source, and an M source to obtain a solid electrolyte precursor; S2: annealing the solid electrolyte precursor and a sulfur source under an inert atmosphere to obtain the solid electrolyte. Thus, the aforementioned solid electrolyte can be obtained by a simple method.
[0010] In some embodiments, the step S1 includes: mixing the titanium source, the lithium source, the phosphorus source, the M source, the organic monomer, the first solvent, the initiator and the catalyst to obtain a mixture; heating the mixture to obtain a first solid electrolyte precursor; pre-sintering the first solid electrolyte precursor to obtain a second solid electrolyte precursor; and sintering the second solid electrolyte precursor to obtain the solid electrolyte precursor. In this way, uniform mixing of multiple raw materials can be achieved to avoid local segregation.
[0011] In some embodiments, the organic monomer includes at least one of acrylamide, methylenebisacrylamide, styrene, butadiene and methyl methacrylate; and / or, the first solvent includes at least one of water, N-methyl-2-pyrrolidone, phthalate, dibasic lipid, long-chain alcohol and pyrrolidone; and / or, the initiator includes at least one of benzoyl peroxide, (NH4)2S2O8 and K2S2O8; and / or, the catalyst includes at least one of N,N,N′N′-tetramethylethylenediamine, N,N,N',N'-tetramethyl-1,6-hexanediamine, N,N-diisopropylethylamine, N-(3-aminopropyl)-N-dodecyl-1,3-propylenediamine.
[0012] In some embodiments, the temperature of the heating treatment is 80°C-200°C; and / or, the temperature of the pre-sintering treatment is 300°C-600°C, and the time of the pre-sintering treatment is 2h-6h; and / or, the temperature of the sintering treatment is 650°C-900°C, and the time of the sintering treatment is 4h-10h. Thus, pure phase preparation of the target sample can be achieved.
[0013] In some embodiments, the solid electrolyte precursor D v50 The particle size is 5nm-500nm. Therefore, the solid electrolyte precursor has high reactivity and dispersibility.
[0014] In some embodiments, the amount of the sulfur source added is 0.1 wt%-3 wt% of the solid electrolyte precursor, thereby helping to make the solid electrolyte contain an appropriate amount of sulfur.
[0015] In some embodiments, the annealing temperature is 120° C.-600° C., and the annealing time is 2 h-6 h. Thus, the material can be recrystallized, and the crystal structure of the material is more compact.
[0016] In a third aspect of the present application, the present application proposes a positive electrode active material, comprising: a core; a coating layer, wherein the coating layer is at least partially located on the surface of the core, and the coating layer includes the aforementioned solid electrolyte. By arranging the coating layer containing the aforementioned solid electrolyte on the surface of the core, the space charge layer and the interface side reaction between the core and the coating layer can be reduced.
[0017] In some embodiments, based on the total mass of the core, the mass fraction of the solid electrolyte is 0.05wt%-1.5wt%, thereby further improving the interface contact performance of the positive electrode active material.
[0018] In some embodiments, the core includes at least one of lithium nickel oxide, lithium cobalt oxide, lithium manganese oxide, lithium nickel manganese oxide, lithium nickel cobalt manganese oxide, lithium nickel cobalt aluminum oxide, lithium nickel cobalt manganese aluminum oxide, layered oxides of lithium-rich manganese and its derivatives, lithium iron phosphate, and lithium manganese iron phosphate. Thus, the positive electrode active material can be applied to a variety of battery systems.
[0019] In a fourth aspect of the present application, the present application proposes a method for preparing the aforementioned positive electrode active material, comprising: heat treating the inner core and the solid electrolyte to form a coating layer including the solid electrolyte on at least a portion of the surface of the inner core, wherein the solid electrolyte includes the aforementioned solid electrolyte. Thus, the aforementioned positive electrode active material can be obtained by a simple method.
[0020] In some embodiments, the heat treatment temperature is 200° C.-700° C., and the heat treatment time is 2 h-10 h. Thus, the bonding strength between the coating layer and the core can be significantly improved.
[0021] In the fifth aspect of the present application, the present application proposes a positive electrode plate, comprising the above-mentioned positive electrode active material. Therefore, the positive electrode plate has all the characteristics and advantages of the above-mentioned positive electrode active material, which will not be repeated here.
[0022] In a sixth aspect of the present application, the present application proposes a solid-state battery, comprising the aforementioned positive electrode plate, so that the solid-state battery has lower impedance, higher capacity, and better cycle performance and rate performance.
[0023] In the seventh aspect of the present application, the present application proposes an electrical device, comprising the aforementioned solid-state battery. Therefore, the electrical device has all the features and advantages of the aforementioned solid-state battery, which will not be described in detail here. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] The above and / or additional aspects and advantages of the present application will become apparent and easily understood from the description of the embodiments in conjunction with the following drawings, in which:
[0025] Figure 1 is the XRD pattern of the solid electrolyte of Example 1 of the present application;
[0026] Figure 2 is the XRD diagram of the solid electrolyte of Comparative Example 1 of the present application;
[0027] Figure 3 This is the EDS test mapping diagram of the NASICON solid electrolyte phase prepared in Example 1;
[0028] Figure 4 The first charge and discharge curves of the all-solid-state batteries of Example 1 and Comparative Example 4. DETAILED DESCRIPTION
[0029] The embodiments of the present application are described in detail below, and examples of the embodiments are shown in the accompanying drawings. The embodiments described with reference to the accompanying drawings are exemplary and are intended to be used to explain the present application, but cannot be understood as limiting the present application.
[0030] The endpoints and any values of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values should be understood to include values close to these ranges or values. For numerical ranges, the endpoint values of each range, the endpoint values of each range and the individual point values, and the individual point values can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.
[0031] In this application, by optimizing the material composition, regulating the element ratio, changing the unit cell structure of the solid electrolyte by introducing the S element, improving the specific surface area and structural stability of the solid electrolyte, and limiting the unit cell of the solid electrolyte to be elongated along the c-axis direction by a specific unit cell parameter c / a value, the specific surface area of the solid electrolyte is large, thereby jointly providing an improvement in the interface contact performance of the solid electrolyte. On this basis, the structural stability is improved by doping elements inside the lattice, and the solid electrolyte is made to achieve a uniform atomic-level mixing of the doping elements and the main phase, thereby obtaining a solid electrolyte with a high specific surface area and high ionic conductivity, significantly increasing the effective sites of solid-phase contact, and providing more paths for the transmission of lithium ions between solid phases.
[0032] The solid electrolyte in the present application is a NASICON type solid electrolyte (Na+superionic conductor) having high ionic conductivity and excellent chemical and electrochemical stability.
[0033] In the first aspect of the present application, the present application proposes a solid electrolyte satisfying the chemical formula: Li 1+x A x D 2-x (PO 4-y S y)3, wherein A is at least one of Mg, B, Na, K, Zn, Ga, Sc, In, Y, Ce, Co, La, Cr, Mo, Mn, Fe, W, Si, Nb, Sm, Al, D is at least one of Ti, Zr, Hf and Ge, 0.01≤x≤5, 0.0001≤y≤0.3, wherein the unit cell parameter c / a of the solid electrolyte is 2.448-2.520. The introduction of the S element can change the unit cell structure of the solid electrolyte, and improve the specific surface area and structural stability of the solid electrolyte. The unit cell parameter c / a value in the above range can improve the interface contact performance of the solid electrolyte. At the same time, its main elements Li, A, and D can also improve the ionic conductivity of the solid electrolyte.
[0034] The introduction of sulfur (sulfur) element allows the active free cations on the surface of the solid electrolyte to react with it, forming a dispersed inert phase on the surface, making it resistant to sulfur. 2- The further corrosion of the strong reducing environment can be improved in the subsequent application of sulfide all-solid-state battery system, which can improve the interface stability of the solid electrolyte. The introduction of elements A and D is inconsistent with the chemical composition and element valence of conventional NASICON solid electrolytes, so that the charge balance is maintained in the solid electrolyte in the form of point defects (for example, one atom is missing at a certain position in the unit cell). Such point defects, especially vacancy defects, will increase the transmission channel of lithium ions and improve ionic conductivity.
[0035] When the unit cell parameter c / a of the solid electrolyte is 2.448-2.520, the unit cell of the solid electrolyte is elongated along the c-axis direction, so that the specific surface area of the solid electrolyte is larger, which can improve the interface contact performance of the solid electrolyte.
[0036] As an example, x can be 0.01, 0.05, 0.1, 0.5, 1, 1.5, 2, 2.5, 3, 3.5, 4, 4.5, or 5.
[0037] As an example, y may be 0.0001, 0.0005, 0.001, 0.005, 0.01, 0.05, 0.1, 0.15, 0.2, 0.25, or 0.3.
[0038] The elemental composition of the solid electrolyte can be determined using instruments and methods known in the art, such as inductively coupled plasma atomic emission spectrometry: the instrument standard refers to EPA6010D-2014 "Inductively coupled plasma atomic emission spectrometry". The sample is treated by chemical methods to be digested into a solution, atomized into a plasma and excited to produce characteristic spectral lines of the elements. The element content is qualitatively and quantitatively analyzed based on the wavelength and intensity of the spectral lines (which are proportional to the concentration).
[0039] In some embodiments, the lattice constants a, b, c, α, β, and γ of the solid electrolyte satisfy at least one of the following conditions: a is b is c is α is 90.005°-91.050°; β is 90.005°-91.050°; γ is 120.005°-120.050°. Therefore, the interface performance of the solid electrolyte can be significantly improved by introducing doping elements.
[0040] In some embodiments, the unit cell parameter c / a of the solid electrolyte is 2.450-2.500. Thus, the unit cell of the solid electrolyte is elongated along the c-axis direction, so that the specific surface area of the solid electrolyte is increased, and the interface contact performance of the solid electrolyte is further improved.
[0041] In some embodiments, the unit cell volume of the solid electrolyte is As a result, the solid electrolyte has a higher lattice stability and is less prone to structural collapse and material self-degradation.
[0042] In some embodiments, the average grain radius of the solid electrolyte is
[0043] As an example, the average grain radius of the solid electrolyte can be or
[0044] The solid electrolyte refinement data is based on the standard LiTi2(PO4)3 lattice parameters and is processed by the whole-powder pattern fitting method to obtain unit cell quantitative description data, wherein the average grain radius can describe the average value of the radial distance from the unit cell center to the unit cell edge. The smaller the value, the less close the solid electrolyte unit cell being measured is to a circle.
[0045] In some embodiments, the lattice distortion rate of the solid electrolyte is 0.05%-0.5%.
[0046] As an example, the lattice distortion rate of the solid electrolyte may be 0.05%, 0.1%, 0.15%, 0.2%, 0.25%, 0.3%, 0.35%, 0.4%, 0.45% or 0.5%.
[0047] The lattice distortion rate is the average rate of change of the lattice constant of the solid electrolyte being measured compared to the lattice constant of the standard LiTi2(PO4)3 unit cell. The larger the value, the more the lattice constant of the solid electrolyte being measured deviates from the lattice constant of the standard unit cell.
[0048] Compared with the standard LiTi2(PO4)3 unit cell, the solid electrolyte has a smaller average grain radius and a larger lattice distortion rate, which causes the unit cell of the solid electrolyte to deform and increases the effective solid-phase contact sites.
[0049] In some embodiments, the solid electrolyte has a crystallinity of 95.0%-99.5%, thereby increasing the effective sites for solid-phase contact.
[0050] As an example, the crystallinity of the solid electrolyte may be 95.0%, 95.5%, 96.0%, 96.5%, 97.0%, 97.5%, 98.0%, 98.5%, 99.0% or 99.5%.
[0051] The solid electrolyte refinement data is based on the standard LiTi2(PO4)3 lattice parameters and processed by the whole-powder pattern fitting method to obtain the crystallinity, indicating the percentage of the diffraction intensity of the solid electrolyte being tested compared to the diffraction intensity of the standard LiTi2(PO4)3 crystal.
[0052] Compared with standard LiTi2(PO4)3, the solid electrolyte has a lower degree of crystallinity and a higher degree of disorder, providing more pathways for lithium ion transmission between solid phases.
[0053] The test methods for the average grain radius, lattice constant (a, b, c, α, β and γ), lattice distortion rate and crystallinity of solid electrolytes include: using the spectrum obtained from the X-ray diffraction test (XRD) to analyze the phase composition of the target material; by fine-tuning and fitting the line spectrum of the theoretical diffraction intensity with the line spectrum of the XRD measured intensity, the quantitative analysis of the average grain radius, lattice constant, lattice distortion rate and crystallinity is achieved by using the whole-powder pattern fitting method. Its basic working principle is based on the lattice interference phenomenon between the periodic arrangement of the material lattice atoms and the incident high-energy X-ray particles, so that it can receive a specific strong interference signal. Materials with different lattices have different lattice interference signals, which can be used for qualitative or quantitative analysis. The test target material was Cu and the analysis was performed under Cu Kα radiation. The tube voltage of the equipment was set to 40 kV, the tube current was set to 200 mA, the test angle range of the sample was 5° to 120°, the scanning rate was 1° / min, and the scanning step was 0.02°.
[0054] In some embodiments, the solid electrolyte has a D v50The particle size is 0.01μm-0.2μm. Therefore, the particle size of the solid electrolyte is small, and it has good interface contact performance. After coating the core of the positive electrode active material, the contact performance between the two is good, and the contact point density is greater, which is conducive to the lithium ion transmission at the interface.
[0055] As an example, the D v50 The particle size may be 0.01 μm, 0.03 μm, 0.05 μm, 0.08 μm, 0.10 μm, 0.15 μm, 0.18 μm or 0.2 μm.
[0056] D v50 It refers to the particle size corresponding to when the cumulative volume distribution percentage reaches 50%, and is measured with reference to the standard GB / T 19077-2016 using a laser particle size analyzer (such as Malvern Master Size 3000).
[0057] In some embodiments, the specific surface area of the solid electrolyte is 30 m 2 / g-300m 2 / g. As a result, the solid electrolyte has a larger specific surface area and more solid-phase contact sites, which can further improve the interface contact performance of the solid electrolyte.
[0058] As an example, the specific surface area of the solid electrolyte can be 30 m 2 / g, 40m 2 / g, 50m 2 / g, 70m 2 / g、100m 2 / g, 120m 2 / g, 150m 2 / g, 170m 2 / g, 180m 2 / g, 200m 2 / g, 230m 2 / g, 250m 2 / g, 280m 2 / g or 300m 2 / g.
[0059] The specific surface area can be measured using instruments and methods known in the art. For example, it can be tested by referring to the following method: Use the American Micromeritics multi-station fully automatic specific surface area and pore analyzer GeminiVII2390, take about 7g of sample and put it into a 9cc long tube with a bulb, degas at 200℃ for 2h, and then put it into the host to test to obtain the BET specific surface area data of the positive electrode active material.
[0060] In some embodiments, the ionic conductivity of the solid electrolyte is 4×10 -4S / cm-1×10 -3 S / cm. Thus, the ion transport performance of the solid electrolyte can be further improved.
[0061] As an example, the ionic conductivity of a solid electrolyte can be 4×10 -4 S / cm, 6×10 -4 S / cm, 8×10 -4 S / cm or 1×10 -3 S / cm.
[0062] The ionic conductivity test method is to use an electrochemical workstation to perform electrochemical impedance spectroscopy (EIS) test and direct current polarization (DC) test. The frequency range of the electrical signal of the EIS test is 0.01Hz to 10000000Hz, and the disturbance amplitude of the AC voltage is 10mV. The constant voltage of the DC test is 1.0V, which lasts for 3000s. σ=L / RS is used to calculate ionic conductivity and electronic conductivity, where R is the resistance value, L is the thickness, and S is the area of the particle. Specifically, the ionic conductivity test of the above-mentioned solid electrolyte is tested at the mold battery level, and the specific composition of the mold battery is: stainless steel electrode / / conductive carbon / / solid electrolyte / / conductive carbon / / stainless steel electrode. The assembly method of the test mold battery device is: pre-press about 100mg of solid electrolyte sample, add conductive carbon on both sides of the sample, press it under 300MPa to form a battery sheet, and place the battery sheet between two stainless steel electrodes to assemble the mold battery.
[0063] In a second aspect of the present application, the present application proposes a method for preparing the aforementioned solid electrolyte, comprising:
[0064] S1: Sintering of titanium source, lithium source, phosphorus source and M source
[0065] In some embodiments, in this step, the titanium source, lithium source, phosphorus source, and M source are mixed, sintered, and crushed to obtain a solid electrolyte precursor.
[0066] In some embodiments, the titanium source, lithium source, and M source may include, but are not limited to, oxides, hydroxides, oxalates, organic alcohol salts, or carbonates of the corresponding elements. The phosphorus source may be phosphoric acid or phosphates. At the same time, the titanium source, lithium source, and M source may also be phosphates of the corresponding elements, and when at least one of the titanium source, lithium source, and M source is a phosphate of the corresponding element, it is not necessary to add a phosphorus source separately.
[0067] In some embodiments, step S1 comprises the following steps:
[0068] S11: Mixing the titanium source, the lithium source, the phosphorus source, the M source, the organic monomer, the first solvent, the initiator and the catalyst
[0069] In some embodiments, in this step, a titanium source, a lithium source, a phosphorus source, an M source, a first solvent, an organic monomer, an initiator, and a catalyst are mixed to obtain a mixture.
[0070] In some embodiments, the titanium source, lithium source, phosphorus source, and M source are added in an amount based on the stoichiometric ratio of the target product. The first solvent is added in an amount based on a target mixed slurry solid content of 20%-60%. The organic monomer, initiator, and catalyst are added in an amount of 40wt%-60wt% of the mixed slurry.
[0071] In some embodiments, the organic monomer includes at least one of acrylamide, methylenebisacrylamide, styrene, butadiene and methyl methacrylate; and / or, the first solvent includes at least one of water, N-methyl-2-pyrrolidone, phthalate, dibasic lipid, long-chain alcohol and pyrrolidone; and / or, the initiator includes at least one of benzoyl peroxide, (NH4)2S2O8 and K2S2O8; and / or, the catalyst includes at least one of N,N,N′N′-tetramethylethylenediamine, N,N,N',N'-tetramethyl-1,6-hexanediamine, N,N-diisopropylethylamine, N-(3-aminopropyl)-N-dodecyl-1,3-propylenediamine.
[0072] S12: heating the mixed material
[0073] In some embodiments, in this step, the mixture is heated to initiate a polymerization reaction to obtain a bulk first solid electrolyte precursor.
[0074] In some embodiments, the temperature of the heating treatment is 80°C-200°C, preferably 90°C-150°C, and more preferably 96°C-120°C. Thus, at this polymerization temperature, the organic monomer undergoes a polymerization reaction under the action of the initiator, so that the raw material elements can be evenly combined at the molecular level. After subsequent sintering, the polymer is oxidized and volatilized, and the raw materials react to each other to easily form a uniform NASICON phase.
[0075] S13: Pre-sintering the first solid electrolyte precursor
[0076] In some embodiments, in this step, the bulk first solid electrolyte precursor is pre-sintered and crushed to obtain a powdery second solid electrolyte precursor. Thus, the organic polymer in the first solid electrolyte precursor can be removed to prevent organic residues from affecting the electrical performance, and then the powdery second solid electrolyte precursor is obtained by crushing.
[0077] In some embodiments, the pre-sintering temperature is 300°C-600°C, preferably 350°C-575°C, and more preferably 380°C-560°C.
[0078] In some embodiments, the pre-sintering treatment time is 2h-6h, preferably 2h-5h, and more preferably 2h-4h.
[0079] By adopting the above-mentioned pre-sintering treatment conditions, the organic polymer in the first solid electrolyte precursor can be significantly removed, reducing the adverse effects of organic residues on electrical performance.
[0080] S14: performing the sintering treatment on the second solid electrolyte precursor to obtain the solid electrolyte precursor.
[0081] In some embodiments, in this step, the powdered second solid electrolyte precursor is sintered and crushed to obtain a solid electrolyte precursor.
[0082] In some embodiments, the sintering temperature is 650°C-900°C, preferably 700°C-875°C, and preferably 730°C-860°C.
[0083] In some embodiments, the sintering treatment time is 4h-10h, preferably 5h-9h, and more preferably 6h-8h.
[0084] In some embodiments, the solid electrolyte precursor D v50 The particle size is 5nm-500nm, preferably 10nm-200nm, and more preferably 50nm-100nm. Thus, the solid electrolyte precursor has high reactivity and dispersibility.
[0085] S2: Under an inert atmosphere, annealing the solid electrolyte precursor and the sulfur source
[0086] In some embodiments, in this step, the solid electrolyte precursor and the sulfur source are mixed and ground under the protection of an inert atmosphere and then annealed to obtain a solid electrolyte.
[0087] In some embodiments, the mixed grinding method includes but is not limited to planetary ball milling, high energy ball milling, etc.
[0088] In some embodiments, the amount of the sulfur source added is 0.1 wt%-3 wt% of the solid electrolyte precursor, preferably 0.1 wt%-1 wt%, thereby helping to make the solid electrolyte contain an appropriate amount of sulfur.
[0089] During the annealing process, sulfur will be lost, so the amount of sulfide added in this process is slightly excessive compared to the sulfur content in the NASICON solid electrolyte composition.
[0090] By way of example, the sulfur source includes, but is not limited to, elemental sulfur, phosphorus pentasulfide, lithium sulfide, thiourea, and the like.
[0091] In some embodiments, the annealing temperature is 120° C.-600° C., and the annealing time is 2 h-6 h. Thus, the material can be recrystallized, and the crystal structure of the material is more compact.
[0092] In solid-state batteries, the poor interface stability and high impedance between the positive electrode active material and the solid electrolyte are important factors leading to the capacity decay and poor cyclability of solid-state batteries. Especially in the sulfide solid electrolyte system, there is a high resistance layer, i.e., a space charge layer, at the interface between the oxide positive electrode active material and the sulfide solid electrolyte, and the interface stability is poor at high temperatures, which greatly reduces the ion conductivity at the interface, thereby adversely affecting the battery performance. The solid electrolyte reaction between the positive electrode active material and the sulfide at high temperatures can be inhibited by setting a niobium-containing coating on the surface of the positive electrode active material. However, niobium salts are expensive and have high production costs, which is not conducive to commercial promotion. The interface between the positive electrode active material and the inorganic solid electrolyte can be improved by setting a lithium metal oxide coating on the surface of the positive electrode active material, but the preparation method is complex and has high equipment requirements, which is not conducive to large-scale production. The NASICON-type solid electrolyte obtained by the method of the present application has its metal elements (elements A and D) introduced during the thermal polymerization process to achieve uniform mixing of the elements at the atomic level. The lattice has better structural stability due to the presence of internal transition elements. Furthermore, by introducing sulfur elements during the annealing process, the prepared solid electrolyte has more transmission paths between the solid phases and higher ionic conductivity, and is suitable for the preparation of solid electrodes and ceramic coated diaphragms.
[0093] In a third aspect of the present application, the present application proposes a positive electrode active material, comprising: a core; a coating layer, wherein the coating layer is at least partially located on the surface of the core, and the coating layer includes the aforementioned solid electrolyte. By arranging the coating layer containing the aforementioned solid electrolyte on the surface of the core, the space charge layer and the interface side reaction between the core and the coating layer can be reduced.
[0094] In some embodiments, by forming a coating layer containing a solid electrolyte on the surface of the inner core, when the positive electrode active material is assembled into a solid-state battery, the coating layer containing the solid electrolyte is located between the inner core and the solid electrolyte layer. On the one hand, the solid electrolyte can buffer the large gradient effect of the chemical potential energy between the inner core and the solid electrolyte layer. On the other hand, it can inhibit the formation of a lithium depletion layer at the interface between the inner core and the solid electrolyte layer, which can effectively reduce the large interface resistance caused by the space charge layer, and also play a role in inhibiting interface side reactions. At the same time, since the solid electrolyte has excellent interface stability and ionic conductivity, it can improve the interface stability and ionic conductivity of the positive electrode active material, so that it can be applied to solid-state batteries, which can reduce the space charge layer and interface side reactions between the inner core and the solid electrolyte layer and the impedance of the solid-state battery, and improve the capacity, cycle performance and rate performance of the solid-state battery.
[0095] In some embodiments, based on the total mass of the core, the mass fraction of the solid electrolyte is 0.05wt%-1.5wt%, preferably 0.1wt%-1.0wt%, more preferably 0.2wt%-0.75wt%. Thus, the interface contact performance of the positive electrode active material can be further improved.
[0096] In some embodiments, the core includes at least one of lithium nickel oxide, lithium cobalt oxide, lithium manganese oxide, lithium nickel manganese oxide, lithium nickel cobalt manganese oxide, lithium nickel cobalt aluminum oxide, lithium nickel cobalt manganese aluminum oxide, layered oxides of lithium-rich manganese and its derivatives, lithium iron phosphate, and lithium manganese iron phosphate. Thus, the positive electrode active material can be applied to a variety of battery systems.
[0097] In the fourth aspect of the present application, the present application proposes a method for preparing the aforementioned positive electrode active material, comprising: heat treating the inner core and the solid electrolyte to form a coating layer including the solid electrolyte on at least a portion of the surface of the inner core, wherein the solid electrolyte includes the aforementioned solid electrolyte. Thus, the aforementioned positive electrode active material can be obtained by a simple method. The slurry of the solid electrolyte can maintain a pure phase state for a long time without phase decomposition. Thus, it can be effectively coated on the inner core.
[0098] In some embodiments, the heat treatment temperature is 200-700°C, preferably 300-500°C, and the heat treatment time is 2h-10h, preferably 4h-9h, and more preferably 5h-8h. Thus, the bonding strength between the coating layer and the core can be significantly improved.
[0099] In the fifth aspect of the present application, the present application proposes a positive electrode plate, comprising the above-mentioned positive electrode active material. Therefore, the positive electrode plate has all the characteristics and advantages of the above-mentioned positive electrode active material, which will not be repeated here.
[0100] In some embodiments, the positive electrode plate includes a positive electrode collector and a positive electrode active material layer disposed on the positive electrode collector, the positive electrode active material layer includes the above-mentioned positive electrode active material, wherein the positive electrode collector can be a metal foil or a composite current collector (the metal material can be disposed on a polymer substrate to form a composite current collector), for example, the positive electrode collector can be an aluminum foil.
[0101] In some embodiments, the positive electrode active material layer may further include a binder. As an example, the binder may include at least one of polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), vinylidene fluoride-tetrafluoroethylene-propylene terpolymer, vinylidene fluoride-hexafluoropropylene-tetrafluoroethylene terpolymer, tetrafluoroethylene-hexafluoropropylene copolymer, or fluorine-containing acrylate resin.
[0102] In some embodiments, the positive electrode active material layer may further include a conductive agent. As an example, the conductive agent may include at least one of superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, or carbon nanofibers.
[0103] In some embodiments, the positive electrode sheet can be prepared in the following manner: the components for preparing the positive electrode sheet, such as the positive electrode active material, the conductive agent, the binder and any other components are dispersed in a solvent (such as N-methylpyrrolidone) to form a positive electrode slurry; the positive electrode slurry is coated on the positive electrode collector, and after drying, cold pressing and other processes, the positive electrode sheet can be obtained.
[0104] In a sixth aspect of the present application, the present application proposes a solid-state battery, comprising the aforementioned positive electrode plate, so that the solid-state battery has lower impedance, higher capacity, and better cycle performance and rate performance.
[0105] As an example, a solid-state battery includes a positive electrode sheet, a negative electrode sheet, and a solid electrolyte layer, wherein the solid electrolyte layer is located between the positive electrode sheet and the negative electrode sheet.
[0106] In some embodiments, the negative electrode plate includes a negative electrode current collector and a negative electrode active material layer disposed on the negative electrode current collector, the negative electrode active material layer includes a negative electrode active material, wherein the negative electrode current collector can be a metal foil or a composite current collector (a metal material can be disposed on a polymer substrate to form a composite current collector), for example, the positive electrode current collector can be a copper foil.
[0107] In some embodiments, the negative electrode active material may include at least one of the following materials: artificial graphite, natural graphite, soft carbon, hard carbon, silicon-based materials, tin-based materials, lithium titanate, etc.
[0108] In some embodiments, the negative electrode active material layer may further include a conductive agent, which may include at least one of superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, or carbon nanofibers.
[0109] In some embodiments, the negative electrode active material layer may further include other additives, such as a thickener (eg, sodium carboxymethyl cellulose (CMC-Na)).
[0110] In some embodiments, the negative electrode sheet can be prepared by the following method: the above-mentioned components for preparing the negative electrode sheet, such as the negative electrode active material, the conductive agent, and the binder are dispersed in a solvent (such as deionized water) to form a negative electrode slurry; the negative electrode slurry is coated on the negative electrode collector, and after drying, cold pressing and other processes, the negative electrode sheet can be obtained.
[0111] In some embodiments, the negative electrode plate may include a metal lithium plate or a lithium alloy, such as a lithium-indium alloy.
[0112] In some embodiments, the solid electrolyte layer between the positive electrode sheet and the negative electrode sheet may include, but is not limited to, at least one of LiPSCl, LiGePS, LiSnPS, LiSiPSCl, LiSiPSBr, and LiSiPSI.
[0113] In the seventh aspect of the present application, the present application proposes an electrical device, comprising the aforementioned solid-state battery. Therefore, the electrical device has all the features and advantages of the aforementioned solid-state battery, which will not be described in detail here.
[0114] In some embodiments, the power-consuming device may include but is not limited to a mobile phone, a laptop computer, an electric vehicle, etc.
[0115] Hereinafter, the embodiments of the present application will be described. The embodiments described below are exemplary and are only used to explain the present application, and should not be construed as limiting the present application. If no specific techniques or conditions are indicated in the embodiments, the techniques or conditions described in the literature in this area or the product specifications are used. If the manufacturer is not indicated in the reagents or instruments used, they are all conventional products that can be obtained commercially.
[0116] Example 1
[0117] Preparation of solid electrolyte:
[0118] Step S1 includes:
[0119] S11: weighing Li2CO3, Al2O3, MgO, TiO2, LiH2PO4, and NH4H2PO4 compounds according to a target stoichiometric ratio, adding a certain amount of pure water to mix, and then mixing and crushing them in a ball mill to obtain a mixed slurry A with a solid content of 50%; adding 50 wt % of acrylamide (monomer), (NH4)2S2O8 (initiator) and N,N,N′N′-tetramethylethylenediamine (TEMED) catalyst to the mixed slurry A, and dispersing them evenly in a stirring device to obtain a mixed slurry B;
[0120] S12: pouring the mixed slurry B into a sagger container and drying it in a 100° C. forced air oven to initiate a polymerization reaction of the substances in the mixed slurry B, and obtaining a bulk first solid electrolyte precursor after 12 hours;
[0121] S13: pre-sintering the first solid electrolyte precursor at 500° C. in a muffle furnace for 2 hours, crushing the sintered product in a wall-breaking machine for 5 minutes to obtain a second solid electrolyte precursor in powder form;
[0122] S14: sintering the second solid electrolyte precursor, sintering the powdered second solid electrolyte precursor at 750° C. in a muffle furnace for 6 hours, and crushing the sintered product in a jet mill to obtain a solid electrolyte precursor.
[0123] Step S2 includes:
[0124] In a nitrogen atmosphere, the solid electrolyte precursor obtained in step S1 is mixed with P2S5, wherein the solid electrolyte and P2S5 are mixed in a mass ratio of 1:0.03. Annealing treatment is performed at an annealing temperature of 300°C, and the powder obtained after annealing treatment is further dissociated by air jet milling to obtain a powder with a chemical composition of Li 1.3 Mg 0.05 Al 0.25 Ti 1.7 (PO 3.998 S 0.002 )3's NASICON-type solid electrolyte SE1.
[0125] The remaining embodiments and comparative examples are consistent with Example 1, except that:
[0126] Example 2
[0127] The difference from Example 1 is that the raw materials used in step S1 are different, and step S11: the compounds of Li2CO3, Al2O3, La2O3, TiO2, and P2O5 are weighed according to the target stoichiometric ratio.
[0128] The process of step S2 is different: in a nitrogen atmosphere, the solid electrolyte precursor obtained in step S1 is mixed with Li2S, wherein the solid electrolyte and Li2S are mixed in a mass ratio of 1:0.01. Annealing treatment is performed at an annealing temperature of 400°C, and the powder obtained after annealing treatment is further dissociated by air jet milling.
[0129] Example 3
[0130] The difference from Example 1 is that the raw materials used in step S1 are different, and step S11: weighing the compounds of LiOH, Al2O3, ZrO2, TiO2, and NH4H2PO4 according to the target stoichiometric ratio.
[0131] The process of step S2 is different: under a nitrogen atmosphere, the solid electrolyte precursor obtained in step S1 is mixed with single substance S, wherein the solid electrolyte and S are mixed in a mass ratio of 1:0.01. Annealing treatment is performed at an annealing temperature of 200°C, and the powder obtained after annealing treatment is further dissociated by air jet milling.
[0132] Example 4
[0133] The difference from Example 1 is that the raw materials used in step S1 are different, and step S11: weigh the compounds of Li3PO4, AlPO4, ZrO2, TiO2, and WO3 according to the target stoichiometric ratio.
[0134] The process of step S2 is different: under a nitrogen atmosphere, the solid electrolyte precursor obtained in step S1 is mixed with single substance S, wherein the solid electrolyte and S are mixed in a mass ratio of 1:0.005. Annealing treatment is performed at an annealing temperature of 180°C, and the powder obtained after annealing treatment is further dissociated by air jet milling.
[0135] Example 5
[0136] The difference from Example 1 is that the process of step S2 is different: in a nitrogen atmosphere, the solid electrolyte precursor obtained in step S1 is mixed with Li2S, wherein the solid electrolyte and Li2S are mixed in a mass ratio of 1:0.05. Annealing treatment is performed at an annealing temperature of 350°C, and the powder obtained after annealing treatment is further dissociated by air jet milling.
[0137] Example 6
[0138] The difference from Example 1 is that the process of step S2 is different: under a nitrogen atmosphere, the solid electrolyte precursor obtained in step S1 is mixed with Li2S, wherein the solid electrolyte and Li2S are mixed in a mass ratio of 1:0.06. Annealing treatment is performed at an annealing temperature of 400°C, and the powder obtained after annealing treatment is further dissociated by air jet milling.
[0139] Example 7
[0140] The difference from Example 1 is that the process of step S2 is different: under a nitrogen atmosphere, the solid electrolyte precursor obtained in step S1 is mixed with P2S5, wherein the solid electrolyte and P2S5 are mixed in a mass ratio of 1:0.05. Annealing treatment is performed at an annealing temperature of 350°C, and the powder obtained after annealing treatment is further dissociated by using a jet mill.
[0141] Example 8
[0142] The difference from Example 1 is that the process of step S2 is different: under a nitrogen atmosphere, the solid electrolyte precursor obtained in step S1 is mixed with P2S5, wherein the solid electrolyte and P2S5 are mixed in a mass ratio of 1:0.04. Annealing treatment is performed at an annealing temperature of 350°C, and the powder obtained after annealing treatment is further dissociated by air jet milling.
[0143] Example 9
[0144] The difference from Example 1 is that the process of step S2 is different: in a nitrogen atmosphere, the solid electrolyte precursor obtained in step S1 is mixed with Li2S, wherein the solid electrolyte and Li2S are mixed in a mass ratio of 1:0.2. Annealing treatment is performed at an annealing temperature of 300°C, and the powder obtained after annealing treatment is further dissociated by air jet milling.
[0145] Example 10
[0146] The difference from Example 1 is that the process of step S2 is different: in a nitrogen atmosphere, the solid electrolyte precursor obtained in step S1 is mixed with Li2S, wherein the solid electrolyte and Li2S are mixed in a mass ratio of 1:0.25. Annealing treatment is performed at an annealing temperature of 350°C, and the powder obtained after annealing treatment is further dissociated by air jet milling.
[0147] Embodiment 11
[0148] The difference from Example 1 is that the process of step S2 is different: in a nitrogen atmosphere, the solid electrolyte precursor obtained in step S1 is mixed with Li2S, wherein the solid electrolyte and Li2S are mixed in a mass ratio of 1:0.2. Annealing treatment is performed at an annealing temperature of 350°C, and the powder obtained after annealing treatment is further dissociated by air jet milling.
[0149] Example 12
[0150] The difference from Example 1 is that the process of step S2 is different: under a nitrogen atmosphere, the solid electrolyte precursor obtained in step S1 is mixed with P2S5, wherein the solid electrolyte and P2S5 are mixed in a mass ratio of 1:0.25. Annealing treatment is performed at an annealing temperature of 350°C, and the powder obtained after annealing treatment is further dissociated by using a jet mill.
[0151] Example 13
[0152] The difference from Example 1 is that the process of step S2 is different: under a nitrogen atmosphere, the solid electrolyte precursor obtained in step S1 is mixed with elemental S, wherein the solid electrolyte and S are mixed in a mass ratio of 1:0.25. Annealing treatment is performed at an annealing temperature of 250°C, and the powder obtained after annealing treatment is further dissociated by using a jet mill.
[0153] Embodiment 14
[0154] The difference from Example 1 is that the process of step S2 is different: under a nitrogen atmosphere, the solid electrolyte precursor obtained in step S1 is mixed with elemental S, wherein the solid electrolyte and S are mixed in a mass ratio of 1:0.28. Annealing treatment is performed at an annealing temperature of 250°C, and the powder obtained after annealing treatment is further dissociated by air jet milling.
[0155] Embodiment 15
[0156] The difference from Example 1 is that the process of step S2 is different: under a nitrogen atmosphere, the solid electrolyte precursor obtained in step S1 is mixed with P2S5, wherein the solid electrolyte and P2S5 are mixed in a mass ratio of 1:0.15. Annealing treatment is performed at an annealing temperature of 400°C, and the powder obtained after annealing treatment is further dissociated by air jet milling.
[0157] Example 16
[0158] The difference from Example 1 is that the process of step S2 is different: under a nitrogen atmosphere, the solid electrolyte precursor obtained in step S1 is mixed with single substance S, wherein the solid electrolyte and S are mixed in a mass ratio of 1:0.2. Annealing treatment is performed at an annealing temperature of 300°C, and the powder obtained after annealing treatment is further dissociated by air jet milling.
[0159] Embodiment 17
[0160] The difference from Example 1 is that the raw materials used in step S1 are different, and step S11: the compounds of Li2CO3, Al2O3, MgO, TiO2, and P2O5 are weighed according to the target stoichiometric ratio.
[0161] The process of step S2 is different: in a nitrogen atmosphere, the solid electrolyte precursor obtained in step S1 is mixed with Li2S, wherein the solid electrolyte and Li2S are mixed in a mass ratio of 1:0.005. Annealing treatment is performed at an annealing temperature of 350°C, and the powder obtained after annealing treatment is further dissociated by air jet milling.
[0162] Embodiment 18
[0163] The difference from Example 1 is that the raw materials used in step S1 are different, and step S11: weigh the compounds of Li3PO4, AlPO4, ZrO2, TiO2, and MgO according to the target stoichiometric ratio.
[0164] The process of step S2 is different: under a nitrogen atmosphere, the solid electrolyte precursor obtained in step S1 is mixed with single substance S, wherein the solid electrolyte and S are mixed in a mass ratio of 1:0.008. Annealing treatment is performed at an annealing temperature of 350°C, and the powder obtained after annealing treatment is further dissociated by air jet milling.
[0165] Embodiment 19
[0166] The difference from Example 1 is that the raw materials used in step S1 are different, and step S11: weigh the compounds of LiOH, Al2O3, MgO, TiO2, and NH4H2PO4 according to the target stoichiometric ratio.
[0167] The process of step S2 is different: under nitrogen atmosphere, the solid electrolyte precursor obtained in step S1 is mixed with P2S5, wherein the solid electrolyte and P2S5 are mixed in a mass ratio of 1:0.015. Annealing treatment is performed at an annealing temperature of 250°C, and the powder obtained after annealing treatment is further dissociated by air jet milling.
[0168] Comparative Example 1
[0169] The difference from Example 1 is that step S2 does not contain the introduction of S component: the solid electrolyte precursor obtained in step S1 is annealed under a nitrogen atmosphere at a temperature of 300° C., and the powder obtained after annealing is further dissociated by a jet mill.
[0170] Comparative Example 2
[0171] The difference from Example 1 is that step S2 is not performed.
[0172] Comparative Example 3
[0173] The difference from Example 1 is that the raw materials used in step S1 are different, and step S11 does not contain the heating and pre-sintering steps after adding monomers, initiators, and catalysts, and only physical mixing is performed.
[0174] Comparative Example 4
[0175] Directly add the positive electrode active material LiNi 0.93 Co 0.05 Mn 0.02 O2 was heat treated at 500℃ in an atmosphere furnace for 2 hours to obtain the heat-treated LiNi 0.93 Co 0.05 Mn 0.02 O2 material.
[0176] Comparative Example 5
[0177] The difference from Example 1 is that the raw materials used in step S1 are different, and step S11: weigh the compounds of LiOH, Al2O3, MgO, TiO2, and NH4H2PO4 according to the target stoichiometric ratio.
[0178] The process of step S2 is different: under nitrogen atmosphere, the solid electrolyte precursor obtained in step S1 is mixed with P2S5, wherein the solid electrolyte and P2S5 are mixed in a mass ratio of 1:0.2. Annealing treatment is performed at an annealing temperature of 400°C, and the powder obtained after annealing treatment is further dissociated by air jet milling.
[0179] Comparative Example 6
[0180] The difference from Example 1 is that the raw materials used in step S1 are different, and step S11: weigh the compounds of Li2CO3, LiOH, Al2O3, La2O3, TiO2, and P2O5 according to the target stoichiometric ratio.
[0181] The process of step S2 is different: in a nitrogen atmosphere, the solid electrolyte precursor obtained in step S1 is mixed with Li2S, wherein the solid electrolyte and Li2S are mixed in a mass ratio of 1:0.006. Annealing treatment is performed at an annealing temperature of 250°C, and the powder obtained after annealing treatment is further dissociated by air jet milling.
[0182] Comparative Example 7
[0183] The difference from Example 1 is that the raw materials used in step S1 are different, and step S11: weigh the compounds of Li2CO3, LiOH, Al2O3, La2O3, TiO2, and P2O5 according to the target stoichiometric ratio.
[0184] The process of step S2 is different: in a nitrogen atmosphere, the solid electrolyte precursor obtained in step S1 is mixed with Li2S, wherein the solid electrolyte and Li2S are mixed in a mass ratio of 1:0.004. Annealing treatment is performed at an annealing temperature of 250°C, and the powder obtained after annealing treatment is further dissociated by air jet milling.
[0185] The NASICON solid electrolytes in the above embodiments and comparative examples were subjected to XRD (after fitting and refinement), EIS, BET and particle size tests. The average radius of the crystal grains, lattice constants (a, b, c, α, β and γ), lattice distortion rate and crystallinity of each embodiment and comparative example are shown in Table 1, and the particle size distribution, specific surface area and ionic conductivity are shown in Table 2.
[0186] The XRD pattern of the solid electrolyte in Example 1 is shown in Figure 1 The XRD pattern of the solid electrolyte in Comparative Example 1 is shown in Figure 2 The EDS test mapping diagram of the NASICON solid electrolyte phase prepared in Example 1 is shown in Figure 3 , the signal response of elements Al, Ti, and S can be observed from the figure. Figure 4 As shown, the battery of Example 1 exhibits higher first cycle discharge capacity and first coulombic efficiency than that of Comparative Example 4. Therefore, it is shown that the positive electrode material coated with the NASICON type solid electrolyte has more excellent electrochemical performance.
[0187] Table 1
[0188]
[0189]
[0190] Table 2
[0191]
[0192] At the same time, it can be seen from Table 1 that after fitting and refinement calculation, compared with the comparative example, the average grain radius of the solid electrolyte in the embodiment is smaller than The lattice distortion rate is greater than 0.05%; the material crystallinity is less than 99.5%; the lattice constants a and b are both less than c is greater than α and β are both greater than 90.005°, and γ is greater than 120.005°, indicating that the grain size of the sulfur-modified NASICON solid electrolyte decreases, the lattice becomes refined and elongated, and the crystallinity of the material decreases.
[0193] As shown in Table 2, compared with the comparative example, the NASICON solid electrolyte in the embodiment has higher ion conductivity, higher specific surface area, and a particle size Dv 50 The Dv of the solid electrolyte in the embodiment is lower. 50 All are less than 0.2μm, and the specific surface area is >30m 2 / g, ionic conductivity>4.0×10 -4 S / cm, indicating that the sulfur-modified NASICON solid electrolyte is a nanoscale raw material with good dispersibility and is a good ion conductor.
[0194] Preparation of positive electrode active materials:
[0195] The core LiNi 0.93 Co 0.05 Mn 0.02 O2 is mixed with the aforementioned solid electrolyte, the mass fraction of the solid electrolyte is 0.08wt% based on the total mass of the inner core, and they are put into a high-speed mixer and mixed evenly to obtain a mixture, which is heat-treated at 500°C in an atmosphere furnace for 2h to obtain a positive electrode active material coated with a solid electrolyte.
[0196] The positive electrode active materials corresponding to the above-mentioned Examples 1-4 and Comparative Examples 1-4 are assembled into batteries in the following manner:
[0197] Perform the following operations in a glove box filled with argon or in a laboratory with humidity controlled at a dew point of -40°C:
[0198] The positive electrode active material, polyvinylidene fluoride binder, carbon black conductive agent and solid electrolyte sulfide Li6PS5Cl were fully dissolved in n-heptane (the mass ratio of positive electrode active material, binder, conductive agent and solid electrolyte was 70:0.5:1.5:28) to prepare a uniformly dispersed slurry, which was evenly coated on the surface of aluminum foil (loading amount was 36 mg / cm 2 ), and then transferred to a vacuum drying oven for complete drying, the obtained electrode sheet was roll-pressed, and then punched to obtain the positive electrode sheet.
[0199] Lithium-indium alloy is used as the negative electrode sheet, and 100 mg of sulfide Li6PS5Cl is used as the solid electrolyte, which is pressed into sheets under a pressure of 300 MPa to obtain a solid electrolyte layer, which is then stacked and assembled into a solid-state battery in the order of positive electrode sheet, solid electrolyte layer and negative electrode sheet.
[0200] The above-mentioned battery was tested as follows, and the test results are shown in Table 3.
[0201] Test of the real part of total impedance before cycling: Before cycling, the assembled solid-state battery is subjected to electrochemical impedance spectroscopy (EIS). The frequency range of the electrical signal of the EIS test is 0.01Hz to 10000000Hz, and the disturbance amplitude of the AC voltage is 10mV. The Nyquis graph obtained after the test is fitted by Zview software to obtain the real part of the total impedance of the battery before cycling. The smaller the real part of the total impedance, the better the chemical stability at the battery interface.
[0202] First discharge specific capacity, first cycle coulomb efficiency and cycle performance test: At 25°C, the solid-state battery was charged to 3.7V at a constant current of 0.1C to obtain the first charge specific capacity C0 of the solid-state battery, and then discharged to 2.0V at a constant current of 0.1C to obtain the first cycle discharge specific capacity C1 of the solid-state battery, and then charged and discharged at a constant current of 0.1C for 80 cycles, and the discharge specific capacity C of the 80th cycle was obtained. 80 . Battery first cycle coulombic efficiency = C1 / C0×100%. Battery capacity retention rate after 80 cycles = C 80 / C1×100%.
[0203] Rate performance test method: the solid-state battery is charged to 3.7V at a constant current of 0.33C, and then discharged to 2.0V at a constant current of 0.33C to obtain the first discharge specific capacity corresponding to 0.33C; then the solid-state battery is charged to 3.7V at a constant current of 0.5C, and then discharged to 2.0V at a constant current of 0.5C to obtain the discharge specific capacity corresponding to 0.5C; then the solid-state battery is charged to 3.7V at a constant current of 1C, and then discharged to 2.0V at a constant current of 1C to obtain the discharge specific capacity corresponding to 1C; finally, the solid-state battery is charged to 3.7V at a constant current of 0.33C, and then discharged to 2.0V at a constant current of 0.33C to obtain the second discharge specific capacity corresponding to 0.33C.
[0204] Table 3
[0205]
[0206] As shown in Table 3, the first discharge capacity, first cycle coulomb efficiency, 80-week cycle capacity retention rate, first discharge capacity corresponding to 0.33C, discharge capacity corresponding to 0.5C, discharge capacity corresponding to 1.0C, and second discharge capacity corresponding to 0.33C of the solid-state battery equipped with the positive active material corresponding to Examples 1-4 are all higher than those of Comparative Examples 1-4, and the real part of the total impedance before the cycle is lower than that of Comparative Examples 1-4. The positive active material of the present invention uses a high-nickel material as a matrix, and forms a NASICON-type solid electrolyte coating layer on the surface of the matrix, has good interface stability, and can improve the charge and discharge capacity and rate performance of the all-solid-state battery containing it, reduce the interface resistance, and improve the cycle capacity.
[0207] In the description of this specification, the description with reference to the terms "one embodiment", "some embodiments", "example", "specific example", or "some examples" etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present application. In this specification, the schematic representations of the above terms do not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described may be combined in any one or more embodiments or examples in a suitable manner. In addition, those skilled in the art may combine and combine the different embodiments or examples described in this specification and the features of the different embodiments or examples, without contradiction.
[0208] Although the embodiments of the present application have been shown and described above, it can be understood that the above embodiments are exemplary and cannot be understood as limitations on the present application. Ordinary technicians in this field can change, modify, replace and modify the above embodiments within the scope of the present application.
Claims
1. A solid electrolyte, characterized in that Satisfy the chemical formula: Li 1+x A x D 2-x (PO 4-y S y )3, wherein A is at least one of Mg, B, Na, K, Zn, Ga, Sc, In, Y, Ce, Co, La, Cr, Mo, Mn, Fe, W, Si, Nb, Sm, and Al, and D is at least one of Ti, Zr, Hf, and Ge, 0.01≤x≤5, 0.0001≤y≤0.3, and the unit cell parameter c / a of the solid electrolyte is 2.448-2.
520.
2. The solid electrolyte according to claim 1, characterized in that The lattice constants a, b, c, α, β, and γ of the solid electrolyte satisfy at least one of the following conditions: a is b is c is α is 90.005°-91.050°; β is 90.005°-91.050°; γ is 120.005°-120.050°.
3. The solid electrolyte according to claim 1 or 2, characterized in that The unit cell parameter c / a of the solid electrolyte is 2.450-2.
500.
4. The solid electrolyte according to claim 1 or 2, characterized in that The unit cell volume of the solid electrolyte is 5. The solid electrolyte according to claim 1 or 2, characterized in that: The average grain radius of the solid electrolyte is And / or, the lattice distortion rate of the solid electrolyte is 0.05%-0.5%; and / or, the crystallinity of the solid electrolyte is 95.0%-99.5%.
6. The solid electrolyte according to claim 1 or 2, characterized in that: The solid electrolyte satisfies at least one of the following conditions: D v50 Particle size is 0.01μm-0.2μm; The specific surface area is 30m 2 / g-300m 2 / g; The ionic conductivity is 4.0×10 -4 S / cm-1×10 -3 S / cm.
7. A method for preparing the solid electrolyte according to any one of claims 1 to 6, characterized in that: include: S1: sintering the titanium source, lithium source, phosphorus source and M source to obtain a solid electrolyte precursor; S2: Under an inert atmosphere, annealing the solid electrolyte precursor and the sulfur source to obtain the solid electrolyte.
8. The method according to claim 7, characterized in that The step S1 comprises: Mixing the titanium source, the lithium source, the phosphorus source, the M source, an organic monomer, a first solvent, an initiator and a catalyst to obtain a mixture; Heating the mixture to obtain a first solid electrolyte precursor; Pre-sintering the first solid electrolyte precursor to obtain a second solid electrolyte precursor; The second solid electrolyte precursor is subjected to the sintering treatment to obtain the solid electrolyte precursor.
9. The method according to claim 8, characterized in that The organic monomer includes at least one of acrylamide, methylenebisacrylamide, styrene, butadiene and methyl methacrylate; and / or, The first solvent comprises at least one of water, N-methyl-2-pyrrolidone, phthalate, dibasic lipid, long-chain alcohol and pyrrolidone; and / or, The initiator comprises at least one of benzoyl peroxide, (NH4)2S2O8 and K2S2O8; and / or, The catalyst includes at least one of N,N,N'N'-tetramethylethylenediamine, N,N,N',N'-tetramethyl-1,6-hexanediamine, N,N-diisopropylethylamine, and N-(3-aminopropyl)-N-dodecyl-1,3-propylenediamine.
10. The method according to claim 8 or 9, characterized in that: The temperature of the heating treatment is 80°C-200°C; and / or, The pre-sintering temperature is 300° C.-600° C., and the pre-sintering time is 2 h-6 h; and / or, The sintering temperature is 650° C.-900° C., and the sintering time is 4 h-10 h.
11. The method according to any one of claims 7 to 9, characterized in that: The solid electrolyte precursor D v50 The particle size is 5nm-500nm.
12. The method according to any one of claims 7 to 9, characterized in that: The added amount of the sulfur source is 0.1wt%-3wt% of the solid electrolyte precursor.
13. The method according to any one of claims 7 to 9, characterized in that: The temperature of the annealing treatment is 120° C.-600° C., and the time of the annealing treatment is 2 h-6 h.
14. A positive electrode active material, characterized in that: include: Kernel; A coating layer, wherein the coating layer is at least partially located on the surface of the inner core, and the coating layer comprises the solid electrolyte according to any one of claims 1 to 6.
15. The positive electrode active material according to claim 14, characterized in that Based on the total mass of the inner core, the mass fraction of the solid electrolyte is 0.05wt%-1.5wt%.
16. The positive electrode active material according to claim 14 or 15, characterized in that: The core includes at least one of lithium nickel oxide, lithium cobalt oxide, lithium manganese oxide, lithium nickel manganese oxide, lithium nickel cobalt manganese oxide, lithium nickel cobalt aluminum oxide, lithium nickel cobalt manganese aluminum oxide, lithium-rich manganese-based layered oxides and their derivatives, lithium iron phosphate and lithium manganese iron phosphate.
17. A method for preparing the positive electrode active material according to any one of claims 14 to 16, characterized in that: include: The inner core and the solid electrolyte are heat-treated to form a coating layer including the solid electrolyte on at least a portion of the surface of the inner core, wherein the solid electrolyte includes the solid electrolyte according to any one of claims 1 to 6.
18. The method according to claim 17, characterized in that The temperature of the heat treatment is 200° C.-700° C., and the time of the heat treatment is 2 h-10 h.
19. A positive electrode plate, characterized in that: The positive electrode active material comprises the positive electrode active material according to any one of claims 14 to 16.
20. A solid-state battery, characterized in that: Including the positive electrode sheet as described in claim 19.
21. An electrical device, characterized in that: Including the solid-state battery as described in claim 20.
Citation Information
Cited By
Solid-state electrolyte, solid-state electrolyte membrane and preparation method thereof, and solid-state battery
CN121905944A