Electrolyte additive, electrolyte and lithium ion battery

By using benzonitrile compounds containing 2,2,2-trifluoroethoxy groups as electrolyte additives in lithium-ion batteries, the problem of nitrile additives destroying the graphite structure is solved, and the excellence of lithium-ion batteries is achieved It takes into account both cycling performance and high temperature resistance, and improves the stability of the electrolyte through water removal and acid removal function.

CN118970190APending Publication Date: 2024-11-15EVE ENERGY CO LTD

Patent Information

Application Number
CN202411210881.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-29
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

Nitrile additives destroy the graphite structure in lithium-ion batteries, resulting in deterioration of the circulation performance of lithium-ion batteries, making it difficult to take into account excellent circulation performance and high temperature resistance.

Method used

Use benzonitrile compounds containing 2,2,2-trifluoroethoxy groups as electrolyte additives, and participate in the generation of solid electrolyte interface masks through their fluorine elements to repair the negative electrode interface masks destroyed by nitrile additives, and with Nitrile additives coexist to take into account both circulation and high temperature properties, and have water removal and acid removal and oxidation resistance.

Benefits of technology

It effectively repairs the negative electrode interface mask destroyed by nitrile additives, ensures that the circulation performance of lithium-ion batteries is not degraded, takes into account excellent circulation performance and high temperature resistance, and improves the stability of the electrolyte through the water removal and acid removal function.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118970190A_ABST
    Figure CN118970190A_ABST
Patent Text Reader

Abstract

The invention discloses an electrolyte additive, an electrolyte and a lithium ion battery, and belongs to the field of secondary batteries. The chemical structural formula of the electrolyte additive is as follows: # imgabs0 #, wherein R1 and R2 are respectively and independently selected from hydrogen, halogen, halogenated alkyl containing 1-10 carbon atoms, alkoxy containing 1-10 carbon atoms or alcoholic hydroxyl containing 3-5 carbon atoms. When the cyanobenzene compound and the nitrile additive coexist, the cyanobenzene compound can repair a negative electrode interface film damaged by the nitrile additive based on the negative electrode film forming function of the cyanobenzene compound, and the cyanobenzene compound also has water removal and acid removal functions, so that the lithium ion battery can have excellent cycle performance and high temperature resistance at the same time.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to secondary battery technology, and in particular to electrolyte additives, electrolytes and lithium-ion batteries. Background Art

[0002] Lithium-ion batteries achieve charging and discharging by embedding and de-embedding lithium ions between the positive electrode and the negative electrode. The electrolyte serves as a transmission carrier for lithium ions between the positive electrode and the negative electrode, and generally includes a lithium salt electrolyte, a solvent, and additives.

[0003] As a common high-temperature additive, nitrile additives are beneficial to improving the high-temperature resistance of lithium-ion batteries. However, for lithium-ion batteries with a graphite negative electrode, nitrile additives will destroy the graphite structure, thereby deteriorating the battery's cycle performance.

[0004] It can be seen that in the presence of nitrile additives, it is necessary to further improve the cycle performance of lithium-ion batteries so that the lithium-ion batteries have both excellent cycle performance and high temperature resistance. Summary of the invention

[0005] In view of this, the present application provides an electrolyte additive, an electrolyte and a lithium-ion battery, which can solve the technical problems existing in the related technologies. Specifically, the present application provides the following technical solutions:

[0006] In one aspect, an electrolyte additive is provided, wherein the chemical structural formula of the electrolyte additive is as follows:

[0007]

[0008] Wherein, R1 and R2 are each independently selected from hydrogen, halogen, a halogenated hydrocarbon group containing 1 to 10 carbon atoms, an alkoxy group containing 1 to 10 carbon atoms or an alcoholic hydroxyl group containing 3 to 5 carbon atoms.

[0009] In some possible implementations, the chemical structural formula of the electrolyte additive is any one of the following:

[0010]

[0011] On the other hand, an electrolyte is provided, comprising: 1 mol / L-3 mol / L of lithium salt, 2 wt%-30 wt% of additives, and the remainder of solvent; wherein the additives include: nitrile additives and any of the above-mentioned electrolyte additives.

[0012] In some possible implementations, the mass percentage of the nitrile additive is 0.2 wt%-2 wt%; the mass percentage of the electrolyte additive is 2 wt%-8 wt%.

[0013] In some possible implementations, the nitrile additive includes at least one of carbonitrile, acetonitrile, propionitrile, butyronitrile, succinonitrile, adiponitrile, glutaronitrile, suberonitrile, 1,3,6-hexanetricarboxylic acid nitrile, 1,3,5-pentanetricarboxylic acid nitrile, p-fluorobenzonitrile, p-methylbenzonitrile, 2-fluoroadiponitrile, and 2,2-difluorosuccinonitrile.

[0014] In some possible implementations, the lithium salt is selected from at least one of lithium hexafluorophosphate, lithium difluorophosphate, lithium tetrafluoroborate, lithium perchlorate, lithium bis(oxalatoborate), lithium difluorobis(oxalatoborate), lithium bis(fluorosulfonyl)imide, and lithium bis(trifluoromethylsulfonyl)imide.

[0015] In some possible implementations, the solvent includes at least one of linear carbonates, cyclic carbonates, hydroxy acid esters, sulfites, and nitrites.

[0016] In some possible implementations, the additive also includes: at least one of a carbonate additive, a sulfur-containing additive, and a lithium salt additive; the mass percentage of the carbonate additive is 1wt%-10wt%; the mass percentage of the sulfur-containing additive is 0.1wt%-2wt%; the mass percentage of the lithium salt additive is 0.2wt%-1wt%.

[0017] In some possible implementations, the carbonate additive is selected from at least one of vinylene carbonate and ethylene carbonate; the sulfur-containing additive is selected from at least one of propylene sulfite, propylene-1,3-sultone, vinyl sulfate, and methylene disulfonate. The lithium salt additive is selected from at least one of lithium bis(fluorosulfonyl)imide, lithium difluorophosphate, lithium bis(oxalatoborate), and lithium difluorobis(oxalatophosphate).

[0018] On the other hand, a lithium-ion battery is provided, comprising: a shell, a positive electrode, a negative electrode, a separator and an electrolyte located inside the shell, wherein the positive electrode and the negative electrode are separated by the separator; wherein the electrolyte is as described above.

[0019] The beneficial effects of the technical solution provided by the embodiments of the present application include at least:

[0020] The present application embodiment provides the application of benzonitrile compounds containing 2,2,2-trifluoroethoxy groups as electrolyte additives. Studies have found that the 2,2,2-trifluoroethoxy groups contained in the benzonitrile compounds, the fluorine element can participate in the formation of SEI film at the negative electrode of the battery, and realize negative electrode film formation. When the benzonitrile compound coexists with the nitrile additive, the benzonitrile compound can repair the negative electrode interface film destroyed by the nitrile additive based on its negative electrode film-forming function, thereby ensuring that the cycle performance of the lithium-ion battery is not deteriorated. In this way, the lithium-ion battery can take into account excellent cycle performance and high temperature resistance based on the coexistence of benzonitrile compounds and nitrile additives. In addition, the benzonitrile compound can also combine with trace amounts of water and acid in the electrolyte based on its nitrile group, eliminate moisture and reduce acidity, and play a role in removing water and acid. In addition, the benzonitrile compound has a strong oxidation resistance based on its rigid benzene ring, which is conducive to improving the stability of the electrolyte itself, thereby further optimizing the cycle performance of the lithium-ion battery. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] In order to more clearly illustrate the technical solutions in the embodiments of the present application, the drawings required for use in the description of the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work.

[0022] Figure 1 A schematic diagram of the structure of an exemplary lithium-ion battery provided in an embodiment of the present application. DETAILED DESCRIPTION

[0023] The following will be combined with the drawings in the embodiments of the present disclosure to clearly and completely describe the technical solutions in the embodiments of the present disclosure. Obviously, the described embodiments are part of the embodiments of the present disclosure, not all of the embodiments. Based on the embodiments in the present disclosure, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present disclosure.

[0024] For lithium-ion batteries, nitrile additives are usually added to their electrolytes to improve the high temperature resistance of lithium-ion batteries. However, for lithium-ion batteries with graphite as the negative electrode, nitrile additives will destroy the graphite structure, thereby deteriorating the cycle performance of the battery. It can be seen that in the presence of nitrile additives, it is necessary to further improve the cycle performance of lithium-ion batteries, so that lithium-ion batteries can have both excellent cycle performance and high temperature resistance (i.e., high temperature storage performance).

[0025] In view of the technical problems existing in the related art, the embodiment of the present application provides an electrolyte additive, and the chemical structure of the electrolyte additive is as follows:

[0026]

[0027] In the chemical structures mentioned above, the wavy line It means that the oxygen atom can be connected to any of the three vacant carbon atoms on the benzene ring, so that the 2,2,2-trifluoroethoxy group is in the ortho, para or meta position with respect to the CN group.

[0028] Wherein, R1 and R2 are each independently selected from hydrogen, halogen, a halogenated hydrocarbon group containing 1 to 10 carbon atoms, an alkoxy group containing 1 to 10 carbon atoms or an alcoholic hydroxyl group containing 3 to 5 carbon atoms.

[0029] As for the halogen, it may be fluorine, chlorine, bromine, iodine, for example, it may be fluorine.

[0030] For the halogenated hydrocarbon group containing 1-10 carbon atoms, it can be fluorocarbon, chlorocarbon, bromocarbon, iodocarbon, and the halogenated hydrocarbon group can be halogenated alkane, halogenated alkene, etc. For further examples, this includes but is not limited to: halogenated methyl (for example, CF3), halogenated ethyl, halogenated propyl, halogenated butyl (n-butyl, isobutyl, tert-butyl, etc.), halogenated pentyl, halogenated hexyl, halogenated heptyl, halogenated octyl, etc.

[0031] The alkoxy group containing 1 to 10 carbon atoms includes, but is not limited to, methoxy, ethoxy, propoxy, butoxy (n-butyl, isobutyl, tert-butyl, etc.), pentyloxy, hexyloxy, heptyloxy, octyloxy, nonyloxy, and the like.

[0032] For the alcohol hydroxyl group containing 3-5 carbon atoms, the number of hydroxyl groups contained therein can be one or two. Some applicable alcohol hydroxyl groups include but are not limited to: n-propanol, isopropanol, n-butanol, isobutanol, n-pentanol, isopentanol, propylene glycol, butylene glycol, pentanediol and the like.

[0033] The embodiment of the present application provides the application of benzonitrile compounds containing 2,2,2-trifluoroethoxy groups as electrolyte additives. Studies have found that the 2,2,2-trifluoroethoxy groups contained in the benzonitrile compounds, the fluorine element of which can participate in the formation of the solid electrolyte interface membrane (Solid Electrolyte Interface membrane, SEI) at the negative electrode of the battery, to achieve negative electrode film formation. When the benzonitrile compounds coexist with nitrile additives, the benzonitrile compounds can repair the negative electrode interface film destroyed by the nitrile additives based on their negative electrode film-forming function, thereby ensuring that the cycle performance of the lithium-ion battery is not deteriorated. In this way, the lithium-ion battery can take into account both excellent cycle performance and high temperature resistance based on the coexistence of benzonitrile compounds and nitrile additives. In addition, the benzonitrile compound can also combine with trace amounts of water and acid in the electrolyte based on its nitrile group, eliminate moisture and reduce acidity, and play a role in removing water and acid. In addition, the benzonitrile compound has strong oxidation resistance based on its rigid benzene ring, which is beneficial to improving the stability of the electrolyte itself, thereby further optimizing the cycle performance of the lithium-ion battery.

[0034] In addition, for the above-mentioned benzonitrile compounds containing a 2,2,2-trifluoroethoxy group, when R1 and R2 are independently selected from a halogenated hydrocarbon group containing 1 to 10 carbon atoms, an alkoxy group containing 1 to 10 carbon atoms, or an alcoholic hydroxyl group containing 3 to 5 carbon atoms, the presence of these substituent groups can further promote the negative electrode film-forming effect of the benzonitrile compound when used as an electrolyte additive, which is beneficial to optimize the cycle performance of the battery.

[0035] In some examples, the chemical structural formula of the electrolyte additive involved above is shown as any one of the following:

[0036]

[0037] For any of the benzonitrile compounds containing a 2,2,2-trifluoroethoxy group involved in the embodiments of the present application, the benzonitrile compound can be prepared by the following preparation method.

[0038] In the presence of a catalyst, a benzonitrile compound and a halogenated hydrocarbon compound are subjected to condensation reflux reaction in a solvent to prepare the electrolyte additive.

[0039] Among them, the chemical structural formula of benzonitrile compounds is as follows:

[0040]

[0041] The R1 and R2 groups can refer to the R1 and R2 groups in the above-mentioned electrolyte additives, which will not be repeated here.

[0042] The M group includes, but is not limited to: -OH, -NO2, -Cl, etc. For example, the benzonitrile compound can be 3-hydroxybenzonitrile, 4-hydroxybenzonitrile, 3-chlorobenzonitrile, p-chlorobenzonitrile, 3-nitrobenzonitrile, p-nitrobenzonitrile, etc.

[0043] Exemplary halogenated hydrocarbon compounds include, but are not limited to, 2,2,2-trifluoroiodoethane, sodium 2,2,2-trifluoroethoxide, and the like.

[0044] Illustratively, the catalyst includes, but is not limited to, KF, alkali metal carbonate, sodium hydroxide, etc. Based on such catalyst, the benzonitrile compound and the halogenated hydrocarbon compound can smoothly achieve a nucleophilic reaction.

[0045] Exemplarily, the reaction temperature is 110°C-150°C, and the reaction time is 3h-7h.

[0046] Taking 4-(2,2,2-trifluoroethoxy)benzonitrile as an electrolyte additive, it can be prepared by the following method:

[0047] 4-Hydroxybenzonitrile (1mmol) and KF (1mmol) are dissolved in methanol (10ml) and mixed evenly, then the methanol is gradually distilled out, washed with dry ether (30ml) and dried under vacuum to obtain a mixture. The mixture is dissolved in dimethyl sulfoxide DMSO (15ml) for pre-dissolution, and then added to a mixed solution of dimethyl sulfoxide (3ml) and halogenated hydrocarbon (3mmol), and heated in a closed reactor at a temperature of 110°C-150°C, such as 120°C, for 3h-7h. After the reaction is completed, the reaction product is diluted with ice water, and then the reaction product is extracted with ethyl acetate to separate and obtain high-purity 4-(2,2,2-trifluoroethoxy)benzonitrile.

[0048] On the other hand, an embodiment of the present application also provides an electrolyte, which includes: 1 mol / L-3 mol / L of lithium salt, 2wt%-30wt% of additives, and the remainder of solvent; wherein the additives include: nitrile additives and any one of the electrolyte additives mentioned above.

[0049] The electrolyte provided in the embodiment of the present application further uses the electrolyte additives mentioned above to ensure and improve the cycle performance of the lithium-ion battery based on the use of nitrile additives to improve the high temperature resistance of the battery. In this way, the lithium-ion battery can take into account both excellent cycle performance and high temperature resistance based on the coexistence of benzonitrile compounds and nitrile additives. On this basis, by combining the components in the electrolyte in a specific ratio, the comprehensive performance of the lithium-ion battery is ensured to be excellent.

[0050] Lithium salt is used as the electrolyte, and some applicable lithium salt concentrations are 1mol / L-3mol / L, including but not limited to: 1mol / L, 1.1mol / L, 1.2mol / L, 1.3mol / L, 1.4mol / L, 1.5mol / L, 2mol / L, 2.5mol / L, 3mol / L, etc.

[0051] Some lithium salts suitable for the electrolyte system involved in the embodiments of the present application can be selected from at least one of lithium hexafluorophosphate, lithium difluorophosphate, lithium tetrafluoroborate, lithium perchlorate, lithium bis(oxalatoborate), lithium difluorobis(oxalatoborate), lithium bis(fluorosulfonyl)imide, and lithium bis(trifluoromethylsulfonyl)imide.

[0052] As described above, the additives include at least nitrile additives and electrolyte additives. In some examples, the mass percentage of the nitrile additives is 0.2wt%-2wt%, which includes but is not limited to: 0.2wt%, 0.5wt%, 0.8wt%, 1wt%, 1.1wt%, 1.2wt%, 1.3wt%, 1.4wt%, 1.5wt%, 1.6wt%, 1.7wt%, 1.8wt%, 1.9wt%, 2wt%, etc.

[0053] The mass percentage of electrolyte additives based on benzonitrile compounds is 2wt%-8wt%, which includes but is not limited to: 2wt%, 2.5wt%, 3wt%, 3.5wt%, 4wt%, 4.5wt%, 5wt%, 5.5wt%, 6wt%, 6.5wt%, 7wt%, 7.5wt%, 8wt% and the like.

[0054] Normally, nitrile additives are continuously consumed during the battery cycle. Therefore, the more electrolyte additives based on benzonitrile compounds are added, the more stable the negative electrode film-forming performance is, and the better the performance of maintaining battery cycle stability is.

[0055] In some examples, the nitrile additive is selected from at least one of methyl nitrile, acetonitrile (AN), propionitrile, butyronitrile, succinonitrile (SN), adiponitrile, glutaronitrile, suberonitrile, 1,3,6-hexanetricarbonitrile, 1,3,5-pentanetricarbonitrile, p-fluorobenzonitrile, p-methylbenzonitrile, 2-fluoroadiponitrile, and 2,2-difluorosuccinonitrile. The above-mentioned nitrile additives are all conducive to improving the high temperature storage performance of lithium-ion batteries.

[0056] The solvent serves as a carrier for carrying and dispersing the lithium salt. In the embodiment of the present application, the solvent can be at least one of linear carbonates, cyclic carbonates, hydroxy acid esters, sulfites, and nitrites. For example, this includes ethylene carbonate (EC for short), propylene carbonate (PC for short), dimethyl carbonate (DMC for short), ethyl methyl carbonate (EMC for short), diethyl carbonate (DEC for short), etc.

[0057] Furthermore, the solvent is selected from at least two of ethylene carbonate, propylene carbonate, dimethyl carbonate, ethyl methyl carbonate, and diethyl carbonate. For example, based on the volume of the solvent as 100%, the solvent includes the following components in volume percentage: 15% to 30% of ethylene carbonate, 10% to 50% of dimethyl carbonate, 0% to 20% of diethyl carbonate, and 20% to 50% of ethyl methyl carbonate.

[0058] In some implementations, in the electrolyte provided in the embodiments of the present application, the additive further includes: at least one of a carbonate additive, a sulfur-containing additive, and a lithium salt additive.

[0059] Carbonate additives mainly form films at the negative electrode, with high film potential and high film impedance at low temperatures. Carbonate additives are used to improve the low-temperature performance of the electrolyte, form a SEI film with better performance, and improve the cycle performance of lithium-ion batteries. The mass percentage of carbonate additives is 1wt%-10wt% to ensure the above performance effects.

[0060] Illustratively, the mass percentage of the carbonate additive includes, but is not limited to, 1 wt%, 2 wt%, 3 wt%, 4 wt%, 5 wt%, 6 wt%, 7 wt%, 8 wt%, 9 wt%, 10 wt%, etc.

[0061] Some applicable carbonate additives are selected from at least one of vinylene carbonate VC and ethylene carbonate EC.

[0062] Sulfur-containing additives can assist film formation at the positive and negative electrodes, and have high thermal stability. Sulfur-containing additives are not only beneficial for improving the electrical performance, cycle performance, and low-temperature discharge performance of the battery, but also beneficial for inhibiting gas production and capacity decay. Too little addition of sulfur-containing additives cannot form a dense SEI film at the negative electrode, and too much addition of sulfur-containing additives will result in excessive film formation, resulting in a decrease in battery cycle performance. Therefore, the mass percentage of sulfur-containing additives is 0.1wt%-2wt%.

[0063] Exemplarily, the mass percentage of the sulfur-containing additive includes but is not limited to 0.1wt%, 0.2wt%, 0.3wt%, 0.4wt%, 0.5wt%, 0.6wt%, 0.7wt%, 0.8wt%, 0.9wt%, 1wt%, 1.1wt%, 1.2wt%, 1.3wt%, 1.4wt%, 1.5wt%, 1.6wt%, 1.7wt%, 1.8wt%, 1.9wt%, 2wt%, etc.

[0064] Some suitable sulfur-containing additives are selected from at least one of propylene sulfite PS, propylene-1,3-sultone PST, vinyl sulfate DTD, and methylene methane disulfonate MMDS.

[0065] The lithium salt additive can increase the number of lithium ion migration and participate in the film formation of the positive and negative electrodes of the battery, thereby improving the stability of the interface film and the cycle performance of the lithium ion battery. The above performance effect can be ensured by setting the mass percentage of the lithium salt additive to 0.2wt%-1wt%.

[0066] Illustratively, the mass percentage of the lithium salt additive includes, but is not limited to, 0.1 wt%, 0.2 wt%, 0.3 wt%, 0.4 wt%, 0.5 wt%, 0.6 wt%, 0.7 wt%, 0.8 wt%, 0.9 wt%, 1 wt%, and the like.

[0067] Some suitable lithium salt additives are selected from at least one of lithium bis(fluorosulfonyl)imide (LiFSI), lithium difluorophosphate (LiPO2F2), lithium bis(oxalatoborate) (LiBOB), and lithium difluorobis(oxalatophosphate) (LiODFP).

[0068] Based on the above electrolyte formula, the electrolyte can be prepared by the following preparation method: in a glove box filled with argon atmosphere, an additive is added to a solvent and stirred evenly, and then a lithium salt is added and stirred evenly to prepare the electrolyte.

[0069] For example, for adding additives, carbonate additives, lithium salt additives, sulfur-containing additives, nitrile additives and electrolyte additives based on benzonitrile compounds may be added to the solvent in sequence and stirred evenly.

[0070] In summary, for the electrolyte provided in the embodiments of the present application, through the synergistic effect of the electrolyte additive with dual functions and the carbonate additive, lithium salt additive, sulfur-containing additive, and nitrile additive, on the basis of ensuring that the battery has good high-temperature storage performance, it is also possible to enhance the negative electrode interface stability and solve the battery's normal temperature / high temperature cycle diving problem under low current.

[0071] On the other hand, an embodiment of the present application further provides a lithium-ion battery, which includes: a shell, a positive electrode, a negative electrode, a diaphragm and an electrolyte located inside the shell, and the positive electrode and the negative electrode are separated by the diaphragm; wherein the electrolyte is as described above.

[0072] The lithium-ion battery provided in the embodiment of the present application has all the advantages brought by the electrolyte involved above, which will not be described in detail here.

[0073] Figure 1 An example of a lithium-ion battery structure is shown in the attached Figure 1As shown, the lithium-ion battery includes a negative electrode 100, a positive electrode 200, an electrolyte 300, a separator 400, and a housing 500 (also known as a packaging housing). Among them, the electrolyte 300 is filled in the housing 500, and the negative electrode 100, the positive electrode 200, and the separator 400 are all in the electrolyte 300. The separator 400 is ion-conductive but electron-insulating, and is used to ensure the migration of lithium ions while separating the negative electrode 100 and the positive electrode 200 to prevent short circuits.

[0074] For the positive electrode (also known as the positive electrode tab) and the negative electrode (also known as the negative electrode tab) of the lithium-ion battery, both can include a current collector and an active layer bonded to the surface of the current collector. The active layer usually includes a positive or negative electrode active material and a conductive agent.

[0075] For the positive electrode of the lithium-ion battery, the positive electrode active material includes, but is not limited to, at least one of a lithium-containing layered metal oxide, a lithium-containing spinel structure metal oxide, a lithium metal phosphate, a lithium metal fluorosulfate, and a lithium metal vanadate. For example, the lithium-containing layered metal oxide includes, but is not limited to, at least one of lithium cobalt oxide (LiCoO2), nickel cobalt manganese ternary material (NCM), and nickel cobalt aluminum ternary material (NCA); the lithium-containing spinel structure metal oxide includes, but is not limited to, lithium manganese oxide (LiMn2O4), etc.; the lithium metal phosphate includes, but is not limited to, lithium iron phosphate (LiFePO4), etc.; the lithium metal fluorosulfate includes, but is not limited to, lithium cobalt fluorosulfate (LiCoFSO4), etc.; the lithium metal vanadate includes, but is not limited to, lithium nickel vanadate (LiNiVO4), etc.

[0076] In some examples, a nickel cobalt manganese ternary material can be used as the positive electrode active material. For example, the chemical general formula of the nickel cobalt manganese ternary material is (Li(Ni x Co y Mn z )O2), where x, y, and z are atomic percentages, 0.5 ≤ x < 0.8, 0 < y ≤ 0.3, 0 < z ≤ 0.3, and x + y + z = 1.

[0077] For the negative electrode of the lithium-ion battery, the negative electrode active material can be graphite-based carbon, silicon carbon, etc., where the graphite-based carbon includes, but is not limited to, natural graphite, artificial graphite, graphite-like materials, etc.

[0078] The specific embodiments of the present application will be described in more detail below. Although the specific embodiments of the present application are described below, it should be understood that the present application can be implemented in various forms and should not be limited by the embodiments set forth herein. For those where specific techniques or conditions are not indicated in the examples, the techniques or conditions described in the literature in the art or according to the product specifications are followed. For reagents or instruments where the manufacturer is not indicated, they are all conventional products that can be obtained commercially.

[0079] Example 1

[0080] This embodiment 1 provides an electrolyte, which includes a lithium salt, an additive and a balance solvent, wherein the lithium salt is lithium hexafluorophosphate with a concentration of 1.1 mol / L. Taking the total volume of the solvent as 100%, the electrolyte includes 30% by volume of ethylene carbonate, 50% by volume of dimethyl carbonate and 20% by volume of ethyl methyl carbonate.

[0081] The additives include electrolyte additive A based on benzonitrile compounds containing 2,2,2-trifluoroethoxy groups, nitrile additives, carbonate additives, lithium salt additives, and sulfur-containing additives.

[0082] The chemical structural formula of the electrolyte additive A is shown below, and the mass percentage of the electrolyte additive A in the electrolyte is 3%.

[0083]

[0084] The nitrile additive is succinonitrile SN, and the mass percentage of succinonitrile in the electrolyte is 1%; the carbonate additive is ethylene carbonate EC, and the mass percentage of it in the electrolyte is 8%; the lithium salt additive is lithium difluorophosphate LiPO2F2, and the mass percentage of it in the electrolyte is 1%; the sulfur-containing additive is propylene sulfite PS, and the mass percentage of it in the electrolyte is 0.5wt%.

[0085] The electrolyte is prepared by the following method: under an argon atmosphere, a carbonate additive, a lithium salt additive, a sulfur-containing additive, a nitrile additive and an electrolyte additive A are added to a solvent in a formulated amount, stirred evenly, and then a lithium salt in a formulated amount is added, stirred and mixed evenly at a temperature of 10° C., to prepare the electrolyte of Example 1.

[0086] Example 2

[0087] This embodiment 2 provides an electrolyte, which includes a lithium salt, an additive and a balance solvent, wherein the lithium salt is lithium hexafluorophosphate with a concentration of 1.1 mol / L. Taking the total volume of the solvent as 100%, the electrolyte includes 30% by volume of ethylene carbonate, 50% by volume of dimethyl carbonate and 20% by volume of ethyl methyl carbonate.

[0088] The additives include electrolyte additive B based on benzonitrile compounds containing 2,2,2-trifluoroethoxy groups, nitrile additives, carbonate additives, lithium salt additives, and sulfur-containing additives.

[0089] The chemical structural formula of the electrolyte additive B is shown below, and the mass percentage of the electrolyte additive B in the electrolyte is 3%.

[0090]

[0091] The nitrile additive is succinonitrile SN, and the mass percentage of succinonitrile in the electrolyte is 1%; the carbonate additive is ethylene carbonate EC, and the mass percentage of it in the electrolyte is 8%; the lithium salt additive is lithium difluorophosphate LiPO2F2, and the mass percentage of it in the electrolyte is 1%; the sulfur-containing additive is propylene sulfite PS, and the mass percentage of it in the electrolyte is 0.5%.

[0092] The electrolyte was prepared by the following method: in an argon atmosphere, a carbonate additive, a lithium salt additive, a sulfur-containing additive, a nitrile additive and an electrolyte additive B were added to a solvent in a prescribed amount and stirred evenly. Then, a lithium salt in a prescribed amount was added, stirred and mixed evenly at a temperature of 15° C., to prepare the electrolyte of Example 2.

[0093] Example 3

[0094] Example 3 provides an electrolyte, which differs from Example 1 in that the electrolyte additive based on benzonitrile compounds used is different from that in Example 1. Example 3 uses electrolyte additive C, whose chemical structure is as follows:

[0095]

[0096] Example 4

[0097] Example 4 provides an electrolyte, which differs from Example 1 in that the concentration of the lithium salt is 3 mol / L, the amount of the electrolyte additive A is 8%, the mass percentage of the nitrile additive is 2 wt%, the mass percentage of the carbonate additive is 2%, the mass percentage of the sulfur-containing additive is 1.5%, and the mass percentage of the lithium salt additive is 0.5 wt%.

[0098] Example 5

[0099] Example 5 provides an electrolyte, which differs from Example 1 in that the concentration of the lithium salt is 2 mol / L, the amount of the electrolyte additive A is 2%, the mass percentage of the nitrile additive is 0.5wt%, the mass percentage of the carbonate additive is 5%, the mass percentage of the sulfur-containing additive is 1%, and the mass percentage of the lithium salt additive is 0.8%.

[0100] Comparative Example 1

[0101] Comparative Example 1 provides an electrolyte, which differs from Example 1 only in that the electrolyte does not contain nitrile additives, and based on the total mass of the electrolyte as 100%, the mass percentage of lithium difluorophosphate is adjusted to 1.3%, and the mass percentage of ethylene carbonate is adjusted to 13%.

[0102] Comparative Example 2

[0103] Comparative Example 2 provides an electrolyte, which differs from Example 1 only in that the electrolyte does not contain an electrolyte additive based on a benzonitrile compound containing a 2,2,2-trifluoroethoxy group. Based on the total mass of the electrolyte as 100%, the mass percentage of lithium difluorophosphate is adjusted to 1.3%, and the mass percentage of ethylene carbonate is adjusted to 13%.

[0104] Test Case

[0105] Based on the electrolyte provided in the above embodiments and comparative examples, it is applied to lithium-ion batteries, and the performance of the lithium-ion batteries is tested. The preparation method of the lithium-ion battery used for the test is as follows:

[0106] The negative electrode active material graphite, the conductive agent acetylene black and the binder sodium carboxymethyl cellulose CMC and styrene butadiene rubber SBR are prepared by mixing them in mass percentages of 95%, 1%, 2% and 2% respectively to obtain a negative electrode slurry, which is then coated on a copper foil current collector and vacuum dried to obtain a negative electrode sheet.

[0107] The positive electrode active material NCM523, the conductive agent acetylene black and the binder polyvinylidene fluoride PVDF were prepared by mixing them in a mass percentage of 94%, 4% and 2% respectively, and the prepared positive electrode slurry was coated on an aluminum foil current collector and vacuum dried to prepare a positive electrode sheet.

[0108] The positive electrode sheet, the negative electrode sheet, the separator and each electrolyte are assembled into 18650 lithium-ion batteries, and the lithium-ion batteries are electrochemically tested using a Xinwei charge and discharge test cabinet. The specific test processes involved are shown below, and the test results are shown in Table 1.

[0109] (1) Cycle performance test of lithium-ion batteries

[0110] At 25℃ / 45℃, the lithium-ion battery is charged at a constant current of 1.0C (nominal capacity) to a voltage of 4.2V, then charged at a constant voltage of 4.2V to a current ≤0.05C, left for 10 minutes, and then discharged at a constant current of 1C to 2.5V. The above is one charge and discharge cycle. The lithium-ion battery is subjected to 800 charge and discharge cycles at 25℃ / 45℃ under the above conditions.

[0111] The capacity retention rate (%) of a lithium-ion battery after N cycles = (discharge capacity at the Nth cycle / initial discharge capacity) × 100%, where N is the number of cycles of the lithium-ion battery.

[0112] (2) High temperature storage performance test of lithium-ion batteries

[0113] At 25°C, the lithium-ion battery was charged at a constant current of 1C to a voltage of 4.2V, and then charged at a constant voltage of 4.2V to a current of 0.05C, an initial capacity of C0, and an initial voltage of OCV1. The lithium-ion battery was then placed in a constant temperature box at 60°C and stored for 60 days. The lithium-ion battery was taken out and its voltage was measured to be OCV2, the capacity was maintained at C1, and the capacity recovered to C2.

[0114] Among them, the capacity retention rate (%) of the lithium-ion battery after storage at 60°C for 60 days = (C1 / C0) × 100%;

[0115] The capacity recovery rate (%) of the lithium-ion battery after storage at 60°C for 60 days = (C2 / C0)×100%.

[0116] Table 1

[0117]

[0118] The above description is only for the purpose of facilitating those skilled in the art to understand the technical solution of the present application and is not intended to limit the present application. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present application shall be included in the protection scope of the present application.

Claims

1. An electrolyte additive, characterized in that: The chemical structural formula of the electrolyte additive is as follows: Wherein, R1 and R2 are each independently selected from hydrogen, halogen, a halogenated hydrocarbon group containing 1 to 10 carbon atoms, an alkoxy group containing 1 to 10 carbon atoms or an alcoholic hydroxyl group containing 3 to 5 carbon atoms.

2. The electrolyte additive according to claim 1, characterized in that: The chemical structural formula of the electrolyte additive is shown in any of the following:

3. An electrolyte, characterized in that: The electrolyte comprises: 1 mol / L-3 mol / L of lithium salt, 2 wt%-30 wt% of additives, and the remainder of solvent; Wherein, the additives include: nitrile additives and the electrolyte additives according to any one of claims 1-2.

4. The electrolyte according to claim 3, characterized in that The mass percentage of the nitrile additive is 0.2wt%-2wt%; The mass percentage of the electrolyte additive is 2wt%-8wt%.

5. The electrolyte according to claim 3, characterized in that The nitrile additive includes at least one of carbonitrile, acetonitrile, propionitrile, butyronitrile, succinonitrile, adiponitrile, glutaronitrile, suberonitrile, 1,3,6-hexanetricarboxylic acid nitrile, 1,3,5-pentanetricarboxylic acid nitrile, p-fluorobenzonitrile, p-methylbenzonitrile, 2-fluoroadiponitrile, and 2,2-difluorosuccinonitrile.

6. The electrolyte according to claim 3, characterized in that The lithium salt is selected from at least one of lithium hexafluorophosphate, lithium difluorophosphate, lithium tetrafluoroborate, lithium perchlorate, lithium bis(oxalatoborate), lithium difluorobis(oxalatoborate), lithium bis(fluorosulfonyl)imide and lithium bis(trifluoromethylsulfonyl)imide.

7. The electrolyte according to claim 3, characterized in that The solvent includes at least one of chain carbonate, cyclic carbonate, hydroxy acid ester, sulfite and nitrite.

8. The electrolyte according to any one of claims 3 to 7, characterized in that: The additives also include: at least one of carbonate additives, sulfur-containing additives, and lithium salt additives; The mass percentage of the carbonate additive is 1wt%-10wt%; The mass percentage of the sulfur-containing additive is 0.1wt%-2wt%; The mass percentage of the lithium salt additive is 0.2wt%-1wt%.

9. The electrolyte according to claim 8, characterized in that The carbonate additive is selected from at least one of vinylene carbonate and ethylene carbonate; The sulfur-containing additive is selected from at least one of propylene sulfite, propylene-1,3-sultone, vinyl sulfate, and methylene methanedisulfonate. The lithium salt additive is selected from at least one of lithium bis(fluorosulfonyl)imide, lithium difluorophosphate, lithium bis(oxalatoborate), and lithium difluorobis(oxalatophosphate).

10. A lithium ion battery, characterized in that: The lithium-ion battery comprises: a shell, a positive electrode, a negative electrode, a separator and an electrolyte located inside the shell, and the positive electrode and the negative electrode are separated by the separator; Wherein, the electrolyte is as described in any one of claims 3-9.

Citation Information

Patent Citations

  • Non-aqueous organic high-voltage electrolyte additive, non-aqueous organic high-voltage electrolyte and lithium ion secondary battery

    CN104701570A

  • Electrolyte and preparation method and application thereof

    CN113381071A

  • Electrolyte additive for improving high-temperature and high-voltage cycling stability of lithium-rich electrode material and electrolyte

    CN117393854A

  • Electrolyte additive, electrolyte containing additive and lithium ion battery

    CN117410561A

  • Nonaqueous electrolyte and lithium secondary battery using the same

    JP2012195223A

Cited By

  • Electrolyte and electrochemical device

    CN119601774A

  • Compound containing TTF and pyridazine groups, preparation method thereof and organic photoelectric device

    CN119751481A

  • Secondary battery and electrical apparatus

    WO2026149028A1