Secondary battery and packaging method and sealing head thereof
By setting a recessed structure on the edge sealing part of the secondary battery, the problem of easy leakage of electrolyte is solved, the packaging strength and sealing performance are improved, and the long-term battery life and lightweighting of electronic products are met.
Patent Information
- Application Number
- CN202411044527.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-31
- Publication Date
- 2024-11-15
AI Technical Summary
The secondary battery can easily cause electrolyte to leak liquid during collision, resulting in battery failure, and the prior art is difficult to effectively solve the problem that seals are easily flushed.
A secondary battery is designed, and its edge sealing part includes a structure with several recesses, which increases the packaging area, improves the packaging strength, and reduces the risk of liquid leakage and thermal stress concentration through the heat diffusion effect during thermal compression packaging.
It effectively reduces the risk of liquid leakage in secondary batteries, improves packaging strength and sealing performance, optimizes heat conduction path, enhances the fit between the head and the edge, and ensures the long-term battery life and lightweight design of the battery.
Smart Images

Figure CN118970301A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the field of battery technology, and in particular to a secondary battery and a packaging method and a sealing head thereof. Background Art
[0002] With the development of electronic product technology, electronic products are increasingly pursuing thin and light designs, such as tablets, mobile phones, and e-books. Long battery life and thin and light designs have gradually become the mainstream. Secondary batteries, as the power source of electronic products, need to have a higher electrolyte retention volume to meet the needs of long battery life and thinness. However, during a collision, the electrolyte inside the secondary battery can easily break the battery seal, causing the secondary battery to leak and fail. Summary of the invention
[0003] The present application aims to provide a secondary battery and a packaging method and a sealing head thereof, aiming to improve the technical problem that the battery seal is easily broken.
[0004] The embodiment of the present application adopts the following technical solutions:
[0005] In the first aspect, the present application proposes a secondary battery, including a packaging bag and an electrode assembly, the packaging bag including a main body and an edge sealing portion that encapsulates the main body, the electrode assembly is arranged in the main body, the edge sealing portion includes a first edge sealing portion connected to the main body, along the thickness direction of the first edge sealing portion, the first edge sealing portion includes a first surface and a second surface that are arranged opposite to each other, the first surface is provided with a plurality of first recessed portions, and the first recessed portions are recessed toward the second surface.
[0006] In the above technical solution, the setting of the first recessed portion increases the packaging area of the first edge seal. Compared with the plane, the first recessed portion can make the layers of the first edge seal fit more closely, reduce the gap, improve the packaging strength of the first edge seal, and effectively reduce the risk of leakage of the secondary battery. At the same time, the heat conduction path can be optimized. The convex portion of the head can penetrate through the first recessed portion, so that the head seal is closer to the various layers of the first edge seal, and the heat during hot pressing packaging can be effectively conducted to the various layers of the first edge seal, and the hot pressing packaging is more sufficient, thereby improving the efficiency and effect of hot pressing packaging. In addition, the setting of the first recessed portion has a better heat diffusion effect during hot pressing packaging. When the head seal contacts the first recessed portion, the heat will first be absorbed and accumulated. As the heat continues to accumulate, the heat will gradually diffuse to the surroundings of the first recessed portion, forming a heat diffusion effect. The temperature around the first recessed portion rises rapidly, which can facilitate the temperature of each part of the first edge seal to be consistent, and can reduce the problems of thermal stress concentration and deformation caused by temperature differences in the first edge seal.
[0007] In some preferred embodiments, the edge seal also includes a second edge seal, the first edge seal is connected between the main body and the second edge seal, and the second edge seal is folded toward the first surface or the second surface. The structure of multiple folded edges can further improve the sealing performance of the secondary battery, improve the mechanical strength and stability of the packaging bag, and multiple folded edges can ensure that the edge seal will not occupy the space in the thickness direction of the secondary battery after folding, which is more conducive to adapting to ultra-thin secondary batteries.
[0008] In some preferred embodiments, along the thickness direction of the second edge seal, the second edge seal has a third surface and a fourth surface that are arranged opposite to each other, the third surface is connected to the first surface, and the fourth surface is connected to the second surface. The third surface is provided with a plurality of second recessed portions, and the second recessed portions are recessed toward the fourth surface, thereby improving the packaging strength of the second edge seal and further reducing the risk of leakage of the secondary battery.
[0009] In some preferred embodiments, the second surface is a flat surface, which allows the first recessed portion to be closer to the two sealing layers, facilitates the diffusion of heat in the two sealing layers, and is beneficial to the bonding of the first sealing layer and the second sealing layer. At the same time, the second surface is flatly arranged, so that the raised portion on the head can serve as a support, thereby reducing overpressure on the first edge seal.
[0010] In some preferred embodiments, the first surface has a first flat portion, and a first flat portion is arranged between two adjacent first recessed portions. The combination of the first recessed portion and the first flat portion can improve the packaging strength of the first edge seal, and the first flat portion can be in contact with the entire surface of the head, which can facilitate the raised portion on the head to penetrate into the first edge seal to a predetermined position, thereby reducing excessive hot pressing of the raised portion 2 on the first edge seal and reducing hot pressing damage to the first edge seal.
[0011] In some preferred embodiments, the secondary battery includes a tab, one end of which is electrically connected to the electrode assembly, and the other end of which extends out of the packaging bag from the flat portion of the first edge seal. The first flat portion can serve as a circumvention of the tab for the first recessed portion, which is beneficial for the extension of the tab.
[0012] In some preferred embodiments, along the thickness direction of the first edge seal, the first edge seal includes a first part and a second part that are arranged opposite to each other. The first part includes a first protective layer, a first sealing layer, and a first metal layer arranged between the first protective layer and the first sealing layer. The second part includes a second protective layer, a second sealing layer, and a second metal layer arranged between the second protective layer and the second sealing layer. The first sealing layer is bonded to the second sealing layer, and the first recessed portion is arranged on the surface of the first protective layer away from the second part. In the first flattened portion, along the thickness direction of the first edge seal, the thickness of the first protective layer is T1, the thickness of the first metal layer is T2, the thickness of the first sealing layer is T3, and the thickness of the second sealing layer is T4. Along the thickness direction of the first edge seal, the depth of the first recessed portion is H, T1+T2≤H≤T1+T2+T3+T4. The first recessed portion at least reaches the first metal layer, which has a high thermal conductivity, and can facilitate the transfer or diffusion of heat. The first recessed portion can also reach the first sealing layer and / or the second sealing layer, and can facilitate the direct transfer of heat to the first sealing layer and / or the second sealing layer, which is beneficial to the bonding of the first sealing layer and the second sealing layer. In addition, the first recessed portion does not exceed the second metal layer, and the second metal layer has a higher strength, which can reduce the bending, tearing or damage of the first sealing edge.
[0013] In some preferred embodiments, along the thickness direction of the first edge seal, the depth of the first recessed portion is H, 0.02T≤H≤0.2T, T is the thickness of the secondary battery, so as to reduce the influence of the first edge seal on the width of the secondary battery when folding.
[0014] In some preferred embodiments, along the width direction of the first edge seal, the maximum width of the first recessed portion is W, 0.3W1≤W≤0.85W1, W1 is the width of the first edge seal, which can improve the heat diffusion effect while reducing the risk of damage and tearing of the first edge seal and improve the packaging strength of the first edge seal.
[0015] In some preferred embodiments, the distance between two adjacent first recessed portions is S, and 0.1W≤S≤W, which can facilitate heat diffusion and folding of the first edge seal.
[0016] In some preferred embodiments, the first recessed portion includes a peripheral wall, a bottom wall, and an arc-shaped chamfered surface connecting the peripheral wall and the bottom wall. The radius of the arc-shaped chamfered surface is R, 0.0015T≤R≤0.15T, T is the thickness of the secondary battery, which can not only reduce the damage and tearing of the first edge seal 121 and improve the packaging strength, but also effectively disperse the stress.
[0017] In some preferred embodiments, the peel strength between the first portion and the second portion is G, 1 N / mm≤G≤5 N / mm.
[0018] In some preferred embodiments, along the width direction of the first edge seal, the first edge seal has a first edge and a second edge that are arranged opposite to each other, and the first edge is connected to the main body. The distance between the first edge and the first recessed portion is L1, 0.25mm≤L1≤0.75mm, which can facilitate the folding of the first edge seal while reducing the impact of the first edge seal on the energy density of the secondary battery. The distance between the second edge and the first recessed portion is L2, 0.25mm≤L2≤0.75mm. When the second edge seal 122 is present, a secondary folding is required, and the limit of 0.25mm≤L2≤0.75mm can facilitate the folding process of the secondary folding and reduce the impact of the folding on the energy density of the secondary battery.
[0019] In the second aspect, the present application further proposes a sealing head for hot pressing and packaging a secondary battery as described in any embodiment of the first aspect, the sealing head comprising a first sealing head and a second sealing head. The first sealing head has a fifth surface, the fifth surface is provided with a plurality of raised portions, and a second flat portion is provided between two adjacent raised portions. The second sealing head has a sixth surface, and the sixth surface faces the fifth surface.
[0020] In the third aspect, the present application also proposes a packaging method, characterized in that it includes a secondary battery as described in any embodiment of the first aspect and a head as described in any embodiment of the second aspect. The method includes the following steps: placing the first head and the second head on both sides of the first edge seal thickness direction, respectively, with the fifth surface of the first head facing the first surface of the first edge seal, and the sixth surface of the second head facing the second surface; the first head and the second head are hot-pressed to form the first edge seal, the convex part is hot-pressed to form the first concave part on the first surface, and the second flat part is hot-pressed to form the first flat part on the first surface.
[0021] Additional aspects and advantages of the embodiments of the present application will be described, shown, or explained in part in the subsequent description through implementation of the embodiments of the present application. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] One or more embodiments are exemplarily described by corresponding drawings, which do not constitute limitations on the embodiments. Elements with the same reference numerals in the drawings represent similar elements, and the figures in the drawings do not constitute proportional limitations unless otherwise stated.
[0023] Figure 1 A schematic diagram of the structure of a secondary battery in some embodiments of the present application;
[0024] Figure 2 An exploded schematic diagram of a secondary battery according to some embodiments of the present application;
[0025] Figure 3 Schematic diagram of the structure of each layer of the first bag body and the second bag body in some embodiments of the present application;
[0026] Figure 4 This is a schematic structural diagram of the first edge sealing in some embodiments of the present application;
[0027] Figure 5 A schematic diagram of the structure of a secondary battery in some embodiments of the present application;
[0028] Figure 6 A schematic diagram of the structure of a secondary battery (secondary folding structure) according to some embodiments of the present application;
[0029] Figure 7 Schematic diagram of the secondary folding structure of some embodiments of the present application;
[0030] Figure 8 Schematic diagram of the secondary folding structure of some embodiments of the present application;
[0031] Fig. 9 Schematic diagram of the secondary folding structure of some embodiments of the present application (straight state);
[0032] Fig.10 Schematic diagram of the structure of each layer of the first edge sealing of some embodiments of the present application;
[0033] Fig.11 This is a schematic structural diagram of the first edge sealing in some embodiments of the present application;
[0034] Fig.12 A cross-sectional view of a first edge seal of some embodiments of the present application;
[0035] Fig.13 This is a schematic diagram of the structure of the head of some embodiments of the present application;
[0036] Fig.14 This is a schematic diagram of hot pressing of a first edge seal by a sealing head in some embodiments of the present application.
[0037] Description of reference numerals:
[0038] 100. Secondary battery;
[0039] 10. Packaging bags;
[0040] 11. Main body; 10a. First bag body; 10a1. First cavity; 10a2. First protective layer; 10a3. First metal layer; 10a4. First sealing layer; 10b. Second bag body; 10b1. Second cavity; 10b2. Second protective layer; 10b3. Second metal layer; 10b4. Second sealing layer;
[0041] 12, edge sealing portion; 12a, top edge sealing; 12b, first side edge sealing; 12c, second side edge sealing; 121, first edge sealing; 1211, first surface; 1212, second surface; 1213, first recessed portion; 12131, peripheral wall; 12132, bottom wall; 12133, arc chamfered surface; 1214, first flat portion; 1215, first edge; 1216, second edge; 122, second edge sealing; 1221, third surface; 1222, fourth surface; 1223, second recessed portion;
[0042] 20. Electrode assembly;
[0043] 30. Tab; 31. Positive tab; 32. Negative tab;
[0044] 200, end cap; 210, first end cap; 211, fifth surface; 212, raised portion; 213, second flat portion; 220, second end cap; 221, sixth surface;
[0045] X, first direction; Y, second direction; Z, third direction; M, fourth direction; N, fifth direction; Q, sixth direction. DETAILED DESCRIPTION
[0046] In order to make the purpose, technical solutions and advantages of the embodiments of the present application clearer, the technical solutions in the embodiments of the present application will be clearly described below in conjunction with the drawings in the embodiments of the present application. Obviously, the described embodiments are only part of the embodiments of the present application, not all of the embodiments.
[0047] Reference to "embodiment" in this application means that a particular feature, structure, or characteristic described in conjunction with the embodiment may be included in at least one embodiment of the present application. The appearance of the phrase in various places in the specification does not necessarily refer to the same embodiment, nor is it an independent or alternative embodiment that is mutually exclusive with other embodiments.
[0048] In the description of the embodiments of the present application, the technical terms "first", "second", etc. are only used to distinguish different objects, and cannot be understood as indicating or implying relative importance or implicitly indicating the number, specific order or primary and secondary relationship of the indicated technical features. In the description of the embodiments of the present application, the meaning of "multiple" is more than two, unless otherwise clearly and specifically defined.
[0049] In the description of the embodiments of the present application, the term "and / or" is only a description of the association relationship of the associated objects, indicating that there may be three relationships. For example, A and / or B can represent: A exists alone, A and B exist at the same time, and B exists alone. In addition, the character " / " in this article generally indicates that the associated objects before and after are in an "or" relationship.
[0050] The technical features involved in the different embodiments of the present application described below can be combined with each other as long as they do not conflict with each other.
[0051] In the first aspect, the present application proposes a secondary battery 100, please refer to Figure 1 and Figure 2 The secondary battery 100 includes a packaging bag 10, an electrode assembly 20 and a tab 30. The electrode assembly 20 is arranged in the packaging bag 10. One end of the tab 30 is electrically connected to the electrode assembly 20 in the packaging bag 10, and the other end extends out of the packaging bag 10. The tab 30 includes a positive tab 31 and a negative tab 32, which are used to lead out the positive and negative electrodes of the secondary battery 100.
[0052] For the above packaging bag 10, please refer to Figure 1 and Figure 2 The packaging bag 10 includes a main body 11 and a sealing edge 12. The main body 11 encloses a receiving cavity (not shown in the figure), which can accommodate the electrode assembly 20 and the electrolyte (not shown in the figure). The sealing edge 12 can be arranged on the side of the main body 11 to encapsulate the receiving cavity of the main body 11 to prevent the electrolyte from leaking.
[0053] For example, the packaging bag 10 includes a first bag body 10a and a second bag body 10b that are arranged opposite to each other, the first bag body 10a is provided with a first pit cavity 10a1, and the second bag body 10b is provided with a second pit cavity 10b1. The electrode assembly 20 can be placed in the first pit cavity 10a1 or the second pit cavity 10b1, and one end of the tab 30 is electrically connected to the electrode assembly 20, and the other end extends out of the first pit cavity 10a1 and the second pit cavity 10b1. The second pit cavity 10b1 of the second bag body 10b is arranged opposite to the first pit cavity 10a1, and the edges of the first bag body 10a and the second bag body 10b are hot-pressed to connect the first bag body 10a and the second bag body 10b, and the first pit cavity 10a1 and the second pit cavity 10b1 are communicated to form a receiving cavity. The portion enclosed to form the accommodating cavity is the main body 11 , and the edges of the first bag body 10 a and the second bag body 10 b form a sealed edge portion 12 after hot pressing. The sealed edge portion 12 can improve the sealing performance of the packaging bag 10 .
[0054] In some other embodiments, the second bag body 10b may not be provided with the second cavity 10b1, and the second bag body 10b may directly adopt a flat structure, directly covering the cavity of the first bag body 10a, and after hot pressing packaging, the first cavity 10a1 may be directly made to form a receiving cavity. Alternatively, the first bag body 10a is not provided with the first cavity 10a1, and only the second bag body 10b is provided with the second cavity 10b1, and the second cavity 10b1 forms a receiving cavity.
[0055] Please refer to Figure 2 and Figure 3The first bag body 10a includes a first protective layer 10a2, a first sealing layer 10a4 and a first metal layer 10a3, and the first metal layer 10a3 is arranged between the first protective layer 10a2 and the first sealing layer 10a4. The second bag body 10b includes a second protective layer 10b2, a second sealing layer 10b4 and a second metal layer 10b3, and the second metal layer 10b3 is arranged between the second protective layer 10b2 and the second sealing layer 10b4. The first protective layer 10a2 and the second protective layer 10b2 can be made of polypropylene, polyethylene, polyamide, polyvinylidene chloride, etc., which have better barrier properties and can effectively block external water vapor. The first metal layer 10a3 and the second metal layer 10b3 can be made of metals such as aluminum, copper or stainless steel, which can improve the thermal conductivity and mechanical strength of the packaging bag 10. The first sealing layer 10a4 and the second sealing layer 10b4 can be made of cast polypropylene, blown polypropylene, linear low-density polyethylene, and ethylene-methacrylate copolymer, etc., which have good hot air performance and chemical resistance. During hot pressing packaging, the first sealing layer 10a4 faces the second sealing layer 10b4, which can directly make the first sealing layer 10a4 and the second sealing layer 10b4 bonded, so that the first bag body 10a and the second bag body 10b form a complete packaging bag 10.
[0056] In the embodiments of this application, please refer to Figure 1 , Figure 4 and Figure 5 The edge seal 12 includes a first edge seal 121. The first edge seal 121 may be a top edge seal 12a (the edge seal extending from the tab 30 is usually regarded as the top edge seal), a first side edge seal 12b, a second side edge seal 12c, or a bottom edge seal in other embodiments. Along the thickness direction (third direction Z) of the first edge seal 121, the first edge seal 121 includes a first surface 1211 and a second surface 1212 that are arranged opposite to each other. The first surface 1211 is provided with a plurality of first recessed portions 1213, and the first recessed portions 1213 are recessed toward the second surface 1212. The sealing head 200 (refer to Fig.13 ) The first edge seal 121 is hot-pressed and packaged, and a convex portion 212 is correspondingly provided on the sealing head 200. During the hot-pressing packaging, a first concave portion 1213 can be directly formed on the first edge seal 121.
[0057] The first recessed portion 1213 is provided to increase the packaging area of the first edge seal 121. Compared with a plane, the first recessed portion 1213 can make the layers of the first edge seal 121 fit more closely, reduce the gap, improve the packaging strength of the first edge seal 121, and effectively reduce the risk of leakage of the secondary battery 100. At the same time, the heat conduction path can be optimized, and the raised portion 212 of the head 200 can penetrate through the first recessed portion 1213, so that the head 200 is closer to the various layers of the first edge seal 121, and the heat during hot pressing packaging can be effectively conducted to the various layers of the first edge seal 121, so that the hot pressing packaging is more sufficient, and the hot pressing packaging efficiency and hot pressing packaging effect are improved. In addition, the setting of the first recessed portion 1213 has a better heat diffusion effect during hot pressing packaging. When the head 200 contacts the first recessed portion 1213, the heat will be absorbed and accumulated first. As the heat continues to accumulate, the heat will gradually diffuse to the surroundings of the first recessed portion 1213, forming a heat diffusion effect. The temperature around the first recessed portion 1213 rises rapidly, which can facilitate the temperature of various parts of the first edge seal 121 to tend to be consistent, and can reduce the thermal stress concentration and deformation of the first edge seal 121 caused by temperature differences.
[0058] For the above-mentioned edge sealing portion 12, the edge sealing portion 12 can adopt a single folding, and in some other embodiments, multiple folding such as double folding and triple folding can also be adopted. The structure of multiple folding can further improve the sealing performance of the secondary battery 100, improve the mechanical strength and stability of the packaging bag 10, and multiple folding can make the edge sealing portion 12 not occupy the space in the thickness direction (fourth direction M) of the secondary battery 100 after folding, which is more conducive to adapting to the ultra-thin secondary battery 100.
[0059] Taking the secondary folding as an example, the edge sealing portion 12 also includes a second edge sealing 122, please refer to Figures 6 to 8 The first edge seal 121 is connected between the main body 11 and the second edge seal 122, and the second edge seal 122 is folded toward the first surface 1211 or the second surface 1212. The second edge seal 122 may be provided with a second recessed portion 1223. For example, along the thickness direction of the second edge seal 122, the second edge seal 122 has a third surface 1221 and a fourth surface 1222 that are relatively arranged, and the third surface 1221 is provided with a plurality of second recessed portions 1223, and the second recessed portions 1223 are recessed toward the fourth surface 1222, thereby improving the packaging strength of the second edge seal 122 and further reducing the risk of leakage of the secondary battery 100.
[0060] Optionally, the third surface 1221 is connected to the first surface 1211, and the fourth surface 1222 is connected to the second surface 1212. When not folded, the first edge seal 121 is connected to the second edge seal 122 and presents a straight state (see Fig. 9), the first edge seal 121 and the second edge seal 122 can be simultaneously hot-pressed by the sealing head 200, that is, a first recessed portion 1213 is formed on the first edge seal 121, and a second recessed portion 1223 is formed on the second edge seal 122. The second edge seal 122 is folded toward the first edge seal 121, and then the first edge seal 121 and the second edge seal 122 are folded toward a side wall of the main body 11, so as to form a secondary folding structure.
[0061] In some embodiments, a first recessed portion 1213 is provided on the first surface 1211 of the first edge seal 121, and a second recessed portion 1223 is provided on the third surface 1221 of the second edge seal 122. After the second edge seal 122 is folded toward the first edge seal 121, the first surface 1211 and the third surface 1221 are arranged opposite to each other, and then the first recessed portion 1213 is directly covered by the second edge seal 122, and the second recessed portion 1223 is covered by the first edge seal 121, thereby reducing the accumulation of impurities such as dust in the first recessed portion 1213 and the second recessed portion 1223.
[0062] In some other embodiments, the edge sealing portion 12 may also adopt a multiple folding structure such as triple folding, quadruple folding, etc., and the triple folding, quadruple folding, etc. may also be arranged similarly to the double folding.
[0063] The second surface 1212 may also be provided with a first recessed portion 1223, or, in some embodiments, the second surface 1212 is a flat surface. During hot pressing packaging, the raised portion 212 of the sealing head 200 first contacts and hot presses the first edge seal 121. After the raised portion 212 penetrates to a certain depth, the first recessed portion 1213 may be directly formed on the first edge seal 121. The flat setting of the second surface 1212 can facilitate the first recessed portion 1213 to be closer to the two sealing layers (the first sealing layer 10a4 and the second sealing layer 10b4), facilitate the diffusion of heat in the two sealing layers, and facilitate the bonding of the first sealing layer 10a4 and the second sealing layer 10b4, thereby improving the packaging strength of the first edge seal 121. At the same time, the flat setting of the second surface 1212 can make the raised portion 212 on the sealing head 200 serve as a support to reduce the overpressure of the first edge seal 121.
[0064] In some embodiments, please refer to Figure 4, the first surface 1211 has a first flat portion 1214, and a first flat portion 1214 is provided between two adjacent first recessed portions 1213. During hot pressing, the raised portion 212 on the sealing head 200 first contacts and hot presses the first edge seal 121, and after the raised portion 212 penetrates into the first edge seal 121 to a certain depth, the first flat portion 1214 between the two sealing heads 200 can be hot pressed against the first edge seal 121. The combination of the first recessed portion 1213 and the first flat portion 1214 can improve the packaging strength of the first edge seal 121, and the first flat portion 1214 can contact the entire surface of the sealing head 200, which can facilitate the raised portion 212 on the sealing head 200 to penetrate into the first edge seal 121 to a predetermined position, thereby reducing excessive hot pressing of the raised portion 212 on the first edge seal 121 and reducing hot pressing damage of the first edge seal 121.
[0065] Please refer to further Figure 5 The packaging bag 10 includes a top seal 12a, a first side seal 12b and a second side seal 12c. The tab 30 extends from the top seal 12a. Along the width direction (fifth direction N) of the packaging bag 10, the first side seal 12b and the second side seal 12c are arranged opposite to each other. The first seal 121 can be used as the top seal 12a, or as the first side seal 12b or the second side seal 12c. When the first seal 121 is used as the top seal 12a, one end of the tab 30 is electrically connected to the electrode assembly 20, and the other end can extend directly from the first flat portion 1214 of the first seal 121 to the packaging bag 10. The setting of the first flat portion 1214 is conducive to the extension of the tab 30, and the setting of the first recessed portion 1213 can improve the packaging strength of the first seal 121.
[0066] When the first edge seal 121 is used as the first side edge seal 12b or the second side edge seal 12c, the combination of the first straight portion 1214 and the first recessed portion 1213 can improve the strength of the first edge seal 121 to a certain extent, and improve the packaging strength of the first edge seal 121. Optionally, in some other embodiments, the packaging bag 10 further includes a bottom edge seal (not shown in the figure), and along the length direction (sixth direction Q) of the packaging bag 10, the top edge seal 12a is arranged opposite to the bottom edge seal, and the first edge seal 121 can also be used as the bottom edge seal.
[0067] In some embodiments, please refer to Fig.10, along the thickness direction (third direction Z) of the first edge seal 121, the first edge seal 121 includes a first portion 121a and a second portion 121b arranged opposite to each other, wherein the first portion 121a is a portion of the first bag body 10a, and the second portion 121b is a portion of the second bag body 10b. After hot pressing and packaging, the first portion 121a and the second portion 121b are bonded to form the first edge seal 121. In the embodiment of the present application, by providing the first recessed portion 1213 on the first edge seal 121, the peeling strength between the first portion 121a and the second portion 121b can be improved, and the leakage risk of the secondary battery 100 can be effectively reduced. For example, the peeling strength between the first portion 121a and the second portion 121b is G, which can make 1N / mm≤G≤5N / mm, or even higher.
[0068] The first portion 121a includes a first protective layer 10a2, a first sealing layer 10a4, and a first metal layer 10a3 disposed between the first protective layer 10a2 and the first sealing layer 10a4. The second portion 121b includes a second protective layer 10b2, a second sealing layer 10b4, and a second metal layer 10b3 disposed between the second protective layer 10b2 and the second sealing layer 10b4.
[0069] The first sealing layer 10a4 is bonded to the second sealing layer 10b4. After hot pressing, the first sealing layer 10a4 is bonded to the second sealing layer 10b4, so that the first part 121a and the second part 121b are connected as a whole to form the first edge seal 121. The first recessed portion 1213 can be provided on the surface of the first protective layer 10a2 away from the second part 121b (the first surface 1211 of the first edge seal 121). In the first flattened portion 1214, along the thickness direction of the first edge seal 121 (the third direction Z), the thickness of the first protective layer 10a2 is T1, the thickness of the first metal layer 10a3 is T2, the thickness of the first sealing layer 10a4 is T3, and the thickness of the second sealing layer 10b4 is T4. Along the thickness direction of the first edge seal 121 (the third direction Z), the depth of the first recessed portion 1213 is H, and T1+T2≤H≤T1+T2+T3+T4. That is, the first recessed portion 1213 at least penetrates into the first metal layer 10a3, and the first metal layer 10a3 has a high thermal conductivity, which can facilitate the transfer or diffusion of heat, and the first recessed portion 1213 can also penetrate into the first sealing layer 10a4 and / or the second sealing layer 10b4, which can facilitate the direct transfer of heat to the first sealing layer 10a4 and / or the second sealing layer 10b4, which is beneficial to the bonding of the first sealing layer 10a4 and the second sealing layer 10b4. In addition, the first recessed portion 1213 does not exceed the second metal layer 10b3, and the second metal layer 10b3 has a high strength, which can reduce the bending, tearing or damage of the first edge seal 121.
[0070] For the measurement of the depth of the first recessed portion 1213, the depth of each first recessed portion 1213 can be detected by a line laser scanner, or the height of the protrusion 212 on the head 200 can be detected, and the depth of the first recessed portion 1213 or the height of the protrusion 212 can be calculated using the triangulation principle to ensure that the parameters such as the depth of each first recessed portion 1213 / height of the protrusion 212, spacing and diameter are within the specified range.
[0071] For the measurement of the thickness of each layer of edge banding, a high-magnification optical microscope with a measuring function can be used to observe the cross-section of each layer and measure the thickness of each layer by measuring the interlayer distance in the image.
[0072] In some other embodiments, along the thickness direction of the first edge seal 121 (third direction Z), the depth of the first recessed portion 1213 is H, 0.02T≤H≤0.2T, T is the thickness of the secondary battery 100, and the depth of the first recessed portion 1213 is too small, and it is difficult to penetrate into the metal layer, which is not conducive to heat diffusion and the hot pressing packaging effect is not good. If the depth of the first recessed portion 1213 is too large, it may cause the first edge seal 121 to be relatively weak, and may cause the first edge seal 121 to be torn and damaged when folded, which is not conducive to improving the packaging strength of the first edge seal 121. In addition, the present application also stipulates that the depth of the first recessed portion 1213 is less than 0.2T, reducing the impact of the first edge seal 121 on the width of the secondary battery 100 when folding.
[0073] Please refer to Figure 4 and Fig.11 , a single row or multiple rows of first recessed portions 1213 may be provided on the first edge seal 121 (a plurality of first recessed portions 1213 along the length direction / second direction Y of the first edge seal 121 is called a row, and the corresponding head seal may also be provided with a single row or multiple rows of raised portions). With respect to the width of the first recessed portion 1213, in some embodiments, the maximum width of the first recessed portion 1213 is W, 0.3W1≤W≤0.85W1, and if the width of the first recessed portion 1213 is too small, the hot pressing contact area between the head seal 200 and the first edge seal 121 may be small, and the heat diffusion effect may be poor. If the width of the first recessed portion 1213 is too large, the recessed portion may occupy a larger area of the first edge seal 121, which may weaken the strength of the first edge seal 121 and easily cause the first edge seal 121 to be damaged or torn. In the present application, 0.3W1≤W≤0.85W1 is defined, which can improve the heat diffusion effect while reducing the risk of damage and tearing of the first edge seal 121 and improving the packaging strength of the first edge seal 121.
[0074] In some embodiments, please refer to Fig.11, the distance between two adjacent first recesses 1213 is S, 0.1W≤S≤W, and if the spacing is too wide, it may lead to insufficient heat diffusion. During hot pressing packaging, it is difficult for heat to be transferred to various parts of the first edge seal 121 in a short time. If the spacing is reduced, the first recesses 1213 will be too dense, which may cause the folding of the first edge seal 121 to be damaged, which is not conducive to the folding of the first edge seal 121, and may cause hot melt adhesive bridging between two adjacent first recesses 1213, affecting the packaging quality. In this application, the limitation of 0.1W≤S≤W can facilitate the folding of the first edge seal 121 while facilitating heat diffusion, and can also reduce hot melt adhesive bridging.
[0075] When only one row of first recessed portions 1213 is provided on the first sealing edge 121, please refer to Figure 4 , along the length direction (second direction Y) of the first edge seal 121, the distance between two adjacent first recessed portions 1213 must satisfy 0.1W≤S≤W. When multiple rows of first recessed portions 1213 are provided on the first edge seal 121, please refer to Fig.11 , along the length direction of the first edge seal 121 (the second direction Y), and along the width direction of the first edge seal 121 (the first direction X), the distance between two adjacent first recessed portions 1213 must satisfy 0.1W≤S≤W.
[0076] In some embodiments, please refer to Fig.11 , along the width direction (first direction X) of the first edge seal 121, the first edge seal 121 has a first edge 1215 and a second edge 1216 that are arranged opposite to each other, and the first edge 1215 is connected to the main body 11. The distance between the first edge 1215 and the first recessed portion 1213 is L1, 0.25mm≤L1≤0.75mm. If the distance between the first recessed portion 1213 and the first edge 1215 is too small, when the first edge seal 121 is folded, it may cause the crease to often contact the first recessed portion 1213, causing the first recessed portion 1213 to interfere with the folding of the first edge seal 121. If the distance between the first recessed portion 1213 and the first edge is too large, after the first edge seal 121 is folded, it may cause the first edge seal 121 to exceed the thickness of the secondary battery 100, affecting the energy density of the secondary battery 100. In the embodiment of the present application, 0.25 mm ≤ L1 ≤ 0.75 mm is defined, which can facilitate the folding of the first edge seal 121 and reduce the influence of the first edge seal 121 on the energy density of the secondary battery 100 .
[0077] In some other embodiments, the distance between the second edge 1216 and the first recessed portion 1213 is L2, 0.25mm≤L2≤0.75mm. For example, when the second edge seal 122 is present, secondary folding is required, and the limit of 0.25mm≤L2≤0.75mm can facilitate the folding process of the secondary folding and reduce the impact of the folding on the energy density of the secondary battery 100.
[0078] Regarding the shape of the first recessed portion 1213, the first recessed portion 1213 may be columnar, prism-shaped, or conical. Taking the columnar first recessed portion 1213 as an example, please refer to Fig.12 The first recessed portion 1213 includes a peripheral wall 12131, a bottom wall 12132, and an arc-shaped chamfered surface 12133 connecting the peripheral wall 12131 and the bottom wall 12132. The arc-shaped chamfered surface 12133 is more conducive to uniformly dispersing stress, reducing the influence of the first recessed portion 1213 on the strength of the first edge seal 121, and reducing the damage and tearing at the first recessed portion 1213. At the same time, during hot pressing packaging, by providing a protruding portion 212 with an arc-shaped chamfered surface 12133 on the sealing head 200, during hot pressing, the first recessed portion 1213 with an arc-shaped chamfered surface 12133 can be directly formed on the first edge seal 121, and the protruding portion 212 with an arc-shaped chamfered surface 12133 on the sealing head 200 is in smooth contact with the first edge seal 121, which can reduce the crimping damage to the first edge seal 121.
[0079] For the radius of the arc chamfered surface 12133, if the radius is too large or too small, it may be difficult to fully disperse the stress. In this application, 0.0015T≤R≤0.15T is limited, which can not only reduce the damage and tearing of the first edge seal 121, improve the packaging strength, but also effectively disperse the stress. Among them, R is the radius of the arc chamfered surface 12133 itself or the radius of the fitting circle where the arc chamfered surface 12133 is located.
[0080] In a second aspect, the present application further proposes a sealing head 200 for hot pressing and packaging the secondary battery 100 as described in any embodiment of the first aspect. Fig.13 and Fig.14 The end cap 200 includes a first end cap 210 and a second end cap 220. The first end cap 210 has a fifth surface 211, and the fifth surface 211 is provided with a plurality of protrusions 212, and a second flat portion 213 is provided between two adjacent protrusions 212. The second end cap 220 has a sixth surface 221, and the sixth surface 221 faces the fifth surface 211.
[0081] During hot pressing packaging, the first edge seal 121 can be placed between the first head 210 and the second head 220, and the raised portion 212 is first contacted with the first edge seal 121 for hot pressing. After the raised portion 212 penetrates to a certain depth, a first recessed portion 1213 is directly formed on the first edge seal 121. The raised portion 212 can quickly transfer heat to each layer structure of the first edge seal 121.
[0082] The setting of the raised portion 212 increases the contact area between the sealing head 200 and the first edge seal 121. Compared with the plane contact, the raised portion 212 can fit the first edge seal 121 more closely, reduce the gap, and thus improve the efficiency of heat transfer. The raised portion 212 plays the role of a "bridge" in the hot pressing packaging process, effectively transferring the heat generated by the heat source to the various layers of the first edge seal 121. The heat sealing pressure of the raised portion 212 and the first edge seal 121 is more reasonable, which helps to maintain the stability of the first edge seal 121, helps to improve the sealing performance of the first edge seal 121, and ensures the safety and reliability of the secondary battery 100. At the contact point between the raised portion 212 and the first edge seal 121, the heat will first be absorbed and accumulated. As the heat continues to accumulate, the heat will gradually diffuse to the surroundings, forming a heat diffusion effect. The heat diffusion effect causes the temperature of the various layers of the structure around the raised portion 212 to gradually increase and tend to be consistent. Such temperature uniformity helps to reduce problems such as thermal stress concentration or deformation of the first edge sealing 121 caused by temperature differences, thereby improving the overall performance and stability of the secondary battery 100 .
[0083] In a third aspect, the present application further proposes a packaging method, using the secondary battery 100 as described in any embodiment of the first aspect and the sealing head 200 as described in any embodiment of the second aspect. The method comprises the following steps:
[0084] The first end cap 210 and the second end cap 220 are respectively placed on both sides of the first edge seal 121 in the thickness direction, the fifth surface 211 of the first end cap 210 faces the first surface 1211 of the first edge seal 121, and the sixth surface 221 of the second end cap 220 faces the second surface 1212;
[0085] The first sealing head 210 and the second sealing head 220 heat press the first edge seal 121 , the raised portion 212 heat presses the first edge seal 121 to form a first recessed portion 1213 on the first surface 1211 , and the second flattened portion 213 heat presses the first edge seal 121 to form a first flattened portion 1214 on the first surface 1211 .
[0086] The raised portion 212 serves as the main contact point of the heat source during the hot pressing packaging process, and helps to transfer heat more fully to the various layers of the first edge sealing 121 by increasing the contact area, optimizing the heat conduction path, and generating a heat diffusion effect. This heat transfer is effective in improving the packaging strength, safety, and reliability of the secondary battery 100.
[0087] Example 1
[0088] <Preparation of positive electrode sheet>:
[0089] The positive electrode active material lithium iron phosphate, the positive electrode conductive agent acetylene black, and the positive electrode binder polyvinylidene fluoride (PVDF, weight average molecular weight 5×10 5 ) were mixed in a mass ratio of 94:3:3, N-methylpyrrolidone (NMP) was added as a solvent, and the mixture was stirred in a vacuum mixer until the solid content was 75wt% and the system was uniform. An aluminum foil with a thickness of 8um was selected as the positive current collector, and the positive electrode slurry was evenly coated on one surface of the positive current collector aluminum foil, and dried at 110°C to obtain a positive electrode sheet with a single-sided positive electrode active material layer (thickness 80μm). After that, the above steps were repeated on the other surface of the aluminum foil to obtain a positive electrode sheet with a double-sided positive electrode active material layer.
[0090] <Preparation of negative electrode sheet>
[0091] The negative electrode active material graphite powder, silicon powder, conductive carbon black (Super P), and binder styrene-butadiene rubber (SBR) are mixed in a weight ratio of 87:10.5:1:1.5, and then deionized water is added as a solvent to prepare a negative electrode slurry with a solid content of 50wt%, and stirred evenly. A copper foil with a thickness of 5μm is selected as the negative electrode current collector, and the negative electrode slurry is evenly coated on one surface of the negative electrode current collector copper foil, and dried at 90°C to obtain a single-sided negative electrode sheet. After the above steps are completed, the single-sided coating of the negative electrode sheet has been completed. After that, the above steps are repeated on the other surface of the negative electrode sheet to obtain a negative electrode sheet with a double-sided coating of the negative electrode active material layer.
[0092] <Preparation of Separator Film>
[0093] A polyethylene (PE) porous film with a thickness of 7 μm was used as the isolation membrane.
[0094] <Electrolyte Preparation>
[0095] In a dry argon atmosphere, ethylene carbonate, ethyl methyl carbonate and diethyl carbonate were mixed in a mass ratio of 30:50:20 to obtain an organic solution, and then lithium hexafluorophosphate was added to the organic solvent to dissolve and mix evenly to obtain an electrolyte with a lithium salt concentration of 1.15 mol / L.
[0096] <Preparation of lithium-ion batteries>
[0097] The prepared separator, positive electrode sheet, separator, and negative electrode sheet are stacked in order, wound to obtain an electrode assembly, and the electrode assembly is hot pressed at a pressure of 5 MPa, a temperature of 65°C, and a holding time of 10 seconds. The electrode assembly is placed in an aluminum-plastic film packaging bag, and the positive electrode tab and the negative electrode tab are extended from the top seal of the packaging bag. After dehydration at 80°C, the electrolyte is injected and packaged.
[0098] Among them, during packaging, a first head and a second head are used, and the first head and the second head are respectively placed on both sides of the first side seal of the packaging bag. The raised portion of the first head corresponds to one surface (first surface) of the first side seal, and the second head corresponds to the other surface (second surface) of the first side seal. After hot pressing packaging, a first recessed portion is formed on the first surface. The first side edge seal is folded once, and a lithium ion battery with a thickness of 2.9 mm is obtained through formation, degassing, shaping and other process flows. The length of the first side edge seal is 50 mm (along the length direction of the battery, that is, the direction in which the pole ear extends, wherein the width W1 of the first side edge seal is 1 mm, the maximum width W of the first recessed portion is 0.5 mm, and the distance S between two adjacent first recessed portions is 0.25 mm. The thicknesses of the layers of the first side edge seal are: the thickness of the first protective layer is (30 um) T1, the thickness of the first metal layer is (70 um) T2, the thickness of the first sealing layer is (70 um) T3, the thickness of the second sealing layer is (70 um) T4, the thickness of the second metal layer is (70 um) T5, and the depth of the first recessed portion is H.
[0099] Peel strength test: Cut out the sample, the sample includes the first side edge seal and part of the main body, the sample size is 3mm in the length direction of the lithium-ion battery, and 1.5 times the width of the first side edge seal in the width direction (for example, if the above embodiment is 1mm, then 1.5mm is selected, 1mm is the first seal edge width, and 0.5mm is the width of part of the main body). Use a tensile testing machine to fix one layer of the main body at the lower end of the tensile testing machine, and the other layer is fixed on the top of the tensile testing machine, keeping both sides on the same vertical plane, setting the tensile testing machine speed to 50mm / min, pulling the sample until the first side edge seal is pulled open, and recording the pulling force f (in N) when the first side edge seal is pulled open. The packaging strength / peel strength of the first side edge seal is G (N / mm) = f / W1, W1 is the packaging width of the first side edge seal.
[0100] The relevant parameters in Comparative Example 1 and Examples 2 to 23 are shown in Table 1 below.
[0101] Table 1
[0102]
[0103]
[0104]
[0105] According to the above Table 1, combined with Examples 1 to 22 and Comparative Example 1, it can be known that when the first recessed portion is provided on the first side seal of the lithium-ion battery, the packaging strength of the first side seal can be effectively improved. This is because the provision of the first recessed portion increases the packaging area of the first side seal. Compared with the plane, the first recessed portion can make the layers of the first side seal fit more closely, reduce the gap, improve the packaging strength of the first side seal, and effectively reduce the risk of battery leakage. At the same time, the heat conduction path can be optimized, and the raised portion of the seal head can penetrate deeper through the first recessed portion, so that the seal head is closer to the various layers of the first side seal, and the heat during hot pressing packaging can be effectively conducted to the various layers of the first side seal, so that the hot pressing packaging is more sufficient, and the hot pressing packaging efficiency and hot pressing packaging effect are improved. In addition, the setting of the first recessed portion has a better heat diffusion effect during hot pressing packaging. When the head contacts the first recessed portion, the heat will be absorbed and accumulated first. As the heat continues to accumulate, the heat will gradually diffuse to the surroundings of the first recessed portion, forming a heat diffusion effect. The temperature around the first recessed portion rises rapidly, which can facilitate the temperature of various parts of the first side edge sealing to tend to be consistent, and can reduce the thermal stress concentration and deformation of the edge sealing caused by temperature differences, thereby making the packaging strength of the edge sealing higher.
[0106] In combination with Examples 1 to 4, in Examples 2 and 3, the peel strength of the first side edge seal is higher than that of Examples 1 and 4. In Example 1, the first recessed portion only penetrates into the first protective layer, and it is difficult for heat to be transferred to the first metal layer, the first sealing layer, the second sealing layer and the second metal layer in a timely manner, which may lead to poor heat diffusion and affect the packaging effect. In Example 4, the first recessed portion penetrates into the second metal layer, and both the first metal layer and the second metal layer are crimped and recessed, which may make the first side edge seal weaker at the first recessed portion. During testing, it is easy to cause the first side edge seal to tear. Therefore, in this application, in combination with Examples 2 and 3, the depth of the first recessed portion can be selected to be T1+T2≤H≤T1+T2+T3+T4.
[0107] In combination with Examples 6 to 12, in Examples 8 to 11, the peel strength of the first side edge seal is higher than that of Examples 6 and 7. In Examples 6 and 7, the width of the first recessed portion is relatively small, which may make it difficult for the heat to diffuse to the entire edge seal in a timely and sufficient manner during hot pressing packaging, affecting the packaging effect. In Example 12, the width of the first recessed portion is too large, which may easily cause the fold line to pass through the first recessed portion when folding the edge seal, causing interference with the folding of the first side edge seal, and the width of the first recessed portion is too large, which may make the first side edge seal relatively weak and its strength weakened, and may also directly cause the first side edge seal to tear during testing. In combination with Examples 8 to 11, in the present application, the minimum width of the first recessed portion can be selected as 0.3W1≤W≤0.85W1.
[0108] In combination with Examples 14 to 21, in Examples 15 to 20, the peel strength of the first side edge seal is higher than that of Example 14. In Example 14, the spacing between the first recessed portions is small, resulting in the first recessed portions being denser, so that the overall strength of the first side edge seal is weaker, which may directly cause the first side edge seal to tear during testing and is not conducive to the folding of the first side edge seal. In Example 21, the distance between two adjacent first recessed portions is too large, which may make it difficult to fully diffuse the heat during hot pressing packaging, affecting the packaging effect. In combination with Examples 15 to 20, in the embodiments of the present application, the distance between two adjacent first recessed portions can be selected to be 0.1W≤S≤W.
[0109] Combined with Example 5 and Examples 1 to 4, Example 13 and Examples 6 to 12, Example 22 and Examples 14 to 21. In Example 5, the peel strength of the first side edge seal is higher than that of Examples 1 to 4; in Example 13, the peel strength of the first side edge seal is higher than that of Examples 6 to 12; in Example 22, the peel strength of the first side edge seal is higher than that of Examples 14 to 21. This is because the arc chamfered surface is more conducive to uniformly dispersing stress, reducing the influence of the first recessed portion on the strength of the first side edge seal, and reducing the damage and tearing at the first recessed portion. At the same time, during hot pressing packaging, by providing a convex portion with an arc chamfered surface on the head, during hot pressing, the first recessed portion with an arc chamfered surface can be directly formed on the edge seal, and the convex portion with an arc chamfered surface on the head is in smooth contact with the first side edge seal, which can facilitate the diffusion of heat and thus improve the packaging strength.
[0110] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present application, rather than to limit them. Under the concept of the present application, the technical features in the above embodiments or different embodiments can also be combined, the steps can be implemented in any order, and there are many other changes in different aspects of the present application as described above, which are not provided in detail for the sake of simplicity. Although the present application has been described in detail with reference to the aforementioned embodiments, a person of ordinary skill in the art should understand that the technical solutions described in the aforementioned embodiments can still be modified, or some of the technical features can be replaced by equivalents. These modifications or replacements do not deviate the essence of the corresponding technical solutions from the scope of the technical solutions of the embodiments of the present application.
Claims
1. A secondary battery, comprising a packaging bag and an electrode assembly, wherein the packaging bag comprises a main body and an edge sealing portion sealing the main body, and the electrode assembly is arranged in the main body, characterized in that: The edge sealing portion includes a first edge sealing portion connected to the main body portion. Along the thickness direction of the first edge sealing portion, the first edge sealing portion includes a first surface and a second surface arranged opposite to each other. The first surface is provided with a plurality of first recessed portions, and the first recessed portions are recessed toward the second surface.
2. The secondary battery according to claim 1, characterized in that: The edge seal portion further includes a second edge seal, the first edge seal is connected between the main body portion and the second edge seal, and the second edge seal is folded toward the first surface or the second surface.
3. The secondary battery according to claim 1, characterized in that: Along the thickness direction of the second edge seal, the second edge seal has a third surface and a fourth surface that are arranged opposite to each other, the third surface is connected to the first surface, and the fourth surface is connected to the second surface; The third surface is provided with a plurality of second recessed portions, and the second recessed portions are recessed toward the fourth surface.
4. The secondary battery according to claim 1, characterized in that: The second surface is a flat surface.
5. The secondary battery according to claim 1, characterized in that: The first surface has a first flat portion, and the first flat portion is disposed between two adjacent first recessed portions.
6. The secondary battery according to claim 5, characterized in that: The secondary battery comprises a tab, one end of which is electrically connected to the electrode assembly, and the other end of which extends out of the packaging bag from the flat portion of the first edge seal.
7. The secondary battery according to claim 5, characterized in that: Along the thickness direction of the first edge seal, the first edge seal includes a first portion and a second portion which are arranged opposite to each other; The first part includes a first protective layer, a first sealing layer, and a first metal layer disposed between the first protective layer and the first sealing layer; The second portion includes a second protective layer, a second sealing layer, and a second metal layer disposed between the second protective layer and the second sealing layer; The first sealing layer is bonded to the second sealing layer, and the first recessed portion is disposed on a surface of the first protective layer away from the second portion; In the first flattened portion, along the thickness direction of the first edge seal, the thickness of the first protective layer is T1, the thickness of the first metal layer is T2, the thickness of the first sealing layer is T3, and the thickness of the second sealing layer is T4; Along the thickness direction of the first edge seal, the depth of the first recessed portion is H, and T1+T2≤H≤T1+T2+T3+T4.
8. The secondary battery according to claim 1, characterized in that: Along the thickness direction of the first edge seal, the depth of the first recessed portion is H, 0.02T≤H≤0.2T, and T is the thickness of the secondary battery.
9. The secondary battery according to claim 1, characterized in that: Along the width direction of the first edge seal, the maximum width of the first recessed portion is W, 0.3W1≤W≤0.85W1, and W1 is the width of the first edge seal.
10. The secondary battery according to claim 9, characterized in that: The distance between two adjacent first recessed portions is S, and 0.1W≤S≤W.
11. The secondary battery according to claim 1, characterized in that: The first recessed portion includes a peripheral wall, a bottom wall, and an arc-shaped chamfered surface connecting the peripheral wall and the bottom wall. The radius of the arc-shaped chamfered surface is R, 0.0015T≤R≤0.15T, and T is the thickness of the secondary battery.
12. The secondary battery according to claim 7, characterized in that: The peel strength between the first portion and the second portion is G, 1N / mm≤G≤5N / mm.
13. The secondary battery according to any one of claims 1 to 12, characterized in that: Along the width direction of the first edge seal, the first edge seal has a first edge and a second edge that are oppositely arranged, and the first edge is connected to the main body; The distance between the first edge and the first recessed portion is L1, 0.25 mm ≤ L1 ≤ 0.75 mm; A distance between the second edge and the first recessed portion is L2, 0.25 mm≤L2≤0.75 mm.
14. A sealing head for hot pressing and packaging the secondary battery according to any one of claims 1 to 13, characterized in that: The end cap comprises a first end cap and a second end cap; The first end cap has a fifth surface, the fifth surface is provided with a plurality of raised portions, and a second flat portion is provided between two adjacent raised portions; The second head has a sixth surface, and the sixth surface faces the fifth surface.
15. A packaging method, characterized in that: A secondary battery according to any one of claims 1 to 13 and a sealing head according to claim 13; The first end cap and the second end cap are respectively placed on both sides of the first edge seal in the thickness direction, with the fifth surface of the first end cap facing the first surface of the first edge seal, and the sixth surface of the second end cap facing the second surface; The first end cap and the second end cap are hot pressed to form the first edge seal, the raised portion is hot pressed to form the first recessed portion on the first surface, and the second flat portion is hot pressed to form the first edge seal to form the first flat portion on the first surface.